Lithium secondary battery
By using a combination of oxalate complex and low viscosity fluorocyclic monoether in lithium secondary batteries, a uniform SEI coating is formed, which solves the problem of reduced discharge capacity of lithium secondary batteries at high temperatures and improves cycling stability and electrolyte properties.
Patent Information
- Application Number
- CN202380034682.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-22
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-26
AI Technical Summary
When existing lithium secondary batteries are repeatedly charged and discharged at high temperatures, the discharge capacity is easily reduced, and the uneven expansion of the negative electrode leads to cracks or cuts.
Anions containing an oxalate complex and low viscosity fluorocyclic monoethers are used as solvent components in the non-aqueous electrolyte to form a uniform SEI film through the decomposition of the oxalate complex to inhibit dendrite of lithium metal. The viscosity and ion conductivity of the electrolyte are optimized by combining non-fluoro chain ethers and fluorocyclic monoethers.
The reduction in discharge capacity during repeated charging and discharging at high temperatures is significantly reduced, and the circulation stability of lithium secondary batteries and the excellent characteristics of electrolyte are improved.
Smart Images

Figure CN119032447A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a lithium secondary battery. Background Art
[0002] In a lithium secondary battery, lithium metal is deposited on the negative electrode during charging, and on the other hand, lithium metal is dissolved in a non-aqueous electrolyte during discharging. Various lithium secondary batteries have been proposed.
[0003] Patent Document 1 (Japanese Patent Application Laid-Open No. 2013-211095) discloses a non-aqueous electrolyte for a secondary battery, which contains a lithium salt, a specific hydrofluoroether, a specific ether compound other than the hydrofluoroether, and a cyclic lactone.
[0004] Patent document 2 (International Publication No. 2020 / 202845) discloses the following: "In a non-aqueous electrolyte secondary battery having a positive electrode, a negative electrode and a non-aqueous electrolyte having lithium ion conductivity, the solvent in the non-aqueous electrolyte comprises a solvent having the general formula (1): R1-(OCH2CH2) n -OR2 (in the formula (1), R1 and R2 are each independently an alkyl group having 1 to 5 carbon atoms, and n is 1 to 3.) and a first ether compound represented by the general formula (2): C a1 H b1 F c1 O d1 (CF2OCH2)C a2 H b2 F c2 O d2 (In formula (2), a1≥1, a2≥0, b1≤2a1, b2≤2a2, c1=(2a1+1)-b1, c2=(2a2+1)-b2, d1≥0, d2≥0.) represents a second ether compound having a fluorination rate of 60% or more. The total amount of the first ether compound and the second ether compound is 80% or more of the solvent. ".
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2013-211095
[0008] Patent Document 2: International Publication No. 2020 / 202845 Summary of the invention
[0009] Problems to be solved by the invention
[0010] At present, there is a need for a lithium secondary battery whose characteristics (such as discharge capacity) are less reduced even when repeatedly charged and discharged at high temperatures. In such a case, one of the purposes of the present disclosure is to provide a lithium secondary battery whose characteristics (such as discharge capacity) are less reduced even when repeatedly charged and discharged at high temperatures.
[0011] Means for solving problems
[0012] The first aspect of the present disclosure relates to a lithium secondary battery. The lithium secondary battery is a lithium secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte having lithium ion conductivity, wherein lithium metal is precipitated at the negative electrode during charging, and the lithium metal is dissolved in the non-aqueous electrolyte during discharging, the non-aqueous electrolyte comprises a solvent and a lithium salt, the solvent comprises a non-fluorinated ether and a fluorinated cyclic monoether, the fluorinated cyclic monoether comprises a cyclic structure having one ether bond, and the lithium salt comprises an anion of an oxalate complex.
[0013] As long as the combinations are possible, the matters described in two or more claims arbitrarily selected from a plurality of claims described in the appended claims may be combined.
[0014] Effects of the Invention
[0015] According to the present disclosure, a lithium secondary battery can be obtained in which the reduction in discharge capacity is small even when charge and discharge are repeated at high temperature.
[0016] The novel features of the present invention are described in the appended claims, but the present invention relates to both the configuration and the content, and can be better understood through the following detailed description together with other objects and features of the present invention and with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] [ Figure 1 ] Figure 1 A longitudinal cross-sectional view of a lithium secondary battery according to an embodiment is shown.
[0018] [ Figure 2 ] Figure 2 The lithium secondary battery is shown in the fully discharged state along Figure 1 An enlarged cross-sectional view obtained by cutting along the line II-II contained therein. DETAILED DESCRIPTION
[0019] Hereinafter, the embodiments of the present disclosure will be illustrated, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values and materials are sometimes illustrated, but other numerical values and other materials may also be applied as long as the invention to which the present disclosure relates can be implemented. In this specification, a description such as "numerical value A to numerical value B" includes numerical value A and numerical value B, which may be replaced by "above numerical value A and below numerical value B". In the following description, when the lower limit and upper limit of numerical values related to specific physical properties, conditions, etc. are illustrated, as long as the lower limit is not above the upper limit, any of the illustrated lower limits may be arbitrarily combined with any of the illustrated upper limits.
[0020] (Lithium secondary battery)
[0021] The lithium secondary battery involved in this embodiment is sometimes referred to as "lithium secondary battery (S)" below. The lithium secondary battery (S) includes a positive electrode, a negative electrode and a non-aqueous electrolyte with lithium ion conductivity. At the negative electrode, lithium metal is precipitated during charging, and the lithium metal is dissolved in the non-aqueous electrolyte during discharge. The non-aqueous electrolyte includes a solvent and a lithium salt. The solvent includes a non-fluorinated ether and a fluorinated cyclic monoether. The fluorinated cyclic monoether includes a cyclic structure having one ether bond. The lithium salt includes an anion of an oxalate complex.
[0022] In the negative electrode of a lithium secondary battery, lithium metal dissolves during discharge and precipitates during charging. In the negative electrode, lithium metal is almost normally present, so side reactions between the lithium metal at the negative electrode and the non-aqueous electrolyte are prone to occur. In addition, in the negative electrode, during charging, a SEI (Solid Electrolyte Interface) film from the components contained in the non-aqueous electrolyte is formed. In other words, during charging, the precipitation of lithium metal and the formation of the SEI film are carried out in parallel at the negative electrode. Therefore, during charging and discharging, it is difficult to uniformly dissolve and precipitate lithium metal in the entire negative electrode. In addition, if charging and discharging are repeated, the deviation of the dissolution and precipitation of lithium metal becomes significant. In such a state, lithium metal becomes easy to precipitate in a dendritic form.
[0023] Lithium metal precipitated in a dendrite shape (hereinafter sometimes referred to as lithium dendrites) leads to a decrease in discharge capacity. In addition, if the specific surface area of the negative electrode increases due to the generation of lithium dendrites, side reactions become significant, and in addition, the volume change during charge and discharge becomes larger. If the negative electrode expands unevenly due to the generation of lithium dendrites during charging, it is difficult to alleviate the stress caused by the expansion of the negative electrode, resulting in cracking or cutting of the negative electrode. As a result, the discharge capacity becomes easy to decrease. As described above, in conventional lithium secondary batteries, the decrease in discharge capacity accompanying charge and discharge has become a problem. In particular, there is the following problem: if charge and discharge are repeated at high temperature, it is easy to form an SEI film more unevenly. Therefore, in conventional lithium secondary batteries, there is a problem that the discharge capacity decreases greatly when repeatedly charged and discharged at high temperature.
