Mechanical ion current generator, manufacturing method thereof and mechanical ion self-powered drug release patch
By using the opposite electrodes of activated carbon cloth and hydrogel in the mechanical ion current generator, the asymmetric ion adsorption and diffusion characteristics are used to solve the problem of insufficient current output under low frequency and low speed mechanical energy in the prior art, and high current and High charge transfer, suitable for biomedical applications.
Patent Information
- Application Number
- CN202410710484.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-06
- Filing Date
- 2024-06-03
- Publication Date
- 2024-12-06
AI Technical Summary
The existing mechanical ion current generators have insufficient current output at low frequency and low speed mechanical energy, which cannot meet the needs of many biomedical applications, especially in terms of electrical muscle stimulation and bone regeneration.
Mechanical ion current generator using a working electrode made of activated carbon cloth and an opposing electrode made of carbon cloth and hydrogel, by introducing multiple flexible and asymmetrical structures and oxygen-containing functional groups into the hydrogel , leverages the asymmetric ion adsorption characteristics of the electrode and the differential diffusion rates of cations and anions in the hydrogel to synergize the engineering structure and chemical asymmetry to enhance the generation of net ion current.
The peak current is generated at 0.1Hz (5.5A m-2) with a charge transmitted up to 916mC m-2 per cycle, significantly improving the current output, suitable for biomedical applications such as self-powered drug delivery functions wound healing patch.
Smart Images

Figure CN119075177A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates generally to electric current generators. More particularly, the present invention relates to hydrogel-based mechano-ionic current generators. Background Art
[0002] The development of tight integration of electronic devices into biological bodies requires soft and biocompatible electromechanical energy converters that can respond to mechanical stimulation for physiological sensing / monitoring or harvest biomechanical energy to provide electricity. Conventional electromagnetic generators, although they have large electrical output at relatively high frequencies, are obviously insufficient due to the mechanical mismatch with biological systems. However, triboelectric and piezoelectric nanogenerators developed using various soft materials are generally characterized by high internal impedance and low output current. Given that some important biomedical applications (such as muscle electrical stimulation and bone regeneration, etc.) require high currents, while most of the biomechanical energy generated by human physiological activities is low-frequency and low-speed, the development of soft electromechanical devices that use low-frequency and low-speed mechanical energy to generate high currents and high transfer charges is particularly important.
[0003] Current generation through mechanical ionic mechanisms is a promising approach to meet these requirements. Analogous to the piezoelectric mechanism of polarizing dipoles in dielectric materials through mechanical pressure, electrolytic materials (such as hydrogels, etc.) can also be polarized due to the unbalanced distribution of cations and anions caused by mechanical deformation. Its essence is to produce gradient deformation at the interface of two electrodes / hydrogels, thereby producing an asymmetric cation / anion distribution. This asymmetry can be induced by the current of polyelectrolyte hydrogels with free ions of a single positive and negative sign, or in neutral hydrogels with cations and anions diffusing at different rates. The latter mechanism has recently been confirmed as the piezoelectric ionic effect. In fact, similar asymmetric ion distribution / diffusion has been thermally manifested in temperature gradients for thermoelectric power generation, or chemically manifested in functional group gradients for moisture or water vapor power generation. However, the current output achievable by existing mechanical ionic effects remains at a low level of about 1μA, which is not enough to serve as a power source for most practical devices. Summary of the invention
[0004] According to a first aspect of the present invention, a mechanical ion current generator is provided, comprising: a working electrode comprising an activated carbon cloth; and an opposing electrode comprising a native carbon cloth and a hydrogel; wherein the hydrogel has a plurality of flexible and asymmetric structures; and the working electrode has a surface immersed in the hydrogel and having a plurality of oxygen-containing functional groups.
[0005] According to a second aspect of the present invention, a method for manufacturing a mechanical ion current generator is provided, the mechanical ion current generator comprising a working electrode made of activated carbon cloth, and an opposing electrode made of carbon cloth and a hydrogel. The method comprises: preparing the working electrode by the following operations: cleaning a piece of carbon cloth; oxidizing the cleaned carbon cloth in a two-electrode system containing an aqueous (NH4)2SO4 solution; and reducing the oxidized carbon cloth in a three-electrode system containing an aqueous NH4Cl solution to form the working electrode; and preparing the opposing electrode by the following operations: pouring a first PVA solution into a mold to obtain a molded PVA; repeatedly freezing and thawing the molded PVA to obtain a cross-linked hydrogel; immersing a piece of cleaned carbon cloth into a second PVA solution to obtain a carbon cloth soaked in PVA; placing the carbon cloth soaked in PVA on the back side of the cross-linked hydrogel to obtain a combined structure; repeatedly freezing and thawing the combined structure to obtain a combined electrode; and keeping the combined electrode in an electrolyte solution for 1 day to load the combined electrode with mobile ions to form the opposing electrode.
[0006] According to the third aspect of the present invention, a mechanical ion self-powered drug release patch is provided. The mechanical ion self-powered drug release patch comprises: a substrate; an electrolyte-containing pad; and a drug release pad placed between the electrolyte-containing pad and the substrate. The drug release pad comprises: a drug-carrying layer having a surface in contact with the electrolyte-containing pad; a printed circuit in contact with the drug-carrying layer; and a mechanical ion current generator according to the first aspect of the present invention, wherein the working electrode is electrically connected to the electrolyte-containing pad through the printed circuit; and the counter electrode is electrically connected to the drug-carrying layer.
