Preparation method of polydimethylsiloxane elastomer with oil permeation resistant coating
By forming a flexible molecular brush on the surface activation and grafting reaction of the polydimethylsiloxane elastomer, the problem of mechanical properties and transparency loss when the oil-resistant penetration performance of PDMS elastomers is improved in the prior art. Excellent anti-oil penetration and liquid repellency properties are achieved.
Patent Information
- Application Number
- CN202411386150.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-30
AI Technical Summary
The prior art often destroys its mechanical properties and optical transparency when improving the oil permeability of polydimethylsiloxane (PDMS) elastomers.
By surfactant treatment of the clean and dry polydimethylsiloxane elastomer, active functional groups are formed, and non-contact or contact grafting reaction is adopted to form flexible molecular brushes, fill nanopores and form them. Space barriers enhance their oil penetration resistance.
On the basis of not damaging the mechanical properties and optical transparency of the PDMS elastomer, it significantly improves its oil permeability and liquid repellency, solving the problem of performance losses in the prior art.
Smart Images

Figure CN119081205A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polydimethylsiloxane surface modification, and relates to a method for preparing a polydimethylsiloxane elastomer with an oil-penetration-resistant coating. Background Art
[0002] Polydimethylsiloxane (PDMS) is one of the most important silicone polymers ever, with different applications in many fields. The Si-O-Si bond of the siloxane backbone of PDMS has an extremely low torsion barrier, and the weak intermolecular interaction of the methyl groups on both sides makes the PDMS molecular chain highly flexible. After chemical cross-linking, the chain PDMS molecules will be transformed into an elastomeric material with an adjustable Young's modulus. Due to its excellent optical transparency, temperature and weather resistance, and biocompatibility, PDMS elastomers are widely used in various fields. For example, PDMS can be used as a mold resin for soft lithography to prepare microfluidic devices; PDMS elastomers can be used as an insulating layer for wearable electronic products to protect complex circuits from environmental pressure; PDMS elastomers can be used as biocompatible contact matrices in the food and medical fields, and are used in Class II or Class III medical tubes for extracorporeal circulation in aqueous cerebrospinal shunts, cardiac surgery, and pacemaker leads. For another example, the high dissociation energy of the Si-O bond in PDMS (444KJ / mol) allows it to be used as a sealing material to seal components used in extreme environments.
[0003] Although PDMS elastomers are widely used in science and industry, due to their porous network structure, when they come into contact with non-polar liquids, especially hydrocarbons (such as oil), small liquid molecules will penetrate into the PDMS elastomer, causing the PDMS elastomer to swell and deform, seriously affecting the performance of the PDMS elastomer components. For example, this will make organic synthesis in microchannels unfeasible, reduce the sensing accuracy of encapsulated flexible sensors, cause contamination of implanted medical devices, and lead to elastic failure of mechanical seals. At present, strategies to improve the anti-permeation performance of PDMS elastomers are mainly divided into two categories: bulk modification and surface functionalization. Bulk modification includes vulcanization (see MMKim, Y.Huang, K.Choi et al.Microelectron.Eng. (2014)), compatibilization (see HWu, XZhang, DXu et al.J.Membr.Sci. (2009)), blending (see BKaur, SKumar, TMondal et al.ACS Omega (2020)), etc. Surface functionalization usually involves setting a solvent-resistant solid coating on the surface of the PDMS elastomer (see ARAbate, D.Lee, T.Do et al.LabChip (2008)). Although these methods can enhance the resistance of PDMS elastomers to non-polar liquids, they will inevitably destroy the excellent mechanical properties and optical transparency of the PDMS elastomer itself. PDMS elastomers are used everywhere in daily life, scientific research and industry. Improving the oil penetration resistance of PDMS elastomers without changing their unique properties such as mechanical properties and optical transparency will be of great significance to further expand their application scope. Summary of the invention
[0004] In view of the problem that the mechanical properties and optical transparency of PDMS elastomers will be destroyed when the prior art adopts bulk modification and surface functionalization strategies to improve the anti-penetration performance of PDMS elastomers, the present invention provides a method for preparing a polydimethylsiloxane elastomer with an oil-resistant penetration coating, which imparts excellent oil-resistant penetration performance and improves its liquid-repellent ability without destroying the mechanical properties and optical transparency of the polydimethylsiloxane elastomer by filling the nanopores of the polydimethylsiloxane elastomer with a synergistic effect of spatial barriers and molecular brush-like liquid properties.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:
[0006] A method for preparing a polydimethylsiloxane elastomer having an oil-penetration-resistant coating comprises the following steps:
[0007] (1) treating a clean and dry polydimethylsiloxane elastomer with oxygen plasma for surface activation to obtain an activated polydimethylsiloxane elastomer substrate;
[0008] (2) grafting the active end-capped silane onto the surface of an activated polydimethylsiloxane elastomer substrate to form a flexible molecular brush on the surface of the activated polydimethylsiloxane elastomer substrate to obtain a polydimethylsiloxane elastomer having an oil-resistant penetration coating;
[0009] The active end-group-terminated silane is an active end-group-terminated silane monomer or an active group-terminated silane polymer; during the grafting reaction, the active end-group-terminated silane monomer will polymerize to form a polydimethylsiloxane flexible molecular chain and grafted onto the surface of an activated polydimethylsiloxane elastomer substrate, and the silane polymer chain of the active group-terminated silane polymer is directly grafted onto the surface of an activated polydimethylsiloxane elastomer substrate.
[0010] In the above technical solution, the active end-group terminated silane monomer is active end-group terminated tetramethyldisiloxane, and the active group terminated silane polymer is active end-group terminated polydimethylsiloxane or active end-group terminated perfluoropolyether silane.
[0011] In the above technical solution, the active end groups in the active end group-terminated silane include at least one of a chlorine end group, a hydroxyl group, a carboxyl group, an amino group, an alkoxy group, an epoxy group, and an isocyanate group.
