Laminate and method for manufacturing eyeglass lens

The laminate structure with a water-repellent and metal layer addresses the challenge of precise grinding and efficient metal layer removal in eyeglass lens manufacturing, achieving small deviations and easy metal layer removal.

WO2024219214A1PCT designated stage expired Publication Date: 2024-10-24NIKON ESSILOR
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013575
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-02
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing methods for manufacturing eyeglass lenses struggle with achieving precise grinding with minimal axial and horizontal deviation, and efficient removal of metal layers, particularly when using laminates with water-repellent and metal layers.

Method used

A laminate structure comprising an eyeglass lens base material, a water-repellent layer, and a metal layer in that order, where the metal layer includes aluminum, zinc, or copper, allowing for precise fixation and grinding with a fixing member, followed by removal of the metal layer post-grinding.

Benefits of technology

This approach enables grinding with small axial and horizontal deviations and facilitates easy removal of the metal layer, improving the manufacturing process for eyeglass lenses by ensuring accurate shaping and efficient layer removal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013575_24102024_PF_FP_ABST
    Figure JP2024013575_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure addresses the problem of providing a laminate that can be polished with small axial and horizontal deviations. This laminate has an eyeglass lens substrate, a water-repellent layer, and a metal layer in this order. The metal layer contains at least one selected from the group consisting of aluminum, zinc, copper, and nickel.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate and method for manufacturing eyeglass lenses

[0001] The present disclosure relates to a laminate and a method for manufacturing an eyeglass lens.

[0002] Patent Document 1 discloses "a method for edging an oil-repellent coated eyeglass lens by edging an oil-repellent coated lens into various lens shapes using an edging machine, the method comprising the steps of: attaching adhesive tape, which has a thickness of 10 to 100 μm and a Young's modulus of 1 GPa or more and has a silicone adhesive coated on the surface of the polymer film, to both sides of the lens to be processed; and then setting the lens in the edging machine."

[0003] Japanese Patent Application Laid-Open No. 2004-347660

[0004] The present disclosure relates to a laminate having an eyeglass lens substrate, a water-repellent layer, and a metal layer in this order, wherein the metal layer contains at least one selected from the group consisting of aluminum, zinc, copper, and nickel (embodiment 1). The laminate of the present disclosure enables grinding with small axial and horizontal deviations.

[0005] The present disclosure also relates to a method for manufacturing a spectacle lens (embodiment 2), which includes step 1 of pressing a fixing member against the metal layer of a laminate having a spectacle lens substrate, a water-repellent layer, and a metal layer in this order to fix the laminate and grinding the periphery of the laminate, and step 2 of removing the metal layer in the ground laminate, wherein the metal layer contains at least one selected from the group consisting of aluminum, zinc, copper, and nickel.

[0006] 1 is a schematic cross-sectional view of a laminate;

[0007] The laminate of the present disclosure will be described in detail below. In this specification, the word "to" means that the numerical values ​​before and after it are included as the lower limit and upper limit.

[0008] [First embodiment: Laminate] The laminate is preferably used to fix the laminate by pressing a fixing member against the metal layer in the laminate and then grinding. In other words, it is preferably used in step 1 of the manufacturing method of an eyeglass lens, which will be described later. FIG. 1 is a cross-sectional schematic diagram of a laminate 100. The laminate 100 has an antireflection layer 4 on an eyeglass lens substrate 2, a water-repellent layer 6 on the antireflection layer 4, and a metal layer 8 on the water-repellent layer 6. The laminate 100 does not necessarily have to have the antireflection layer 4. The laminate 100 may also further have a primer layer and / or a hard coat layer, which will be described later. Unlike the laminate 100 of FIG. 1 , the laminate may have a water-repellent layer and a metal layer on only one surface of the eyeglass lens substrate, or may have a water-repellent layer and a metal layer on both surfaces of the eyeglass lens substrate.

[0009] The luminous transmittance of the laminate is preferably less than 100%, more preferably 90% or less, and even more preferably 88% or less. The lower limit is preferably 0% or more, more preferably 10% or more, and even more preferably 20% or more. An example of a method for adjusting the luminous transmittance is a method for adjusting the thickness of each layer (e.g., a metal layer) of the laminate. The luminous transmittance is the average value of transmittance in the wavelength range of 380 to 780 nm, and can be measured using a spectrometer.

