Antibacterial textile fabric and preparation method thereof

By interwoven and blending mugwort modified fibers with cotton fibers and combining specific antibacterial agents, the problems of poor antibacterial performance and low safety of cotton fabrics are solved, achieving lasting antibacterial, deworming and health care effects, while improving the comfort of the fabric.

CN119082927AInactive Publication Date: 2024-12-06ANBEL PLASTIC MFG LTD

Patent Information

Application Number
CN202411416649.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing cotton fabrics have poor antibacterial properties and low safety. Traditional antibacterial materials have adverse reactions to human physiology, making it difficult to meet the needs of high-quality life.

Method used

Mugwort modified fibers and cotton fibers are mixed with interwoven and blended, and are prepared by composite antibacterial agents, including mugwort powder, diatomaceous earth-loaded titanium dioxide, silicone quaternary ammonium salts and α-methacrylic acid, combined with aqueous polyurethane binder and stable The agent forms a long-lasting antibacterial textile fabric to ensure safety performance and comfort.

Benefits of technology

It significantly improves the long-lasting antibacterial properties of textile fabrics, exerts the pharmacological effects of mugwort, has a deworming effect, and provides health care effects of warming meridians and dispelling cold, promoting blood circulation and removing blood stasis while ensuring safety performance, while improving comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005079636680000101
    Figure BDA0005079636680000101
  • Figure BDA0005079636680000111
    Figure BDA0005079636680000111
Patent Text Reader

Abstract

The invention discloses an antibacterial textile fabric and a preparation method thereof, and belongs to the field of textile fabric preparation. After the prepared wormwood modified fiber and the cotton fiber are interwoven and blended, the fabric is endowed with remarkable lasting antibacterial property, the pharmacological action of wormwood can be fully played, and the safety performance is high. The composite antibacterial agent is prepared by compounding the wormwood powder, the diatomite-loaded titanium dioxide, the organosilicon quaternary ammonium salt and the alpha-methacrylic acid, so that the pharmacological action of the wormwood can be exerted, and a certain wormwood powder loading effect can be achieved by compounding the wormwood powder with the diatomite-loaded titanium dioxide with a porous structure; according to the present invention, the alpha-methacrylic acid can promote the compatibility between the components and promote the cross-linking between the composite antibacterial agent and the binder, such that the more stable adhesion effect can be achieved on the premise of ensuring the safety performance so as to ensure the lasting antibacterial property of the fabric, such that the lasting antibacterial property of the fabric can be further ensured by using the alpha-methacrylic acid to promote the compatibility between the components and promote the cross-linking between the composite antibacterial agent and the binder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textiles, and in particular to an antibacterial textile fabric and a preparation method thereof. Background Art

[0002] Cotton fabric is one of the commonly used fabrics in the textile field, but single-function cotton fabric can no longer meet people's pursuit of high-quality life. Cotton textiles are widely used in all aspects of life due to their excellent properties such as breathability, moisture absorption, heat resistance, acid resistance, softness, close fit, and warmth. However, the antibacterial function of pure cotton textiles is relatively poor, and their own structure and properties are very likely to cause bacteria to grow. Therefore, it is extremely important to give cotton fabrics better antibacterial functions. Traditional antibacterial finishing of cotton fabrics mainly revolves around two mechanisms: a. Contact-type persistent sterilization; b. Release of bactericidal components for antibacterial (dissolution-type antibacterial). Among them, the materials used on cotton fabrics based on the contact-type persistent sterilization method include chitosan, guanidine salt polymers, halogenamine compounds, betaine and other materials. These materials generally adsorb bacteria and move closer to them when in contact with bacteria, and a large amount of charge distribution can cause the rupture of bacterial cell membranes. The method based on the release of bactericidal components usually pre-loads or embeds the bactericide, and then uses it for antibacterial finishing of cotton fabrics, such as silver nanoparticles, various antibiotics, and some metal oxides. However, these materials have certain adverse effects on human physiology, including skin allergies and inflammatory reactions such as rashes, which limits their application. Therefore, it is extremely important to study the durability and safety of the antibacterial properties of cotton fabrics. Summary of the invention