[0012] In the above technical solution, the molecular weight of the active end-group terminated silane is 203 to 100,000 g / mol.
[0013] Furthermore, in the above technical solution, when the molecular weight of the active terminal silane is less than 10000 g / mol, the grafting reaction is carried out in step (2) by a non-contact method, and when the molecular weight of the active terminal silane is greater than or equal to 10000 g / mol, the grafting reaction is carried out by a contact method.
[0014] In the above technical scheme, the operation of step (2) in which the grafting reaction is carried out in a non-contact manner is as follows: adding the active end-group-capped silane into a container, fixing the activated polydimethylsiloxane elastomer substrate in the container to avoid direct contact between the activated polydimethylsiloxane elastomer substrate and the liquid active end-group-capped silane, sealing the container to allow the active end-group-capped silane molecules to evaporate and undergo a grafting reaction with the surface of the activated polydimethylsiloxane elastomer substrate, then taking out, rinsing with deionized water, and drying to obtain a polydimethylsiloxane elastomer with an oil-resistant penetration coating.
[0015] In the above technical scheme, the operation of the contact grafting reaction in step (2) is as follows: the active end-group-capped silane is applied to the surface of the activated polydimethylsiloxane elastomer substrate, and the substrate is placed in a sealed container to allow the active end-group-capped silane to undergo a grafting reaction with the surface of the activated polydimethylsiloxane elastomer substrate, and then the substrate is taken out, rinsed with water, and dried to obtain a polydimethylsiloxane elastomer with an oil-resistant penetration coating.
[0016] In the above technical solution, when step (2) adopts a non-contact method to carry out the grafting reaction, the amount of each 1 cm 2 Add the active end-capped silane to the container in a ratio of 2 to 50 μL of the active end-capped silane to the bottom area of the container.
[0017] In the above technical solution, when step (2) adopts a contact grafting reaction, the active end-group-capped silane is applied to the surface of the activated polydimethylsiloxane elastomer substrate to completely cover the area where the oil-proof penetration coating is to be formed. 2 The area of the activated polydimethylsiloxane elastomer substrate on which the oil penetration-resistant coating is to be formed is coated with 50 to 500 μL of the active end-group-capped silane, and the active end-group-capped silane is coated on the surface of the activated polydimethylsiloxane elastomer substrate.
[0018] In the above technical solution, during the grafting reaction in step (2), the pressure in the container is controlled not to exceed 1013.25 mbar.
[0019] In the above technical solution, during the grafting reaction process of step (2), the temperature in the container is preferably controlled to be 10-100° C., and the grafting reaction time is preferably controlled to be 1-720 min.
[0020] In step (1) of the above technical solution, when the clean and dry polydimethylsiloxane elastomer is subjected to surface activation treatment with oxygen plasma, the surface activation treatment can be performed on a certain part of the surface of the clean and dry polydimethylsiloxane elastomer or on the entire surface, depending on the actual application requirements. The grafting reaction in step (2) mainly occurs at the site subjected to the surface activation treatment.
[0021] In the above technical solution, when the grafting reaction is carried out in a non-contact manner, in order to facilitate the active end-group-terminated silane molecules volatilized from the bottom of the container to fully contact with the surface of the activated polydimethylsiloxane elastomer substrate and undergo a grafting reaction, it is preferred that the activated polydimethylsiloxane elastomer substrate is suspended in the container. For example, a bracket may be placed in the container, or a hook may be provided in the container, and the activated polydimethylsiloxane elastomer substrate may be suspended in the air through the bracket or the hook.
[0022] In step (1) of the above technical solution, it is preferred to control the power of the oxygen plasma for surface activation treatment to be 10 to 1500 W and the time to be 10 s to 10 min.
[0023] In the above technical solution, the clean and dry polydimethylsiloxane elastomer is obtained by ultrasonically cleaning the polydimethylsiloxane elastomer with an organic solvent (such as ethanol) and water to remove organic pollutants and solid particles on the surface, and then drying. The drying method adopted can be compressed air purging, nitrogen and other non-reactive gas purging, inert gas purging and other drying methods, and can also be drying methods such as drying and natural air drying.
[0024] Compared with the prior art, the technical solution of the present invention can produce the following beneficial technical effects:
[0025] 1. The present invention provides a method for preparing a PDMS elastomer with an oil-resistant permeation coating. The method firstly performs surface activation treatment on a clean and dry PDMS elastomer with oxygen plasma to form a large number of active functional groups (such as hydroxyl groups) on the surface of the PDMS elastomer to facilitate subsequent grafting reactions. Then, a non-contact method or a contact method is used for grafting reactions to form a flexible molecular brush on the surface of the activated PDMS elastomer substrate to obtain a PDMS elastomer with an oil-resistant permeation coating. On the one hand, the flexible molecular brush grafted on the surface of the PDMS elastomer fills the nanopores on the surface of the PDMS elastomer and forms a spatial barrier. On the other hand, the flexible molecular brush grafted on the surface of the PDMS elastomer has good dynamic compliance, so that the oil-resistant permeation coating formed by the molecular brush has a fluidity similar to that of a liquid. These two reasons enable the method of the present invention to give the PDMS elastomer excellent oil-resistant permeation performance and improve its liquid-repelling ability without destroying the mechanical properties and optical transparency of the PDMS elastomer. The problem of destroying the mechanical properties and optical transparency of the PDMS elastomer in the prior art using bulk modification and surface functionalization strategies is solved.
[0026] 2. The method of the present invention is simple to operate. The PDMS elastomer can be endowed with excellent oil-resistant and liquid-repellent properties simply by adjusting the molecular structure of the surface of the PDMS elastomer. The requirements for instruments, reagents and process conditions are not high. The preparation of the PDMS elastomer with an oil-resistant coating can be completed under conventional operating conditions. It is easy to promote and apply under existing simple process conditions, which is conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1The present invention is a schematic diagram of the process of preparing a PDMS elastomer with an oil-resistant penetration coating by grafting reaction in a non-contact manner, in which 1-PDMS elastomer, 2-activated PDMS elastomer substrate, 3-active end-group-capped silane molecules, 4-liquid active end-group-capped silane, 5-container, 6-PDMS elastomer grafted with a flexible molecular brush.
