High-temperature-resistant electrolyte and lithium ion battery
By using optimized high-temperature resistant electrolytes, including lithium salts, functional additives and other additives in lithium-ion batteries, the problem of electrolyte decomposition and capacity loss in lithium-ion batteries under high temperature conditions is solved, and the high-temperature capacity maintenance and recovery rate is achieved The improvement meets the high-temperature use needs of special equipment.
Patent Information
- Application Number
- CN202411112497.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-06
AI Technical Summary
Existing lithium-ion batteries have electrolyte decomposition, voltage drop and irreversible capacity loss under high temperature conditions, making it difficult to meet the high-temperature use needs of special equipment.
A high-temperature resistant electrolyte is adopted, including lithium salts, functional additives and other additives. By optimizing the composition of the electrolyte, the high-temperature capacity retention rate and recharge and discharge capacity recovery rate of lithium-ion batteries are improved.
The electrolyte is stored at 60℃ for 28 days and the voltage remains above 4.25V, which significantly improves the high-temperature capacity retention and recovery rate of lithium-ion batteries and reduces safety hazards.
Smart Images

Figure CN119092826A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a high temperature resistant electrolyte and a lithium ion battery. Background Art
[0002] Lithium-ion batteries are currently the battery system with the best comprehensive performance. They have the characteristics of high specific energy, high cycle life, small size, light weight, no memory effect, and no pollution. They have developed into a new generation of energy storage power sources, used for power support for information technology, electric and hybrid vehicles, special equipment, etc. With the widespread use of electronic products, the industry has put forward higher requirements for the battery performance of lithium-ion batteries.
[0003] As the "blood" system of lithium-ion batteries, the electrolyte is in contact with the positive and negative electrodes and the diaphragm. It is an important medium for transmitting lithium ions and is closely related to the performance of the battery. The electrochemical performance of lithium-ion batteries is closely related to the interfacial properties of the electrode / electrolyte, and modifying the interfacial chemical composition and properties of the electrode through electrolyte additives is a simple and efficient means. Through the design and optimization of the electrolyte, not only can the cycle life of the battery be improved, but also the high-temperature performance of the battery can be improved. Especially for the power supply use scenarios of special equipment for certain environmental information collection work, the capacity retention and capacity utilization after long-term storage under high temperature conditions are particularly important. On the other hand, the lithium salts and organic solvents in the electrolyte have poor stability. Under high temperature conditions, they will decompose and produce a large amount of gas, causing the battery to swell, increasing safety hazards while reducing the effective migration of active lithium in the electrolyte. In summary, the high-temperature performance of lithium-ion battery electrolytes in the prior art is poor, and it is difficult to meet the use of special situations. Therefore, it is urgent to develop an electrolyte with good high-temperature performance to compensate for the above problems. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes a high temperature resistant electrolyte and a lithium ion battery.
[0005] The invention provides a high temperature resistant electrolyte comprising lithium salt, solvent, functional additives and other additives.
[0006] The functional additives include compounds of the structures shown in Formula I and Formula II:
[0007]
[0008] The R1, R2, and R3 are independently selected from one or more of H, C1-C12 alkyl, C1-C12 alkoxy, amine, and heterocyclic group.
[0009] Preferably, the heteroatom of the heterocyclic group is selected from one or more of oxygen and nitrogen.
[0010] The role of functional additives is to alleviate the problems of voltage drop, severe gas production or electrolyte decomposition caused by high temperature after lithium-ion batteries are stored at high temperatures, and to improve the high-temperature capacity retention rate of lithium-ion batteries and the capacity recovery rate of re-charge and discharge.
[0011] Preferably, the mass of the functional additive accounts for 0.1% to 5% of the total mass of the high temperature resistant electrolyte.
[0012] The quality of functional additives within a certain range helps to improve the high temperature resistance of the electrolyte.
[0013] Preferably, the other additives are selected from one or more of vinylene carbonate, vinyl carbonate, fluoroethylene carbonate, 4-methyl vinyl sulfate, 4-ethyl vinyl sulfate, 4-propyl vinyl sulfate, tris(trimethylsilyl)borate, trimethyl phosphate, dimethyl methylphosphonate, hexamethyldisilazane, methyl methyl disulfonate, 1,3-propane sultone, vinyl sulfate, vinyl sulfite, and ethylene carbonate.