[0003] Based on this, in order to solve the problems of poor antibacterial performance and low safety of the prior art fabrics, the present invention provides an antibacterial textile fabric and a preparation method thereof, and the specific technical scheme is as follows:

[0004] An antibacterial textile fabric, comprising the following raw materials in parts by weight: 35 to 50 parts of modified wormwood fiber and 15 to 35 parts of cotton fiber;

[0005] The modified wormwood fiber comprises the following raw materials in parts by weight: 20 to 35 parts of wormwood-based viscose, 10 to 20 parts of cellulose, 1 to 10 parts of a composite antibacterial agent, 5 to 10 parts of a binder, and 1 to 3 parts of a stabilizer;

[0006] The composite antibacterial agent is composed of wormwood powder, diatomaceous earth-loaded titanium dioxide, organosilicon quaternary ammonium salt and alpha-methacrylic acid in a mass ratio of (1-5): (1-2): (3-15): (20-30).

[0007] Furthermore, the binder is water-based polyurethane.

[0008] Furthermore, the stabilizer is at least one of sodium alginate, hydroxyethyl cellulose and sodium carboxymethyl cellulose.

[0009] In addition, the present invention also provides a method for preparing an antibacterial textile fabric, the preparation method comprising the following steps:

[0010] S1, adding wormwood powder, diatomaceous earth-loaded titanium dioxide, organosilicon quaternary ammonium salt and α-methacrylic acid into a mixing kettle, stirring and treating to obtain a composite antibacterial agent;

[0011] S2, adding wormwood-based viscose, cellulose, composite antibacterial agent, binder and stabilizer into a mixing kettle, stirring, aging, and then spinning to obtain wormwood modified fiber;

[0012] S3, interweaving and blending the modified wormwood fiber and the cotton fiber to prepare a blank;

[0013] S4, soaking the blank in a treatment solution A to which an antifouling agent and an antioxidant have been added in advance, leaving it to stand for 20 minutes to 60 minutes, washing, drying, and then soaking it in a treatment solution B to which a softener has been added in advance, leaving it to stand for 10 minutes to 20 minutes, washing, and drying to obtain an antibacterial textile fabric.

[0014] Furthermore, the antifouling agent is ethylene terephthalate.

[0015] Furthermore, the softener is at least one of softeners MS-20, AS-23N and GL-54.

[0016] Furthermore, the antioxidant is at least one of antioxidant 1010, antioxidant 168 and ultraviolet absorber UV-P.

[0017] Furthermore, the stirring conditions in step S1 are: temperature of 85° C. to 110° C., rotation speed of 50 r / min to 150 r / min, and time of 25 min to 40 min.

[0018] Furthermore, the stirring conditions in step S2 are: temperature of 80° C. to 100° C., rotation speed of 50 r / min to 150 r / min, and time of 20 min to 30 min.

[0019] Furthermore, the aging treatment is carried out at a temperature of 35°C to 60°C and for a time of 5h to 8h.

[0020] Compared with the prior art, this application has the following beneficial effects:

[0021] The fabric obtained by interweaving and blending the prepared wormwood modified fiber and cotton fiber has significant lasting antibacterial performance, and can give full play to the pharmacological effect of wormwood, has high safety performance, has certain anthelmintic effect, and also has certain health care effects of warming meridians and dispelling cold, promoting blood circulation and removing blood stasis; Moreover, the fabric after being processed by the present application has excellent comfort. In addition, the present invention prepares a composite antibacterial agent by compounding wormwood powder, diatomaceous earth-loaded titanium dioxide, organosilicon quaternary ammonium salt and α-methacrylic acid, which can not only play the pharmacological effect of wormwood itself, but also compound diatomaceous earth-loaded titanium dioxide with a porous structure, which can also play the load effect of wormwood powder, and realize synergistic enhancement with organosilicon quaternary ammonium salt, delay the release of organosilicon quaternary ammonium salt, α-methacrylic acid can promote the compatibility between components, and promote the crosslinking between the composite antibacterial agent and the binder, and achieve a more stable adhesion effect under the premise of ensuring safety performance, thereby ensuring the lasting antibacterial of the fabric. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0024] An antibacterial textile fabric in an embodiment of the present invention comprises the following raw materials in parts by weight: 35 to 50 parts of modified wormwood fiber and 15 to 35 parts of cotton fiber;