[0028] Figure 2 These are optical images comparing the absorption of hexadecane by a blank PDMS elastomer and a PDMS elastomer with an oil-resistant coating prepared in Example 1 at different times.
[0029] Figure 3 The graph is a comparative test result of the absorption rate of hexadecane by a blank PDMS elastomer and a PDMS elastomer with an oil-resistant coating prepared in Example 1 at different times.
[0030] Figure 4 3 are stress-strain curves of a blank PDMS elastomer and a PDMS elastomer with an oil-resistant coating prepared in Example 1.
[0031] Figure 5 These are the transmittance spectrum test results of the blank PDMS elastomer and the PDMS elastomer with oil-resistant coating prepared in Example 1.
[0032] Figure 6 These are the contact angle hysteresis test results of water and hexadecane on the surface of a blank PDMS elastomer and the PDMS elastomer with an oil-resistant coating prepared in Example 1.
[0033] Figure 7 These are time series images of 20 μL water droplets and hexadecane droplets sliding on the surface of a blank PDMS elastomer and a PDMS elastomer with an oil-resistant coating prepared in Example 1. DETAILED DESCRIPTION
[0034] The following examples further illustrate the preparation method of the polydimethylsiloxane elastomer with an oil-resistant coating provided by the present invention. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention according to the above invention content and implement them specifically, which still falls within the scope of protection of the present invention.
[0035] In the following examples, the polydimethylsiloxane (PDMS) elastomer (Sylgard 184) was purchased from Dow Chemical Company, and other reagents were all commercially available products, which could be purchased directly from the market or customized by manufacturers.
[0036] Example 1
[0037] In this embodiment, a method for preparing a PDMS elastomer having an oil-penetration-resistant coating is provided, and the steps are as follows:
[0038] (1) Using ethanol (purity ≥ 99.7%) and deionized water, ultrasonically clean the sheet PDMS elastomer for 60 seconds to remove organic pollutants and solid particles on the surface of the PDMS elastomer, and then using compressed nitrogen to blow dry the surface of the PDMS elastomer for later use.
[0039] (2) The PDMS elastomer treated in step (1) is placed in a plasma cleaning machine, and the surface of the PDMS elastomer is activated by oxygen plasma. The power of the oxygen plasma treatment is controlled to be 50 W and the treatment time is controlled to be 30 s. In this step, only one surface of the PDMS elastomer is activated, and a large number of active functional groups including hydroxyl groups are formed on the activated surface to obtain an activated PDMS elastomer substrate.
[0040] (3) The grafting reaction is carried out in a non-contact manner, and the operation is as follows:
[0041] According to every 1cm 2 Add 4 μL of chlorine-terminated polydimethylsiloxane (molecular weight is about 3000 g / mol) to the bottom area of the container. Add chlorine-terminated polydimethylsiloxane into the glass container, stick the activated PDMS elastomer substrate to the top of the glass container, make the activated PDMS elastomer substrate face down after activation, avoid direct contact between the activated PDMS elastomer substrate and the liquid chlorine-terminated polydimethylsiloxane, seal the glass container, control the temperature in the glass container to 60° C. and the pressure to 1.33 mbar, and after the chlorine-terminated polydimethylsiloxane molecules volatilize, they contact with the surface of the activated PDMS elastomer substrate and undergo a grafting reaction. The grafting reaction time is controlled to be 60 min, and a flexible molecular brush is formed on the surface of the activated PDMS elastomer substrate, that is, a flexible molecular brush is formed on the surface of the activated PDMS elastomer substrate by vapor phase chemical deposition, and then taken out, rinsed with deionized water, and the surface is blown dry with compressed nitrogen to obtain a PDMS elastomer with an oil-resistant penetration coating.
[0042] Example 2
[0043] In this example, the performance of the PDMS elastomer with the oil-resistant coating prepared in Example 1 was tested.
[0044] (1) Take a number of PDMS elastomers (blank PDMS elastomers) used in Example 1 and a number of PDMS elastomers with an oil-resistant permeation coating prepared in Example 1, and drip 5 μL of hexadecane onto each blank PDMS elastomer and each PDMS elastomer with an oil-resistant permeation coating (drop onto the oil-resistant permeation coating), wipe off the residual hexadecane droplets on the surface at regular intervals, take photos with a digital camera, and record the diffusion of the hexadecane droplets on the blank PDMS elastomer and the PDMS elastomer with an oil-resistant permeation coating prepared in Example 1 at different diffusion times. The results are shown in FIG. Figure 2 As shown, Figure 2 “Before treatment” represents a blank PDMS elastomer, and “after treatment” represents the PDMS elastomer with an oil-resistant coating prepared in Example 1.
[0045] Depend on Figure 2 It can be seen that the hexadecane droplets will quickly diffuse into the internal network of the blank PDMS elastomer within the first 10 minutes and leave obvious swelling marks on the surface, corresponding to Figure 2 The "before treatment" group of pictures in the figure; after adding hexadecane to the oil-resistant penetration coating, no obvious traces were left on the surface after wiping off the residual hexadecane droplets on the surface during the 720-minute contact process, corresponding to Figure 2 The “after treatment” group of pictures in the figure illustrate that the oil-resistant penetration coating formed on the surface of the PDMS elastomer in Example 1 has excellent oil-resistant penetration performance.