[0024] As a result of repeated studies under such circumstances, the inventors of the present application have found for the first time that, in a lithium secondary battery (S) having the above-mentioned structure, even if charge and discharge are repeated at high temperatures, the decrease in discharge capacity is significantly small. The present disclosure is based on this new finding.
[0025] In the case where the non-aqueous electrolyte contains anions of the oxalate complex, a portion of the anions of the oxalate complex decomposes as the battery is charged and discharged. It is believed that the anions decompose at a high potential compared to other additives and solvents contained in the non-aqueous electrolyte. It is believed that the decomposition products of the anions are precipitated on the surface of the lithium metal to form a thin and uniform SEI film. The lithium metal is mainly precipitated between the film and the negative electrode collector. By pressing the lithium metal with the film, the elongation of the dendritic precipitate can be suppressed. However, at high temperatures, the decomposition rate of the anions of the oxalate complex increases, and it is easy to form an SEI film unevenly, and the reduction in discharge capacity becomes larger.
[0026] In contrast, in the lithium secondary battery (S), a fluorinated cyclic monoether having a relatively low viscosity is used, which is considered to allow a more uniform formation of the SEI film and to suppress a decrease in the discharge capacity.
[0027] Furthermore, in the lithium secondary battery (S), it is considered that a particular synergistic effect is exerted by combining a solvent containing a non-fluorinated chain ether and a fluorinated cyclic monoether having a low viscosity with a specific lithium salt.
[0028] The total of the ratio shared by non-fluorinated ether in solvent and the ratio shared by fluorinated cyclic monoether in solvent can be more than 70 mol %, more than 90 mol % or more than 95 mol %.If this total is high, then easily improve the effect realized by the disclosure.Solvent can also only consist of non-fluorinated ether and fluorinated cyclic monoether.When solvent comprises other solvents except non-fluorinated ether and fluorinated cyclic monoether, the example of these other solvents includes the 3rd solvent described later.
[0029] The ratio MF / MLi of the number of moles MF of the fluorinated cyclic monoether contained in the non-aqueous electrolyte to the number of moles MLi of the lithium salt contained in the non-aqueous electrolyte may be within the range described in (1) below.
[0030] (1) The ratio MF / MLi may be greater than 0.25, greater than 1.0 or greater than 3.0. The ratio MF / MLi may be less than 10, less than 8.0 or less than 5.0. The ratio MF / MLi may be in the range of 0.25 to 10 (e.g., in the range of 1.0 to 5.0). By making the ratio MF / MLi greater than 0.25, the proportion of low-viscosity fluorinated cyclic monoethers increases, the viscosity of the electrolyte decreases, and the ion conductivity of the electrolyte increases. On the other hand, by making the ratio MF / MLi less than 10, the decrease in ion conductivity caused by the low lithium ion concentration in the electrolyte can be suppressed. By making the ratio MF / MLi within the above range, a high lithium ion concentration and a low viscosity of the electrolyte can be achieved simultaneously, and a high ion conductivity in the electrolyte can be achieved. As a result, it exhibits excellent properties as an electrolyte for a lithium secondary battery.
[0031] The ratio MF / MNF of the molar number MF of the fluorinated cyclic monoether contained in the non-aqueous electrolyte to the molar number MNF of the non-fluorinated ether contained in the non-aqueous electrolyte may be within the range described in (2) below.
[0032] (2) The ratio MF / MNF may be greater than 0.1, greater than 0.5, greater than 1.0 or greater than 2.0. The ratio MF / MNFi may be less than 10, less than 5.0 or less than 3.0. The ratio MF / MNF may be in the range of 0.1 to 10 (e.g., in the range of 1.0 to 5.0). In the case where the viscosity of the fluorinated cyclic monoether is lower than that of the non-fluorinated ether, by making the value of MF / MNF greater than 0.1, the proportion of the low-viscosity fluorinated cyclic monoether becomes larger. As a result, the viscosity of the electrolyte decreases and the ion conductivity of the electrolyte increases. On the other hand, the interaction between the fluorinated cyclic monoether and the lithium ion is weak, and the dissociation of the lithium ion is easily reduced. Therefore, by making the ratio MF / MNF less than 10, the decrease in the ion conductivity of the electrolyte can be suppressed. By making the ratio MF / MNF within the above range, low viscosity and high lithium ion dissociation of the electrolyte can be achieved simultaneously, and high ion conductivity in the electrolyte can be achieved. As a result, the electrolyte solution exhibits excellent characteristics as a lithium secondary battery.
[0033] The concentration X of the lithium salt containing anions of the oxalate complex in the non-aqueous electrolyte may be within the range described in (3) below.
[0034] (3) The concentration X may be 0.01 mol / L or more, 0.05 mol / L or more, or 0.1 mol / L or more. The concentration X may be 0.5 mol / L or less, 0.3 mol / L or less, or 0.2 mol / L or less. The concentration X may be in the range of 0.01 to 0.5 mol / L (e.g., in the range of 0.05 to 0.3 mol / L). By setting the concentration to this range, the film formation caused by the decomposition of the oxalate complex anion can be carried out appropriately, and a uniform film can be formed. By setting the concentration X to 0.01 mol / L or more, the film formation can be carried out appropriately. By setting the concentration X to 0.5 mol / L or less, the discharge capacity can be prevented from being reduced due to excessive thickness of the film.
[0035] The fluorinated cyclic monoether may include a 5-membered ring containing one ether bond or a 6-membered ring containing one ether bond. According to this structure, the stability against oxidation / reduction is high and a low viscosity can be achieved.
[0036] The above-mentioned lithium salt containing an anion of an oxalate complex may be lithium difluorooxalatoborate (LiBF2(C2O4)).
[0037] The fluorinated cyclic monoether may be at least one selected from 3,3,4,4-tetrafluorotetrahydrofuran and 4-difluoromethyltetrahydro-2H-pyran, or 3,3,4,4-tetrafluorotetrahydrofuran. These molecules have a small volume and therefore a low viscosity. Therefore, by using the compound, a high effect due to low viscosity can be obtained, and an electrolyte having excellent characteristics can be obtained.
[0038] Lithium secondary batteries (S) are also called lithium metal secondary batteries. In lithium secondary batteries (S), for example, more than 70% of the rated capacity is presented by the precipitation and dissolution of lithium metal. The movement of electrons in the negative electrode during charging and discharging is mainly based on the precipitation and dissolution of lithium metal in the negative electrode. Specifically, 70% to 100% (for example, 80% to 100%, 90% to 100%) of the movement of electrons in the negative electrode during charging and discharging (current from other perspectives) is based on the precipitation and dissolution of lithium metal. That is, the negative electrode of the lithium secondary battery (S) is different from the negative electrode in which the movement of electrons in the negative electrode during charging and discharging is mainly based on the absorption and release of lithium ions achieved by the negative electrode active material (graphite, etc.).