[0007] In the present invention, the engineered structure and chemical asymmetry in the hydrogel are synergistically optimized to enhance the generation of net ionic current, achieving several orders of magnitude amplification of mechano-ionic current generation. Under compressive loading, the relief structure in the hydrogel enhances the net ionic flux induced by the deformation gradient, which synergizes with the asymmetric ion adsorption properties of the electrode and the differential diffusion rates of cations and anions in the hydrogel matrix. This engineered mechano-ionic process can generate 4 mA (5.5 A m) under cyclic compression of 80 kPa applied at 0.1 Hz. -2 ) with a peak current of up to 916 mCm per cycle. -2The ionic current generation mechanism is naturally compatible with living organisms and living hydrogels, where ions are the main charge / information / energy carriers, providing good current and charge transport, which is beneficial for various biomedical applications, such as wound healing patches with self-powered drug delivery. On the other hand, hydrogel materials can be further engineered to have additional properties, such as bioactivity, biodegradability, bioadhesion, and other properties useful for advanced biological interfaces. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Embodiments of the present invention are described in more detail below with reference to the accompanying drawings, in which:
[0009] Figure 1 A schematic structural diagram of a mechanical ion current generator according to an embodiment of the present invention is shown.
[0010] Figure 2A and 2B It is shown that before compression is applied to the hydrogel structure ( Figure 2A ) and after ( Figure 2B )-simulated strain.
[0011] Figure 3 The working mechanism of the mechanical ionic current generator is shown. The strain gradient in the hydrogel layer causes Cl - In comparison + Higher diffusivity shifts.
[0012] Figures 4A to 4C The short-circuit current I generated by the mechanical ionic current generator is shown respectively. SC , open circuit voltage V OC And the time series distribution curve of the applied pressure P.
[0013] Figure 5A and 5B The voltage and corresponding current and power density of the mechanical ionic current generator for various loads are shown.
[0014] Figure 6 Shown is the change in current output when the layout of the working electrode and the counter electrode is changed.
[0015] Figure 7 The current output of the optimized electrode layout CC-ACC at various activation times of the ACC electrode is shown.
[0016] Figure 8 Shown in CC / Li + / H2O system and ACC / Li + Simulated charge redistribution in the H2O system.
[0017] Fig. 9The calculated adsorption energies of various species on the electrode counter-electrode materials are shown.
[0018] Fig. 10A and 10B The contact angles of the steel foil before (91°) and after (32°) plasma treatment are shown respectively.
[0019] Fig.11A shows the response current as a function of applied pressure for various devices using steel foil as the working electrode; and Fig. 11B A schematic image showing a corresponding device configuration.
[0020] Fig. 12A Schematic diagram showing the response current and corresponding configuration of various devices using PI / Au as working electrodes as a function of applied pressure; Fig. 12B A schematic image showing a corresponding device configuration.
[0021] Fig.13 Shown is a schematic representation of the process of polyethyleneimine (PEI, a typical cationic polymer) treatment of ACC, which modifies the ion adsorption properties of ACC.
[0022] Fig.14 Different current outputs of the device under different treatments of the ACC working electrode are shown.
[0023] Fig.15 Fourier transform infrared spectroscopy (FTIR) spectra of ACC at four stages during the PEI modification process are shown.
[0024] Fig.16 An enlarged FTIR spectrum image is shown, indicating that a small amount of residual PEI is still present on the surface of ACC even after 2 days of rinsing.
[0025] Fig.17 The peak short-circuit current is shown as a function of applied pressure, where the hydrogel is soaked with different electrolytes.
[0026] Fig.18 Peak current and charge delivered per cycle are shown as a function of recovery time between cycles.
[0027] Fig.19 The output current is shown at various recovery times.
[0028] Fig. 20 Peak current and charge delivered per cycle are shown as a function of strain rate.
[0029] Fig.21 The output current at various strain rates is shown.
[0030] Fig. 22Shown is the charging profile of a 2 F capacitor charged by a hydrogel-based current generator.
[0031] Fig.23 The voltage of a 2 F capacitor is shown during charging of the 2 F capacitor by an electrochemical workstation.
[0032] Fig.24 Shown is a demonstration setup using a mechano-ionic current generator as a power source to harvest mechanical energy and drive electronics.
[0033] Fig.25 The current output over 7500 cycles of 5 kPa compression is shown, illustrating the durability and stability of the device.
[0034] Fig.26 The pressure-distance curves for the 1st and 500th compression-disengagement cycles are shown.
[0035] Fig.27A The pressure-response characteristics of a large-scale device are shown, where the device area is increased to 29 cm 2 ; Fig.27B shows the current and voltage when the large-scale device is loaded with different resistances; Fig.27C The power density of a large-scale device is shown as a function of external resistance.
[0036] Fig.28 The current signal when a 122Ω resistor is loaded at low humidity and high humidity is shown.
[0037] Fig.29 The recycling process of the CC-PVA electrode is shown.
[0038] Fig.30 A comparison of the mechanical ionic current generator provided by the present invention with the current state of the art in terms of internal resistance, current density, softness, transferred charge and density is shown.
[0039] Fig.31 The current output of this hydrogel-based current generator under various frequencies of mechanical input is shown compared with TENG and EMG.
[0040] Fig.32 Schematic diagram showing the drug loading process with electrodeposition.
[0041] Fig.33A SEM images of the drug release patch are shown at a scale of 1:50 μm; and Fig.33B SEM images of the drug release patch are shown at a scale of 1:5 μm.
[0042] Fig.34 Schematic diagram showing electrically responsive drug release in vitro.
[0043] Fig.35 A standard calibration curve of cefazolin sodium is shown.
[0044] Fig.36 An in vitro demonstration of electrically controlled drug release with "on-off" cycling driven by a hydrogel-based current generator is shown. The "on" state represents tapping the device to provide an output current.