[0046] (2) A blank PDMS elastomer and a PDMS elastomer with an oil-resistant coating prepared in Example 1 were taken as samples, and their oil-resistant performance was evaluated by measuring the absorption rate η of the samples to a hexadecane droplet. The absorption rate measurement steps were as follows:
[0047] ①Place the sample on the test platform of the contact angle measuring instrument;
[0048] ② Drop 5 μL of hexadecane on the sample surface. For the PDMS elastomer with an oil-resistant coating prepared in Example 1, drop hexadecane on the oil-resistant coating;
[0049] ③The built-in camera of the contact angle meter captures the cross-sectional image of the droplet at a certain interval;
[0050] ④ Use analysis software to extract w and θ data from the captured image. w is the contact width of the droplet on the surface, and θ is the contact angle of the droplet.
[0051] ⑤ Use the following formula to calculate the absorption rate η: η=(V0-V t ) / V0×100%, where V0 is the initial volume of the hexadecane droplet on the sample surface, V tis the residual volume of the hexadecane droplet on the sample surface after absorption time t. The entire hexadecane droplet is regarded as a spherical cap for volume calculation. The droplet volume (V) calculation formula is: V = πw 3 (2+cosθ)(1-cosθ) 2 / (24sin 3 θ).
[0052] The positions of the sample and the camera remained fixed throughout the measurement. To avoid evaporation of hexadecane, all experiments were performed at a constant room temperature of 20 °C. The measurements were performed three times and the average of the three measurements was taken. The measurement results are shown in Figure 3 As shown, Figure 3 “Before treatment” represents a blank PDMS elastomer, and “after treatment” represents the PDMS elastomer with an oil-resistant coating prepared in Example 1.
[0053] Depend on Figure 3 It can be seen that the PDMS elastomer with an anti-oil penetration coating on the surface has significantly better anti-oil penetration performance than the blank PDMS elastomer. For example, when hexadecane diffuses on the surface for 720 minutes, the absorption rate of hexadecane on the blank PDMS elastomer is as high as 20.8%, while the absorption rate on the PDMS elastomer with an anti-oil penetration coating is only 2.4%, and the absorption rate is reduced by 88.5%.
[0054] (3) Take a blank PDMS elastomer and a PDMS elastomer with an oil-resistant coating prepared in Example 1 as samples, and use a tensile testing machine to perform a tensile test on the samples to obtain a stress-strain curve, such as Figure 4 As shown, Figure 4 “Before treatment” represents a blank PDMS elastomer, and “after treatment” represents the PDMS elastomer with an oil-resistant coating prepared in Example 1.
[0055] Depend on Figure 4 It can be seen that the ultimate tensile strength of the blank PDMS elastomer and the PDMS elastomer with an oil-resistant penetration coating prepared in Example 1 is almost the same, which is 4.77MPa and 4.63MPa respectively. At the same time, the fracture strain of the two is the same, both of which are 140%. This shows that the oil-resistant penetration coating formed by grafting a flexible molecular brush on the surface of the PDMS elastomer will basically not cause damage to the mechanical properties of the PDMS elastomer. The elastic modulus of the blank PDMS elastomer and the PDMS elastomer with an oil-resistant penetration coating prepared in Example 1 are calculated to be 1.32MPa and 1.27MPa respectively, and the elastic modulus has only undergone a slight change of 3.8%, which also shows that the oil-resistant penetration coating formed by grafting a flexible molecular brush on the surface of the PDMS elastomer will basically not affect the macroscopic elasticity of the PDMS elastomer.
[0056] (4) A blank PDMS elastomer and a PDMS elastomer with an oil-resistant coating prepared in Example 1 were taken as samples, and the transmittance of the samples was tested using a spectrophotometer. The test results are as follows: Figure 5 As shown, Figure 5 “Before treatment” represents a blank PDMS elastomer, and “after treatment” represents the PDMS elastomer with an oil-resistant coating prepared in Example 1.
[0057] Depend on Figure 5 It can be seen that the transmittance of the blank PDMS elastomer and the PDMS elastomer with the oil-resistant coating prepared in Example 1 is basically the same, for example, the transmittance of the blank PDMS elastomer is 93.7% at 555nm, and the transmittance of the PDMS elastomer with the oil-resistant coating prepared in Example 1 is 93.6%. This indicates that the oil-resistant coating formed by grafting the flexible molecular brush on the surface of the PDMS elastomer will not affect the light transmittance of the PDMS elastomer.
[0058] (5) Take a blank PDMS elastomer and a PDMS elastomer with an oil-resistant coating prepared in Example 1 as samples, use water and hexadecane as probe liquids, and use a contact angle meter to measure the contact angle hysteresis of the sample surface. For the PDMS elastomer with an oil-resistant coating prepared in Example 1, it is necessary to drop the probe liquid on the oil-resistant coating for measurement. The measurement is performed 3 times, and the average value of the 3 measurements is taken. The measurement results are shown in FIG. Figure 6 As shown, Figure 6 “Before treatment” represents a blank PDMS elastomer, and “after treatment” represents the PDMS elastomer with an oil-resistant coating prepared in Example 1.
[0059] Depend on Figure 6 It can be seen that compared with the blank PDMS elastomer, the contact angle hysteresis values of water and hexadecane on the surface of the PDMS elastomer with an oil-resistant coating prepared in Example 1 are significantly reduced, the contact angle hysteresis value of water on the surface of the PDMS elastomer with an oil-resistant coating prepared in Example 1 is reduced from 37.9° to 10.5°, and the contact angle hysteresis value of hexadecane on the surface of the PDMS elastomer with an oil-resistant coating prepared in Example 1 is reduced from 15° to 3.1°, indicating that the oil-resistant coating formed by grafting a flexible molecular brush on the surface of the PDMS elastomer can improve the liquid repellency of the PDMS elastomer.
[0060] (6) Take a blank PDMS elastomer and a PDMS elastomer with an oil-resistant coating prepared in Example 1 as samples, and drip 20 μL of water and hexadecane on the sample surface respectively. For the PDMS elastomer with an oil-resistant coating prepared in Example 1, it is necessary to drip on the oil-resistant coating. Use a digital camera to record the time series images of water and hexadecane sliding on the inclined sample surface. The results are as follows: Figure 7 As shown, Figure 7 Figures (a) and (b) represent water and hexadecane, respectively. "Before treatment" represents a blank PDMS elastomer, and "after treatment" represents the PDMS elastomer with an oil-resistant coating prepared in Example 1.