[0025] The modified wormwood fiber comprises the following raw materials in parts by weight: 20 to 35 parts of wormwood-based viscose, 10 to 20 parts of cellulose, 1 to 10 parts of a composite antibacterial agent, 5 to 10 parts of a binder, and 1 to 3 parts of a stabilizer;

[0026] The composite antibacterial agent is composed of wormwood powder, diatomaceous earth-loaded titanium dioxide, organosilicon quaternary ammonium salt and alpha-methacrylic acid in a mass ratio of (1-5): (1-2): (3-15): (20-30).

[0027] In one embodiment, the binder is water-based polyurethane.

[0028] In one embodiment, the stabilizer is at least one of sodium alginate, hydroxyethyl cellulose, and sodium carboxymethyl cellulose.

[0029] In one embodiment, the average particle size of the wormwood powder is 40nm to 80nm.

[0030] In addition, the present invention also provides a method for preparing an antibacterial textile fabric, the preparation method comprising the following steps:

[0031] S1, adding wormwood powder, diatomaceous earth-loaded titanium dioxide, organosilicon quaternary ammonium salt and α-methacrylic acid into a mixing kettle, stirring and treating to obtain a composite antibacterial agent;

[0032] S2, adding wormwood-based viscose, cellulose, composite antibacterial agent, binder and stabilizer into a mixing kettle, stirring, aging, and then spinning to obtain wormwood modified fiber;

[0033] S3, interweaving and blending the modified wormwood fiber and the cotton fiber to prepare a blank;

[0034] S4, soaking the blank in a treatment solution A to which an antifouling agent and an antioxidant have been added in advance, leaving it to stand for 20 minutes to 60 minutes, washing, drying, and then soaking it in a treatment solution B to which a softener has been added in advance, leaving it to stand for 10 minutes to 20 minutes, washing, and drying to obtain an antibacterial textile fabric.

[0035] In one embodiment, the stirring treatment conditions in step S1 are: temperature of 85° C. to 110° C., rotation speed of 50 r / min to 150 r / min, and time of 25 min to 40 min.

[0036] In one embodiment, the stirring treatment conditions in step S2 are: temperature of 80°C to 100°C, rotation speed of 50 r / min to 150 r / min, and time of 20 min to 30 min.

[0037] In one embodiment, the antifouling agent is ethylene terephthalate.

[0038] In one embodiment, the concentration of the antifouling agent in the treatment liquid A is 1 g / L to 5 g / L.

[0039] In one embodiment, the antioxidant is at least one of antioxidant 1010, antioxidant 168 and ultraviolet absorber UV-P.

[0040] In one embodiment, the concentration of the antioxidant in the treatment solution A is 1 g / L to 5 g / L.

[0041] In one embodiment, the softener is at least one of softeners MS-20, AS-23N and GL-54.

[0042] In one embodiment, the concentration of the softener in the treatment solution B is 1 g / L to 10 g / L.

[0043] In one embodiment, in step S2, the aging treatment is carried out at a temperature of 35°C to 60°C and for a time of 5h to 8h.

[0044] In one embodiment, in step S4, the bath ratio of the blank to the treatment liquid A is 1:50 to 1:100.

[0045] In one embodiment, in step S4, the bath ratio of the blank to the treatment liquid B is 1:50 to 1:100.

[0046] In one embodiment, in step S4, the drying temperature is 60°C to 100°C.

[0047] In one embodiment, the fineness of the modified mugwort fiber and the cotton fiber is 70D-130D.

[0048] After the prepared modified wormwood fiber is interwoven and blended with cotton fiber, the fabric is given significant lasting antibacterial properties, and the pharmacological effects of wormwood can be fully exerted, with a certain insect repellent effect and high safety performance. At the same time, it also has a certain health care effect of warming the meridians and dispelling cold, promoting blood circulation and removing blood stasis; moreover, the fabric treated by the present application has excellent comfort.

[0049] The embodiments of the present invention will be described in detail below with reference to specific examples.

