A method for treating metal with an efficient cleaning agent
An electrochemical polishing method with a specialized cleaning agent and power supply regimen addresses surface defects in aluminum alloys, achieving low roughness and high corrosion resistance for improved surface quality.
Patent Information
- Application Number
- CN202210963510.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-11
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-08-11
AI Technical Summary
Aluminum and aluminum alloy workpieces suffer from surface defects such as pores, abrasions, and scratches, which affect their surface flatness, brightness, and corrosion resistance, making them unsuitable for high-quality applications.
An electrochemical polishing method using a cleaning agent composed of polyol, perchloric acid, polyol amine, mercaptosulfonyl ionic compound, and pyridinium salt compound, combined with a specific power supply regimen, to achieve low roughness, high flatness, and corrosion resistance.
The method effectively polishes metal surfaces to achieve low roughness, high flatness, and improved corrosion resistance, enhancing their decorative and functional properties.
Smart Images

Figure CN115261966B_ABST
Abstract
Description
Technical Field
[0001] The invention discloses a method for treating metal with a high-efficiency cleaning agent, and particularly relates to the field of aluminum alloy surface cleaning. Technical Background
[0002] In nature, aluminum is the most abundant metal element, accounting for 8.3% of the earth's crust. Aluminum and aluminum alloy products have the advantages of low specific gravity, good electrical and thermal conductivity, high specific strength, high temperature resistance, corrosion resistance of various media, fatigue resistance and good reflection of light and heat. They are typical light alloy materials and are widely used in civil, construction, machinery manufacturing, science and technology, military, electronics and electrical, transportation, aerospace and chemical industries. The continuous development of science and technology and industrial technology has put forward higher requirements and standards for the surface quality of aluminum and aluminum alloy workpieces, especially for the gloss and flatness of the workpiece surface. Therefore, in order to make aluminum and aluminum alloy workpieces meet the use standards of industrial production and life, the surface of aluminum and aluminum alloy workpieces usually needs to achieve a sand surface or mirror decorative effect.
[0003] However, aluminum and aluminum alloys have low hardness and poor wear resistance. Aluminum and aluminum alloy materials cause mechanical damage to workpieces during manufacturing, and produce defects such as pores, abrasions, bumps, scratches, and wear on the surface of aluminum and aluminum alloy workpieces. Due to the existence of these surface defects, the beauty and application value of aluminum and aluminum alloy workpieces are greatly affected, and the surface flatness and brightness of aluminum and aluminum alloy workpieces are reduced. Not only that, the existence of these defects particularly affects the chemical stability of the workpiece, and the impact on corrosion resistance is particularly obvious. Local corrosion often occurs preferentially at the surface defects of the workpiece, greatly shortening the service life of the workpiece. Therefore, solving the problem of surface defects of aluminum and aluminum alloy products is a top priority for achieving the continued development of the aluminum and aluminum alloy industry. In order to eliminate these surface defects and obtain higher surface brightness and better decorative effects, aluminum and aluminum alloy workpieces are usually surface treated.
[0004] According to different working principles and process characteristics, polishing technology can be divided into three categories: mechanical polishing, electrochemical polishing (electrolytic polishing) and chemical polishing. Surface polishing technology can be used as the final treatment of the surface of aluminum and aluminum alloy workpieces, or as a pre-treatment process for anodizing and electroplating of aluminum and aluminum alloys. Each polishing method has its advantages and disadvantages. Different polishing methods will result in different polishing effects on aluminum and aluminum alloys after treatment, which are mainly reflected in the polishing process, polishing cost, surface finish of the workpiece and the impact on the atmospheric environment.
[0005] Mechanical polishing is to grind and roll the very fine polishing paste applied on the polishing disc and the surface of the workpiece to be processed under the action of external force, remove the raised part of the workpiece to be processed, and make the uneven surface flat and smooth. However, during the mechanical polishing process, the surface of the workpiece is affected by factors such as extrusion and heat, and a new crystal deformation layer will be formed on the surface of the workpiece, destroying the surface structure of the workpiece, so that the polished aluminum alloy workpiece still has problems and cannot meet the product use requirements. For example, the surface finish of the workpiece after polishing is not enough, the corrosion resistance is poor, and stress corrosion or intergranular corrosion is easy to occur. Although the surface of the workpiece can be sufficiently flat and bright after mechanical polishing, if such a workpiece is directly anodized, a high-quality film layer with excellent decorative effect cannot be obtained. In addition, mechanical polishing can only polish some workpieces with simple appearance and structure. For those decorative materials, precision parts and optical parts with high requirements on the surface performance of the workpiece and complex shapes, mechanical polishing alone cannot achieve the required mirror reflectivity and surface flatness of the workpiece.
[0006] For example, CN105081941A discloses a mechanical polishing process for the inner wall of a stainless steel storage tank, which includes the following steps:
[0007] 1) Rough polishing: Use 60#~100# diamond grinding wheel to grind, polish or grind the surface of the workpiece to remove burrs, scratches, rust marks, oxide scale, weld excess height, weld nodules, welding slag, etc. on the surface, remove the surface oxide layer, and expose the metallic luster;
[0008] 2) Fine polishing: Use 80# diamond grinding wheel and flap wheel to further process the rough polished surface, remove the scratches left by rough polishing, and produce a smooth to medium-bright surface;
[0009] 3) Fine polishing: Use 240#~320# fiber wheels and cloth wheels coated with polishing paste to polish the surface of the stainless steel storage tank to further reduce the roughness of the stainless steel surface and achieve the purpose of microscopic flatness;
[0010] 4) Polishing test: The center line average method is used for testing. During the test, the roughness tester is moved horizontally on the surface of the stainless steel tank to record the peak-to-valley change amplitude.