[0039] In a battery that precipitates lithium metal in the negative electrode during charging, the open circuit potential (OCV: Open Circuit Voltage) of the negative electrode when fully charged is, for example, 70 mV or less for lithium metal (lithium dissolution potential). When fully charged, the battery is charged until, for example, a state of charge (SOC: State of Charge) of 0.98×C or more is reached when the rated capacity of the battery is recorded as C. For the open circuit potential (OCV) of the negative electrode when fully charged, the fully charged battery is disassembled under an argon atmosphere, the negative electrode is removed, and the battery cell is assembled using lithium metal as the counter electrode and measured. The non-aqueous electrolyte of the battery cell may have the same composition as the non-aqueous electrolyte in the disassembled battery.
[0040] An example of the configuration of the lithium secondary battery (S) will be described below. As components other than the non-aqueous electrolyte, known components can be applied.
[0041] (Non-aqueous electrolyte)
[0042] The non-aqueous electrolyte includes a solvent (more specifically, a non-aqueous solvent) and a lithium salt dissolved in the solvent. The liquid non-aqueous electrolyte can be prepared by dissolving the lithium salt in the non-aqueous solvent. The lithium salt is dissolved in the non-aqueous solvent to generate lithium ions and anions. The non-aqueous electrolyte has lithium ion conductivity.
[0043] The non-aqueous electrolyte may be in a liquid state or in a gel state. The gel-like non-aqueous electrolyte comprises a lithium salt, a solvent and a matrix polymer. As the matrix polymer, for example, a polymer material that can absorb the solvent and gel can be used. As the polymer material, fluororesin, acrylic resin, polyether resin, etc. can be cited.
[0044] (Lithium Salt)
[0045] The lithium salt at least includes a lithium salt containing an anion of an oxalate complex. The anion of the oxalate complex may contain fluorine. The anion of the oxalate complex may contain at least one of boron and phosphorus. The anion of the oxalate complex may contain boron (or phosphorus) and fluorine. The anion of the oxalate complex may also be composed of boron (or phosphorus), fluorine and (C2O4) 2- By using an anion of a fluorine-containing oxalate complex, the inorganic component of LiF is contained in the SEI film, so that the solubility of the SEI film in the electrolyte solution is reduced and the film is thinned, resulting in a low-resistance and high-quality film.
[0046] Examples of the anion of the oxalate complex include bis(oxalatoborate) anion and difluoro(oxalatoborate) anion (BF2(C2O4) - )、PF4(C2O4) - PF2(C2O4)2- The lithium salt may also include a lithium salt containing anions other than the oxalate complex. Examples of anions constituting such a lithium salt include known anions used in non-aqueous electrolytes of lithium secondary batteries. Specifically, BF4 - 、ClO4 - PF6 - CF3SO3 - CF3CO2 - , anions of imide compounds, etc. Examples of anions of imide compounds include N(SO2F)2 - 、N(SO2CF3)2 - The non-aqueous electrolyte may contain one type of anion or a combination of two or more types of anions. In other words, the non-aqueous electrolyte may contain one type of lithium salt or a combination of two or more types of lithium salts.
[0047] When the lithium salt contains anions of the oxalate complex, the lithium metal is easily precipitated more uniformly in the form of fine particles. The non-aqueous electrolyte may also contain anions of the oxalate complex and anions other than the anions of the oxalate complex. Examples of anions other than the anions of the oxalate complex include, for example, PF6 - and at least one anion of an imide compound.
[0048] (Solvent)
[0049] As mentioned above, the solvent (nonaqueous solvent) contained in the nonaqueous electrolyte comprises non-fluorinated ether and fluorinated cyclic monoether. Hereinafter, fluorinated cyclic monoether is sometimes referred to as "cyclic monoether (F)". In addition, hereafter, non-fluorinated ether is sometimes referred to as "ether (NF)", chain ether as non-fluorinated ether is sometimes referred to as "chain ether (NF)", and cyclic ether as non-fluorinated ether is sometimes referred to as "cyclic ether (NF)". They are described below.
[0050] (Cyclic monoether (F))
[0051] Cyclic monoether (F) (fluorinated cyclic monoether) contains fluorine atoms and a cyclic structure. Cyclic monoether (F) has only one ether bond (-O-) in the molecule, and the ether bond is present in the cyclic structure. The non-aqueous electrolyte may contain only one compound as a cyclic monoether (F), or may contain multiple compounds as cyclic monoether (F). The cyclic structure of the cyclic monoether (F) may contain a double bond or may not contain a double bond. The cyclic structure may or may not have aromaticity. The viscosity of the cyclic monoether (F) is relatively low. In a preferred embodiment, the viscosity of the cyclic monoether (F) is lower than the viscosity of other compounds constituting the solvent.
[0052] The cyclic structure of the cyclic monoether (F) may be a 5- to 10-membered ring, a 5- to 8-membered ring, or a 5- or 6-membered ring. Examples of the 5-membered ring include furan, dihydrofuran, tetrahydrofuran, and the like. Examples of the 6-membered ring include pyran, dihydropyran, tetrahydropyran, and the like.
[0053] Examples of cyclic monoethers (F) include compounds having a structure in which hydrogen atoms contained in a prescribed ether are replaced with fluorine atoms. Examples of ethers before fluorination include tetrahydrofuran, alkyltetrahydrofurans (e.g., 2-methyltetrahydrofuran), propylene oxide, 1,2-butylene oxide, furan, alkylfurans (e.g., 2-methylfuran), tetrahydropyran, and alkyltetrahydropyrans. Examples of ethers before fluorination include compounds having a structure in which hydrogen atoms of the above-mentioned 5-membered ring or 6-membered ring are replaced with fluorine atoms or fluoroalkyl groups. Examples of alkyl groups contained in the above-mentioned compounds include methyl, ethyl, etc.
[0054] The hydrogen atom substituted with a fluorine atom may be a hydrogen atom directly bonded to the cyclic structure or a hydrogen atom bonded to an atomic group (eg, an alkyl group) bonded to the cyclic structure.
[0055] The ratio of hydrogen atoms replaced by fluorine atoms is referred to as the fluorination rate (%). If the number of fluorine atoms in the cyclic monoether (F) is recorded as N1, and the number of hydrogen atoms contained in the molecule when all fluorine atoms in the cyclic monoether (F) are replaced by hydrogen atoms is recorded as N0, the fluorination rate is represented by the following formula.
[0056] Fluorination rate (%) = 100 × N1 / N0
[0057] For example, in the case of 3,3,4,4-tetrafluorotetrahydrofuran, the number of fluorine atoms in the molecule N1 = 4. When all the fluorine atoms in the molecule are replaced with hydrogen atoms, the number of hydrogen atoms contained in the molecule N0 = 8. Therefore, the fluorination rate is 50%.
[0058] As long as the effects achieved by the present disclosure can be obtained, there is no particular limitation on the fluorination rate. The fluorination rate may be 10% or more, 20% or more, 30% or more, 40% or more, or 50% or less, or 80% or less, or 60% or less. The fluorination rate may be in the range of 10 to 80% (e.g., 30 to 80%, 30 to 60%).
[0059] The cyclic structure of the cyclic monoether (F) may be bonded to an alkyl group or a fluoroalkyl group. The number of carbon atoms of the alkyl group or the fluoroalkyl group is, for example, 1 to 6, 1 to 4, 1 to 3, or 1 or 2.