[0014] Adding other additives to the electrolyte can help reduce ion transfer impedance and improve capacity retention.
[0015] More preferably, the mass of the other additives accounts for 0.5% to 5% of the total mass of the high temperature resistant electrolyte.
[0016] The quality of other additives within a certain range can help improve the high temperature resistance of the electrolyte.
[0017] Preferably, the solvent is selected from one or more of chain carbonate compounds, cyclic carbonate compounds or carboxylate compounds.
[0018] The function of the solvent is to dissolve the solute in the electrolyte and improve the high temperature resistance of the electrolyte.
[0019] More preferably, the cyclic carbonate compounds include ethylene carbonate and propylene carbonate; the chain carbonate compounds include dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate; and the carboxylate compounds include ethyl propionate and ethyl acetate.
[0020] More preferably, the mass of the solvent accounts for 65% to 85% of the total mass of the high temperature resistant electrolyte.
[0021] The quality of the solvent is within a certain range so that the prepared electrolyte has high-temperature storage characteristics.
[0022] Preferably, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(fluorosulfonyl imide), and lithium bis(trifluoromethanesulfonyl imide).
[0023] Preferably, the mass of the lithium salt accounts for 8% to 12.5% of the total mass of the high temperature resistant electrolyte.
[0024] Preferably, the molar concentration of the lithium salt is 0.5-1.5M.
[0025] The type, mass range, and molar concentration range of the lithium salt are appropriately selected to provide an appropriate amount of lithium source, synergize with the solvent, and enhance high temperature resistance.
[0026] The present invention also provides a lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator, and the above-mentioned electrolyte.
[0027] Preferably, the positive electrode material in the positive electrode sheet is one or more of transition metal lithium-intercalated oxides, metal oxides and metal sulfides.
[0028] Preferably, the negative electrode material in the negative electrode sheet is one or more of carbon-containing materials, silicon, silicon-carbon, silicon-oxygen, ferrite, nitride and alloy materials.
[0029] The beneficial effects of the present invention are:
[0030] The present invention provides a high temperature resistant electrolyte to meet the use scenarios of special equipment. The high temperature resistant electrolyte prepared by the present invention has high temperature storage characteristics, which solves the problems of many lithium ion batteries on the market that have voltage drop, severe gas production, or electrolyte decomposition caused by high temperature, and irreversible capacity loss after high temperature storage. The high temperature resistant electrolyte provided by the present invention has a voltage of more than 4.25V after being stored at 60°C for 28 days. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a performance data chart of a lithium battery prepared with the electrolyte proposed in the present invention after being stored at high temperature for 21D.
[0032] Figure 2 This is a performance data chart of a lithium battery prepared with the electrolyte proposed in the present invention after being stored at high temperature for 28D. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is described in detail through specific embodiments.
[0034] Unless otherwise specified, the materials, reagents, etc. used in the following examples and comparative examples can be obtained from commercial sources.
[0035] In the following examples and comparative examples, the structural formulas of the functional additives used are shown in Table 1:
[0036] Table 1 Structural formula of functional additive compounds 1 to 4
[0037]
[0038]
[0039] Example 1
[0040] Preparation of electrolyte: In an inert atmosphere glove box with a water content and an oxygen content of less than 5 ppm, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), ethyl acetate (EA), and ethyl propionate (EP) are prepared into an organic solvent in a mass ratio of 15:25:20:40, 3-(3-boran-2,4-dioxapent-3-yl)-1,3-oxaazacyclopentan-2-one (Compound 1) is slowly added, lithium hexafluorophosphate and lithium bistrifluoromethanesulfonyl imide are mixed in a mass ratio of 1:1 as lithium salt, added to the organic solution and stirred until dissolved, and then other additives are added, stirred thoroughly and completely dissolved to obtain an electrolyte. The other additives are composed of vinylene carbonate, 4-methyl vinyl sulfate, 4-ethyl vinyl sulfate, and 4-propyl vinyl sulfate in a mass ratio of 1:0.25:0.25:0.5. The mass fractions of lithium salt, organic solvent, other additives and functional additives in the electrolyte are 12%, 85%, 2% and 1% respectively.
