Magnetic tunnel junction

By using a diffusion layer and a reinforcement layer to combine the seed layer in a magnetic tunnel junction, the perpendicular magnetic anisotropy and damping factor of the pinned layer is solved, and the problem of insufficient magnetic stability of the synthetic antiferromagnetic structure is significantly improved. The MTJ device is significantly improved performance.

CN119031823APending Publication Date: 2024-11-26ZHEJIANG HIKSTOR TECHOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310613918.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The synthetic antiferromagnetic structures of existing magnetic tunnel junctions have poor magnetic stability, resulting in high write error rate and increased write voltage, affecting the performance of MTJ devices.

Method used

Using a combined seed layer composed of a diffusion layer and a reinforcement layer, the perpendicular magnetic anisotropy of the pinned layer is enhanced by the diffusion and stress of Cr element, and the damping factor is enhanced by the spin-orbit coupling effect, thereby enhancing the magnetic stability of the SAF structure. sex.

Benefits of technology

It significantly improves the magnetic stability of the SAF structure, reduces the write error rate and write voltage, and improves the overall performance of MTJ devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031823A_ABST
    Figure CN119031823A_ABST
Patent Text Reader

Abstract

A magnetic tunnel junction provided by the present invention comprises a combined seed crystal layer, a fixed layer with a fixed magnetization direction, a barrier layer and a free layer with a variable magnetization direction which are stacked from bottom to top, the fixed layer adopts a synthetic antiferromagnetic structure and comprises a reference layer, a coupling layer and a pinning layer, and the combined seed crystal layer comprises a diffusion layer and an enhancement layer which are stacked. The diffusion layer is used for diffusing chromium (Cr) into the pinning layer in the synthetic antiferromagnetic structure so as to enhance the vertical magnetic anisotropy of the pinning layer, the enhancement layer enables lattices of the pinning layer to be distorted through the stress effect so as to enhance the vertical magnetic anisotropy of the pinning layer, and the enhancement layer improves the damping factor of the pinning layer through the spin-orbit coupling effect. According to the invention, the magnetic stability of the synthesized antiferromagnetic structure is improved, and the performance of the MTJ device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of magnetic memory, and in particular to a magnetic tunnel junction. Background Art

[0002] In recent years, people have used the characteristics of magnetic tunnel junction (MTJ) to make magnetic random access memory, namely MRAM (Magnetic Random Access Memory). MTJ is composed of dozens of layers of ultra-thin films. For MTJ film stacking, the film structure and interface characteristics have an extremely important impact on the performance.

[0003] The bottom-pinned perpendicular magnetization MTJ is the mainstream structure in the industry today, with advantages such as relatively low difficulty in preparation, high thermal stability, and low write power consumption. The pinned layer generates antiferromagnetic coupling with the reference layer through the coupling layer Ir or Ru, thereby fixing the magnetization direction of the reference layer. The whole formed by the pinned layer, coupling layer, and reference layer is called a synthetic antiferromagnetic (SAF) structure.

[0004] The magnetic stability of the SAF structure is one of the main factors affecting the performance of the MTJ device. When the magnetic stability of the SAF structure is poor, it will bring many adverse effects on the performance of the MTJ device, such as a high write error rate, a significant increase in the write voltage, and even cause the MTJ device to fail to work properly. Therefore, in order to improve the magnetic stability, write error rate, write voltage and other performance of the MTJ device, it is necessary to enhance the magnetic stability of the SAF structure. Summary of the invention

[0005] In view of this, the present invention provides a magnetic tunnel junction, which can improve the magnetic stability of the synthetic antiferromagnetic structure and improve the performance of the MTJ device.