[0045] Fig.37 Schematic (top) and photograph (bottom) showing a self-powered drug-delivery patch (SDP).
[0046] Fig.38A Schematic diagram showing application of SDP on the dorsal side of a mouse; and Fig.38B A schematic image showing the working mechanism of the developed SDP.
[0047] Fig.39 An equivalent circuit of SDP is shown.
[0048] Fig.40 The relative area of the wound as a function of healing time is shown. On the last day, the wound area covered by the normal patch and SDP was reduced to 32% and 11% of the initial wound area, respectively.
[0049] Fig.41 Photographs of wounds during the healing process with a standard patch (upper) and SDP (lower) are shown. DETAILED DESCRIPTION
[0050] In the following description, mechanical ion current generators and the like are described as preferred examples. It will be apparent to those skilled in the art that modifications including additions and / or substitutions may be made without departing from the scope and spirit of the invention. Certain details may be omitted so as not to obscure the invention; however, this disclosure is written to enable those skilled in the art to practice the teachings herein without undue experimentation.
[0051] Figure 1 The schematic diagram of the structure of a mechanical ion current generator according to an embodiment of the present invention is shown. As shown in the figure, the mechanical ion current generator includes a working electrode 110 and an opposing electrode 120.
[0052] The working electrode 110 is made of activated carbon cloth (ACC). The counter electrode 120 is made of virgin carbon cloth (CC) 121 and a hydrogel 122. The hydrogel 122 has a plurality of flexible and asymmetrically shaped structures. The bottom surface of the working electrode 110 is immersed in the hydrogel 122 and has a plurality of oxygen-containing functional groups. The plurality of oxygen-containing functional groups are configured to face the tip portions of the plurality of flexible and asymmetrically shaped structures of the hydrogel 122. Each of the flexible and asymmetrically shaped structures has a pyramidal shape.
[0053] The ACC working electrode 101 can be manufactured by the following operations: cleaning a piece of CC with acetone, isopropyl alcohol (IPA) and deionized water (DI water) before activation; and subjecting the CC to an electrochemical oxidation process, which is carried out in a two-electrode system in a 0.1M (NH4)2SO4 aqueous solution using a Pt electrode as a counter electrode and applying a voltage of 10V for 15 minutes. The oxidized CC is subjected to an electrochemical reduction process, which is carried out in a three-electrode system in a 1MNH4Cl aqueous solution, where Pt and Ag / AgCl electrodes serve as counter electrodes and reference electrodes, respectively. The oxidized carbon cloth is reduced at -1.2V for 30 minutes. After cleaning and drying, the manufactured ACC is collected and used as a working electrode.
[0054] The CC-PVA counter electrode can be made by pouring a 15wt% PVA solution into a 3D printed PTFE mold, freeze-molding the PVA at -18°C for 8 hours, and thawing the frozen PVA at 25°C for 3 hours; and repeating the freezing and thawing steps four times to obtain a physically cross-linked hydrogel. A piece of clean CC was then immersed in a 10wt% PVA solution and placed on the back side of the cross-linked PVA hydrogel. After repeating the freeze-thaw process twice, the CC-PVA electrode was kept in an electrolyte solution (4M LiCl) for 1 day to react with mobile ions Li. + and Cl - Loading CC-PVA electrodes.
[0055] Figure 2A and 2B It is shown that before compression is applied to the hydrogel structure ( Figure 2A ) and after ( Figure 2B )-simulated strain. The cross-sectional area of the hydrogel pyramid changes with height, resulting in a high strain gradient under normal compression. This strain gradient causes water to shift from areas with large compressive strain to areas with less strain, and then the resulting gradient in ion concentration leads to cation / anion diffusion along the strain gradient.
[0056] Figure 3 The working mechanism of the mechanical ionic current generator is shown. The strain gradient in the hydrogel layer causes Cl- (Blue) + (red) higher diffusion rate shift. On the other hand, ACC in the working electrode has a higher diffusion rate shift to Li + Cation ratio to Cl - Stronger adsorption of anions leads to enhanced separation of charges. The enlarged image shows the electrode-ion interaction at the ACC / hydrogel interface. Due to the different diffusion rates of cations and anions, a net ionic current will be generated inside the hydrogel and therefore a current will be generated through the external circuit.
[0057] Figures 4A to 4C The short-circuit current I generated by the mechanical ionic current generator is shown respectively. SC , open circuit voltage V OC The timing distribution curve of the applied pressure P. As shown in the figure, the current generator outputs a large current pulse under compression deformation. The current can be as high as 4mA (5.5A m) at a pressure of 80kPa. -2 ), where the transferred charge is 916 mC m -2 , three to five orders of magnitude greater than existing devices (Table 1), reaching the threshold for direct electrical stimulation of muscles.
[0058] Table 1: Comparison with other mechanical-electrical energy conversions. #Drive method: Press and slide. #1: Pressure 50kPa; #2: Pressure 30kPa
[0059] The amount of charge transferred (Q) is calculated as follows Q=∫Idt (1) Where I is the current and t is the time. Prior to testing, the surfaces of the hydrogel and counter electrode were wiped dry.
[0060] Figure 5A and 5B The voltage and corresponding current and power density of the mechanical ionic current generator for various loads are shown.
[0061] The power density (P) is calculated as follows P=I 2 / (R×S) (2) where I, R, and S are the recorded current, loaded resistance, and area of the device, respectively.