[0061] Depend on Figure 7 It can be seen that compared with the blank PDMS elastomer, after the flexible molecular brush is grafted on the surface of the PDMS elastomer to form an oil-resistant penetration coating in Example 1, the liquid repellency of the PDMS elastomer is effectively improved, and water and hexadecane can be better repelled.
[0062] Example 3
[0063] In this embodiment, a method for preparing a PDMS elastomer having an oil-penetration-resistant coating is provided, and the steps are as follows:
[0064] (1) The PDMS elastomer was ultrasonically cleaned for 30 seconds using ethanol (purity ≥ 99.7%) and deionized water in sequence to remove organic pollutants and solid particles on the surface of the PDMS elastomer, and then the surface of the PDMS elastomer was blown dry using compressed nitrogen gas for later use.
[0065] (2) placing the PDMS elastomer treated in step (1) into a plasma cleaning machine, and performing surface activation treatment on the PDMS elastomer using oxygen plasma, wherein the power of the oxygen plasma treatment is controlled to be 300 W and the treatment time is controlled to be 10 min, thereby forming a large number of active functional groups including hydroxyl groups on the surface of the PDMS elastomer, thereby obtaining an activated PDMS elastomer substrate.
[0066] (3) The grafting reaction is carried out in a non-contact manner, and the operation is as follows:
[0067] According to every 1cm 2 Add 10 μL of chlorine-terminated polydimethylsiloxane (molecular weight is about 425 g / mol) to the bottom area of the container. Add chlorine-terminated polydimethylsiloxane into the glass container, suspend the activated PDMS elastomer substrate in the glass container to avoid direct contact between the activated PDMS elastomer substrate and the liquid chlorine-terminated polydimethylsiloxane, seal the glass container, control the temperature in the glass container to room temperature (20-25° C.) and the pressure to normal pressure (1013.25 mbar), and after the chlorine-terminated polydimethylsiloxane molecules volatilize, they contact with the surface of the activated PDMS elastomer substrate and undergo a grafting reaction. The grafting reaction time is controlled to be 5 minutes, and a flexible molecular brush is formed on the surface of the activated PDMS elastomer substrate. Then, take it out, rinse it with deionized water, and blow dry the surface with compressed nitrogen to obtain a PDMS elastomer with an oil-resistant penetration coating.
[0068] Example 4
[0069] In this embodiment, a method for preparing a PDMS elastomer having an oil-penetration-resistant coating is provided, and the steps are as follows:
[0070] (1) The PDMS elastomer was ultrasonically cleaned for 30 seconds using ethanol (purity ≥ 99.7%) and deionized water in sequence to remove organic pollutants and solid particles on the surface of the PDMS elastomer, and then the surface of the PDMS elastomer was blown dry using compressed nitrogen gas for later use.
[0071] (2) placing the PDMS elastomer treated in step (1) into a plasma cleaning machine, and performing surface activation treatment on the PDMS elastomer using oxygen plasma, wherein the power of the oxygen plasma treatment is controlled to be 1500 W and the treatment time is controlled to be 10 s, thereby forming a large number of active functional groups including hydroxyl groups on the surface of the PDMS elastomer, thereby obtaining an activated PDMS elastomer substrate.
[0072] (3) The grafting reaction is carried out in a contact manner, and the operation is as follows:
[0073] According to every 1cm 2 The surface area of the activated PDMS elastomer substrate is coated with 50 μL of alkoxy-terminated polydimethylsiloxane (molecular weight 100,000 g / mol), the alkoxy-terminated polydimethylsiloxane is evenly coated on the surface of the activated PDMS elastomer substrate, and then placed in a container, the container is sealed, the temperature in the container is controlled to 100°C and the pressure is controlled to normal pressure (1013.25 mbar), so that the alkoxy-terminated polydimethylsiloxane and the surface of the activated PDMS elastomer substrate undergo a grafting reaction, the grafting reaction time is controlled to 720 minutes, a flexible molecular brush is formed on the surface of the activated PDMS elastomer substrate, and then the substrate is taken out, rinsed with deionized water and the surface is blown dry with compressed nitrogen to obtain a PDMS elastomer with an oil-resistant penetration coating.
[0074] Example 5
[0075] In this embodiment, a method for preparing a PDMS elastomer having an oil-penetration-resistant coating is provided, and the steps are as follows:
[0076] (1) The PDMS elastomer was ultrasonically cleaned for 180 seconds using ethanol (purity ≥ 99.7%) and deionized water in sequence to remove organic pollutants and solid particles on the surface of the PDMS elastomer, and then the surface of the PDMS elastomer was dried in a forced air drying oven for later use.
[0077] (2) placing the PDMS elastomer treated in step (1) into a plasma cleaning machine, and performing surface activation treatment on the PDMS elastomer using oxygen plasma, wherein the power of the oxygen plasma treatment is controlled to be 10 W and the treatment time is controlled to be 60 s, thereby forming a large number of active functional groups including hydroxyl groups on the surface of the PDMS elastomer, thereby obtaining an activated PDMS elastomer substrate.