[0006] In a first aspect, the present invention provides a magnetic tunnel junction, comprising: a combined seed layer, a fixed layer with a fixed magnetization direction, a barrier layer, and a free layer with a variable magnetization direction stacked from bottom to top, wherein:

[0007] The fixed layer adopts a synthetic antiferromagnetic structure, including a reference layer, a coupling layer and a pinning layer, the reference layer is close to the barrier layer, the pinning layer is close to the combined seed layer, and the coupling layer is located between the reference layer and the pinning layer;

[0008] The combined seed layer includes a diffusion layer and an enhancement layer which are stacked. The diffusion layer is used to diffuse chromium (Cr) into the pinned layer to enhance the perpendicular magnetic anisotropy of the pinned layer. The enhancement layer is used to distort the pinned layer lattice through stress to enhance the perpendicular magnetic anisotropy of the pinned layer, and is also used to improve the damping factor of the pinned layer through spin-orbit coupling.

[0009] Optionally, the diffusion layer is close to the pinning layer, and the reinforcement layer is located below the diffusion layer; or, the reinforcement layer is close to the pinning layer, and the diffusion layer is located below the reinforcement layer.

[0010] Optionally, the reinforcement layer has a face-centered cubic lattice structure or a body-centered cubic lattice structure, and adopts a single-layer structure containing one or any combination of Pt, Pd, Ir, W, Au and Mo, or adopts a Z / X composite layer structure, wherein Z is Co or CoFe, and X is one or any combination of Pt, Pd, Ir, W, Au and Mo, or adopts a Y / Pt composite layer structure, wherein Y is one or any combination of Pd, Ir, W, Au and Mo.

[0011] Optionally, the diffusion layer is a body-centered cubic structure and is made of chromium (Cr) or an alloy containing chromium (Cr).

[0012] Optionally, a lattice mismatch between the enhancement layer and the diffusion layer is greater than a lattice mismatch between the diffusion layer and the pinning layer, and is no more than 10%.

[0013] In a second aspect, the present invention provides a magnetic tunnel junction, comprising: a combined seed layer, a fixed layer with a fixed magnetization direction, a barrier layer, and a free layer with a variable magnetization direction stacked from bottom to top, wherein:

[0014] The fixed layer adopts a synthetic antiferromagnetic structure, including a reference layer, a coupling layer and a pinning layer, the reference layer is close to the barrier layer, the pinning layer is close to the combined seed layer, and the coupling layer is located between the reference layer and the pinning layer;

[0015] The combined seed layer includes a diffusion layer and two enhancement layers which are stacked, wherein the diffusion layer is located between the two enhancement layers, and the diffusion layer is used to diffuse chromium (Cr) into the pinned layer to enhance the perpendicular magnetic anisotropy of the pinned layer. The two enhancement layers are used to distort the pinned layer lattice through stress to enhance the perpendicular magnetic anisotropy of the pinned layer, and are also used to improve the damping factor of the pinned layer through spin-orbit coupling.

[0016] Optionally, the two reinforcement layers adopt the same structure or different structures, and the reinforcement layers have a face-centered cubic lattice structure or a body-centered cubic lattice structure, and adopt a single-layer structure containing one or any combination of Pt, Pd, Ir, W, Au and Mo, or adopt a Z / X composite layer structure, wherein Z is Co or CoFe, and X is one or any combination of Pt, Pd, Ir, W, Au and Mo, or adopt a Y / Pt composite layer structure, wherein Y is one or any combination of Pd, Ir, W, Au and Mo.

[0017] Optionally, the diffusion layer is a body-centered cubic structure and is made of chromium (Cr) or an alloy containing chromium (Cr).

[0018] Optionally, a lattice mismatch between the two enhancement layers and the diffusion layer is greater than a lattice mismatch between the diffusion layer and the pinning layer and is no more than 10%.

[0019] Optionally, a lattice mismatch between the diffusion layer and the pinning layer is less than 3%.