[0062] like Figure 5A and 5B As shown, 475mW m is achieved with an external load of 122W. -2The maximum peak power density of 1.3 MW was obtained, indicating that the internal resistance of the hydrogel-based current generator is less than one thousandth of that of triboelectric or piezoelectric nanogenerators (TENG or PENG). Compared with the recently reported generators based on the piezoelectric effect, the presented hydrogel-based mechano-ionic current generator also shows significant improvements in current (4 mA vs. 1 μA) and power (475 mW m -2 For 0.85 μW cm -3 ) output.
[0063] By exploiting asymmetric surface functionalization of electrodes, mechano-ion generation can be significantly improved. Specifically, high current output is achieved by exploiting the synergistic effect between the differential ion adsorption properties of the electrodes and the differential ion diffusion in the hydrogel matrix. - Anions and Li + The difference in the diffusivity of cations can be enhanced in PVA hydrogels. + The configuration of anchoring the ACC electrode and interfacing with the high strain region can further reduce the Li + The diffusion flux increases, thereby enhancing the generation of ionic current.
[0064] A set of controlled experiments demonstrates these effects well. Figure 6 , two generators with symmetric electrode pairs (using two CC or ACC electrodes) were measured for comparison, both showing current generation but with much smaller peaks. On the other hand, if the ACC working electrode and CC counter electrode are reversed, very little current generation is observed, since the ion anchoring effect is flipped and offset by the differential diffusion of cations and anions.
[0065] Figure 7 The current output of the optimized electrode layout CC-ACC at various activation times of the ACC electrode is shown. As shown, the current increases with the duration of electrochemical oxidation of the ACC working electrode.
[0066] In order to confirm the use of Li + The role of the anchored oxygen-containing functional groups was investigated by density functional theory (DFT) calculations on the charge redistribution when CC and ACC were in contact with electrolytes. Figure 8 Shown in CC / Li + / H2O system and ACC / Li + / H2O system. For CC / Li + / H2O system, the charge redistribution process mainly occurs between H2O molecules and CC; while for ACC / Li + / H2O system, obviously Li +The adsorption energy of LiCl on ACC (1.2 eV) is higher than that on CC (0.18 eV).
[0067] Fig. 9 The calculated adsorption energies of various species on the electrode counter electrode materials are shown. For ACC, the calculated Li + and Cl - The adsorption energies of Li and ACC are 2.515 eV and -0.384 eV, respectively. These results indicate that when ACC is in contact with the hydrogel, Li + Cations tend to accumulate at the ACC-hydrogel interface, while Cl - Anions tend to remain away from the interface.
[0068] In some embodiments, the top working electrode can be changed from ACC to a gold (Au) film or stainless steel foil. Oxygen plasma treatment is applied to these metal electrodes to introduce oxygen-containing groups on the surface.
[0069] In a typical fabrication process of PI / Au electrodes, a piece of PI film (thickness: 50 μm) was cleaned with acetone, IPA and DI water, and then a double layer of chromium (Cr, 5 nm) and gold (Au, 200 nm) was sputtered (Denton desktop professional sputtering system) on the PI film.
[0070] In a typical manufacturing process for steel electrodes, a piece of stainless steel foil (50 μm) was cleaned with sandpaper (7000 grit), acetone, IPA, and DI water.
[0071] Oxygen plasma treatment (40 sccm oxygen gas flow, 100 W, and 30 seconds) was performed by RIE etcher (Tailong Electronics). Fig. 10A and 10B The contact angles of the steel foil before (91°) and after (32°) plasma treatment are shown, respectively. The lower contact angle after plasma treatment indicates the introduction of oxygen-containing functional groups.
[0072] Fig.11A Shown are the response currents of various devices as a function of applied pressure using steel foil as the working electrode. Fig. 11B Schematic images of the corresponding device configurations are shown. After plasma treatment, the output current increased significantly in both cases. This result is consistent with the results when ACC and CC were used as working electrodes. Figure 6 The results mentioned above are in good agreement, showing the importance of oxygen-containing functional groups.
[0073] Fig. 12A Schematic diagram showing the response current as a function of applied pressure and the corresponding configuration for various devices using PI / Au as the working electrode. Fig. 12BA schematic image showing the corresponding device configuration is shown. Fig. 12A and 12B , the huge difference in the response current before and after plasma treatment also shows that oxygen-containing functional groups are extremely important. At the same time, the difference between the yellow line and the red line proves that the engineered pyramid structure also plays a key role in improving the current. The PI / Au film was chosen because it is extremely flat and clean, which can significantly reduce the impact of undesirable surface deformation of the hydrogel. The value of the blue line is below zero. The possible reason is that when using a carbon electrode, due to the cation-π interaction, the cation can be preferably adsorbed on the anion, which is in contrast to the metal-electrolyte interface, where there is no cation-π interaction and anion adsorption can dominate. 3 . Therefore, the direction of the current is reversed.
[0074] Therefore, it is clear that the surface functionalization of the working electrode with sufficient oxygen-containing groups can be due to Li + The current output is greatly enhanced by the anchoring effect of the activated carbon cloth. The selective adsorption triggers the separation of anions and cations at the surface between the activated carbon cloth and the hydrogel. Increasing the asymmetry of the diffusion flux can effectively improve the efficiency. In addition, improving the selective ion adsorption by matching the electrolyte and the electrode can further improve the response current.
[0075] Another set of control experiments further demonstrated the importance of selective ion adsorption for the generation of mechanoionic currents. Specifically, the surface functionalization of the ACC working electrode was modified to enable anion adsorption by treatment with polyethyleneimine (PEI), a typical cationic polymer, which is contrary to its optimal design.