[0060] The cyclic monoether (F) may be a cyclic ether having a structure in which at least a part of the hydrogen atoms of tetrahydrofuran are substituted with fluorine atoms, or may be a cyclic ether having a structure in which at least a part of the hydrogen atoms of tetrahydrofuran bonded with an alkyl group are substituted with fluorine atoms. Examples of cyclic monoethers (F) in such cases are shown in the following formula (i).
[0061]
[0062] (In formula (i), R 4 ~R 11 Each independently represents a hydrogen atom, a fluorine atom, an alkyl group or a fluoroalkyl group, and R 4 ~R 11 At least one of them is a fluorine atom or a fluorinated alkyl group.)
[0063] R 4 ~R 11 The number of carbon atoms of the alkyl or fluoroalkyl represented by formula (i) is, for example, 1 to 6, 1 to 4, 1 to 3, or 1 or 2. The alkyl or fluoroalkyl group may be branched, but preferably linear. The fluorination rate may also be within the above range. Examples of the cyclic monoether (F) represented by formula (i) include R 6 ~R 9 3,3,4,4-tetrafluorotetrahydrofuran containing a fluorine atom.
[0064] The cyclic monoether (F) may be a cyclic ether having a structure in which at least a portion of hydrogen atoms of tetrahydropyran are substituted with fluorine atoms, or may be a cyclic ether having a structure in which at least a portion of hydrogen atoms of tetrahydrofuran bonded with an alkyl group are substituted with fluorine atoms. For the alkyl group and the fluoroalkyl group of the cyclic ether, the description of formula (i) may be applied. The fluorination ratio may also be within the above range.
[0065] (Non-fluorinated ether)
[0066] Non-fluorinated ether (ether (NF)) is an ether that is not fluorinated. In other words, non-fluorinated ether is an ether that does not contain a fluorine atom. Non-fluorinated ether comprises one or more ether bonds. The ether bond can be contained in a chain structure and / or a cyclic structure. Non-fluorinated ether can be a chain ether or a cyclic ether. The following examples of chain ether (NF) as non-fluorinated ether and cyclic ether (NF) as non-fluorinated ether are described.
[0067] (Nuclear Ether (NF))
[0068] Chain ether (NF) (non-fluorinated chain ether) is a compound having an ether bond in the chain portion. Chain ether (NF) can be a chain compound having an ether bond. Chain ether (NF) can include a chain portion having an ether bond and a cyclic structure bonded to the chain portion and not including an ether bond. Chain ether (NF) can have 1 ether bond (-O-) in the molecule, or it can have more than 2 ether bonds (-O-) in the molecule. In the molecule, the ether bond is, for example, 5 or less, or 4 or less or 3 or less. From the viewpoint of easily ensuring high affinity for lithium ions, chain ether (NF) can have more than 2 (for example, 2 or more and 5 or less, or 2 or more and 4 or less) ether bonds.
[0069] The chain ether (NF) may contain, for example, at least one compound selected from the group consisting of compounds represented by the following formula (ii).
[0070]
[0071] (In formula (ii), R 1 and R 2 are each independently an alkyl group having 1 to 5 carbon atoms, R 3 is an alkylene group having 1 to 5 carbon atoms, and n is an integer of 0 to 4.
[0072] R 3 The carbon number of the alkylene group represented by may be 2 or more and 4 or less, or may be 2 or 3. It should be noted that when n is 2 or more, formula (ii) contains 2 or more -OR 3 -represented by a unit. In this case, it can be that R 3 The same can also be R in all units 3 different.
[0073] Among the compounds represented by formula (ii), the compounds represented by the following formula (iia) are preferred. In other words, the chain ether (NF) may contain at least one compound selected from the compounds represented by formula (iia). Formula (iia) corresponds to the alkylene R in formula (ii). 3 For the case of ethylene.
[0074]
[0075] (In formula (iia), R 1 , R 2 , n are the same as those in formula (ii).
[0076] In each of formula (ii) and (iia), R 1 and R 2The number of carbon atoms in the alkyl group represented by each is, for example, 1 to 5, 1 to 3, or 1 or 2. 1 With R 2 It can be the same or different.
[0077] n may be an integer of 0 to 3. From the viewpoint of easily ensuring a high affinity for lithium ions, n is preferably an integer of 1 to 3, and may be 1 or 2.
[0078] If a compound of formula (ii) or formula (iia) (especially a compound of formula (iia)) is used, it is easy to make lithium ions into solvates. In addition, by using these compounds and cyclic monoether (F) together, the side reactions in which the solvent participates can be suppressed in both the positive electrode and the negative electrode, so that the charge and discharge reaction can be carried out. Therefore, it is easy to suppress the reduction of the discharge capacity.
[0079] Examples of the chain ether (NF) include diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,1-dimethoxymethane, 1,1-diethoxyethane, etc. The chain ether (NF) preferably contains at least a chain ether having two or more ether bonds. Examples of such chain ethers include 1,2-dimethoxyethane (DME), 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol dibutyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, triethylene glycol ethyl methyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol ethyl methyl ether and the like.
[0080] Specific examples of the chain ether (NF) include the following compounds.
[0081] CH3-O-CH2CH2-O-CH3
[0082] CH3CH2-O-CH2CH2-O-CH3
[0083] CH3CH2-O-CH2CH2-O-CH3
[0084] CH3CH2-O-CH2CH2-O-CH2CH3
[0085] CH3-O-CH2CH2CH2CH2-O-CH3
[0086] CH3CH2-O-CH(CH3)CH2-O-CH2CH3
[0087] CH3CH2-O-(CH2CH2-O)3-CH2CH3
[0088] (Cyclic ether (NF))
[0089] Cyclic ether (NF) (non-fluorinated cyclic monoether) has an ether bond (-O-) at least in the cyclic structure. The non-aqueous electrolyte may contain only one compound as the cyclic ether (NF), or may contain multiple compounds as the cyclic ether (NF). The cyclic structure of the cyclic ether (NF) may contain a double bond or may not contain a double bond. The cyclic structure may have aromaticity or may not have aromaticity. A chain structure containing an ether bond may also be bonded to the cyclic structure.
[0090] Examples of cyclic ethers (NF) include compounds having a structure in which the fluorine atoms of the compounds exemplified for the above-mentioned cyclic monoethers (F) (fluorinated cyclic monoethers) are replaced with hydrogen atoms. Examples of cyclic ethers (NF) include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, and crown ethers.
[0091] As non-fluorinated ether (NF) and fluorinated cyclic monoether (F), the compound that can be used as the solvent of the non-aqueous electrolyte of lithium secondary battery can be adopted.Non-fluorinated ether (NF) can be the compound consisting of carbon, oxygen and hydrogen.Fluorinated cyclic monoether (F) can also be the compound consisting of carbon, oxygen, hydrogen and fluorine.Their oxygen atom can be only contained in ether bond.
[0092] The non-aqueous electrolyte may contain only one non-fluorinated ether (NF) or a combination of two or more non-fluorinated ethers (NF). The non-aqueous electrolyte may contain only one fluorinated cyclic monoether (F) or a combination of two or more fluorinated cyclic monoethers (F).