[0020] The magnetic tunnel junction provided by the present invention adopts a combined seed layer formed by a diffusion layer and an enhancement layer. After high-temperature annealing, the Cr element in the diffusion layer diffuses into the pinned layer, and the Cr element and the pinned layer element form a Cr-containing alloy at high temperature, presenting a stronger perpendicular magnetic anisotropy (PMA); the pinned layer with a stronger PMA acts on the reference layer through antiferromagnetic coupling, making the magnetization direction of the reference layer more vertical and more stable. In addition, the enhancement layer distorts the lattice of the pinned layer through stress, thereby further enhancing the perpendicular magnetic anisotropy of the pinned layer. In addition, there is an interface coupling effect between the diffusion layer and the enhancement layer. Since the enhancement layer is composed of a heavy metal with strong spin-orbit coupling, this spin-orbit coupling effect is transmitted and strengthened through the interface diffusion layer, affecting the pinned layer, improving the damping factor of the pinned layer, thereby significantly enhancing the magnetic stability of the SAF structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A schematic diagram of the structure of a magnetic tunnel junction provided by an embodiment of the present invention;

[0022] Figure 2 A schematic diagram of the structure of a magnetic tunnel junction provided by an embodiment of the present invention;

[0023] Figure 3 A schematic diagram of the structure of a magnetic tunnel junction provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present application described here. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0026] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0027] An embodiment of the present invention provides a magnetic tunnel junction, such as Figure 1 As shown, the magnetic tunnel junction includes: a combined seed layer 10, a fixed layer 11 with a fixed magnetization direction, a barrier layer 12 and a free layer 13 with a variable magnetization direction, which are stacked from bottom to top.

[0028] The fixed layer 11 adopts a synthetic antiferromagnetic structure, including a reference layer 111, a coupling layer 112 and a pinning layer 113, wherein the reference layer 111 is close to the barrier layer 12, the pinning layer 113 is close to the combined seed layer 10, and the coupling layer 112 is located between the reference layer 111 and the pinning layer 113;

[0029] The combined seed layer 10 includes a diffusion layer 101 and an enhancement layer 102 which are stacked. The diffusion layer 101 is close to the pinning layer 113, and the enhancement layer 102 is located below the diffusion layer 101. The diffusion layer 101 is used to diffuse chromium (Cr) into the pinning layer 113 to enhance the perpendicular magnetic anisotropy of the pinning layer 113. The enhancement layer 102 is used to distort the lattice of the pinning layer 113 through stress so as to enhance the perpendicular magnetic anisotropy of the pinning layer 113. In addition, there is interface coupling between the enhancement layer 102 and the adjacent interface of the diffusion layer 101. The strong spin-orbit coupling of the enhancement layer 102 affects the pinning layer 113 through the transmission and strengthening of the interface of the diffusion layer 101, thereby improving the damping factor of the pinning layer 113 and thus improving the magnetic stability of the SAF.

[0030] Furthermore, in one embodiment, the reinforcement layer 102 has a face-centered cubic lattice structure or a body-centered cubic lattice structure, and adopts a single-layer structure containing one or any combination of Pt, Pd, Ir, W, Au and Mo, or adopts a Z / X composite layer structure, wherein Z is Co or CoFe, and X is one or any combination of Pt, Pd, Ir, W, Au and Mo, or adopts a Y / Pt composite layer structure, wherein Y is one or any combination of Pd, Ir, W, Au and Mo.

[0031] For example, Ir (1 nm) single layer structure, Pt (1 nm) single layer structure, Co (0.8 nm) / Pt (0.8 nm) composite layer structure, the thickness of the layer is indicated in brackets.

[0032] In one embodiment, the diffusion layer 101 is a body-centered cubic structure and is made of chromium (Cr) or an alloy containing chromium (Cr), such as NiCr, NiFeCr, RuCr, IrCr or CoCr.

[0033] In order to ensure the stress and interface coupling between the enhancement layer 102 and the diffusion layer 101, and to ensure that the crystal structure of the SAF does not change, in one embodiment, the lattice mismatch between the enhancement layer and the diffusion layer is greater than the lattice mismatch between the diffusion layer and the pinning layer, and does not exceed 10%. Generally, the lattice mismatch between the diffusion layer and the pinning layer is less than 3%, so the lattice mismatch between the enhancement layer and the diffusion layer is between 3% and 10%.