[0010] <Eyeglass Lens Substrate> Examples of the eyeglass lens substrate include eyeglass lens substrates made of organic or inorganic materials, with eyeglass lens substrates made of organic materials (such as plastic lens substrates) being preferred. Examples of eyeglass lens substrates include finished lenses in which both the convex and concave surfaces are optically finished and molded to the desired dioptric power, semi-finished lenses in which only the convex surface is finished as an optical surface (e.g., spherical, rotationally symmetric aspherical, and progressive surfaces), and semi-finished lenses in which the concave surface is processed and polished to match the wearer's prescription. Examples of organic materials include acrylic resins, methacrylic resins, thiourethane resins, allyl resins, episulfide resins, polycarbonate resins, polyurethane resins, polyester resins, polystyrene resins, polyethersulfone resins, poly(4-methylpentene-1) resins, diethylene glycol bisallyl carbonate resins (CR-39), and polyvinyl chloride resins.

[0011] The thickness of the spectacle lens substrate is preferably 1 to 30 mm from the viewpoint of ease of handling. The spectacle lens substrate may be opaque or colored, as long as it has light-transmitting properties.

[0012] <Water-Repellent Layer> The laminate has a water-repellent layer on the spectacle lens substrate. The water-repellent layer preferably contains at least one selected from the group consisting of organosilicon compounds, their hydrolysates, and their hydrolyzed condensates. The hydrolyzate of an organosilicon compound refers to a compound produced by hydrolyzing the hydrolyzable groups in an organosilicon compound having hydrolyzable groups. The hydrolyzate of an organosilicon compound may be a complete hydrolyzate in which all of the hydrolyzable groups in the organosilicon compound have been hydrolyzed, a partial hydrolyzate in which some of the hydrolyzable groups have been decomposed, or a mixture thereof. The hydrolyzed condensate of an organosilicon compound refers to a compound produced by condensing the hydrolyzed organosilicon compound having hydrolyzable groups. The hydrolyzed condensate of an organosilicon compound may be a complete hydrolyzed condensate in which all of the hydrolyzed groups in the hydrolyzate have been condensed, a partial hydrolyzed condensate in which only some of the hydrolyzed groups have been condensed, or a mixture thereof.

[0013] Examples of the organosilicon compound include a silane compound, a silazane compound, a silanol compound, a siloxane compound, a silicate compound, and a silyl ester compound, with the silane compound being preferred.

[0014] Examples of the hydrolyzable group include an alkoxy group, a halogen atom, a cyano group, an acetoxy group, and an isocyanate group.

[0015] The organosilicon compound preferably has a fluorine atom-containing group, such as a group having a perfluorocarbon structure or a group having a perfluoropolyether structure.

[0016] Examples of the organosilicon compound include those described in WO 2020 / 039795, U.S. Pat. No. 4,410,563, EP 0,203,730, EP 749,021, EP 844,265, and EP 933,377.

[0017] The thickness of the water-repellent layer is preferably 1 to 1000 nm.

[0018] <Metal Layer> The laminate has a metal layer on the water-repellent layer. The laminate preferably has a metal layer adjacent to the water-repellent layer. When the laminate has a metal layer, it has excellent adhesion to the fixing member in step 1 described below, and therefore, when grinding the laminate, it is easy to grind it into a desired shape with little axial deviation, etc. Furthermore, the metal layer is a layer that is removed after grinding.

[0019] The metal layer contains at least one metal selected from the group consisting of aluminum, zinc, copper, and nickel (hereinafter also referred to as the "specific metal"), and preferably contains aluminum. The specific metal may be either a pure metal or an alloy, and a pure metal is preferred. As long as the metal layer contains the specific metal, it may also contain other metals. Examples of other metals include known metals.

[0020] The content of the specific metal (preferably aluminum) is preferably 50% by mass or more, more preferably 80% by mass or more, still more preferably 95% by mass or more, and particularly preferably 99% by mass or more, based on the total mass of the metal layer. The upper limit is preferably 100% by mass or less.