[0093] The molecular weight of the non-fluorinated ether (NF) may be 60 or more, 70 or more, or 80 or more, and may be 300 or less, 200 or less, or 100 or less. The molecular weight may be in the range of 60 to 300 (eg, 70 to 200).
[0094] The molecular weight of the fluorinated cyclic monoether (F) may be 90 or more, 120 or more, or 140 or more, and may be 300 or less, 250 or less, or 200 or less. The molecular weight may be in the range of 90 to 300 (eg, 120 to 200).
[0095] (Ratio of each solvent)
[0096] The shared ratio of fluorinated cyclic monoether (F) in solvent can be more than 5 mol % or more than 30 mol %, can be below 90 mol % or below 70 mol %. The shared ratio of non-fluorinated ether (NF) in solvent can be more than 5 mol % or more than 20 mol %, can be below 80 mol % or below 60 mol %. The shared ratio of chain ether (NF) in non-fluorinated ether (NF) and the shared ratio of cyclic ether (NF) in non-fluorinated ether (NF) are not particularly limited. Non-fluorinated ether (NF) can be composed only of chain ether (NF), can be composed only of cyclic ether (NF), can also be composed of chain ether (NF) and cyclic ether (NF).
[0097] (other)
[0098] The solvent may include a small amount of other solvents (the third solvent) except fluorinated cyclic monoether (F) and non-fluorinated ether (NF). Examples of such a third solvent include fluorinated chain ethers and fluorinated cyclic polyethers (e.g., fluorinated cyclic diethers). Examples of fluorinated chain ethers include compounds having a structure in which at least a portion of hydrogen atoms of non-fluorinated chain ether (NF) are replaced with fluorine atoms. In addition, examples of the third solvent include esters, nitrile, amides, or halogen substitutions thereof. The nonaqueous electrolyte may include only one third solvent, or may include more than two third solvents. The halogen substitution has a structure in which at least one hydrogen element is replaced with a halogen element. As a halogen element, at least one element selected from fluorine, chlorine, bromine, and iodine may be cited. The solvent may consist of only an ether compound, or may consist of an ether compound and a compound that is not an ether compound.
[0099] As esters, for example, carbonates, carboxylates, etc. can be mentioned. As cyclic carbonates, ethylene carbonate, propylene carbonate, butylene carbonate, ethylene fluorocarbonate, etc. can be mentioned. As chain carbonates, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, etc. can be mentioned. As cyclic carboxylates, γ-butyrolactone, γ-valerolactone, etc. can be mentioned. As chain carboxylates, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, methyl fluoropropionate, etc. can be mentioned.
[0100] The non-aqueous electrolyte may contain an additive. The additive may be a substance that forms a film on the negative electrode. By forming a film from the additive on the negative electrode, it is easy to further suppress the formation of dendrites. As the additive, for example, vinylene carbonate and vinyl ethylene carbonate can be cited. The amount of the additive in the non-aqueous electrolyte can be, for example, 5% by mass or less.
[0101] (positive electrode)
[0102] The positive electrode includes, for example, a positive electrode current collector and a positive electrode composite material layer formed on the surface of the positive electrode current collector. The positive electrode current collector can be in sheet form (e.g., foil, film) or porous. The positive electrode composite material layer can be formed on a pair of main surfaces of the sheet-like positive electrode current collector or on one main surface. In addition, the positive electrode composite material layer can also be formed in a state filled in a mesh-like positive electrode current collector.
[0103] Examples of the material of the positive electrode current collector include metal materials including Al, Ti, Fe, etc. The metal material may be Al, Al alloy, Ti, Ti alloy, Fe alloy, etc. The Fe alloy may also be stainless steel.
[0104] The positive electrode composite material layer contains a positive electrode active material. The positive electrode composite material layer may also contain at least one selected from a binder, a conductive material, a thickener and an additive in addition to the positive electrode active material. A conductive carbonaceous material may be configured between the positive electrode collector and the positive electrode composite material layer as needed.
[0105] As the positive electrode active material, a material that electrochemically absorbs and releases lithium ions can be used. As such a material, for example, at least one material selected from transition metal oxides, transition metal fluorides, polyanions, fluorinated polyanions, and transition metal sulfides containing lithium can be cited. From the viewpoint of high average discharge voltage and cost advantage, the positive electrode active material can also be a transition metal oxide containing lithium.
[0106] As the transition metal element contained in the transition metal oxide containing lithium, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, W, etc. can be mentioned. The transition metal oxide containing lithium can contain one transition metal element, and can also contain two or more transition metal elements. The transition metal element can be at least one element selected from Co, Ni and Mn. The transition metal oxide containing lithium can contain one or more typical metal elements as needed. As typical metal elements, Mg, Al, Ca, Zn, Ga, Ge, Sn, Sb, Pb, Bi, etc. can be mentioned. Typical metal elements can be Al, etc.
[0107] Examples of the binder include fluororesins, polyacrylonitrile, polyimide resins, acrylic resins, polyolefin resins, and rubber polymers. Examples of the fluororesins include polytetrafluoroethylene and polyvinylidene fluoride.
[0108] As the conductive material, for example, conductive carbonaceous materials can be mentioned. As the conductive carbonaceous materials, carbon black, carbon nanotubes, graphite, etc. can be mentioned. As the carbon black, acetylene black, Ketjen black, etc. can be mentioned.
[0109] As the thickener, for example, cellulose derivatives such as cellulose ethers can be cited. As cellulose derivatives, carboxymethyl cellulose (CMC) and its modified products, methyl cellulose, etc. can be cited. Modified products of CMC also include salts of CMC. As salts, alkali metal salts (such as sodium salts), ammonium salts, etc. can be cited.
[0110] Examples of the carbonaceous material disposed between the positive electrode current collector and the positive electrode composite material layer include at least one carbonaceous material selected from the conductive carbonaceous materials exemplified as the conductive material.
[0111] The positive electrode can be obtained, for example, by applying or filling a slurry containing the constituent components of the positive electrode composite material layer and a dispersion medium on the positive electrode collector, and drying and compressing the coating. On the surface of the positive electrode collector, a conductive carbonaceous material can be applied as needed. As a dispersion medium, at least one dispersion medium selected from water and an organic medium (N-methyl-2-pyrrolidone, etc.) can be cited.
[0112] (negative electrode)
[0113] The negative electrode includes a negative electrode collector. The negative electrode collector is usually composed of a conductive sheet. The conductive sheet may also be composed of a conductive material other than lithium metal and lithium alloys. The conductive material may be a metal material such as a metal and an alloy. The metal material may be a material that does not react with lithium. More specifically, it may be a material that does not form an alloy or an intermetallic compound with lithium. Such metal materials are, for example, copper, nickel, iron, and alloys containing these metal elements. As alloys, copper alloys, stainless steel, and the like may be used. From the viewpoint of easily ensuring high capacity and high charge and discharge efficiency due to high conductivity, the metal material may include at least one of copper and a copper alloy. The conductive sheet may include one of these conductive materials, or may include two or more.
[0114] As the conductive sheet, foil, film, etc. can be used. The conductive sheet can be porous. From the viewpoint of easily ensuring high conductivity, the conductive sheet can be a metal foil, or a metal foil containing copper. Such a metal foil can be a copper foil or a copper alloy foil.