[0078] (3) The grafting reaction is carried out in a non-contact manner, and the operation is as follows:
[0079] According to every 1cm 2 Add 2 μL of chlorine-terminated 1,3-dichlorotetramethyldisiloxane (molecular weight 203 g / mol) to the bottom area of the container. Add chlorine-terminated 1,3-dichlorotetramethyldisiloxane to the glass container, suspend the activated PDMS elastomer substrate in the glass container to avoid direct contact between the activated PDMS elastomer substrate and the liquid chlorine-terminated 1,3-dichlorotetramethyldisiloxane, seal the glass container, control the temperature in the glass container to room temperature (20-25°C), and the pressure to normal pressure (1013.25 mbar). -After volatilization, the dichlorotetramethyldisiloxane molecules come into contact with the surface of the activated PDMS elastomer substrate and undergo a grafting reaction. During the grafting reaction, the chlorine-terminated 1,3-dichlorotetramethyldisiloxane molecules polymerize to form polydimethylsiloxane flexible molecular chains and are grafted onto the surface of the activated PDMS elastomer substrate. The grafting reaction time is controlled to be 1 minute, and a flexible molecular brush is formed on the surface of the activated PDMS elastomer substrate. After that, it is taken out, rinsed with deionized water, and the surface is blown dry with compressed nitrogen to obtain a PDMS elastomer with an oil-resistant penetration coating.
[0080] Example 6
[0081] In this embodiment, a method for preparing a PDMS elastomer having an oil-penetration-resistant coating is provided, and the steps are as follows:
[0082] (1) The PDMS elastomer was ultrasonically cleaned for 30 seconds using ethanol (purity ≥ 99.7%) and deionized water in sequence to remove organic pollutants and solid particles on the surface of the PDMS elastomer, and then the surface of the PDMS elastomer was blown dry using compressed nitrogen gas for later use.
[0083] (2) placing the PDMS elastomer treated in step (1) into a plasma cleaning machine, and performing surface activation treatment on the PDMS elastomer using oxygen plasma, wherein the power of the oxygen plasma treatment is controlled to be 300 W and the treatment time is controlled to be 60 s, thereby forming a large number of active functional groups including hydroxyl groups on the surface of the PDMS elastomer, thereby obtaining an activated PDMS elastomer substrate.
[0084] (3) The grafting reaction is carried out in a non-contact manner, and the operation is as follows:
[0085] According to every 1cm 2 Add 10 μL of hydroxyl-terminated perfluoropolyether oxide (molecular weight is about 3000 g / mol) to the bottom area of the container. Add hydroxyl-terminated perfluoropolyether oxide to the glass container, suspend the activated PDMS elastomer substrate in the glass container to avoid direct contact between the activated PDMS elastomer substrate and the liquid hydroxyl-terminated perfluoropolyether oxide, seal the glass container, control the temperature in the glass container to 100° C. and the pressure to normal pressure (1013.25 mbar), and after the hydroxyl-terminated perfluoropolyether oxide molecules volatilize, they contact with the surface of the activated PDMS elastomer substrate and undergo a grafting reaction. The grafting reaction time is controlled to be 20 min, and a flexible molecular brush is formed on the surface of the activated PDMS elastomer substrate. Then, take it out, rinse it with deionized water, and blow dry the surface with compressed nitrogen to obtain a PDMS elastomer with an oil-resistant penetration coating.
[0086] Example 7
[0087] In this embodiment, a method for preparing a PDMS elastomer having an oil-penetration-resistant coating is provided, and the steps are as follows:
[0088] (1) The PDMS elastomer was ultrasonically cleaned for 30 seconds using ethanol (purity ≥ 99.7%) and deionized water in sequence to remove organic pollutants and solid particles on the surface of the PDMS elastomer, and then the surface of the PDMS elastomer was blown dry using compressed nitrogen gas for later use.
[0089] (2) placing the PDMS elastomer treated in step (1) into a plasma cleaning machine, and performing surface activation treatment on the PDMS elastomer using oxygen plasma, wherein the power of the oxygen plasma treatment is controlled to be 300 W and the treatment time is controlled to be 60 s, thereby forming a large number of active functional groups including hydroxyl groups on the surface of the PDMS elastomer, thereby obtaining an activated PDMS elastomer substrate.
[0090] (3) The grafting reaction is carried out in a non-contact manner, and the operation is as follows:
[0091] According to every 1cm 2Add 20 μL of carboxyl-terminated perfluoropolyether oxide (molecular weight is about 6000 g / mol) to the bottom area of the container. Add carboxyl-terminated perfluoropolyether oxide into the glass container, suspend the activated PDMS elastomer substrate in the glass container to avoid direct contact between the activated PDMS elastomer substrate and the liquid carboxyl-terminated perfluoropolyether oxide, seal the glass container, control the temperature in the glass container to 80° C. and the pressure to normal pressure (1013.25 mbar), and after the carboxyl-terminated perfluoropolyether oxide molecules volatilize, they contact with the surface of the activated PDMS elastomer substrate and undergo a grafting reaction. The grafting reaction time is controlled to be 20 min, and a flexible molecular brush is formed on the surface of the activated PDMS elastomer substrate. Then, the substrate is taken out, rinsed with deionized water, and the surface is blown dry with compressed nitrogen to obtain a PDMS elastomer with an oil-resistant penetration coating.
[0092] Example 8
[0093] In this embodiment, a method for preparing a PDMS elastomer having an oil-penetration-resistant coating is provided, and the steps are as follows:
[0094] (1) The PDMS elastomer was ultrasonically cleaned for 30 seconds using ethanol (purity ≥ 99.7%) and deionized water in sequence to remove organic pollutants and solid particles on the surface of the PDMS elastomer, and then the surface of the PDMS elastomer was blown dry using compressed nitrogen gas for later use.
[0095] (2) placing the PDMS elastomer treated in step (1) into a plasma cleaning machine, and performing surface activation treatment on the PDMS elastomer using oxygen plasma, wherein the power of the oxygen plasma treatment is controlled to be 50 W and the treatment time is controlled to be 30 s, so that a large number of active functional groups including hydroxyl groups are formed on the surface of the PDMS elastomer, thereby obtaining an activated PDMS elastomer substrate.