[0034] The pinned layer in this embodiment can be one or more of Co / Pt multilayer film, Co / Pd multilayer film, Co / Ni multilayer film, etc. As for the coupling layer, reference layer, barrier layer and free layer, they can be designed according to the conventional method in the art.

[0035] A magnetic tunnel junction provided by an embodiment of the present invention uses a combined seed layer formed by a diffusion layer and an enhancement layer. After high-temperature annealing, the Cr element in the diffusion layer diffuses into the pinned layer, and the Cr element and the pinned layer element form a Cr-containing alloy at high temperature, showing a stronger perpendicular magnetic anisotropy (PMA); the pinned layer with a stronger PMA acts on the reference layer through antiferromagnetic coupling, and makes the magnetization direction of the reference layer more vertical and more stable. In addition, the enhancement layer distorts the lattice of the pinned layer through stress, thereby further enhancing the perpendicular magnetic anisotropy of the pinned layer. In addition, there is an interface coupling effect between the diffusion layer and the enhancement layer. Since the enhancement layer is composed of a heavy metal with strong spin-orbit coupling, this spin-orbit coupling effect is transmitted and strengthened through the interface diffusion layer, which affects the pinned layer, improves the damping factor of the pinned layer, and thus significantly enhances the magnetic stability of the SAF structure. In actual testing, the SAF flip field is one of the main parameters characterizing the magnetic stability of the SAF structure. Experiments have shown that the magnetic tunnel junction provided by the embodiment of the present invention has an SAF switching field that is increased by more than 50%, and the overall performance of the MTJ is improved, which has great application value.

[0036] It should be noted that, in the MTJ of the above-mentioned embodiment, the positions of the diffusion layer 101 and the enhancement layer 102 can be interchanged. Figure 2 As shown, the enhancement layer 102 is close to the pinned layer 113, and the diffusion layer 101 is located under the enhancement layer 102. In this embodiment, although the diffusion layer 101 is not in direct contact with the pinned layer 113, the chromium (Cr) element can still be diffused into the pinned layer 113, thereby enhancing the perpendicular magnetic anisotropy of the pinned layer 113. The enhancement layer 102 is adjacent to the pinned layer 113. In addition to the above-mentioned stress and spin-orbit coupling effects, due to the interface structure of the magnetic layer / heavy metal (that is, the interface structure of the pinned layer / enhancement layer), there will be a spin pumping effect in the structure, which will further increase the damping factor of the pinned layer, thereby further improving the magnetic stability of the pinned layer.

[0037] The materials of each layer can refer to the description of the aforementioned embodiment and will not be described again here.

[0038] On the other hand, an embodiment of the present invention provides a magnetic tunnel junction, such as Figure 3 As shown, the magnetic tunnel junction includes: a combined seed layer 20, a fixed layer 21 with a fixed magnetization direction, a barrier layer 22, and a free layer 23 with a variable magnetization direction, which are stacked from bottom to top.

[0039] The fixed layer 21 adopts a synthetic antiferromagnetic structure, including a reference layer 211, a coupling layer 212 and a pinning layer 213, wherein the reference layer 211 is close to the barrier layer 22, the pinning layer 213 is close to the combined seed layer 20, and the coupling layer 212 is located between the reference layer 211 and the pinning layer 213;

[0040] The combined seed layer 20 includes a stacked diffusion layer and two enhancement layers, which are denoted as a first enhancement layer 201 and a second enhancement layer 203. The diffusion layer 202 is located between the two enhancement layers 201 and 203. The diffusion layer 202 is used to diffuse chromium (Cr) into the pinned layer 213 to enhance the perpendicular magnetic anisotropy of the pinned layer 213. The two enhancement layers 201 and 203 are used to distort the lattice of the pinned layer 213 through stress so as to enhance the perpendicular magnetic anisotropy of the pinned layer, and are also used to improve the damping factor of the pinned layer 213 through spin-orbit coupling.

[0041] On the one hand, the second enhancement layer 203 away from the pinned layer 213 distorts the lattice of the pinned layer 213 through stress, thereby enhancing the perpendicular magnetic anisotropy of the pinned layer 213 . In addition, the damping factor of the pinned layer 213 is improved through spin-orbit coupling.