[0076] Before the measurement, a piece of ACC was cleaned and then immersed in a 25wt% polyethyleneimine (PEI) solution (600MW, Aladdin). During the 24-hour immersion, PEI with positively charged groups was adsorbed onto the surface of ACC. The ACC modified by PEI, i.e., ACC-PEI, was then dried in an oven at 85°C to complete.
[0077] After the measurement, the PEI-modified ACC electrode was rinsed with DI water for 2 minutes and dried again. This step was intended to reduce the content of PEI. After this, the electrode was tested again. The ACC was then immersed in DI water at 85°C for 2 days to remove most of the adsorbed PEI. The manufactured ACC was tested after drying.
[0078] Fig.13 Shown is a schematic representation of the process of polyethyleneimine (PEI, a typical cationic polymer) treatment of ACC, which modifies the ion adsorption properties of ACC. Fig.14Different current outputs of the device under different treatments of the ACC working electrode are shown.
[0079] ACC-PEI electrodes were prepared by applying PEI on the surface of ACC by immersing ACC in a 25wt% PEI solution and drying it in an oven. It was observed that the current direction was reversed when the working electrode was changed from ACC to ACC-PEI. When ACC was used as the working electrode and 1M LiCl hydrogel was used as the electrolyte in the optimal configuration, a positive peak current of 1.051mA was obtained at a pressure of 12kPa. However, when ACC-PEI was used as the working electrode, the output changed to an opposite current of -0.111mA. Subsequently, ACC-PEI was rinsed with DI water for 2 minutes to partially remove PEI and dried again to reduce the PEI content. The response current returned to positive with a small value of 0.0349mA. Further reduction of the PEI content by rinsing ACC-PEI in DI water for 2 days restored the response current back to 0.722mA. A small amount of PEI residue on ACC resulted in a slight decrease in the current compared to the initial value.
[0080] The changes in PEI content in each step were characterized by Fourier transform infrared (FTIR) spectroscopy. Fig.15 Shown are FTIR spectra of ACC at four stages during the PEI modification process. Fig.16 A magnified FTIR spectrum image is shown, showing that there is still a small amount of residual PEI on the surface of ACC even after rinsing for 2 days. As a typical cationic polymer with a strong positive surface charge, PEI easily adsorbs negative ions and repels positive ions. Due to sufficient negatively charged groups, PEI can be adsorbed on the surface of ACC. In this way, the surface charge state changes from negative to positive, thereby giving it the ability to adsorb anions.
[0081] For ν(NH) at 3250cm -1 And for ν(CH) at 2925cm -1 and 2830cm -1 The peak is identified as the characteristic peak of PEI. The change of the intensity of these peaks indicates the gradual removal of successful upgrading and PEI. These results indicate that the anion adsorption superiority of ACC-PEI working electrode can overwhelm the net anion flux caused by strain gradient, and cause the positive and negative sign of the reversal of net cation flux. In this regard, the mechanical ion action can be well adjusted by the asymmetric chemical functionalization of suitably designed electrode, which is convenient for different device applications.
[0082] The performance of these mechano-ionic hydrogel-based current generators was further characterized in the context of practical applications.The optimized electrode layout (ACC as working electrode and CC as counter electrode) was used for all subsequent tests.
[0083] First, the effects of ion concentration and applied pressure on the current output are investigated. Fig.17 Peak short-circuit current as a function of applied pressure is shown, where the hydrogels are soaked with different electrolytes: DI water (grey), 1M LiCl (blue) and 4M LiCl (red). No current signal was observed at any pressure when the DI water-based hydrogel served as the electrolyte. When the hydrogel with 1M LiCl was used, the response current rose significantly from 0mA to 3.3mA as the pressure increased from 0kPa to 88kPa. A higher current output was obtained using a hydrogel with 4M LiCl. The current increased as the pressure increased, but reached a saturation of about 4mA at about 60kPa.
[0084] Next, the effect of the recovery time between cycles and the strain rate on the current generation was investigated. -1 Loading rate (strain rate: 2s -1 ), the response current increases as the recovery time extends from 1 s to 8 s (frequency: 1 Hz to 0.125 Hz), and remains constant when the recovery time exceeds 8 s.
[0085] Fig.18 Peak current and charge delivered per cycle are shown as a function of recovery time between cycles. Fig.19 The output current at various recovery times is shown. Longer recovery times (lower frequencies) generate steadier and higher currents, which can be attributed to the transient distribution of ions.
[0086] This phenomenon can be explained by the inability of the ions to restore their initial uniform distribution within a short recovery time, resulting in a gradual decrease in current at higher frequencies. The charge transferred per press-release cycle shows the same trend. Even if the recovery time is shortened to 1 second, the amount of charge transferred is at most 180 μC per cycle.
[0087] Higher strain rates lead to higher peak currents. After the external pressure is removed, it takes some time for the ions to return to their initial distribution state. Higher strain rates generate more significant deformations of the hydrogel in a short period of time, leading to higher concentration gradients and therefore higher output currents. At the same time, higher strain rates shorten the period of ion redistribution and result in a lower amount of charge transferred per cycle.
[0088] Fig. 20 Peak current and charge delivered per cycle are shown as a function of strain rate. Fig.21The output current at various strain rates is shown. When the recovery time is fixed at 10.4 seconds, the strain rate is increased from 2 mm s -1 Change to 30mm s -1 , where the corresponding peak current increases from 0.4 mA to 2.9 mA. Higher strain rates lead to higher gradients in ion concentration due to the finite response time of ion redistribution, thus enhancing the differential ion diffusion flux. On the other hand, higher strain rates shorten the duration of current output, thereby reducing the charge delivered per cycle. At 2 mm s -1 The charge transferred per cycle was 668 μC (916 mC m -2 ), which outperforms reported electromechanical energy converters. Benefiting from the high capacity of charge transfer, the hydrogel-based current generator can quickly charge the capacitor.