[0021] The thickness of the metal layer is preferably 0.1 to 200.0 nm, more preferably 1.0 to 100.0 nm, and even more preferably 5.0 to 80.0 nm.

[0022] <Other Layers> The laminate may have other layers in addition to the above layers. Examples of other layers include a primer layer, a hard coat layer, an anti-reflection layer, and an intermediate layer. When the laminate has an intermediate layer, the laminate preferably has the intermediate layer on the side of the water-repellent layer opposite the metal layer. When the laminate has other layers, the laminate preferably further has a primer layer, a hard coat layer, and an anti-reflection layer, in this order from the spectacle lens substrate side, between the spectacle lens substrate and the water-repellent layer.

[0023] The primer layer is a layer that improves the adhesion of the hard coat layer to the eyeglass lens substrate. The primer layer preferably contains a resin, more preferably a urethane resin, an epoxy resin, a phenol resin, a polyimide resin, a polyester resin, a bismaleimide resin, or a polyolefin resin. The thickness of the primer layer is preferably 0.3 to 2 μm.

[0024] The hard coat layer is a layer disposed on a spectacle lens substrate and provides scratch resistance to the spectacle lens substrate. Examples of hard coat layers include organic hard coat layers, inorganic hard coat layers, and organic-inorganic hybrid hard coat layers. The thickness of the hard coat layer is preferably 1.0 to 20.0 μm, and more preferably 1.5 to 15.0 μm.

[0025] The composition for forming a hard coat layer preferably contains at least one selected from the group consisting of an inorganic compound, a polymerization initiator, and an organic solvent. Examples of the inorganic compound include inorganic oxides and silsesquioxanes.

[0026] The inorganic oxide is preferably a metal oxide particle. Examples of the metal oxide particle include oxide particles of at least one metal selected from the group consisting of Ti, Zr, Si, Al, Sn, Sb, Ta, Ce, La, Fe, Zn, W, and In, and composite metal oxide particles thereof. Composite metal oxide particles are oxide particles containing two or more metals (metal atoms). The inorganic oxide particle is preferably a SiO 2 (silicon oxide), Al 2 O 3 (aluminum oxide), SnO 2 (tin oxide), ZrO 2 (zirconium oxide) and TiO 2 (titanium oxide), and SiO 2 and ZrO 2 It is more preferable that the composition contains at least one selected from the group consisting of:

[0027] Silsesquioxane is a silane compound obtained by hydrolysis of a trifunctional silane compound such as alkoxysilane, chlorosilane, or silanol.

[0028] The antireflection layer may have either a single-layer structure or a multilayer structure. The antireflection layer is preferably an inorganic antireflection layer. By inorganic antireflection layer is meant an antireflection layer composed of an inorganic compound. An antireflection layer having a multilayer structure may have a structure in which high-refractive-index layers and low-refractive-index layers are alternately laminated. The high-refractive-index layers preferably contain an oxide of titanium, zirconium, aluminum, niobium, tantalum, or lanthanum. The low-refractive-index layers preferably contain a silica compound. The thickness of the antireflection layer is preferably 0.2 to 3.0 μm, more preferably 0.3 to 2.0 μm.

[0029] [Method for producing laminate] Examples of the method for producing the laminate include known production methods. As the method for producing the laminate, a method for producing a laminate including a step of forming a water-repellent layer on a spectacle lens substrate and a step of forming a metal layer on the water-repellent layer is preferred.

[0030] The step of forming the water-repellent layer is preferably a step of applying a water-repellent layer-forming composition onto a spectacle lens substrate and curing it. Examples of methods for applying the water-repellent layer-forming composition include dip coating, roll coating, bar coating, spin coating, spray coating, die coating, and gravure coating. Examples of curing methods include drying, which may or may not be heated during drying. The water-repellent layer-forming composition is a composition containing various components that may be contained in the water-repellent layer described above, and preferably further contains an organic solvent.