[0050] Embodiment 1:

[0051] A method for preparing an antibacterial textile fabric, the method comprising the following steps:

[0052] S1. Adding wormwood powder, diatomaceous earth-loaded titanium dioxide, organosilicon quaternary ammonium salt and α-methacrylic acid in a mass ratio of 3:2:7:25 into a mixing kettle, stirring for 35 minutes at a temperature of 85°C and a rotation speed of 100 r / min to obtain a composite antibacterial agent;

[0053] S2. Add 30 parts of wormwood-based viscose, 13 parts of cellulose, 7 parts of composite antibacterial agent, 8 parts of water-based polyurethane and 1 part of hydroxyethyl cellulose to a mixing kettle by weight, stir at a temperature of 95°C and a speed of 50r / min for 25min, then age at a temperature of 45°C for 6h, and then spin-form to obtain wormwood modified fiber;

[0054] S3. By weight, 45 parts of modified wormwood fiber with a fineness of 100D and 30 parts of cotton fiber with a fineness of 100D are interwoven and blended to prepare a blank;

[0055] S4, according to a bath ratio of 1:50, the blank is immersed in a treatment solution A to which ethylene terephthalate and antioxidant 1010 are added in advance, and the concentration of the antifouling agent is 3 g / L, and the concentration of the antioxidant is 5 g / L. After standing for 45 minutes, the blank is washed, dried at 85°C, and then immersed in a treatment solution B to which softener MS-20 is added in advance, and the concentration of the softener is 8 g / L. After standing for 15 minutes, the blank is washed, and dried at 90°C to obtain an antibacterial textile fabric.

[0056] Embodiment 2:

[0057] A method for preparing an antibacterial textile fabric, the method comprising the following steps:

[0058] S1. Adding wormwood powder, diatomaceous earth-loaded titanium dioxide, organosilicon quaternary ammonium salt and α-methacrylic acid in a mass ratio of 3:2:7:26 into a mixing kettle, stirring for 40 minutes at a temperature of 100°C and a rotation speed of 100 r / min to obtain a composite antibacterial agent;

[0059] S2. Add 32 parts of wormwood-based viscose, 18 parts of cellulose, 7 parts of composite antibacterial agents, 9 parts of water-based polyurethane and 1 part of hydroxyethyl cellulose to a mixing kettle by weight, stir for 25 minutes at a temperature of 100°C and a rotation speed of 50r / min, and then age for 7 hours at a temperature of 50°C, and then spin-form to obtain wormwood modified fiber;

[0060] S3, by weight, 48 parts of modified wormwood fiber with a fineness of 100D and 32 parts of cotton fiber with a fineness of 100D are interwoven and blended to prepare a blank;

[0061] S4, according to a bath ratio of 1:50, the blank is immersed in a treatment solution A to which ethylene terephthalate and antioxidant 1010 are added in advance, and the concentration of the antifouling agent is 3 g / L, and the concentration of the antioxidant is 5 g / L. After standing for 45 minutes, the blank is washed, dried at 95°C, and then immersed in a treatment solution B to which softener MS-20 is added in advance, and the concentration of the softener is 9 g / L. After standing for 20 minutes, the blank is washed, and dried at 100°C to obtain an antibacterial textile fabric.

[0062] Embodiment 3:

[0063] A method for preparing an antibacterial textile fabric, the method comprising the following steps:

[0064] S1. Adding wormwood powder, diatomaceous earth-loaded titanium dioxide, organosilicon quaternary ammonium salt and α-methacrylic acid in a mass ratio of 5:2:5:27 into a mixing kettle, stirring for 40 minutes at a temperature of 95°C and a rotation speed of 100 r / min to obtain a composite antibacterial agent;

[0065] S2. Add 33 parts of wormwood-based viscose, 20 parts of cellulose, 9 parts of composite antibacterial agent, 10 parts of water-based polyurethane and 2 parts of sodium carboxymethyl cellulose to a mixing kettle by weight, stir for 25 minutes at a temperature of 95°C and a rotation speed of 100r / min, and then age for 8 hours at a temperature of 45°C, and then spin-form to obtain wormwood modified fiber;

[0066] S3. By weight, 49 parts of modified mugwort fiber with a fineness of 100D and 34 parts of cotton fiber with a fineness of 100D are interwoven and blended to prepare a blank;

[0067] S4, according to a bath ratio of 1:50, the blank is immersed in a treatment solution A to which ethylene terephthalate and antioxidant 1010 are added in advance, and the concentration of the antifouling agent is 3 g / L, and the concentration of the antioxidant is 5 g / L. After standing for 60 minutes, the blank is washed, dried at 95°C, and then immersed in a treatment solution B to which softener MS-20 is added in advance, and the concentration of the softener is 10 g / L. After standing for 20 minutes, the blank is washed, and dried at 80°C to obtain an antibacterial textile fabric.