[0011] Chemical polishing is similar to electrochemical polishing. Both rely on the etching effect of special chemical reagents to selectively dissolve the uneven areas on the surface of the workpiece, and under certain temperature and time conditions, the surface oxide layer and crystal deformation layer are etched away to eliminate surface wear marks and etching leveling. After chemical polishing, the surface gloss of the workpiece is improved, the surface roughness is reduced, the chemical stability is improved, and the reflection ability of light and heat is enhanced. However, compared with electrochemical polishing, chemical polishing requires less equipment and capital, does not require power equipment and corresponding fixtures, has simple equipment, simple operation, high production efficiency, and can effectively process thin tubes, parts with deep holes, small sizes and complex shapes. Because most aluminum and aluminum alloys do not have special requirements for use, as long as they meet the requirements of daily industry and life for surface gloss and flatness, it is completely sufficient to use chemical polishing technology. Chemical polishing is applicable not only to aluminum and aluminum alloy products, but also to other products such as copper, nickel, titanium and their alloys, and even steel and silver workpieces. Chemical polishing or electrochemical polishing technology can improve the surface finish of materials.
[0012] For example, CN102277575A discloses a chemical polishing liquid for aluminum products and a preparation method thereof, which relates to a chemical polishing liquid. A nitrate-modified "three-acid" polishing process is provided, which not only has the advantages of less yellow smoke, low pollution, and no nitric acid, but also has the polishing quality that can reach the level of the traditional "three-acid" process, and can reduce the release of nitrogen oxides to cause environmental pollution. The chemical polishing liquid for aluminum products and its preparation method. Its raw materials are sulfuric acid, phosphoric acid, boric acid, passivator, fog suppressant brightener, citric acid, tartaric acid and water. The specific steps are to add each solid raw material to water, dissolve it, add phosphoric acid and sulfuric acid in turn, and transfer it to a volumetric flask to make up the volume after the solution is cooled. Usage: Heat the chemical polishing liquid for aluminum products to 95-110°C; immerse the dry and clean aluminum products to be polished in the chemical polishing liquid for aluminum products, and take them out after processing for 30-100s; immerse the aluminum products to be polished taken out in nitric acid to lighten for 25-120s, and wash them, and the polishing of the aluminum products is completed.
[0013] Electrochemical polishing (electrolytic polishing or electropolishing), also known as electrolytic polishing, refers to the surface finishing technology of reducing the surface roughness, improving the brightness, and producing a certain metallic luster by dissolving the anodic part of the metal workpiece in a certain electrolyte. The specific process is: the workpiece to be processed is used as the anode, and the insoluble metal is used as the cathode (mostly lead plate or stainless steel plate), and then both the positive and negative electrodes are placed in the electrolytic cell liquid, and the DC power supply is turned on to start polishing. During the polishing process, the surface of the aluminum and aluminum alloy workpiece is selectively dissolved by the anodic part to obtain a workpiece surface with higher gloss and smoother surface. Electrochemical polishing technology has been developed for decades. It can improve the properties of the metal surface without changing the performance of the workpiece itself. After electrochemical polishing, metals and alloys will become smoother, brighter, and more corrosion-resistant. This process is to dissolve the particles produced by mechanical polishing.
[0014] For example, CN110846710A discloses an electrochemical polishing method for the surface of a copper material, comprising the following steps: preparing a polishing solution; immersing the copper material to be polished in the polishing solution, and turning on the power supply for polishing; wherein, preparing the polishing solution comprises: calculating the amount of each solute according to the total volume of the solution to be prepared, and the solutes include phosphoric acid, glycerol, thiourea and polyoxyethylene alkanolamide; according to the calculation results, weighing phosphoric acid and glycerol into a corrosion-resistant container, adding water to reach the total volume, stirring and dissolving to obtain a first intermediate solution; according to the calculation results, weighing thiourea and adding it to the first intermediate solution, stirring and dissolving to obtain a second intermediate solution; according to the calculation results, measuring polyoxyethylene alkanolamide and adding it to the second intermediate solution, stirring evenly to obtain a polishing solution. The present invention can increase the surface roughness of copper precision parts from Ra0.4μm to Ra0.2μm to meet the use requirements of vacuum electronic devices.
[0015] Compared with chemical polishing and mechanical polishing, electrochemical polishing has the following advantages: (1) It can obtain high surface finish; (2) It can obtain high polishing accuracy; (3) It has a good operating environment and low metal loss; (4) It consumes less energy; (5) It can process workpieces of any shape and size; (6) The polishing speed has nothing to do with the physical and mechanical properties of the metal; (7) It can greatly improve production efficiency; (g) It can improve the physical and mechanical properties, physical and chemical properties and performance of the surface of metal parts; (9) It is relatively easy to master the operating technology; (10) It has a wide range of applications. Summary of the invention
[0016] Based on the above introduction to polishing, the present invention provides a method for treating metal with an efficient cleaning agent. The cleaning agent serves as an electrochemical polishing electrolyte and can effectively polish the metal substrate to obtain a metal surface with low roughness, high flatness, corrosion resistance and good stability.
[0017] The invention discloses a method for treating metal with a high-efficiency cleaning agent. The cleaning agent is composed of polyol, perchloric acid, polyol amine, mercaptosulfonyl ionic compound and pyridinium salt compound.
[0018] The polyol is selected from one of dipropylene glycol, glycerol or butylene glycol.
[0019] The polyol amine is selected from one of diisopropanolamine, triisopropanolamine or triethanolamine.