[0031] Examples of the process for forming the metal layer include dry film-forming methods such as physical vapor deposition and chemical vapor deposition, and wet film-forming methods such as coating, with physical vapor deposition being preferred. Physical vapor deposition methods include vapor deposition methods such as thermal evaporation and electron beam evaporation, and sputtering, with thermal evaporation being preferred in that it can reduce damage to the laminate (e.g., the water-repellent layer, etc.). The dry film-forming method and the wet film-forming method may be carried out under normal pressure, reduced pressure, or high pressure, with reduced pressure being preferred.

[0032] The method for producing the laminate also preferably includes the steps of forming a primer layer on the spectacle lens substrate, forming a hard coat layer on the primer layer, forming an antireflection layer on the hard coat layer, forming a water-repellent layer on the antireflection layer, and forming a metal layer on the water-repellent layer. The steps of forming the water-repellent layer and the metal layer are as described above.

[0033] The step of forming the primer layer is preferably a method of applying a primer layer-forming composition onto a spectacle lens substrate. The step of forming the primer layer may include a drying step. Heating may or may not be performed during drying.

[0034] The step of forming a hard coat layer is preferably a method of applying a hard coat layer-forming composition onto a primer layer and curing it. Examples of the method of applying the hard coat layer-forming composition include the above-mentioned method of applying the water-repellent layer-forming composition. For example, when using a dipping coating method, a spectacle lens substrate having a primer layer is immersed in the hard coat layer-forming composition, and then the spectacle lens substrate having the primer layer is pulled up and dried, thereby forming a coating film derived from the hard coat layer-forming composition on the primer layer of the spectacle lens substrate.

[0035] Examples of the curing method include heat treatment and exposure treatment. The conditions for the heat treatment and the light irradiation treatment can be appropriately adjusted depending on the various components contained in the composition for forming a hard coat layer. Examples of the type of light used for light irradiation include ultraviolet light and visible light. Examples of the light source include a high-pressure mercury lamp. The integrated light amount used for light irradiation is 100 to 10,000 mJ / cm from the viewpoints of productivity and curability of the coating film. 2 is preferred, and 100 to 5000 mJ / cm 2 is more preferred.

[0036] The anti-reflection layer can be formed by a dry method such as vacuum deposition, sputtering, ion plating, ion beam assisted deposition, or CVD.

[0037] Second Embodiment: Manufacturing Method of Spectacle Lens A manufacturing method of a spectacle lens includes Step 1 of pressing a fixing member against the metal layer of a laminate having a spectacle lens substrate, a water-repellent layer, and a metal layer in this order to fix the laminate, and grinding the periphery of the laminate, and Step 2 of removing the metal layer in the ground laminate, wherein the metal layer contains a specific metal.

[0038] The laminate in the method for manufacturing a spectacle lens is the same as the laminate described above, and the preferred embodiments are also the same.

[0039] Step 1 is a so-called edge grinding process, in which the laminate is machined into a predetermined shape by grinding the periphery of the laminate. Grinding can be performed using a known grinding device. FIG. 2 is a schematic diagram of a grinding device 300 used in step 1, and step 1 will be described in detail with reference to FIG. 2. First, the laminate 200 is placed between a fixing member 60 and a lens processing shaft 52 so that the fixing member 60 contacts the metal layer 40 of the laminate 200, and the fixing member 60 is pressed against the fixing member 60 to fix the laminate 200. That is, the laminate 200 is pressed and fixed between the fixing member 60 and the lens processing shaft 52. Also, in FIG. 2, the fixing member 60 includes a lens processing shaft 51, a lens lock cap 30 fixed to the tip of the lens processing shaft 51, and an adhesive tape 20 attached to the surface of the lens lock cap 30. The surface of the adhesive tape 20 opposite the surface of the lens lock cap 30 contacts the metal layer of the laminate 200, but this is not a limitation.

[0040] An example of the grinding device 300 is LE-9000X (manufactured by Nidek Co., Ltd.), and an example of the adhesive tape 20 is LEAPIII (manufactured by 3M Co., Ltd.).

[0041] Next, the laminate 200 is rotated by rotating the fixing member 60 and the lens processing shaft 52, and the laminate 200 is ground into a predetermined shape by pressing a rotating grindstone against the periphery of the laminate 200. Examples of the grinding method in step 1 include the edging processes described in JP-A-2007-156226, JP-A-2003-141607, and JP-A-2007-505937.