[0089] Fig. 22 Figure 2 shows the charging profile of a 2 F capacitor charged by a hydrogel-based current generator. Fig. 22 As shown in Figure 1, a 2 F capacitor can be charged to 29 mV in 350 s, with a charge rate of up to 166 μC s -1 .
[0090] Fig.23 The voltage of a 2 F capacitor is shown during charging of the 2 F capacitor by an electrochemical workstation. To simulate the current pulses generated by the device, the charging parameters were set as follows: 4 mA for 0.5 seconds, 1 mA for 1 second, and 0 mA for 2 seconds. Voltage fluctuations were observed, such as Fig. 22 As mentioned in , this can be attributed to the effect of the internal resistance of the capacitor.
[0091] The fluctuation of current during the cycle is similar to what happens when a capacitor is charged using a potentiometer ( Fig.23 Together with a power management system, the hydrogel-based current generator can harvest mechanical energy and charge a 2F capacitor, which then powers an LED, thermometer, and LCD display ( Fig.24 ). Insoles integrated with hydrogel-based current generators are designed to harvest mechanical energy from walking and store charge in capacitors ( Fig.24 ).
[0092] Furthermore, the hydrogel-based current generator has outstanding durability, showing no significant output degradation over 7,500 compression cycles ( Fig.25 ). This durability comes from the excellent elasticity of the device during loading cycles. Fig.26 The pressure-distance curves for the 1st and 500th compression-disconnection cycles are shown. The highly overlapping curves indicate the mechanical stability of the device.
[0093] The device can also be scaled up. Fig.27A The pressure-response characteristics of a large-scale device are shown, where the device area is increased to 29 cm 2 . A peak current of nearly 13mA is achieved. Fig.27B Shown are the current and voltage when the large-scale device is loaded with different resistances. Fig.27C The power density of a large-scale device is shown as a function of external resistance. The change in area can explain the reduction in internal resistance.
[0094] exist Figures 27A to 27C The change in area can explain the reduction in internal resistance. Since the thickness and composition of this large-scale device are similar to the original device (with 7.29 cm 2 device area), it is reasonable to assume the same resistivity for both. This is close to the measured value of 32Ω.
[0095] Fig.28 The current signal when a 122Ω resistor is loaded at low and high humidity is shown, showing that the electrical output is insensitive to external humidity. It can be seen that the device can maintain a stable output even in a high humidity environment, which is difficult for a triboelectric nanogenerator.
[0096] Additionally, due to the physical cross-linking of PVA, the hydrogel portion can be recycled for disposal. Fig.29 Figure 2 shows the recycling process of CC-PVA electrodes. Placing the counter electrode in hot water can dissolve the physically cross-linked PVA hydrogel, thereby recycling the carbon cloth and PVA.
[0097] Compared with the state-of-the-art electromechanical energy converters including semiconductor direct current triboelectric nanogenerator (SDC-TENG), magnetoelastic generator (MEG), TENG and PENG, this mechano-ionic hydrogel-based current generator is advantageous in terms of internal resistance, current density, transferred charge density and device softness ( Fig.30 and Table 1).
[0098] Fig.31 The current output of this hydrogel-based current generator under various frequencies of mechanical input is shown compared with TENG and EMG. The test parameters are listed in Table 2. Compared with EMG and TENG, the hydrogel-based current generator is particularly suitable for collecting extremely low-frequency mechanical energy, and the current output increases as the frequency decreases. In addition, considering the mechanical softness and biocompatibility of the hydrogel-based current generator, it is promising for application in soft robotics and biomedical devices.
[0099] Table 2: Parameters used in testing and demonstration -: Variable or not applicable. Recovery time: The time interval between pressure peaks in two cycles.
[0100] To demonstrate its utility in biomedical applications, the hydrogel-based electric current generator was used as a power source for an integrated drug release system. Fig.32 Schematic diagram showing the drug loading process with electrodeposition. A polypyrrole (PPy) layer doped with dopamine and antibiotic (cefazolin sodium) was electrodeposited onto carbon cloth ( Fig.33A and 33B ).like Fig.34 As shown in , a two-electrode system was used, in which the drug-loaded carbon cloth was the working electrode, the Pt foil was the counter electrode, and 10 ml of PBS buffer was the electrolyte. Under periodic tapping, the generated current transformed PPy from an oxidized state to a reduced state, thereby releasing negatively charged cefazolin from PPy into the PBS solution.
[0101] The concentration of the drug was calibrated by UV-VIS spectroscopy, and a series of PBS buffers contained different concentrations of the drug (cefazolin sodium). The UV-Vis spectrometer defines the relationship between absorbance at 272nm and drug concentration, which is the characteristic absorbance band of cefazolin sodium. Therefore, a standard calibration curve for cefazolin sodium was drawn ( Fig.35 ), where R 2 =0.99797.
[0102] Due to the high current output of the generator, the drug release rate was much higher when the device was tapped than when it was not tapped ( Fig.36 ), indicating a design for electromechanical controlled release of drugs.
[0103] The integrated drug release system was further integrated with Ag / AgCl electrodes to form a drug release pad. In other words, the drug release pad included a three-electrode system, which was constructed with a clean CC, Pt electrode and Ag / AgCl electrode, acting as a working electrode, a counter electrode and a reference electrode, respectively. A constant voltage of 0.8V was applied to the system for 300 seconds, wherein the electrolyte solution contained 0.1M pyrrole, 0.01M dopamine hydrochloride and 0.01M cefazolin sodium. After that, a layer of chloride-doped polypyrrole was deposited via electrodeposition (0.8V, 60 seconds) to slow down the natural release of the drug (the electrolyte contained 0.1M pyrrole, 0.01M dopamine hydrochloride and 0.1M sodium chloride). The prepared pad was immersed in PBS buffer and DI water to remove residual reagents.