[0020] The mercaptosulfonyl ionic compound is selected from sodium thiazolyl dithiopropane sulfonate, sodium dimethyl dithiocarbonyl propane sulfonate, and sodium 3-(benzothiazole-2-thio)-propane sulfonate.
[0021] The pyridinium salt compound is selected from 1-ethyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide, or 3-(4-tert-butyl 1-pyridyl)propanesulfonate, or 3-(1-pyridyl)propanesulfonate.
[0022] The metal is used as an anode, an inert metal is used as a cathode, and a cleaning agent is used as an electrolyte. A power source is applied between the metal anode and the inert metal cathode to clean the anode metal.
[0023] The cleaning process is as follows:
[0024] (1) Turn on the DC power supply: current density 3-5A / cm 2 , polishing time is 5-7min, temperature is 20-25℃, inter-electrode distance is 15-20mm;
[0025] (2) Turn on the millisecond pulse power supply: the forward pulse current density is 2-3mA / cm 2 , the forward pulse width is 100-150ms, the forward duty cycle is 10-15%, the number of pulses is 5-10, and the reverse pulse current density is 2-3mA / cm 2 , pulse width is 150-170ms, reverse duty cycle is 10-15%, pulse number is 1, temperature is 20-25℃, time is 2-3min;
[0026] (3) Turn on the microsecond pulse power supply: the forward pulse current density is 1-2 mA / cm 2 , forward pulse width is 50-100μs, forward duty cycle is 10-15%, pulse number is 10-15, reverse pulse current density is 1-2mA / cm2, reverse pulse width is 50-100μs, reverse duty cycle is 10-15%, pulse number is 1, temperature is 13-15℃, time is 0.5-1min;
[0027] Furthermore, the content of the polyol is 30-65 vol.%, the content of perchloric acid is 3-5 vol.%, the content of the polyol amine is 10-15 ml / L, the content of the mercaptosulfonyl ionic compound is 3-5 g / L, and the content of the pyridinium salt compound is 1.5-3 g / L.
[0028] Furthermore, the metal is stainless steel, aluminum alloy or titanium alloy, preferably aluminum alloy.
[0029] Furthermore, intermittent steps are provided between step (1) and step (2), and between step (2) and step (3): turning off the power supply, starting stirring, stirring speed of 200-300 rpm, stirring temperature of 17-23° C., and stirring time of 2-3 min.
[0030] Furthermore, after step (3), post-processing is provided: turning off the power supply, washing with anhydrous ethanol, and purging and drying with an inert atmosphere.
[0031] Furthermore, the inert atmosphere is nitrogen or argon, the temperature is 35-40° C., and the time is 1-2 h.
[0032] Regarding the cleaning liquid of the present invention, it is composed of polyol, perchloric acid, polyol amine, mercaptosulfonyl ionic compound, pyridinium salt compound, and the balance is supplemented by ethanol. It is a standard deionized water cleaning system. Generally speaking, the composition of the polishing liquid is relatively complex, and the type of polishing liquid suitable for each material is different. There is no definite formula, and most of them need to be explored by experiment, but the types of components contained therein are roughly divided into three parts, polishing base liquid, oxidant and various additives, and the oxidant is the most important component. The electrochemical polishing liquid is mainly divided into three categories, namely acid-acid system, such as concentrated sulfuric acid-concentrated phosphoric acid and other combinations; acid-alcohol system, such as concentrated sulfuric acid-methanol / ethanol and other combinations; alcohol-salt system, such as ethylene glycol-chloride salt and other combinations. Each polishing liquid system cannot meet all requirements, and there are certain advantages and disadvantages. There is no completely ideal polishing liquid system. Acid-acid system, mostly using strong acid, such as concentrated sulfuric acid, concentrated phosphoric acid, etc., although the polishing quality is good and the polishing efficiency is high, but the corrosiveness is strong, the reaction process is not easy to control, and the use process is prone to danger. Acid-alcohol system, alcohols are generally volatile and difficult to preserve, and alcohols and acids react easily to generate lipids, and the operating process has high requirements for the environment. Although most of the alcohol-salt system does not pollute the environment, due to its low corrosiveness and oxidizability, it causes low polishing efficiency, high production cost, and high requirements for polishing devices during the polishing process. The present invention mainly adopts a polyol-perchloric acid system, and perchloric acid is used as an oxidant and is the most important component in the polishing liquid. It can dissolve metal alloys and generate soluble salts, and also generate a passivation film on the surface of the specimen. Polyols are used as solvents to dissolve the soluble salts generated by the anode. At the same time, the carboxyl and hydroxyl groups they contain can also play a role in corrosion inhibition. Compared with monohydric alcohols such as methanol, the solvent selected by the present invention is a polyol such as dipropylene glycol, glycerol or butanediol, wherein the polyhydroxyl group shows a better slow release effect.
[0033] The polyol and the polyol amine are added simultaneously. The polyol amine is selected from diisopropanolamine, triisopropanolamine or triethanolamine. The polyol amine is weakly alkaline and can be a complexing agent or a leveling agent. It can produce a sticky film on the surface, adsorb on the surface, help polishing, and gradually level the surface.