[0115] It should be noted that, from the perspective of easily ensuring a high volume energy density, the negative electrode may include only a negative electrode collector in the fully discharged state of the lithium secondary battery (S). That is, the lithium secondary battery (S) may not include a negative electrode active material layer. In addition, from the perspective of easily ensuring a high charge and discharge efficiency, in the fully discharged state, the negative electrode may include a negative electrode collector and a negative electrode active material layer disposed on the surface of the negative electrode collector. It should be noted that when assembling the battery, only the negative electrode collector may be used as the negative electrode, or a negative electrode having a negative electrode active material layer and a negative electrode collector may be used.
[0116] As the negative electrode active material contained in the negative electrode active material layer, for example, metallic lithium, lithium alloys, materials that reversibly absorb and release lithium ions, etc. can be cited. As the negative electrode active material, the negative electrode active material used in lithium ion batteries can be used. As lithium alloys, for example, lithium-aluminum alloys, lithium-zinc alloys, lithium-magnesium alloys, lithium-silver alloys, lithium-gold alloys, etc. can be cited. As materials that reversibly absorb and release lithium ions, for example, carbon materials, alloy materials, etc. can be cited. As carbon materials, for example, graphite materials, soft carbon, hard carbon and amorphous carbon can be cited. As alloy materials, for example, silicon-containing materials and tin-containing materials can be cited. As alloy materials, for example, silicon single substance, silicon alloys, silicon compounds, tin single substance, tin alloys and tin compounds can be cited. As silicon compounds and tin compounds, oxides and nitrides can be cited respectively. The negative electrode active material layer can contain one negative electrode active material, or it can contain a combination of two or more negative electrode active materials.
[0117] The negative electrode active material layer can be formed by depositing the negative electrode active material on the surface of the negative electrode collector by a gas phase method such as electrolysis or evaporation. In addition, it can also be formed by applying a negative electrode composite material containing a negative electrode active material, a binding material and other components used as needed to the surface of the negative electrode collector. As other components, conductive materials, thickeners and additives can be cited.
[0118] The thickness of the negative electrode active material layer is not particularly limited, but is, for example, 30 μm to 300 μm in a fully discharged state of the lithium secondary battery (S). The thickness of the negative electrode current collector is, for example, 5 μm to 20 μm.
[0119] In the present disclosure, the fully discharged state of a lithium metal secondary battery refers to a state in which the battery is discharged to a charged state (SOC: State of Charge) of 0.05×C or less when the rated capacity of the battery is recorded as C. For example, it refers to a state in which the battery is discharged at a constant current of 0.05C to a lower limit voltage. The lower limit voltage is, for example, 2.5V.
[0120] The negative electrode may further include a protective layer. The protective layer may be formed on the surface of the negative electrode collector, and may also be formed on the surface of the negative electrode active material layer when the negative electrode has a negative electrode active material layer. The protective layer has the effect of making the surface reaction of the electrode more uniform, and it is easy to precipitate lithium metal more uniformly on the negative electrode. The protective layer is composed of, for example, a material (organic material, inorganic material) that does not inhibit lithium ion conductivity. As organic materials, polymers with lithium ion conductivity may be cited. As such polymers, polyethylene oxide and polymethyl methacrylate may be exemplified. As inorganic materials, ceramics, solid electrolytes, etc. may be cited. The protective layer may include one of these materials, or may include two or more.
[0121] (Diaphragm)
[0122] The lithium secondary battery may include a separator sandwiched between the positive electrode and the negative electrode. As the separator, a porous sheet having ion permeability and insulation may be used. Examples of porous sheets include microporous membranes, fabrics, and nonwoven fabrics. The material of the separator may also be a polymer material. Examples of polymer materials include olefin resins, polyamide resins, and cellulose. Examples of olefin resins include polyethylene, polypropylene, and copolymers of ethylene and propylene. The separator may include additives as needed. Examples of additives include inorganic fillers.
[0123] The separator may include a plurality of layers having at least one different form and composition. Such a separator may be, for example, a laminate of a polyethylene microporous membrane and a polypropylene microporous membrane, or a laminate of a nonwoven fabric containing cellulose fibers and a nonwoven fabric containing thermoplastic resin fibers.
[0124] (other)
[0125] As an example of the structure of a lithium secondary battery, the following structure can be cited: an electrode group and a non-aqueous electrolyte are contained in an outer package body, in which a positive electrode and a negative electrode are wound via a separator. In such a structure, as an electrode group, an electrode group of other forms such as a stacked electrode group in which a positive electrode and a negative electrode are stacked via a separator can also be used. The lithium secondary battery can be, for example, in any form such as a cylindrical, square, coin-shaped, button-shaped, laminated type, etc.
[0126] Figure 1 A longitudinal cross-sectional view of a lithium secondary battery according to an embodiment is shown. Figure 2 The lithium secondary battery is shown in the fully discharged state along Figure 1 An enlarged cross-sectional view obtained by cutting along line II contained therein.
[0127] The lithium secondary battery 10 is a cylindrical battery including a cylindrical battery case, a wound electrode group 14 and a non-aqueous electrolyte (not shown). The electrode group 14 and the non-aqueous electrolyte are contained in the battery case. The battery case is composed of a shell body 15 as a bottomed cylindrical metal container and a sealing body 16 that seals the opening of the shell body 15. A sealing gasket 27 is arranged between the shell body 15 and the sealing body 16, thereby ensuring the airtightness of the battery case. In the shell body 15, insulating plates 17 and 18 are respectively arranged at one end and the other end of the wound electrode group 14.
[0128] The housing body 15 has, for example, a step portion 21 formed by locally pressurizing the side wall of the housing body 15 from the outside. The step portion 21 may be formed in an annular shape on the side wall of the housing body 15 along the circumferential direction of the housing body 15. In this case, the sealing body 16 is supported by the surface of the step portion 21 on the opening side.
[0129] The sealing body 16 includes a filter 22, a lower valve body 23, an insulating member 24, an upper valve body 25, and a cover 26. In the sealing body 16, these components are stacked in this order. The sealing body 16 is mounted on the opening of the housing body 15 in such a manner that the cover 26 is located outside the housing body 15 and the filter 22 is located inside the housing body 15. The above-mentioned components constituting the sealing body 16 are, for example, in a disc shape or an annular shape. The components except the insulating member 24 are electrically connected to each other.
[0130] The electrode group 14 includes a positive electrode 11, a negative electrode 12, and a separator 13. The positive electrode 11, the negative electrode 12, and the separator 13 are all in a strip shape. The positive electrode 11 and the negative electrode 12 are wound into a spiral shape with the separator 13 sandwiched between the electrodes in a manner that the width direction of the strip-shaped positive electrode 11 and the negative electrode 12 is parallel to the winding axis. In a cross section of the electrode group 14 perpendicular to the winding axis, the positive electrode 11 and the negative electrode 12 are alternately stacked along the radial direction of the electrode group 14 with the separator 13 sandwiched between the electrodes.
[0131] The positive electrode 11 is electrically connected to the cap 26 also serving as a positive electrode terminal via a positive electrode lead 19. One end of the positive electrode lead 19 is electrically connected to the strip-shaped positive electrode 11. The positive electrode lead 19 extending from the positive electrode 11 passes through a through hole (not shown) formed in the insulating plate 17 and extends to the filter 22. The other end of the positive electrode lead 19 is welded to the surface of the filter 22 on the electrode group 14 side.