[0104] The drug release liner was further demonstrated in in vivo applications as a self-powered antimicrobial drug patch (SDP) with sustained release of antibiotics, which can be used for the treatment of wound infections.
[0105] Fig.37 Schematic diagram of SDP is shown. As shown in the figure, SDP includes substrate 210, cover liner 230 and drug release liner 220 arranged between substrate 210 and cover liner 230.
[0106] The cover gasket 230 may contain a PBS solution serving as an electrolyte.
[0107] The drug release liner 220 comprises a drug-loaded layer 221 , a printed circuit 222 , and a mechanical ion current generator 223 .
[0108] The drug loaded layer 221 is a layer of polypyrrole (PPy) electrodeposited onto carbon cloth and doped with dopamine and antibiotics. The printed circuit is an Ag / AgCl printed circuit.
[0109] The mechanical ionic current generator 223 includes a working electrode 2231 made of activated carbon cloth (ACC), and a counter electrode 2232 made of carbon cloth (CC) and PVA hydrogel.
[0110] The opposing electrode 2232 can have an arcuate CC-PVA structure, which can be manufactured by the following steps: obtaining a flattened CC-PVA electrode by casting a PVA solution onto a carbon cloth and freezing; after the first freeze-thaw cycle, placing the CC-PVA electrode in a beaker to introduce bending deformation; and applying another three freeze-thaw cycles to manufacture the arcuate CC-PVA electrode.
[0111] The SDP can be manufactured by the following steps: preparing a substrate (e.g., a first aid bandage); printing an Ag / AgCl circuit by applying a layer of Ag / AgCl ink on a central cotton pad using a mask; annealing the printed Ag / AgCl circuit; placing the mechanical ion current generator 230, the drug release liner 220, and the cover cotton pad 210 layer by layer on the substrate. Finally, the cover cotton pad is fixed with a waterproof medical tape.
[0112] Fig.38A A schematic diagram showing the application of SDP on the dorsal flank of a mouse is shown. A wound incision was created below the indicated area. Fig.38B A schematic image showing the working mechanism of the developed SDP is shown. Fig.39 The equivalent circuit of the SDP is shown. The current flows from the ACC electrode, through the Ag / AgCl circuit, the cotton pad containing PBS and the drug-loaded pad CC-CZ, and back to the CC electrode.
[0113] exist Fig.38A and 38BIn the experiment, the soft and biocompatible components allowed the device to directly cover the wound. The movement of the mouse, including eating, breathing, etc., stretched the first aid bandage and caused it to flatten, deforming the bow-shaped hydrogel, thereby increasing the contact area with the working electrode. The carbon fibers of the carbon cloth triggered the uneven deformation of the PVA hydrogel, thereby generating current. The elastic bow-shaped PVA hydrogel recovered its shape after stress relaxation, resulting in the separation of ACC and PVA.
[0114] A piece of drug-loaded pad CC-CZ (1.2 cm×1.4 cm), a Pt electrode, and 10 mL of PBS buffer formed a two-electrode system. The Pt electrode was connected to a piece of ACC. The CC-CZ was fixed by a Pt clamp and connected to a CC-PVA electrode. Hand tapping of the ACC placed on the CC-PVA electrode generated a current pulse and released the drug. After 1 minute of tapping, 2 mL of PBS buffer was moved to a quartz cuvette and tested by a UV-Vis spectrometer. The PBS buffer was then poured back into the two-electrode system and kept for 5 minutes before the next test. This process was repeated 4 times.
[0115] After anesthesia (pentobarbital, 1.5 mg / 100 g, intraperitoneal injection), an electric shaver and hair removal cream were applied to shave the hair from the dorsal area of the mice. Two symmetrical skin incisions were made on both sides of each mouse. 7 CFU mL -1 Wounds were infected with 200 μL of Staphylococcus aureus (S. aureus) at an initial density of . After that, all wounds were covered with a transparent waterproof wound dressing bandage (Nexcare, 3M). Mice were kept in cages overnight.
[0116] The initial area of the wound was recorded on the same day after surgery. After anesthesia, a camera (EOS R5, Canon) was used to record the area of the wound. The wound on one side of the mouse was subsequently covered with a self-powered antibacterial first aid bandage. Before use, the upper cotton pad was moistened with sterile PBS buffer. Another wound was covered with a normal first aid bandage. This process was repeated every two days until the ninth day. The area of the wound was measured using ImageJ software. After the experiment, the mice were euthanized by carbon dioxide asphyxiation.
[0117] Fig.40 The relative area of the wound as a function of healing time is shown. On the last day, the wound area covered by the normal patch and SDP was reduced to 32% and 11% of the initial wound area, respectively. Fig.41 Photographs of wounds during the healing process with a standard patch (upper) and SDP (lower) are shown.
[0118] The functional units and modules of the hydrogel-based current generator according to the embodiments disclosed herein can be implemented using a computing device, a computer processor or an electronic circuit system, including but not limited to an application specific integrated circuit (ASIC), a field programmable gate array (FPGA), a microcontroller, and other programmable logic devices configured or programmed according to the teachings of the present disclosure. The computer instructions or software codes running in the computing device, computer processor or programmable logic device can be easily made by practitioners in the field of software or electronic technology based on the teachings of the present disclosure.