[0034] The composition of the mercaptosulfonyl ionic compound and the pyridinium salt compound has a synergistic leveling and brightening technical effect. The mercaptosulfonyl ionic compound is selected from sodium thiazolinyl dithiopropane sulfonate, sodium dimethyl dithiocarbonyl propane sulfonate, and sodium 3-(benzothiazole-2-thiol)-propane sulfonate; the pyridinium salt compound is selected from 1-ethyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide, or 3-(4-tert-butyl 1-pyridinium) propane sulfonate, or 3-(1-pyridinium) propane sulfonate. The structural formulas of the three pyridinium salts are as follows:
[0035] ; ;
[0036] In theory, during the metal polishing process, when the metal immersed in the electrolyte is energized, it loses electrons at the anode, and the metal dissolves in the electrolyte in the form of ions. The reaction formula is Al→3Al 3+ +3e; in this process, aluminum ions are expected to leave the surface as quickly as possible; after the metal loses electrons, OH- ions migrate under the action of the electric field, causing a large number of OH- ions to gather near the metal anode, resulting in hydrolysis and deposition reaction, that is, Al 3+ +3OH - →Al(OH)3, it is hoped that no hydrolysis will occur in this process. Based on the above theory, the pyridinium salts of the present invention all have a C=N structure and are amphiphilic compounds. Under current conditions, one end of the anion will be adsorbed on the surface of the anode to neutralize the anions therein, and the metal ions released during the polishing and dissolution process, such as aluminum ions, will obviously repel the positively charged nitrogen, accelerating Al 3+ Metal ions enter the electrolyte from the surface of the dissolved metal, and the rejected aluminum ions are very easy to hydrolyze with water to form hydroxide particles, which affects the polishing effect. In order to prevent excessive hydrolysis of aluminum ions, the metal ions (Al 3+ ) will combine with CS=O and N=CS in the mercaptosulfonyl group, and the unshared electron pairs in the functional group are filled in the empty orbits of the metal ions, achieving a strong adsorption effect with the metal ions, thereby avoiding the deposition of the metal. In addition, mercaptosulfonyl ionic compounds and pyridinium salt compounds have rich ring structures, and their adsorption conjugation effect is significant, forming a mucous film structure on the surface, controlling the rapid corrosion of convex parts and slow corrosion of concave parts, and finally obtaining a leveling and brightening effect. Both are indispensable. If there is a lack of pyridinium salts, the metal ions cannot effectively move and diffuse away from the metal surface. If there is a lack of mercaptosulfonyl ionic compounds, the metal ions cannot effectively avoid hydrolysis. Figure 1 and attached Figure 2 shown.
[0037] Another important reason why the cleaning agent of the present invention can achieve excellent surface treatment effect on metal surfaces is the electrochemical electrolysis parameters. The electrochemical polishing power supply mainly used in the prior art is a DC power supply or a pulse power supply. There are few treatment methods that use DC first and then pulse, and even fewer electrochemical treatment processes that use millisecond-level and then micrometer-level.
[0038] The present invention uses the substrate to be treated as the anode, adds the cleaning agent prepared by the above preparation process, and then performs anode electrochemical polishing. The metal to be treated is stainless steel, aluminum alloy or titanium alloy, preferably aluminum alloy. The metal can undergo various surface pretreatments, including but not limited to degreasing, pickling activation, sandblasting, grinding, polishing and the like.
[0039] First, the substrate is subjected to direct current electrolytic polishing. In the early stage of direct current electrolytic polishing, due to the different roughness of the parts surface, that is, the uneven roughness of the metal surface, the electrolyte is adsorbed on the metal surface and an oxidation reaction occurs. The viscous liquid film generated on the protruding parts is thinner than the viscous liquid film generated on the concave parts. In addition, the viscous liquid film on the protruding parts is more affected by the impact of the electric lines and the stirring of the liquid. In addition, the protruding parts are closer to the cathode and the electric field strength is large. According to the principle of tip discharge, it is easy to lose electrons, forming a positive charge that is highly concentrated on the protruding parts. Since the anions around the anode preferentially react with the cations on the protruding parts, the metal dissolution rate on the protruding parts is faster than that on the concave parts. For direct current electrolytic polishing, it has an obvious and relatively fast leveling effect on the obvious concave and convex structures on the metal surface. The whole process appears to be rough and fast. Although it is not fine enough, it is efficient. For example, Figure 3 shown.
[0040] DC electrolysis conditions: current density 3-5A / cm 2 , the polishing time is 5-7min, the temperature is 20-25℃, and the inter-electrode distance is 15-20mm; among them, the current density has the greatest impact on the DC electrolytic polishing process and is the energy source for polishing. Too much or too little current density will have an adverse effect on polishing. When the current density is too small, the polished surface is always in the dissolution stage, the surface roughness is large, there is no metallic luster, and the polishing effect is small. When the current density is too large, the reaction is violent, more heat is generated, the oxidizing property of perchloric acid increases with the increase of temperature, more surface materials are removed, and the surface brightness is enhanced. At the same time, the oxygen precipitation on the anode surface increases, and due to the agitation of the gas, the surface will be unevenly polished and over-polished. In addition, the inter-electrode distance during electrochemical polishing is larger than that during electrolytic processing, mainly to ensure that the metal dissolves more evenly during the polishing process and achieve a better polishing effect. When the inter-electrode distance is too small, the diffusion of reactants is inconvenient, the temperature of the polishing liquid rises faster, and the heat dissipation is poor. When the inter-electrode distance is too large, the current density decreases, the polishing effect is not obvious, and the final optimized reaction condition is a current density of 3-5A / cm 2 The polishing time is 5-7min, the temperature is 20-25℃, and the inter-electrode distance is 15-20mm. Compared with pulse electrolysis, DC electrolytic polishing has a higher current density and a longer time, and can obtain a smooth surface more quickly.