[0068] Embodiment 4:

[0069] A method for preparing an antibacterial textile fabric, the method comprising the following steps:

[0070] S1. Adding wormwood powder, diatomaceous earth-loaded titanium dioxide, organosilicon quaternary ammonium salt and α-methacrylic acid in a mass ratio of 4:2:6:28 into a mixing kettle, stirring for 30 minutes at a temperature of 100°C and a rotation speed of 150 r / min to obtain a composite antibacterial agent;

[0071] S2. Add 35 parts of wormwood-based viscose, 20 parts of cellulose, 10 parts of composite antibacterial agent, 10 parts of water-based polyurethane and 3 parts of sodium carboxymethyl cellulose to a mixing kettle by weight, stir for 25 minutes at a temperature of 100°C and a rotation speed of 150r / min, and then age for 5 hours at a temperature of 60°C, and then spin-form to obtain wormwood-modified fiber;

[0072] S3. By weight, 50 parts of modified wormwood fiber with a fineness of 100D and 35 parts of cotton fiber with a fineness of 100D are interwoven and blended to prepare a blank;

[0073] S4, according to a bath ratio of 1:50, the blank is immersed in a treatment solution A to which ethylene phthalate and antioxidant 1010 are added in advance, and the concentration of the antifouling agent is 3 g / L, and the concentration of the antioxidant is 5 g / L. After standing for 50 minutes, the blank is washed, dried at 95°C, and then immersed in a treatment solution B to which softener MS-20 is added in advance, and the concentration of the softener is 8 g / L. After standing for 20 minutes, the blank is washed, and dried at 100°C to obtain an antibacterial textile fabric.

[0074] Comparative Example 1:

[0075] The difference between Comparative Example 1 and Example 4 is that in Comparative Example 1, only the cotton fiber with a fineness of 100D in Example 4 is used to spin the blank, and the rest is the same as Example 4.

[0076] Comparative Example 2:

[0077] The difference between Comparative Example 2 and Example 4 is that no composite antibacterial agent is added to the raw materials for preparing the modified mugwort fiber in Comparative Example 2, and the rest is the same as Example 4.

[0078] Comparative Example 3:

[0079] The difference between Comparative Example 3 and Example 4 is that no wormwood-based viscose is added to the raw materials for preparing the wormwood-modified fiber in Comparative Example 3, and the rest is the same as Example 4.

[0080] Comparative Example 4:

[0081] The difference between Comparative Example 4 and Example 4 is that no binder is added to the raw materials for preparing the modified mugwort fiber in Comparative Example 4, and the rest is the same as Example 4.

[0082] Comparative Example 5:

[0083] The difference between Comparative Example 5 and Example 4 is that no wormwood powder is added to the composite antibacterial agent in Comparative Example 5, and the rest is the same as Example 4.

[0084] Comparative Example 6:

[0085] The difference between Comparative Example 6 and Example 4 is that diatomaceous earth loaded titanium dioxide is not added to the composite antibacterial agent in Comparative Example 6, and the rest is the same as Example 4.

[0086] Comparative Example 7:

[0087] The difference between Comparative Example 7 and Example 4 is that in Comparative Example 7, ordinary titanium dioxide is used instead of diatomaceous earth to load titanium dioxide, and the rest is the same as Example 4.

[0088] Comparative Example 8:

[0089] The difference between Comparative Example 8 and Example 4 is that no organosilicon quaternary ammonium salt is added to the composite antibacterial agent in Comparative Example 8, and the rest is the same as Example 4.

[0090] Comparative Example 9:

[0091] The difference between Comparative Example 8 and Example 4 is that α-methacrylic acid is not added to the composite antibacterial agent in Comparative Example 8, and the rest is the same as Example 4.