[0132] The negative electrode 12 is electrically connected to the case body 15 also serving as a negative electrode terminal via a negative electrode lead 20. One end of the negative electrode lead 20 is electrically connected to the strip-shaped negative electrode 12. The other end of the negative electrode lead 20 is welded to the inner bottom surface of the case body 15.
[0133] like Figure 2 As shown, the positive electrode 11 includes a positive electrode collector 30 and a positive electrode composite material layer 31 disposed on both surfaces of the positive electrode collector 30. The negative electrode 12 includes a negative electrode collector 32. In the negative electrode 12 of the lithium secondary battery 10, lithium metal is deposited by charging. On the other hand, the deposited lithium metal is dissolved in the non-aqueous electrolyte by discharging.
[0134] (Note)
[0135] The following techniques are disclosed through the description of the above embodiments.
[0136] (Technology 1)
[0137] A lithium secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte having lithium ion conductivity,
[0138] In the negative electrode, lithium metal is deposited during charge, and the lithium metal is dissolved in the nonaqueous electrolyte during discharge.
[0139] The nonaqueous electrolyte comprises a solvent and a lithium salt,
[0140] The solvent comprises a non-fluorinated ether and a fluorinated cyclic monoether,
[0141] The fluorinated cyclic monoether comprises a cyclic structure having one ether bond,
[0142] The lithium salt comprises an anion of an oxalate complex.
[0143] (Technique 2)
[0144] According to the lithium secondary battery of the first aspect, the total of the ratio of the non-fluorinated ether in the solvent and the ratio of the fluorinated cyclic monoether in the solvent is 95 mol % or more.
[0145] (Technique 3)
[0146] According to the lithium secondary battery of technology 1 or 2, the ratio MF / MLi of the mole number MF of the fluorinated cyclic monoether contained in the non-aqueous electrolyte to the mole number MLi of the lithium salt contained in the non-aqueous electrolyte is in the range of 0.25-10.
[0147] (Technique 4)
[0148] According to any one of techniques 1 to 3, the ratio MF / MNF of the mole number MF of the fluorinated cyclic monoether contained in the non-aqueous electrolyte to the mole number MNF of the non-fluorinated ether contained in the non-aqueous electrolyte is in the range of 0.1-10.
[0149] (Technique 5)
[0150] According to the lithium secondary battery of any one of techniques 1 to 4, the concentration of the lithium salt containing the anion of the oxalate complex in the non-aqueous electrolyte is in the range of 0.01 to 0.5 mol / L.
[0151] (Technique 6)
[0152] According to any one of techniques 1 to 5, the lithium secondary battery, wherein the fluorinated cyclic monoether includes a 5-membered ring containing one ether bond or a 6-membered ring containing one ether bond.
[0153] (Technique 7)
[0154] According to any one of technologies 1 to 6, the lithium secondary battery, wherein the lithium salt containing the anion of the oxalate complex is lithium difluorooxalatoborate.
[0155] (Technology 8)
[0156] According to any one of techniques 1 to 7, the lithium secondary battery, wherein the fluorinated cyclic monoether is 3,3,4,4-tetrafluorotetrahydrofuran.
[0157] Example
[0158] Hereinafter, the present disclosure will be specifically described based on examples, but the present disclosure is not limited to the following examples. In this example, a plurality of lithium secondary batteries were produced and evaluated by the following steps.
[0159] (Battery A1)
[0160] The following steps are performed to prepare Figure 1 Battery A1 (lithium secondary battery) of the structure shown.
[0161] (1) Preparation of positive electrode 11
[0162] The positive electrode active material, acetylene black (conductive material) and polyvinylidene fluoride (binding material) are mixed in a mass ratio of 95:2.5:2.5 to obtain a mixture. An appropriate amount of N-methyl-2-pyrrolidone (dispersion medium) is added to the obtained mixture and stirred to prepare a positive electrode composite material slurry. As the positive electrode active material, a lithium-containing transition metal oxide containing Ni, Co and Al is used.
[0163] The positive electrode composite material slurry is applied to both sides of the aluminum foil (positive electrode collector 30) and dried to obtain a dried product. Next, the dried product is compressed in the thickness direction using a roller to obtain a laminate. The obtained laminate is cut according to a specified electrode size to thereby prepare a positive electrode 11 comprising a positive electrode collector 30 and a positive electrode composite material layer 31 formed on both sides of the positive electrode collector 30. It should be noted that in a part of the positive electrode 11, an exposed portion of the positive electrode collector 30 without the positive electrode composite material layer 31 is formed. On the exposed portion of the positive electrode collector 30, one end of an aluminum positive electrode lead 19 is installed by welding.
[0164] (2) Preparation of negative electrode 12
[0165] A 10 μm thick electrolytic copper foil is cut into a predetermined electrode size to form a negative electrode collector 32. This negative electrode collector 32 is used in the manufacture of a battery as the negative electrode 12. One end of a negative electrode lead 20 made of nickel is attached to the negative electrode collector 32 by welding.
[0166] (3) Preparation of non-aqueous electrolyte
[0167] The solvent is prepared by mixing 3,3,4,4-tetrafluorotetrahydrofuran (F-THF) as a cyclic fluoroether (F) with 1,2-dimethoxyethane (DME) as a non-fluorinated chain ether (NF). They are mixed in a manner such that the ratio MF / MNF of the mole number MF of the fluorinated cyclic monoether contained in the non-aqueous electrolyte to the mole number MNF of the non-fluorinated ether contained in the non-aqueous electrolyte is the value shown in Table 1. Lithium hexafluorophosphate (LiPF6) as a lithium salt and lithium difluorooxalatoborate (LiFOB) as a lithium salt are dissolved in the obtained solvent to thereby modulate a non-aqueous electrolyte. At this time, LiFOB and LiPF6 are dissolved in the solvent in a manner such that their concentrations are the concentrations shown in Table 1.
[0168] (4) Battery production
[0169] In an inert gas atmosphere, the positive electrode 11 obtained in the above (1), the negative electrode 12 obtained in the above (2) and the separator 13 are wound to form an electrode group 14. The positive electrode 11, the negative electrode 12 and the separator 13 are wound in a manner in which the separator 13 is arranged between the positive electrode 11 and the negative electrode 12. As the separator 13, a microporous film made of polyethylene is used. The obtained electrode group 14 is contained in a bag-shaped outer packaging body. Next, after the non-aqueous electrolyte obtained in the above (3) is injected into the outer packaging body, the outer packaging body is sealed. Battery A1 is thus produced. The outer packaging body is formed by a laminate sheet including an aluminum layer.
[0170] (Other batteries)
[0171] As shown in Table 1, the type and ratio of the solvent used in the non-aqueous electrolyte, as well as the type and ratio of the lithium salt, were changed. In addition, the same method as the modulation of the non-aqueous electrolyte of battery A1 was used to modulate a variety of non-aqueous electrolytes. It should be noted that "other (X)" in Table 1 refers to solvents other than fluorinated cyclic monoether (F) and non-fluorinated ether (NF). Using the non-aqueous electrolytes modulated, in addition, a plurality of batteries were made using the same method as the preparation method of battery A1.