[0041] The roughness of the metal surface treated by DC electrolytic polishing is about 5-10μm, and the polishing accuracy is obviously insufficient. The main reason may be that the DC voltage is constant, and it is difficult to remove the polishing products and heat. The products accumulate on the anode surface, which increases the surface roughness of the workpiece and leads to poor surface quality.
[0042] Then pulse processing:
[0043] (2) Turn on the millisecond pulse power supply: the forward pulse current density is 2-3mA / cm 2 , the forward pulse width is 100-150ms, the forward duty cycle is 10-15%, the number of pulses is 5-10, and the reverse pulse current density is 2-3mA / cm 2 , pulse width is 150-170ms, reverse duty cycle is 10-15%, pulse number is 1, temperature is 20-25℃, time is 2-3min.
[0044] (3) Intermittent step: turn off the power, start stirring, stirring speed 200-300 rpm, stirring temperature 17-23 ° C, stirring time 2-3 min.
[0045] (4) Turn on the microsecond pulse power supply: the forward pulse current density is 1-2 mA / cm 2 , the forward pulse width is 50-100μs, the forward duty cycle is 10-15%, the number of pulses is 10-15, the reverse pulse current density is 1-2mA / cm2, the reverse pulse width is 50-100μs, the reverse duty cycle is 10-15%, the number of pulses is 1, the temperature is 13-15℃, and the time is 0.5-1min.
[0046] Compared with direct current electrochemical polishing, the surface roughness of the polished surface of pulse current electrochemical polishing is greatly reduced. The reason is that theoretically, at the moment of power on, a pressure wave will be generated in the electrode gap. Due to the effect of the pressure wave, bubbles will be generated in the electrode gap and the anode surface will be corroded. At the moment of power off, the bubbles suddenly expand and merge, and the anode products are washed away, which effectively reduces the phenomenon of surface roughness deterioration caused by the surface products not being removed in time. Generally, the narrower the pulse width of the pulse current and the higher the frequency, the more beneficial it is to improve the flow field, because the smaller the pulse width and the higher the frequency, the faster the electrolyte in the gap is updated, and the more obvious the impact effect of the pressure wave is, which is more conducive to improving the surface quality.
[0047] Based on the above considerations, the present invention adopts a periodic commutation pulse power supply. The periodic commutation pulse is to add one or more reverse pulses after a group of forward pulses, which can further accelerate the migration of the anode product and thus obtain a high polishing effect. In the pulse stage, a relatively high current is first used to perform a long time of millisecond-level anode polishing, and the obtained metal surface roughness is about 400-600nm. Then, a relatively low current is used to perform a short time of microsecond-level anode polishing, and the obtained metal surface roughness is about 50-150nm. Compared with directly performing microsecond-level periodic commutation pulse electrochemical treatment to obtain the same polishing effect, the polishing time can be shortened by 3 / 4, and the polishing effect is greatly satisfied. The polishing effect is as shown in the attached figure. Figure 4 shown.
[0048] Beneficial technical effects
[0049] (1) The present invention has a direct impact on the roughness, high flatness and glossiness of metal surface treatment by effectively configuring the cleaning solution, especially the mercaptosulfonyl ionic compound and pyridinium salt compound therein.
[0050] (2) The present invention processes the metal surface by direct current + millisecond pulse + microsecond pulse, which effectively reduces the time consumption and reduces the loss while ensuring the low roughness, high gloss and low corrosion of the metal surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Attached Figure 1 Aluminum alloy image after being treated according to comparative example 1 of the present invention.
[0052] Attached Figure 2 Figure 2 of the aluminum alloy after being treated by comparative example 2 of the present invention.
[0053] Attached Figure 3 Figure 3 of the aluminum alloy after treatment according to comparative example 3 of the present invention.
[0054] Attached Figure 4 Figure 2 of the aluminum alloy after being treated according to Example 2 of the present invention. DETAILED DESCRIPTION
[0055] The preparation methods of the cleaning agents in Examples 1-3 of the present invention and the comparative examples are as follows:
[0056] (1) Mix polyol amine and polyol at a mixing temperature of 5-10°C and stir evenly;
[0057] (2) Continue stirring and keep the temperature stable, slowly add perchloric acid, and stir evenly;
[0058] (3) Continue stirring and add the mercaptosulfonyl ionic compound and the pyridinium salt compound at the same time, slowly raise the temperature to room temperature, and continue stirring for 1-2 hours to obtain a cleaning agent.
[0059] If the above ingredients are not contained, some adaptability will be deleted.
[0060] Example 1
[0061] A method for treating metal with an efficient cleaning agent. The cleaning agent is composed of a polyol, perchloric acid, a polyol amine, a mercaptosulfonyl ionic compound, and a pyridinium salt compound. The content of the polyol is 30 vol.%, the content of the perchloric acid is 3 vol.%, the content of the polyol amine is 10 ml / L, the content of the mercaptosulfonyl ionic compound is 3 g / L, the content of the pyridinium salt compound is 1.5 g / L, and the balance is deionized water.
[0062] The polyol is selected from dipropylene glycol.
[0063] The polyol amine is selected from diisopropanolamine.
[0064] The mercaptosulfonyl ionic compound is selected from sodium thiazoline dithiopropane sulfonate.
[0065] The pyridinium salt compound is selected from 3-(4-tert-butyl 1-pyridyl) propane sulfonate.
[0066] The metal is used as an anode, an inert metal is used as a cathode, and a cleaning agent is used as an electrolyte. A power source is applied between the metal anode and the inert metal cathode to clean the anode metal.
[0067] The cleaning process is as follows:
[0068] (1) Turn on the DC power supply: current density 3A / cm 2 , polishing time is 5min, temperature is 20℃, and inter-electrode distance is 15mm.