[0092] Comparative Example 10:

[0093] The difference between Comparative Example 10 and Example 4 is that the composition ratio of the composite antibacterial agent in Comparative Example 10 is different, and the other components are the same as Example 4. The composition ratio of the composite antibacterial agent in Comparative Example 10 is as follows:

[0094] Add mugwort powder, diatomaceous earth-loaded titanium dioxide, organosilicon quaternary ammonium salt and α-methacrylic acid in a mass ratio of 1:10:1:7 into a mixing kettle, stir for 30 minutes at a temperature of 100°C and a rotation speed of 150 r / min to obtain a composite antibacterial agent.

[0095] 1. Antibacterial Test

[0096] The antibacterial textile fabric samples prepared in Examples 1 to 4 and the fabric comparison samples prepared in Comparative Examples 1 to 10 were subjected to performance tests. The antibacterial performance test was conducted according to the oscillation method in the FZ / T73023-2006 standard. The results are shown in Table 1 below.

[0097] Table 1: Antibacterial performance test

[0098]

[0099] From the data analysis of Table 1, the antibacterial textile fabric prepared by the present invention has significant antibacterial properties, and the antibacterial properties are stable and long-lasting. The fabric obtained by weaving cotton fibers in Comparative Example 1 has no obvious antibacterial properties, and the cotton fibers are interwoven to improve the comfort of the fabric; the difference between Comparative Example 2 and Example 4 is that no composite antibacterial agent is added to the raw materials for preparing the modified wormwood fiber in Comparative Example 2, but the antibacterial properties of the fabric are significantly reduced, indicating that the composite antibacterial agent added in this application can play a significant health-care and antibacterial effect in the fabric; the difference between Comparative Example 3 and Example 4 is that no wormwood-based viscose is added in Comparative Example 3, but the antibacterial property has a downward trend, indicating that adding a certain amount of wormwood raw materials to prepare and modify the fiber is helpful to improve the antibacterial properties; Comparative Example 4 and Example 4 are different. The difference of Example 4 is that no binder is added in Comparative Example 4, but the antibacterial performance is worse than that of Example 4. During the experiment, it was also found that the problem of uneven mixing of raw materials occurred in Comparative Example 4, indicating that the presence of the binder is helpful to promote the compatibility of the components; the difference between Comparative Examples 5 to 9 and Example 4 is that the components of the composite antibacterial agent are different, and the difference between Comparative Example 10 and Example 4 is that the ratio of the components of the composite antibacterial agent is different, but it can be seen from Table 1 that the antibacterial effect is obviously worse than that of Example 4, indicating that the present application obtains a composite antibacterial agent by compounding specific components in specific proportions, which can achieve a synergistic effect and give the textile fabric health antibacterial properties.

[0100] 2. Mosquito and insect repellent test

[0101] The antibacterial textile fabrics of Examples 1 to 4 were selected to test the insect repellent effect. A subjective evaluation method was adopted, and the fabrics were placed in areas with more mosquitoes. The anti-mosquito and insect repellent effects were observed for 5 days, 10 days and 20 days. Subjective scoring was performed by photography and videography, with 0 to 30 indicating no effect, 31 to 60 indicating average effect, and 61 to 100 indicating marked effect. The results are shown in Table 2 below.

[0102] Table 2: Anti-mosquito and insect repellent effects

[0103]

[0104] From the data analysis in Table 2, it can be seen that the antibacterial textile fabric prepared by the present invention exhibits significant insect repellent and mosquito repellent effects. It should be noted that the test is only for the repellent test of mosquitoes in daily homes, not for all, and the purpose is also to reflect the mosquito repellent and insect repellent effect of the antibacterial textile fabric in daily activities.

[0105] 3. Skin allergy test

[0106] 30 healthy mice, 15 males and 15 females, weighing 25±1 g, were selected; 30 rabbits, 15 males and 15 females, weighing 2.5±0.1 kg, were selected, the hair on the abdomen of the mice and rabbits was shaved, and the antibacterial textile fabrics prepared in Example 4 of equal areas were attached to the abdomen of the mice and the abdomen of the rabbits, respectively, and observed continuously for 3 hours. After 3 hours, no redness, swelling or blisters appeared on the abdomen of the 30 mice and 30 rabbits. It was preliminarily judged that the antibacterial textile fabrics prepared by the present invention did not have adverse reactions such as allergies and inflammation to the skin, and it was preliminarily believed that the safety was relatively high.