[0042] On the other hand, in addition to the above-mentioned stress and spin-orbit coupling effects, the first enhancement layer 201 adjacent to the pinned layer 213 has a spin pumping effect due to the interface structure of the magnetic layer / heavy metal (that is, the interface structure of the pinned layer / enhancement layer), which further increases the damping factor of the pinned layer 213, thereby further improving the magnetic stability of the pinned layer 213. The effects of the two enhancement layers are superimposed, greatly improving the damping factor of the pinned layer.

[0043] Furthermore, in one embodiment, the two reinforcement layers 201 and 203 adopt the same structure or different structures, each reinforcement layer has a face-centered cubic lattice structure or a body-centered cubic lattice structure, and adopts a single-layer structure containing one or any combination of Pt, Pd, Ir, W, Au and Mo, or adopts a Z / X composite layer structure, wherein Z is Co or CoFe, and X is one or any combination of Pt, Pd, Ir, W, Au and Mo, or adopts a Y / Pt composite layer structure, wherein Y is one or any combination of Pd, Ir, W, Au and Mo.

[0044] For example, Ir (1 nm) single layer structure, Pt (1 nm) single layer structure, Co (0.8 nm) / Pt (0.8 nm) composite layer structure, the thickness of the layer is indicated in brackets.

[0045] In one embodiment, the diffusion layer 202 is a body-centered cubic structure, and is made of chromium (Cr), or an alloy containing chromium (Cr), such as NiCr, NiFeCr, RuCr, IrCr, or CoCr.

[0046] In order to ensure the stress and interface coupling effect between the two enhancement layers and the diffusion layer, and to ensure that the crystal structure of the SAF does not change, in one embodiment, the lattice mismatch between the two enhancement layers and the diffusion layer is greater than the lattice mismatch between the diffusion layer and the pinning layer, and does not exceed 10%. Generally, the lattice mismatch between the diffusion layer and the pinning layer is less than 3%, so the lattice mismatch between the two enhancement layers and the diffusion layer is between 3% and 10%.

[0047] The pinned layer in this embodiment can be one or more of Co / Pt multilayer film, Co / Pd multilayer film, Co / Ni multilayer film, etc. As for the coupling layer, reference layer, barrier layer and free layer, they can be designed according to the conventional method in the art.

[0048] A magnetic tunnel junction provided by an embodiment of the present invention uses a combined seed layer formed by a diffusion layer and two enhancement layers. The diffusion layer is located between the two enhancement layers. After high-temperature annealing, the Cr element in the diffusion layer diffuses into the pinned layer. The Cr element and the pinned layer element form a Cr-containing alloy at high temperature, showing a stronger perpendicular magnetic anisotropy (PMA); the pinned layer with a stronger PMA acts on the reference layer through antiferromagnetic coupling, and makes the magnetization direction of the reference layer more vertical and more stable. In addition, the enhancement layer distorts the pinned layer lattice through stress, thereby further enhancing the perpendicular magnetic anisotropy of the pinned layer. In addition, since the enhancement layer is composed of heavy metals with strong spin-orbit coupling, this spin-orbit coupling effect is transmitted and strengthened through the interface diffusion layer. The effects of the two enhancement layers are directly or indirectly applied to the pinned layer, affecting the pinned layer. The effects of the two enhancement layers are superimposed, which significantly improves the damping factor of the pinned layer, thereby significantly enhancing the magnetic stability of the SAF structure. In actual testing, the SAF flip field is one of the main parameters characterizing the magnetic stability of the SAF structure. Experiments have shown that the magnetic tunnel junction provided by the embodiment of the present invention has a SAF switching field that is increased by more than 70%, and the overall performance of the MTJ is improved, which has great application value.