[0069] (2) Intermittent step: turn off the power, start stirring, stirring speed 200 rpm, stirring temperature 17 °C, stirring time 2 min.
[0070] (3) Turn on the millisecond pulse power supply: the forward pulse current density is 2 mA / cm 2 , the forward pulse width is 100ms, the forward duty cycle is 10%, the number of pulses is 5, and the reverse pulse current density is 2mA / cm 2 , pulse width is 150ms, reverse duty cycle is 10%, pulse number is 1, temperature is 20℃, and time is 2min.
[0071] (4) Intermittent step: turn off the power, start stirring, stirring speed 200 rpm, stirring temperature 17 °C, stirring time 2 min.
[0072] (5) Turn on the microsecond pulse power supply: the forward pulse current density is 1mA / cm 2 , the forward pulse width is 50μs, the forward duty cycle is 10%, the number of pulses is 10, and the reverse pulse current density is 1mA / cm 2 , pulse width is 50μs, forward duty cycle is 10%, pulse number is 1, temperature is 13℃, and time is 0.5min.
[0073] There is post-treatment: turn off the power, wash with anhydrous ethanol, purge and dry in an inert atmosphere, the inert atmosphere is nitrogen or argon, the temperature is 35°C, and the time is 1 hour.
[0074] Example 2
[0075] A method for treating metal with an efficient cleaning agent. The cleaning agent is composed of a polyol, perchloric acid, a polyol amine, a mercaptosulfonyl ionic compound, and a pyridinium salt compound. The content of the polyol is 55 vol.%, the content of the perchloric acid is 4 vol.%, the content of the polyol amine is 12.5 ml / L, the content of the mercaptosulfonyl ionic compound is 4 g / L, the content of the pyridinium salt compound is 2 g / L, and the balance is deionized water.
[0076] The polyol is selected from one of glycerols.
[0077] The polyol amine is selected from one of triisopropanolamine.
[0078] The mercaptosulfonyl ionic compound is selected from one of sodium dimethyldithiocarbonylpropane sulfonate.
[0079] The pyridinium salt compound is selected from 1-ethyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide.
[0080] The metal is used as an anode, an inert metal is used as a cathode, and a cleaning agent is used as an electrolyte. A power source is applied between the metal anode and the inert metal cathode to clean the anode metal.
[0081] The cleaning process is as follows:
[0082] (1) Turn on the DC power supply: current density 4A / cm 2 , polishing time is 6min, temperature is 23℃, and inter-electrode distance is 17mm.
[0083] (2) Intermittent step: turn off the power, start stirring, stirring speed 250 rpm, stirring temperature 20 °C, stirring time 2.5 min.
[0084] (3) Turn on the millisecond pulse power supply: the forward pulse current density is 2.5 mA / cm 2 , the forward pulse width is 125ms, the forward duty cycle is 12.5%, the number of pulses is 8, and the reverse pulse current density is 2.5mA / cm 2 , the reverse pulse width is 160ms, the reverse duty cycle is 12.5%, the number of pulses is 1, the temperature is 23℃, and the time is 2.5min.
[0085] (4) Intermittent step: turn off the power, start stirring, stirring speed 250 rpm, stirring temperature 20 °C, stirring time 2.5 min.
[0086] (5) Turn on the microsecond pulse power supply: the forward pulse current density is 1.5 mA / cm 2, the forward pulse width is 75μs, the forward duty cycle is 12.5%, the pulse number is 13, the reverse pulse current density is 1.5mA / cm2, the reverse pulse width is 75μs, the reverse duty cycle is 12.5%, the pulse number is 1, the temperature is 14℃, and the time is 0.75min.
[0087] There is post-treatment: turn off the power, wash with anhydrous ethanol, purge and dry in an inert atmosphere, the inert atmosphere is nitrogen or argon, the temperature is 38°C, and the time is 1.5h.
[0088] Example 3
[0089] A method for treating metal with an efficient cleaning agent. The cleaning agent is composed of a polyol, perchloric acid, a polyol amine, a mercaptosulfonyl ionic compound, and a pyridinium salt compound. The content of the polyol is 65 vol.%, the content of the perchloric acid is 5 vol.%, the content of the polyol amine is 15 ml / L, the content of the mercaptosulfonyl ionic compound is 5 g / L, the content of the pyridinium salt compound is 3 g / L, and the balance is deionized water.
[0090] The polyol is selected from one of butanediols.
[0091] The polyol amine is selected from one of triethanolamines.
[0092] The mercaptosulfonyl ionic compound is selected from one of sodium 3-(benzothiazole-2-mercapto)-propane sulfonate.
[0093] The pyridinium salt compound is selected from one of 3-(1-pyridyl)propanesulfonate salts.
[0094] The metal is used as an anode, an inert metal is used as a cathode, and a cleaning agent is used as an electrolyte. A power source is applied between the metal anode and the inert metal cathode to clean the anode metal.
[0095] The cleaning process is as follows:
[0096] (1) Turn on the DC power supply: current density 5A / cm 2 , polishing time is 7min, temperature is 25℃, and inter-electrode distance is 20mm.
[0097] (2) Intermittent step: turn off the power, start stirring, stirring speed 300 rpm, stirring temperature 23 °C, stirring time 3 min.
[0098] (3) Turn on the millisecond pulse power supply: the forward pulse current density is 3mA / cm 2 , the forward pulse width is 150ms, the forward duty cycle is 15%, the number of pulses is 10, and the reverse pulse current density is 3mA / cm 2, pulse width is 170ms, reverse duty cycle is 15%, pulse number is 1, temperature is 25℃, and time is 3min.