[0041] Example 2
[0042] Preparation of electrolyte: In an inert atmosphere glove box with a water content and an oxygen content of less than 5 ppm, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), ethyl acetate (EA), and ethyl propionate (EP) are prepared into an organic solvent in a mass ratio of 15:25:20:40, 3-[(1,4-oxazacyclohexane-4-ylboryl)methyl]-1,3-oxazacyclopentane-2-one (Compound 2) is slowly added, lithium hexafluorophosphate and lithium bistrifluoromethanesulfonyl imide are mixed in a mass ratio of 1:1 as lithium salt, added to the organic solution and stirred until dissolved, and then other additives are added, stirred thoroughly and completely dissolved to obtain an electrolyte. The other additives are composed of vinylene carbonate, 4-methyl vinyl sulfate, 4-ethyl vinyl sulfate, and 4-propyl vinyl sulfate in a mass ratio of 1:0.25:0.25:0.5. The mass fractions of lithium salt, organic solvent, other additives and functional additives in the electrolyte are 12%, 85%, 2% and 1% respectively.
[0043] Example 3
[0044] Preparation of electrolyte: In an inert atmosphere glove box with a water content and an oxygen content of less than 5 ppm, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), ethyl acetate (EA), and ethyl propionate (EP) are prepared into an organic solvent in a mass ratio of 15:25:20:40, 5-(1,4-oxazacyclohexane-4-yl)-3-(4-bora-3,5-dioxahept-4-yl)-1,3-oxazacyclopentane-2-one (Compound 3) is slowly added, lithium hexafluorophosphate and lithium bistrifluoromethanesulfonyl imide are mixed in a mass ratio of 1:1 to form a lithium salt, added to the organic solution and stirred until dissolved, and then other additives are added, stirred thoroughly to completely dissolve, and an electrolyte is obtained. The other additives are composed of vinylene carbonate, 4-methyl vinyl sulfate, 4-ethyl vinyl sulfate, and 4-propyl vinyl sulfate in a mass ratio of 1:0.25:0.25:0.5. The mass fractions of lithium salt, organic solvent, other additives and functional additives in the electrolyte are 12%, 85%, 2% and 1% respectively.
[0045] Example 4
[0046] Preparation of electrolyte: In an inert atmosphere glove box with a water content and an oxygen content of less than 5 ppm, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), ethyl acetate (EA), and ethyl propionate (EP) are prepared into an organic solvent in a mass ratio of 15:25:20:40, and 3-[(dimethylboryl)methyl]-5-methyl-1,3-oxazacyclopentane-2-one (Compound 4) is slowly added, lithium hexafluorophosphate and lithium bistrifluoromethanesulfonyl imide are mixed in a mass ratio of 1:1 to form a lithium salt, added to the organic solution and stirred until dissolved, and then other additives are added, stirred thoroughly to completely dissolve, and an electrolyte is obtained. Other additives are composed of vinylene carbonate, 4-methyl vinyl sulfate, 4-ethyl vinyl sulfate, and 4-propyl vinyl sulfate in a mass ratio of 1:0.25:0.25:0.5. The mass fractions of lithium salt, organic solvent, other additives, and functional additives in the electrolyte are 12%, 85%, 2%, and 1%, respectively.
[0047] Comparative Example 1
[0048] Preparation of electrolyte: In an inert atmosphere glove box with water content and oxygen content less than 5ppm, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), ethyl acetate (EA), and ethyl propionate (EP) are prepared into an organic solvent in a mass ratio of 15:25:20:40, lithium hexafluorophosphate and lithium bis(trifluoromethanesulfonyl)imide are mixed into lithium salt in a mass ratio of 1:1, and the lithium salt is added into the organic solution and stirred until dissolved to obtain an electrolyte. The mass fractions of lithium salt and organic solvent in the electrolyte are 15% and 85%, respectively.