[0096] (3) The grafting reaction is carried out in a non-contact manner, and the operation is as follows:
[0097] According to every 1cm 2Add 10 μL of amino-terminated polydimethylsiloxane (molecular weight is about 3000 g / mol) to the bottom area of the container. Add amino-terminated polydimethylsiloxane into the glass container, suspend the activated PDMS elastomer substrate in the glass container to avoid direct contact between the activated PDMS elastomer substrate and the liquid amino-terminated polydimethylsiloxane, seal the glass container, control the temperature in the glass container to room temperature (20-25° C.) and the pressure to normal pressure (1013.25 mbar), and after the amino-terminated polydimethylsiloxane molecules volatilize, they contact with the surface of the activated PDMS elastomer substrate and undergo a grafting reaction. The grafting reaction time is controlled to be 5 minutes, and a flexible molecular brush is formed on the surface of the activated PDMS elastomer substrate. Then, take it out, rinse it with deionized water, and blow dry the surface with compressed nitrogen to obtain a PDMS elastomer with an oil-resistant penetration coating.
[0098] Example 9
[0099] In this embodiment, a method for preparing a PDMS elastomer having an oil-penetration-resistant coating is provided, and the steps are as follows:
[0100] (1) The PDMS elastomer was ultrasonically cleaned for 30 seconds using ethanol (purity ≥ 99.7%) and deionized water in sequence to remove organic pollutants and solid particles on the surface of the PDMS elastomer, and then the surface of the PDMS elastomer was blown dry using compressed nitrogen gas for later use.
[0101] (2) placing the PDMS elastomer treated in step (1) into a plasma cleaning machine, and performing surface activation treatment on the PDMS elastomer using oxygen plasma, wherein the power of the oxygen plasma treatment is controlled to be 50 W and the treatment time is controlled to be 30 s, thereby forming a large number of active functional groups including hydroxyl groups on the surface of the PDMS elastomer, thereby obtaining an activated PDMS elastomer substrate.
[0102] (3) The grafting reaction is carried out in a non-contact manner, and the operation is as follows:
[0103] According to every 1cm 2Add 30 μL of alkoxy-terminated polydimethylsiloxane (molecular weight is about 3000 g / mol) to the bottom area of the container. Add alkoxy-terminated polydimethylsiloxane into the glass container, suspend the activated PDMS elastomer substrate in the glass container to avoid direct contact between the activated PDMS elastomer substrate and the liquid alkoxy-terminated polydimethylsiloxane, seal the glass container, control the temperature in the glass container to room temperature (20-25° C.) and the pressure to normal pressure (1013.25 mbar), and after the alkoxy-terminated polydimethylsiloxane molecules volatilize, they contact with the surface of the activated PDMS elastomer substrate and undergo a grafting reaction. The grafting reaction time is controlled to be 5 minutes, and a flexible molecular brush is formed on the surface of the activated PDMS elastomer substrate. Then, take it out, rinse it with deionized water, and blow dry the surface with compressed nitrogen to obtain a PDMS elastomer with an oil-resistant penetration coating.
[0104] Example 10
[0105] In this embodiment, a method for preparing a PDMS elastomer having an oil-penetration-resistant coating is provided, and the steps are as follows:
[0106] (1) The PDMS elastomer was ultrasonically cleaned for 30 seconds using ethanol (purity ≥ 99.7%) and deionized water in sequence to remove organic pollutants and solid particles on the surface of the PDMS elastomer, and then the surface of the PDMS elastomer was blown dry using compressed nitrogen gas for later use.
[0107] (2) placing the PDMS elastomer treated in step (1) into a plasma cleaning machine, and performing surface activation treatment on the PDMS elastomer using oxygen plasma, wherein the power of the oxygen plasma treatment is controlled to be 50 W and the treatment time is controlled to be 30 s, thereby forming a large number of active functional groups including hydroxyl groups on the surface of the PDMS elastomer, thereby obtaining an activated PDMS elastomer substrate.
[0108] (3) The grafting reaction is carried out in a non-contact manner, and the operation is as follows:
[0109] According to every 1cm 2Add 30 μL of epoxy-terminated polydimethylsiloxane (molecular weight is about 3000 g / mol) to the bottom area of the container. Add epoxy-terminated polydimethylsiloxane into the glass container, suspend the activated PDMS elastomer substrate in the glass container to avoid direct contact between the activated PDMS elastomer substrate and the liquid epoxy-terminated polydimethylsiloxane, seal the glass container, control the temperature in the glass container to 80°C and the pressure to normal pressure (1013.25 mbar), and after the epoxy-terminated polydimethylsiloxane molecules volatilize, they contact with the surface of the activated PDMS elastomer substrate and undergo a grafting reaction. The grafting reaction time is controlled to be 5 minutes, and a flexible molecular brush is formed on the surface of the activated PDMS elastomer substrate. Then, take it out, rinse it with deionized water, and blow dry the surface with compressed nitrogen to obtain a PDMS elastomer with an oil-resistant penetration coating.
[0110] Embodiment 11
[0111] In this embodiment, a method for preparing a PDMS elastomer having an oil-penetration-resistant coating is provided, and the steps are as follows:
[0112] (1) The PDMS elastomer was ultrasonically cleaned for 30 seconds using ethanol (purity ≥ 99.7%) and deionized water in sequence to remove organic pollutants and solid particles on the surface of the PDMS elastomer, and then the surface of the PDMS elastomer was blown dry using compressed nitrogen gas for later use.
[0113] (2) placing the PDMS elastomer treated in step (1) into a plasma cleaning machine, and performing surface activation treatment on the PDMS elastomer using oxygen plasma, wherein the power of the oxygen plasma treatment is controlled to be 50 W and the treatment time is controlled to be 30 s, thereby forming a large number of active functional groups including hydroxyl groups on the surface of the PDMS elastomer, thereby obtaining an activated PDMS elastomer substrate.