[0099] (4) Intermittent step: turn off the power, start stirring, stirring speed 200-300 rpm, stirring temperature 17-23 ° C, stirring time 2-3 min.
[0100] (5) Turn on the microsecond pulse power supply: the forward pulse current density is 2 mA / cm 2 , the forward pulse width is 100μs, the forward duty cycle is 15%, the number of pulses is 15, the reverse pulse current density is 2mA / cm2, the reverse pulse width is 100μs, the reverse duty cycle is 15%, the number of pulses is 1, the temperature is 15℃, and the time is 1min.
[0101] There is post-treatment: turn off the power, wash with anhydrous ethanol, blow and dry in an inert atmosphere, the inert atmosphere is nitrogen or argon, the temperature is 40°C, and the time is 2h.
[0102] Comparative Example 1
[0103] A method for treating metal with an efficient cleaning agent, wherein the cleaning agent is composed of a polyol, perchloric acid, and a polyol amine compound, wherein the content of the polyol is 55 vol.%, the content of the perchloric acid is 4 vol.%, the content of the polyol amine is 12.5 ml / L, and the balance is deionized water.
[0104] The polyol is selected from glycerol.
[0105] The polyol amine is selected from one of triisopropanolamine.
[0106] The mercaptosulfonyl ionic compound is selected from one of sodium dimethyldithiocarbonylpropane sulfonate.
[0107] The pyridinium salt compound is selected from 1-ethyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide.
[0108] The metal is used as an anode, an inert metal is used as a cathode, and a cleaning agent is used as an electrolyte. A power source is applied between the metal anode and the inert metal cathode to clean the anode metal.
[0109] The cleaning process is as follows:
[0110] (1) Turn on the DC power supply: current density 4A / cm 2 , polishing time is 6min, temperature is 23℃, and inter-electrode distance is 17mm.
[0111] (2) Intermittent step: turn off the power, start stirring, stirring speed 250 rpm, stirring temperature 20 °C, stirring time 2.5 min.
[0112] (3) Turn on the millisecond pulse power supply: the forward pulse current density is 2.5 mA / cm 2 , the forward pulse width is 125ms, the forward duty cycle is 12.5%, the number of pulses is 8, and the reverse pulse current density is 2.5mA / cm 2 , the reverse pulse width is 160ms, the reverse duty cycle is 12.5%, the number of pulses is 1, the temperature is 23℃, and the time is 2.5min.
[0113] (4) Intermittent step: turn off the power, start stirring, stirring speed 250 rpm, stirring temperature 20 °C, stirring time 2.5 min.
[0114] (5) Turn on the microsecond pulse power supply: the forward pulse current density is 1.5 mA / cm 2 , the forward pulse width is 75μs, the forward duty cycle is 12.5%, the pulse number is 13, the reverse pulse current density is 1.5mA / cm2, the reverse pulse width is 75μs, the reverse duty cycle is 12.5%, the pulse number is 1, the temperature is 14℃, and the time is 0.75min.
[0115] There is post-treatment: turn off the power, wash with anhydrous ethanol, purge and dry in an inert atmosphere, the inert atmosphere is nitrogen or argon, the temperature is 38°C, and the time is 1.5h.
[0116] Comparative Example 2
[0117] A method for treating metal with an efficient cleaning agent. The cleaning agent is composed of a polyol, perchloric acid, a polyol amine, and a mercaptosulfonyl ionic compound. The content of the polyol is 55 vol.%, the content of the perchloric acid is 4 vol.%, the content of the polyol amine is 12.5 ml / L, the content of the mercaptosulfonyl ionic compound is 4 g / L, and the balance is deionized water.
[0118] The polyol is selected from one of glycerols.
[0119] The polyol amine is selected from one of triisopropanolamine.
[0120] The mercaptosulfonyl ionic compound is selected from one of sodium dimethyldithiocarbonylpropane sulfonate.
[0121] The pyridinium salt compound is selected from 1-ethyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide.
[0122] The metal is used as an anode, an inert metal is used as a cathode, and a cleaning agent is used as an electrolyte. A power source is applied between the metal anode and the inert metal cathode to clean the anode metal.
[0123] The cleaning process is as follows:
[0124] (1) Turn on the DC power supply: current density 4A / cm 2 , polishing time is 6min, temperature is 23℃, and inter-electrode distance is 17mm.
[0125] (2) Intermittent step: turn off the power, start stirring, stirring speed 250 rpm, stirring temperature 20 °C, stirring time 2.5 min.
[0126] (3) Turn on the millisecond pulse power supply: the forward pulse current density is 2.5 mA / cm 2 , the forward pulse width is 125ms, the forward duty cycle is 12.5%, the number of pulses is 8, and the reverse pulse current density is 2.5mA / cm 2 , the reverse pulse width is 160ms, the reverse duty cycle is 12.5%, the number of pulses is 1, the temperature is 23℃, and the time is 2.5min.
[0127] (4) Intermittent step: turn off the power, start stirring, stirring speed 250 rpm, stirring temperature 20 °C, stirring time 2.5 min.
[0128] (5) Turn on the microsecond pulse power supply: the forward pulse current density is 1.5 mA / cm 2 , the forward pulse width is 75μs, the forward duty cycle is 12.5%, the pulse number is 13, the reverse pulse current density is 1.5mA / cm2, the reverse pulse width is 75μs, the reverse duty cycle is 12.5%, the pulse number is 1, the temperature is 14℃, and the time is 0.75min.