[0042] Step 2 is a step of removing the metal layer from the ground laminate. Examples of methods for removing the metal layer include a method of removing the metal layer by tape peeling, a method of removing the metal layer using a release agent, a dry wiping method, and a combination thereof. In terms of efficient removal of the metal layer, a method of removing the metal layer by tape peeling or a method of removing the metal layer using a release agent is preferred. Examples of dry wiping include a method of rubbing the metal layer with a wipe. Examples of tape peeling include a method of peeling the metal layer using a known tape. Examples of release agents include organic solvents such as alcohol solvents, water, and mixtures thereof, with alcohol solvents being preferred. The release agent may contain an anionic surfactant, a cationic surfactant, and / or an amphoteric surfactant. The release agent may be acidic, neutral, or alkaline.

[0043] The present disclosure will be explained in more detail below with reference to examples and comparative examples, but is not limited to these examples.

[0044] [Preparation of Laminate] The laminates used in Examples 1 to 3 were prepared by the following procedure. ECC (trade name, manufactured by Nikon-Essilor) was used as the eyeglass lens 1. The eyeglass lens had an eyeglass lens substrate (diameter 70 mm, -10.00D) with a refractive index of 1.60, a primer layer, a hard coat layer, an anti-reflection layer, and a water-repellent layer, in this order. Furthermore, using a physical vapor deposition apparatus (BC-P: manufactured by Shincron, or 1200-DLX2: manufactured by Satisloh), an aluminum layer with a purity of 99% by mass or more was formed by thermal vapor deposition on the water-repellent layer of the eyeglass lens 1 while adjusting the thickness so as to achieve the luminous transmittance shown in the table below, thereby obtaining the laminate 1. Note that when forming the aluminum layer, a boat made of a tungsten-tantalum alloy was used as the deposition board, and the aluminum layer was evaporated under reduced pressure (1 × 10 -3 ~1 x 10 -2 The experiment was carried out at 1000 kJ / min.

[0045] Laminates 2 and 3 were formed by adjusting the thickness of an aluminum layer with a purity of 99% by mass or more on the water-repellent layer of eyeglass lens 1, with reference to the procedure for Laminate 1 described above, so as to achieve the luminous transmittance shown in the table below.

[0046] The spectacle lens used in Comparative Example 1 was used for evaluation as it was, without forming an aluminum layer on the spectacle lens 1.

[0047] <Evaluation> (Luminous transmittance of laminate) The luminous transmittance of the laminate was measured using a spectrometer (LED spectrometer, manufactured by Fuji Kohden Kogyo Co., Ltd.).

[0048] (Axial deviation and horizontal deviation) Step 1 was performed using the obtained laminate or eyeglass lens, and the axial deviation and horizontal deviation after grinding were evaluated. The optical center of the laminate was identified using a lens meter (LM-1200, manufactured by Nidek Co., Ltd.), and a total of three points, including the optical center, were marked on the surface of the metal layer of the laminate so that they were equidistant from the surface of the metal layer on any line passing through the optical center. Next, using a lens blocker (CE-1, manufactured by Nidek Co., Ltd.), double-sided tape (LEAP III, manufactured by 3M Co., Ltd.) was attached to the laminate, centered on a point shifted by the amount of eccentricity from the optical center (a point on a line passing through the above three points and shifted 5 mm from the optical center), and a lens lock cap was further attached on top of the tape. The lens lock cap with the laminate attached was fitted into one of the lens processing shafts of a edging machine, and then the laminate was sandwiched and fixed between the lens lock cap and the other processing shaft. The edging process was performed with the eccentricity set to zero on the edging machine side. The equipment and tools used for the edging process are as follows: The eyeglass lenses were also subjected to edging process using the same procedure as for the laminate.

[0049] Lens grinding machine: LE-9000X (manufactured by Nidek), chuck pressure: 50 kg. Lens shape: Nikon Classico, product number 9018 (approximately octagonal shape, 48 mm wide, 30 mm high and 30 mm long). Lens lock cap: minimum size cap (manufactured by Nidek).