[0172] (1) Charge and discharge cycle test at 25°C (T1)
[0173] The plurality of lithium secondary batteries thus produced were subjected to charge and discharge tests by the following procedure to evaluate the cycle characteristics: First, the lithium secondary batteries were charged in a thermostatic chamber at 25° C. under the following conditions, rested for 20 minutes, and then discharged under the following conditions.
[0174] (Charge)
[0175] The battery was charged at a constant current of 0.1 It until the battery voltage reached 4.3 V, and then charged at a constant voltage of 4.3 V until the current value reached 0.01 It. Here, It is a current value represented by It (A) = rated capacity (Ah) / 1.0 (h).
[0176] (Discharge)
[0177] The battery was discharged at a constant current of 0.1 It until the battery voltage reached 2.5V.
[0178] The above charge and discharge were regarded as one cycle, and the charge and discharge test was carried out for 50 cycles. The discharge capacity of the first cycle was measured as the initial discharge capacity C0. In addition, the discharge capacity C1 of the 50th cycle was measured. Then, the capacity retention rate (%) was calculated by the following formula.
[0179] Capacity retention rate (%) = 100 × C1 / C0
[0180] (2) Charge and discharge cycle test at 45°C (T2)
[0181] For the plurality of lithium secondary batteries thus prepared, the charge and discharge were performed in a thermostatic chamber at 45°C instead of in a thermostatic chamber at 25°C, and a charge and discharge cycle test (T2) was performed in the same manner as in the charge and discharge cycle test (T1). Then, the capacity retention rate (%) was calculated in the same manner as above.
[0182] Some of the preparation conditions of the nonaqueous electrolyte and the evaluation results are shown in Table 1. A higher capacity retention rate is preferred because the deterioration is less. Batteries A1 to A10 are lithium secondary batteries (S), and the other batteries are batteries of comparative examples.
[0183] The "molar ratio MF / MNF / MX" in Table 1 represents the molar ratio of each compound constituting the solvent, MF / MNF / MX = "the number of moles of fluorinated cyclic monoether (F)" / "the number of moles of non-fluorinated ether (NF)" / "the number of moles of others (X)". "0.05 / 1.0" in the lithium salt concentration column of Experimental Example EA1 in Table 1 means that the concentration of LiFOB is 0.05 mol / L and the concentration of LiPF6 is 1.0 mol / L (the same applies to other experimental examples). As mentioned above, the "ratio MF / MLi" in Table 1 is the ratio of the number of moles MF of the fluorinated cyclic monoether (F) contained in the non-aqueous electrolyte to the number of moles MLi of the lithium salt contained in the non-aqueous electrolyte. The number of moles of the lithium salt is the sum of the number of moles of LiPF6 and the number of moles of LiFOB. As described above, the “ratio MF / MNF” in Table 1 is the ratio of the number of moles MF of the fluorinated cyclic monoether (F) contained in the non-aqueous electrolyte to the number of moles MNF of the non-fluorinated ether (NF) contained in the non-aqueous electrolyte.
[0184] [Table 1]
[0185]
[0186] In Table 1, the abbreviations of the compounds represent the following compounds. "F-THF" represents 3,3,4,4-tetrafluorotetrahydrofuran. "F-THP" represents 4-difluoromethyltetrahydro-2H-pyran. "DME" represents 1,2-dimethoxyethane. "F-DOL" represents 2-(trifluoromethyl)dioxolane. "HFE" represents 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether. LiFOB and LiPF6 are as described above.
[0187] As shown in Table 1, batteries A1 to A10, which are lithium secondary batteries (S) involved in the present disclosure, have high capacity retention rates even after a cycle test at 45°C. Battery A1 has a high capacity retention rate after a cycle test at any temperature between 25°C and 45°C. When battery A1 was used, the capacity retention rate in the test at 45°C was 90% (76.4 / 84.6) of the capacity retention rate in the test at 25°C. On the other hand, when battery C1 of the comparative example was used, the capacity retention rate in the test at 45°C was 76% (63.2 / 83.0) of the capacity retention rate in the test at 25°C. In addition, when battery C2 of the comparative example was used, the capacity retention rate in the test at 45°C was 79% (67.1 / 85.2) of the capacity retention rate in the test at 25°C.
[0188] As shown in Table 1, the concentration of the lithium salt containing an anion of the oxalate complex in the non-aqueous electrolyte is preferably in the range of 0.01 to 0.5 mol / L. The ratio MF / MLi is preferably in the range of 0.25 to 10. The ratio MF / MNF is preferably in the range of 0.1 to 10.
[0189] Industrial Availability
[0190] The present disclosure can be used in lithium secondary batteries.
[0191] The present invention has been described with respect to the currently preferred embodiments, but such disclosure is not to be construed as limiting. A person skilled in the art in the art to which the present invention belongs can accurately know various modifications and changes by reading the above disclosure. Therefore, the attached claims should be interpreted as including all modifications and changes in a manner that does not depart from the true spirit and scope of the present invention.
[0192] Description of Reference Numerals
[0193] 10Lithium secondary battery
[0194] 11 Positive electrode
[0195] 12 Negative electrode
[0196] 13 Diaphragm
[0197] 14 electrode set
[0198] 15 Shell body
[0199] 16 Sealing body
[0200] 30 Positive electrode collector
[0201] 31 positive electrode composite material layer
[0202] 32 Negative electrode collector
Claims
1. A lithium secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte having lithium ion conductivity, At the negative electrode, lithium metal is precipitated during charging, and the lithium metal is dissolved in the non-aqueous electrolyte during discharging. The nonaqueous electrolyte comprises a solvent and a lithium salt, The solvent comprises a non-fluorinated ether and a fluorinated cyclic monoether, The fluorinated cyclic monoether comprises a cyclic structure having one ether bond, The lithium salt comprises an anion of an oxalate complex. 2 . The lithium secondary battery according to claim 1 , wherein the total of the ratio of the non-fluorinated ether in the solvent and the ratio of the fluorinated cyclic monoether in the solvent is 95 mol % or more. 3 . The lithium secondary battery according to claim 1 , wherein a ratio MF / MLi of a mole number MF of the fluorinated cyclic monoether contained in the non-aqueous electrolyte to a mole number MLi of the lithium salt contained in the non-aqueous electrolyte is in a range of 0.25 to 10. 4 . The lithium secondary battery according to claim 1 , wherein a ratio MF / MNF of a mole number MF of the fluorinated cyclic monoether contained in the non-aqueous electrolyte to a mole number MNF of the non-fluorinated ether contained in the non-aqueous electrolyte is in the range of 0.1 to 10. 5 . The lithium secondary battery according to claim 1 , wherein the concentration of the lithium salt containing the anion of the oxalate complex in the non-aqueous electrolyte is in the range of 0.01 to 0.5 mol / L. 6 . The lithium secondary battery according to claim 1 , wherein the fluorinated cyclic monoether comprises a 5-membered ring containing one ether bond or a 6-membered ring containing one ether bond. 7 . The lithium secondary battery according to claim 1 , wherein the lithium salt containing the anion of the oxalate complex is lithium difluorooxalatoborate. 8 . The lithium secondary battery according to claim 1 , wherein the fluorinated cyclic monoether is 3,3,4,4-tetrafluorotetrahydrofuran.