[0049] Comparative Example 2
[0050] Preparation of electrolyte: In an inert atmosphere glove box with water content and oxygen content less than 5ppm, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), ethyl acetate (EA), and ethyl propionate (EP) are prepared into an organic solvent in a mass ratio of 15:25:20:40, lithium hexafluorophosphate and lithium bis(trifluoromethanesulfonyl)imide are mixed into lithium salt in a mass ratio of 1:1, added to the organic solution and stirred until dissolved, and then other additives are added, stirred thoroughly and completely dissolved to obtain an electrolyte. Other additives are composed of vinylene carbonate, 4-methyl vinyl sulfate, 4-ethyl vinyl sulfate, and 4-propyl vinyl sulfate in a mass ratio of 1:0.25:0.25:0.5. The mass fractions of lithium salt, organic solvent, and other additives in the electrolyte are 12.3%, 85.6%, and 2.1%, respectively.
[0051] Comparative Example 3
[0052] Preparation of electrolyte: In an inert atmosphere glove box with water content and oxygen content less than 5ppm, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), ethyl acetate (EA), and ethyl propionate (EP) were prepared into an organic solvent in a mass ratio of 15:25:20:40, lithium hexafluorophosphate and lithium bis(trifluoromethanesulfonyl)imide were mixed into lithium salt in a mass ratio of 1:1, added into the organic solution and stirred until dissolved, and a small amount of functional additive 3-[(dimethylboryl)methyl]-5-methyl-1,3-oxazacyclopentane-2-one (Compound 4) was added to obtain an electrolyte. The mass fractions of lithium salt, organic solvent, and functional additive in the electrolyte were 12.3%, 85.6%, and 1.1%, respectively.
[0053] The above electrolyte is assembled with the positive electrode sheet, the negative electrode sheet and the separator into a lithium ion battery, specifically comprising: mixing the positive electrode material active substance (lithium iron phosphate), the conductive agent acetylene black and the binder polytetrafluoroethylene in a mass ratio of 95:2.5:2.5, then adding N-methylpyrrolidone, stirring evenly to obtain a uniform slurry, coating the slurry evenly on a 15um thick aluminum foil, and drying to obtain a positive electrode sheet; making a soft-pack laminated battery in a dry environment with a dew point temperature controlled below -40°C, stacking the prepared positive electrode sheet, separator and graphite negative electrode sheet in sequence, ensuring that the separator completely separates the positive and negative electrode sheets, and packaging and welding the pole ears with aluminum-plastic film to form a battery to be injected, baking the battery water content to below 300ppm before injection, and then injecting the above lithium ion battery electrolyte, sealing and letting it stand and retaining the air bag, and the lithium ion battery is completed.
[0054] The performance of the batteries prepared in the examples of the present invention and the comparative examples was tested.
[0055] High temperature storage capacity retention and recovery test: The battery cell to be tested is placed at room temperature of 22℃ for 6 minutes, then charged to 4.25V at 2.4A with constant current and constant voltage, and the cut-off current is 0.12A, and then discharged to 2.8V at a constant current rate of 0.2C0 to obtain the normal temperature discharge capacity, and the average of the three-week discharge capacity is taken as the reference capacity C0. The battery cell to be tested is fully charged to the cut-off voltage and placed in a 60℃ high temperature cabinet for 28 days, and the capacity is retained after being taken out and cooled to room temperature every seven days. The first discharge capacity C1 is recorded at a constant current charge and discharge rate of 1C / 1C, and the cut-off conditions are the same as those at room temperature. Then, it is charged and discharged at a rate of 0.33C for 3 cycles, and the last small current discharge capacity is recorded as C2, and the above test steps are repeated. Calculate the high temperature storage capacity retention rate, and the specific calculation formula is: high temperature storage capacity retention rate = (C1 / C0)*100%, recovery rate = (C2 / C0)*100%.
[0056] The above comparative examples and embodiments were subjected to a capacity retention test after high temperature storage (60° C., 4*7=28 Days), and the test results are shown in Table 2 (average values of multiple groups of tests were recorded).