[0107] In summary, the antibacterial textile fabric prepared by the present invention has a long-lasting and significant antibacterial effect and high safety performance, and can solve the problem that the antibacterial textile fabric in the prior art has poor antibacterial performance and safety performance and cannot meet market demand.

[0108] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0109] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. An antibacterial textile fabric, characterized in that: The antibacterial textile fabric comprises the following raw materials in parts by weight: 35 to 50 parts of modified wormwood fiber and 15 to 35 parts of cotton fiber; The modified wormwood fiber comprises the following raw materials in parts by weight: 20 to 35 parts of wormwood-based viscose, 10 to 20 parts of cellulose, 1 to 10 parts of a composite antibacterial agent, 5 to 10 parts of a binder, and 1 to 3 parts of a stabilizer; The composite antibacterial agent is composed of wormwood powder, diatomaceous earth-loaded titanium dioxide, organosilicon quaternary ammonium salt and alpha-methacrylic acid in a mass ratio of (1-5): (1-2): (3-15): (20-30).

2. The antibacterial textile fabric according to claim 1, characterized in that: The binder is water-based polyurethane.

3. The antibacterial textile fabric according to claim 1, characterized in that: The stabilizer is at least one of sodium alginate, hydroxyethyl cellulose and sodium carboxymethyl cellulose.

4. A method for preparing an antibacterial textile fabric, characterized in that: The preparation method is used to prepare the antibacterial textile fabric according to any one of claims 1 to 3, and the preparation method comprises the following steps: S1, adding wormwood powder, diatomaceous earth-loaded titanium dioxide, organosilicon quaternary ammonium salt and α-methacrylic acid into a mixing kettle, stirring and treating to obtain a composite antibacterial agent; S2, adding wormwood-based viscose, cellulose, composite antibacterial agent, binder and stabilizer into a mixing kettle, stirring, aging, and then spinning to obtain wormwood modified fiber; S3, interweaving and blending the modified wormwood fiber and the cotton fiber to prepare a blank; S4, soaking the blank in a treatment solution A to which an antifouling agent and an antioxidant have been added in advance, leaving it to stand for 20 minutes to 60 minutes, washing, drying, and then soaking it in a treatment solution B to which a softener has been added in advance, leaving it to stand for 10 minutes to 20 minutes, washing, and drying to obtain an antibacterial textile fabric.

5. The preparation method according to claim 4, characterized in that: The antifouling agent is ethylene phthalate.

6. The preparation method according to claim 4, characterized in that: The softener is at least one of softeners MS-20, AS-23N and GL-54.

7. The preparation method according to claim 4, characterized in that: The antioxidant is at least one of antioxidant 1010, antioxidant 168 and ultraviolet absorber UV-P.

8. The preparation method according to claim 7, characterized in that: The stirring conditions in step S1 are: temperature of 85° C. to 110° C., rotation speed of 50 r / min to 150 r / min, and time of 25 min to 40 min.

9. The preparation method according to claim 7, characterized in that: The stirring conditions in step S2 are: temperature of 80° C. to 100° C., rotation speed of 50 r / min to 150 r / min, and time of 20 min to 30 min.

10. The preparation method according to claim 7, characterized in that: The temperature of the aging treatment is 35° C. to 60° C., and the time is 5 h to 8 h.

Citation Information

Patent Citations

  • Deodorizing and moisture-regulating kieselguhr shoe pad

    CN103564979A

  • Antibacterial degradable composite material and application thereof in preparation of paper diapers

    CN110960720A

  • Medical protective clothing textile fabric and preparation method thereof and medical protective clothing

    CN111455669A

  • Cloth-based antibacterial wallpaper

    CN112227079A

  • Nanometer antifouling and antibacterial textile fabric and preparation method thereof

    CN113290971A

Cited By

  • Environment-friendly wormwood cloud wool and preparation method thereof

    CN121161447A