[0049] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A magnetic tunnel junction, characterized in that: include: A combined seed layer, a fixed layer with a fixed magnetization direction, a barrier layer, and a free layer with a variable magnetization direction are stacked from bottom to top, wherein: The fixed layer adopts a synthetic antiferromagnetic structure, including a reference layer, a coupling layer and a pinning layer, the reference layer is close to the barrier layer, the pinning layer is close to the combined seed layer, and the coupling layer is located between the reference layer and the pinning layer; The combined seed layer includes a diffusion layer and an enhancement layer which are stacked. The diffusion layer is used to diffuse chromium (Cr) into the pinned layer to enhance the perpendicular magnetic anisotropy of the pinned layer. The enhancement layer is used to distort the pinned layer lattice through stress to enhance the perpendicular magnetic anisotropy of the pinned layer, and is also used to improve the damping factor of the pinned layer through spin-orbit coupling.

2. The magnetic tunnel junction according to claim 1, characterized in that: The diffusion layer is close to the pinning layer, and the reinforcement layer is located below the diffusion layer; or, the reinforcement layer is close to the pinning layer, and the diffusion layer is located below the reinforcement layer.

3. The magnetic tunnel junction according to claim 1, characterized in that: The reinforcement layer has a face-centered cubic lattice structure or a body-centered cubic lattice structure, and adopts a single-layer structure containing one or any combination of Pt, Pd, Ir, W, Au and Mo, or adopts a Z / X composite layer structure, wherein Z is Co or CoFe, and X is one or any combination of Pt, Pd, Ir, W, Au and Mo, or adopts a Y / Pt composite layer structure, wherein Y is one or any combination of Pd, Ir, W, Au and Mo.

4. The magnetic tunnel junction according to claim 1, characterized in that: The diffusion layer is a body-centered cubic structure and is made of chromium (Cr) or an alloy containing chromium (Cr).

5. The magnetic tunnel junction according to claim 1, characterized in that: The lattice mismatch between the enhancement layer and the diffusion layer is greater than the lattice mismatch between the diffusion layer and the pinning layer and is no more than 10%.

6. A magnetic tunnel junction, characterized in that: include: A combined seed layer, a fixed layer with a fixed magnetization direction, a barrier layer, and a free layer with a variable magnetization direction are stacked from bottom to top, wherein: The fixed layer adopts a synthetic antiferromagnetic structure, including a reference layer, a coupling layer and a pinning layer, the reference layer is close to the barrier layer, the pinning layer is close to the combined seed layer, and the coupling layer is located between the reference layer and the pinning layer; The combined seed layer includes a diffusion layer and two enhancement layers which are stacked, wherein the diffusion layer is located between the two enhancement layers, and the diffusion layer is used to diffuse chromium (Cr) into the pinned layer to enhance the perpendicular magnetic anisotropy of the pinned layer. The two enhancement layers are used to distort the pinned layer lattice through stress to enhance the perpendicular magnetic anisotropy of the pinned layer, and are also used to improve the damping factor of the pinned layer through spin-orbit coupling.

7. The magnetic tunnel junction according to claim 6, characterized in that: The two reinforcement layers adopt the same structure or different structures, and the reinforcement layers have a face-centered cubic lattice structure or a body-centered cubic lattice structure, and adopt a single-layer structure containing one or any combination of Pt, Pd, Ir, W, Au and Mo, or adopt a Z / X composite layer structure, wherein Z is Co or CoFe, and X is one or any combination of Pt, Pd, Ir, W, Au and Mo, or adopt a Y / Pt composite layer structure, wherein Y is one or any combination of Pd, Ir, W, Au and Mo.

8. The magnetic tunnel junction according to claim 6, characterized in that: The diffusion layer is a body-centered cubic structure and is made of chromium (Cr) or an alloy containing chromium (Cr).

9. The magnetic tunnel junction according to claim 6, characterized in that: The lattice mismatch between the two enhancement layers and the diffusion layer is greater than the lattice mismatch between the diffusion layer and the pinning layer and is no more than 10%.

10. The magnetic tunnel junction according to claim 1 or 6, characterized in that: The lattice mismatch between the diffusion layer and the pinning layer is less than 3%.