[0119] All or part of the method according to the embodiment may be executed in one or more computing devices including a server computer, a personal computer, a laptop computer, a mobile computing device (eg, a smart phone), and a tablet computer.
[0120] Embodiments may include computer storage media, transient and non-transitory memory devices having stored therein computer instructions or software codes that may be used to program or configure a computing device, a computer processor, or an electronic circuit system to perform any of the processes of the present invention. Storage media, transient and non-transitory memory devices may include, but are not limited to, floppy disks, optical disks, Blu-ray disks, DVDs, CD-ROMs and magneto-optical disks, ROMs, RAMs, flash memory devices, or any type of medium or device suitable for storing instructions, codes, and / or data.
[0121] Each of the functional units and modules according to various embodiments may also be implemented in a distributed computing environment and / or a cloud computing environment, where all or part of the machine instructions are executed in a distributed manner by one or more processing devices interconnected by a communication network, such as an intranet, a wide area network (WAN), a local area network (LAN), the Internet, and other forms of data transmission media.
[0122] The foregoing description of the present invention has been provided for the purpose of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed. Many modifications and variations will be apparent to those skilled in the art.
[0123] The embodiment was chosen and described in order to best explain the principles of the invention and its practical application, thereby enabling others skilled in the art to understand the invention for various embodiments and with various modifications as are suited to the particular use contemplated.
Claims
1. A mechanical ion current generator, characterized in that: include: a working electrode comprising an activated carbon cloth; and a counter electrode comprising pristine carbon cloth and hydrogel; The hydrogel has multiple flexible and asymmetric structures; and The working electrode has a surface immersed in the hydrogel and provided with a plurality of oxygen-containing functional groups.
2. The mechanical ion current generator according to claim 1, characterized in that: The plurality of oxygen-containing functional groups are configured to face tip portions of the plurality of flexible and asymmetrically shaped structures.
3. The mechanical ion current generator according to claim 1, characterized in that: Each of the flexible and asymmetrically shaped structures has a pyramid-like shape.
4. The mechanical ion current generator according to claim 1, characterized in that: The hydrogel is loaded with mobile ions.
5. The mechanical ion current generator according to claim 1, characterized in that: The mobile ions include Li + Ions and Cl - ion.
6. A method for manufacturing a mechanical ion current generator, the mechanical ion current generator comprising a working electrode made of activated carbon cloth, and an opposing electrode made of carbon cloth and hydrogel, characterized in that: The method comprises: The working electrode was prepared by the following operations: Clean a piece of carbon cloth; oxidizing the cleaned carbon cloth in a two-electrode system containing an aqueous solution of (NH4)2SO4; and Reducing the oxidized carbon cloth in a three-electrode system containing an aqueous solution of NH4Cl to form the working electrode; and The counter electrode is prepared by the following operations: pouring the first PVA solution into a mold to obtain a molded PVA; repeatedly freezing and thawing the molded PVA to obtain a cross-linked hydrogel; immersing a cleaned carbon cloth into a second PVA solution to obtain a PVA-soaked carbon cloth; placing the PVA-soaked carbon cloth onto the rear side of the cross-linked hydrogel to obtain a combined structure; repeatedly freezing and thawing the combined structure to obtain a combined electrode; and The combined electrode was kept in the electrolyte solution for 1 day to load the combined electrode with mobile ions to form the counter electrode.
7. The method according to claim 6, characterized in that The (NH4)2SO4 aqueous solution has a concentration of 0.1M, and the NH4Cl aqueous solution has a concentration of 1M.
8. The method according to claim 6, characterized in that The freezing and thawing steps included freezing the molded PVA at -18°C for 8 hours and thawing the frozen PVA at 25°C for 3 hours.
9. The method according to claim 6, characterized in that The first PVA solution is a 15 wt % PVA solution and the second PVA solution is a 10 wt % PVA solution.
10. A mechanical ion self-powered drug release patch, characterized in that: include: substrate; A liner containing an electrolyte; as well as a drug release liner disposed between the electrolyte-containing liner and the substrate, The drug release liner comprises: a drug-loaded layer having a surface in contact with the electrolyte-containing liner; a printed circuit in contact with the drug-loaded layer; and The mechanical ionic current generator of claim 1, wherein the working electrode is electrically connected to the electrolyte-containing pad through the printed circuit, and the counter electrode is electrically connected to the drug-loaded layer.
11. The mechanical ion self-powered drug release patch according to claim 10, characterized in that: The plurality of oxygen-containing functional groups are configured to face tip portions of the plurality of flexible and asymmetrically shaped structures.
12. The mechanical ion self-powered drug release patch according to claim 10, characterized in that: Each of the flexible and asymmetrically shaped structures has a pyramid-like shape.
13. The mechanical ion self-powered drug release patch according to claim 10, characterized in that: The hydrogel is loaded with mobile ions.
14. The mechanical ion self-powered drug release patch according to claim 13, characterized in that: The mobile ions include Li + Ions and Cl - ion.
15. The mechanical ion self-powered drug release patch according to claim 10, characterized in that: The counter electrode has an arcuate structure.
16. The mechanical ion self-powered drug release patch according to claim 10, characterized in that: The cover pad is a cotton pad containing PBS solution.
17. The mechanical ion self-powered drug release patch according to claim 10, characterized in that: The drug-loaded layer is a polypyrrole (PPy) layer electrodeposited onto carbon cloth and doped with dopamine and antibiotics.
18. The mechanical ion self-powered drug release patch according to claim 10, characterized in that: The printed circuit is an Ag / AgCl printed circuit.