[0114] (3) The grafting reaction is carried out in a non-contact manner, and the operation is as follows:
[0115] According to every 1cm 2Add 30 μL of isocyanate-terminated polydimethylsiloxane (molecular weight is about 3000 g / mol) to the bottom area of the container. Add isocyanate-terminated polydimethylsiloxane into the glass container, suspend the activated PDMS elastomer substrate in the glass container to avoid direct contact between the activated PDMS elastomer substrate and the liquid isocyanate-terminated polydimethylsiloxane, seal the glass container, control the temperature in the glass container to 10°C and the pressure to normal pressure (1013.25 mbar), and after the isocyanate-terminated polydimethylsiloxane molecules volatilize, they contact with the surface of the activated PDMS elastomer substrate and undergo a grafting reaction. The grafting reaction time is controlled to be 5 minutes, and a flexible molecular brush is formed on the surface of the activated PDMS elastomer substrate. Then take it out, rinse it with deionized water, and blow dry the surface with compressed nitrogen to obtain a PDMS elastomer with an oil-resistant penetration coating.
Claims
1. A method for preparing a polydimethylsiloxane elastomer having an oil-penetration-resistant coating, characterized in that: The following steps are involved: (1) treating a clean and dry polydimethylsiloxane elastomer with oxygen plasma for surface activation to obtain an activated polydimethylsiloxane elastomer substrate; (2) grafting the active end-capped silane onto the surface of an activated polydimethylsiloxane elastomer substrate to form a flexible molecular brush on the surface of the activated polydimethylsiloxane elastomer substrate to obtain a polydimethylsiloxane elastomer having an oil-resistant penetration coating; The active end-group-terminated silane is an active end-group-terminated silane monomer or an active group-terminated silane polymer; during the grafting reaction, the active end-group-terminated silane monomer will polymerize to form a polydimethylsiloxane flexible molecular chain and grafted onto the surface of an activated polydimethylsiloxane elastomer substrate, and the silane polymer chain of the active group-terminated silane polymer is directly grafted onto the surface of an activated polydimethylsiloxane elastomer substrate.
2. The method for preparing the polydimethylsiloxane elastomer having an oil-resistant coating according to claim 1, characterized in that: The active end-group-terminated silane monomer is active end-group-terminated tetramethyl disiloxane, and the active group-terminated silane polymer is active end-group-terminated polydimethylsiloxane or active end-group-terminated perfluoropolyether silane.
3. The method for preparing the polydimethylsiloxane elastomer having an oil-penetration-resistant coating according to claim 1, characterized in that: The active end groups in the active end group-terminated silane include at least one of a chlorine end group, a hydroxyl group, a carboxyl group, an amino group, an alkoxy group, an epoxy group, and an isocyanate group.
4. The method for preparing the polydimethylsiloxane elastomer having an oil-resistant coating according to any one of claims 1 to 3, characterized in that: The molecular weight of the active end-group-capped silane is 203-100000 g / mol.
5. The method for preparing the polydimethylsiloxane elastomer having an oil-penetration-resistant coating according to claim 4, characterized in that: When the molecular weight of the active terminal silane is less than 10000 g / mol, the grafting reaction is carried out in a non-contact manner in step (2); when the molecular weight of the active terminal silane is greater than or equal to 10000 g / mol, the grafting reaction is carried out in a contact manner.
6. The method for preparing the polydimethylsiloxane elastomer having an oil-penetration-resistant coating according to claim 5, characterized in that: The operation of step (2) of carrying out the grafting reaction in a non-contact manner is as follows: adding the active end-group-capped silane into a container, fixing the activated polydimethylsiloxane elastomer substrate in the container to prevent the activated polydimethylsiloxane elastomer substrate from directly contacting the liquid active end-group-capped silane, sealing the container to allow the active end-group-capped silane molecules to volatilize and undergo a grafting reaction with the surface of the activated polydimethylsiloxane elastomer substrate, then taking out, rinsing with deionized water, and drying to obtain a polydimethylsiloxane elastomer with an oil-proof penetration coating; The operation of the step (2) of carrying out the grafting reaction in a contact manner is as follows: applying the active end-group-capped silane to the surface of the activated polydimethylsiloxane elastomer substrate, placing it in a sealed container to allow the active end-group-capped silane to undergo a grafting reaction with the surface of the activated polydimethylsiloxane elastomer substrate, then taking it out, rinsing it with deionized water, and drying it to obtain a polydimethylsiloxane elastomer with an oil-resistant penetration coating.
7. The method for preparing the polydimethylsiloxane elastomer having an oil-penetration-resistant coating according to claim 6, characterized in that: When step (2) is carried out by non-contact grafting reaction, the amount of each 1 cm 2 The active end-group-capped silane is added to the container in a ratio of 2 to 50 μL according to the bottom area of the container; when step (2) adopts a contact method to carry out the grafting reaction, the active end-group-capped silane is applied to the surface of the activated polydimethylsiloxane elastomer substrate to completely cover the area where the oil-proof penetration coating is to be formed.
8. The method for preparing the polydimethylsiloxane elastomer having an oil-penetration resistant coating according to claim 6 or 7, characterized in that: During the grafting reaction of step (2), the pressure in the container is controlled not to exceed 1013.25 mbar.
9. The method for preparing the polydimethylsiloxane elastomer having an oil-penetration resistant coating according to claim 6 or 7, characterized in that: During the grafting reaction process of step (2), the temperature in the container is controlled to be 10-100° C., and the grafting reaction time is controlled to be 1-720 min.
10. The method for preparing the polydimethylsiloxane elastomer having an oil-proof coating according to any one of claims 1 to 3, characterized in that: The power of oxygen plasma for surface activation treatment is controlled to be 10 to 1500 W and the time is 10 s to 10 min.
Citation Information
Patent Citations
Solvent-resistant polydimethylsiloxane polymer having oil repellency, and production method thereof
CN110857334A
Pressure-induced infiltration state and shape-controllable super-hydrophobic silicone rubber elastomer and preparation method thereof
CN118254315A
Silicone elastomer stamp with hydrophilic surfaces and method of making same
EP1193056A1
Method for controlling wettability of solid surface, and the solid surface
JP2012140580A
Smart Temperature Control Device
KR102107473B1