[0050] The positions of the three marked points on the laminate after grinding were evaluated using a profile projector V-16E (manufactured by Nikon Corporation), and the axial deviation (amount of rotational axis deviation) and horizontal deviation (amount of parallel axis deviation) from the design values ​​were measured and evaluated according to the following evaluation criteria.

[0051] - Evaluation criteria for axial deviation - "A": Absolute value of axial deviation is 1.000° or less. "B": Absolute value of axial deviation is more than 1.000° and less than 1.500°. "C": Absolute value of axial deviation is more than 1.500°.

[0052] - Evaluation criteria for horizontal deviation - "A": Absolute value of horizontal deviation is 0.500 mm or less "B": Absolute value of horizontal deviation is more than 0.500 mm and less than 1.000 mm "C": Absolute value of horizontal deviation is more than 1.000 mm

[0053] (Metal Layer Removability) The metal layer of the laminate ground in the evaluation of the axial deviation and the horizontal deviation was removed using tape peeling or ethanol. In the tape peeling, Nichiban 405 cellophane tape (18 mm wide, 10 mm long) was attached to the metal layer and the tape was peeled off three times, and the metal layer remaining on the eyeglass lens was visually confirmed after the tape peeling. In all Examples, the metal layer was almost completely removed. In the removal using ethanol, the metal layer was rubbed several times with a wipe soaked in ethanol, and the metal layer was completely removed in all Examples, and the metal layer was removed more cleanly than with the tape peeling.

[0054] In the table, the thickness of the metal layer was measured using a quartz crystal film thickness meter for each laminate before grinding. The values ​​for axial and horizontal deviation indicate the absolute value of the amount of deviation.

[0055]

[0056] As shown in Table 1, it was confirmed that when the laminate of the present disclosure was used, grinding could be performed with small axial deviation and horizontal deviation. A comparison of Examples 1 to 3 confirmed that horizontal deviation could be further reduced when the luminous transmittance of the laminate was 90% or less. The luminous transmittance of the laminate decreased as the thickness of the metal layer increased. Therefore, it is presumed that the laminates of Examples 1 and 2 had metal layers of appropriate thickness, which made the laminate more easily fixed, and therefore had better horizontal deviation.

[0057] 2: Spectacle lens substrate 4: Anti-reflection layer 6: Water-repellent layer 8: Metal layer 20: Adhesive tape 30: Lens lock cap 51, 52: Lens processing shaft 60: Fixing member 100, 200: Laminate 300: Grinding device

Claims

1. A laminate having, in this order, a spectacle lens substrate, a water-repellent layer, and a metal layer, wherein the metal layer contains at least one selected from the group consisting of aluminum, zinc, copper, and nickel.

2. The laminate according to claim 1, wherein the metal layer contains aluminum, and the content of the aluminum is 95 mass % or more based on the total mass of the metal layer.

3. The laminate according to claim 1 or 2, further comprising a primer layer, a hard coat layer and an anti-reflection layer, in this order from the eyeglass lens substrate side, between the eyeglass lens substrate and the water-repellent layer.

4. The laminate according to any one of claims 1 to 3, which is used for grinding by pressing a fixing member against the metal layer to fix the laminate.

5. A method for manufacturing a spectacle lens, comprising: step 1 of pressing a fixing member against a metal layer of a laminate having a spectacle lens substrate, a water-repellent layer, and a metal layer in this order to fix the laminate, and grinding the periphery of the laminate; and step 2 of removing the metal layer in the ground laminate, wherein the metal layer comprises at least one selected from the group consisting of aluminum, zinc, copper, and nickel.

6. The method of claim 5, wherein the metal layer is formed by thermal evaporation.

7. The method for manufacturing a spectacle lens according to claim 5 or 6, wherein in step 2, the metal layer is removed by tape peeling, or the metal layer is removed using a stripping agent.

Citation Information

Patent Citations

  • Gas barrier film and its manufacture, and laminated material in which gas barrier film is used

    JP2000006297A

  • Method for producing glass suitable for trimming, glass obtained thereby, and method for trimming the glass

    JP2005505427A

  • Adhesive tape and lens shape processing method for spectacle lens

    JP2007156226A

  • Optical articles with antifouling coatings

    JP2010508541A