[0057] Table 2
[0058]
[0059]
[0060] It can be seen from the data in Table 2 that the battery assembled by the electrolyte prepared by the present invention has a high capacity retention rate under the high temperature 60°C shelf test, and the capacity recovery rate of the recharge and discharge after shelf is high, indicating that the electrolyte prepared by the present invention has excellent high temperature resistance. It can be seen from the data of Comparative Example 1 and the embodiment that the addition of high temperature resistant functional additives and the cooperation of other basic film-forming additives can effectively improve the capacity retention and recovery performance of the battery under high temperature conditions of the system, that is, more capacity can be provided under the same high temperature conditions; it can be seen from the data of Comparative Example 2 and the embodiment that the electrolyte system without adding high temperature functional additives reduces the capacity by nearly 10% at 60°C for 28 days, which will be more obvious under the enlarged system; it can be seen from the data of Comparative Example 3 and the embodiment that the absence of basic additives that help positive and negative electrode film formation will greatly reduce the capacity, and the capacity retention cannot be effectively improved despite the presence of high temperature stable additives, which is related to the cooperation between the two in the embodiment. The basic additive forms a stable positive and negative electrode protective film in the formation stage, so that the initial performance is stably improved, and the subsequent high temperature stable additive slowly oxidizes and loses electrons under high temperature conditions to reduce the oxidation of additives, solvents or protective films, thereby stabilizing the high temperature performance of the battery. The above comparative example can effectively show that the cooperation between the two additives is helpful for the stability of the system under high temperature conditions.
[0061] In summary, the lithium-ion battery prepared with the electrolyte provided by the present invention has excellent high temperature resistance.
[0062] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A high temperature resistant electrolyte, characterized in that: Including lithium salts, solvents, functional additives and other additives; The functional additives include compounds of the structures shown in Formula I and Formula II: The R1, R2, and R3 are independently selected from one or more of H, C1-C12 alkyl, C1-C12 alkoxy, amine, and heterocyclic group.
2. The high temperature resistant electrolyte according to claim 1, characterized in that: The mass of the functional additive accounts for 0.1% to 5% of the total mass of the high temperature resistant electrolyte.
3. The high temperature resistant electrolyte according to claim 1, characterized in that: The other additives are selected from one or more of vinyl carbonate, vinyl carbonate, fluoroethylene carbonate, 4-methyl vinyl sulfate, 4-ethyl vinyl sulfate, 4-propyl vinyl sulfate, tris(trimethylsilyl)borate, trimethyl phosphate, dimethyl methylphosphonate, hexamethyldisilazane, methyl disulfonate, 1,3-propane sultone, vinyl sulfate, vinyl sulfite, and ethylene carbonate.
4. The high temperature resistant electrolyte according to claim 1, characterized in that: The mass of the other additives accounts for 0.5% to 5% of the total mass of the high temperature resistant electrolyte.
5. The high temperature resistant electrolyte according to claim 1, characterized in that: The solvent is selected from one or more of chain carbonate compounds, cyclic carbonate compounds or carboxylate compounds; the cyclic carbonate compounds include ethylene carbonate and propylene carbonate; the chain carbonate compounds include dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate; the carboxylate compounds include ethyl propionate and ethyl acetate.
6. The high temperature resistant electrolyte according to claim 1, characterized in that: The mass of the solvent accounts for 65% to 85% of the total mass of the high temperature resistant electrolyte.
7. The high temperature resistant electrolyte according to claim 1, characterized in that: The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalato)borate, lithium difluorooxalato)borate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide; the mass of the lithium salt accounts for 8% to 12.5% of the total mass of the high temperature resistant electrolyte; and the molar concentration of the lithium salt is 0.5 to 1.5M.
8. A lithium ion battery comprising a positive electrode sheet, a negative electrode sheet, a separator, and the electrolyte according to any one of claims 1 to 7.
Citation Information
Patent Citations
Electrolyte and secondary battery containing same
CN105958110A
Electrolyte and lithium ion battery containing same
CN112331922A
Silyl-containing oxazolidinone lithium ion battery electrolyte and battery
CN113363576A
Electrolyte and lithium ion battery
CN115763970A
Electrolyte for lithium ion battery as well as preparation method and application of electrolyte
CN117558986A