[0129] There is post-treatment: turn off the power, wash with anhydrous ethanol, purge and dry in an inert atmosphere, the inert atmosphere is nitrogen or argon, the temperature is 38°C, and the time is 1.5h.
[0130] Comparative Example 3
[0131] A method for treating metal with an efficient cleaning agent. The cleaning agent is composed of a polyol, perchloric acid, a polyol amine, a mercaptosulfonyl ionic compound, and a pyridinium salt compound. The content of the polyol is 55 vol.%, the content of the perchloric acid is 4 vol.%, the content of the polyol amine is 12.5 ml / L, the content of the mercaptosulfonyl ionic compound is 4 g / L, the content of the pyridinium salt compound is 2 g / L, and the balance is deionized water.
[0132] The polyol is selected from glycerol.
[0133] The polyol amine is selected from one of triisopropanolamine.
[0134] The mercaptosulfonyl ionic compound is selected from one of sodium dimethyldithiocarbonylpropane sulfonate.
[0135] The pyridinium salt compound is selected from 1-ethyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide.
[0136] The metal is used as an anode, an inert metal is used as a cathode, and a cleaning agent is used as an electrolyte. A power source is applied between the metal anode and the inert metal cathode to clean the anode metal.
[0137] The cleaning process is as follows:
[0138] (1) Turn on the DC power supply: current density 4A / cm 2 , polishing time is 10min, temperature is 23℃, and inter-electrode distance is 17mm.
[0139] (2) Post-treatment: turn off the power, wash with anhydrous ethanol, and purge and dry in an inert atmosphere of nitrogen or argon at a temperature of 38°C for 1.5 h.
[0140] Comparative Example 4
[0141] A method for treating metal with an efficient cleaning agent. The cleaning agent is composed of a polyol, perchloric acid, a polyol amine, a mercaptosulfonyl ionic compound, and a pyridinium salt compound. The content of the polyol is 55 vol.%, the content of the perchloric acid is 4 vol.%, the content of the polyol amine is 12.5 ml / L, the content of the mercaptosulfonyl ionic compound is 4 g / L, the content of the pyridinium salt compound is 2 g / L, and the balance is deionized water.
[0142] The polyol is selected from one of glycerols.
[0143] The polyol amine is selected from one of triisopropanolamine.
[0144] The mercaptosulfonyl ionic compound is selected from one of sodium dimethyldithiocarbonylpropane sulfonate.
[0145] The pyridinium salt compound is selected from 1-ethyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide.
[0146] The metal is used as an anode, an inert metal is used as a cathode, and a cleaning agent is used as an electrolyte. A power source is applied between the metal anode and the inert metal cathode to clean the anode metal.
[0147] The cleaning process is as follows:
[0148] (1) Turn on the millisecond pulse power supply: the forward pulse current density is 2.5 mA / cm 2 , the forward pulse width is 125ms, the forward duty cycle is 12.5%, the number of pulses is 8, and the reverse pulse current density is 2.5mA / cm 2, the reverse pulse width is 160ms, the reverse duty cycle is 12.5%, the number of pulses is 1, the temperature is 23℃, and the time is 13min.
[0149] (2) Intermittent step: turn off the power, start stirring, stirring speed 250 rpm, stirring temperature 20 °C, stirring time 2.5 min.
[0150] (3) Turn on the microsecond pulse power supply: the forward pulse current density is 1.5 mA / cm 2 , the forward pulse width is 75μs, the forward duty cycle is 12.5%, the number of pulses is 13, the reverse pulse current density is 1.5mA / cm2, the reverse pulse width is 75μs, the reverse duty cycle is 12.5%, the number of pulses is 1, the temperature is 14℃, and the time is 7.4min.
[0151] Post-treatment: turn off the power, wash with anhydrous ethanol, purge and dry in an inert atmosphere of nitrogen or argon, at a temperature of 38°C for 1.5 h.
[0152] Surface roughness: Three different areas were selected on the sample surface for testing using the RSE3000 surface roughness tester, and the average roughness of the three areas was taken as the test result.
[0153] Surface glossiness: Take aluminum as the sample and select 45 o Reflection angle, measure the surface gloss of the sample according to GB8807-88.
[0154] Table 1
[0155]
[0156] As shown in the table above, the roughness of the aluminum alloy surface obtained by Example 2 of the present invention through base liquid + mercaptosulfonyl + pyridinium salt is 53nm, the glossiness is 81.3%, and the corrosion amount of the product is small. In comparison, under the same electrolysis parameter conditions, if the electrolyte is changed, such as deleting mercaptosulfonyl + pyridinium salt in Comparative Example 1 and deleting pyridinium salt in Comparative Example 2, it can be seen that the electrolyte has a significant effect on the glossiness and roughness of the product, which is ten times the order of magnitude. The main reason is that the additive has a significant effect on the migration and diffusion of the generated oxidized particles in the electroplating solution. Comparative Examples 3-4 have the same electrolyte and different electrolysis parameters. If only direct current electrolysis is used, the polishing degree and glossiness cannot meet the industrial requirements of low roughness and high metallic gloss. Compared with direct pulse treatment, the millisecond and microsecond pulse time of Comparative Example 3 is adjustable. By adjusting the time parameters of Comparative Example 3, the surface roughness effect consistent with that of Example 2 is obtained. Although both can obtain a high mirror effect, the time, loss consumption, and equipment burden are significantly higher than those of Example 2 of the present invention.
[0157] Finally, it should be noted that the above implementation modes are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the preferred implementation modes, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention.
Claims
1. A method for treating metal with a cleaning agent, Features The cleaning agent is composed of polyol, perchloric acid, polyol amine, mercaptosulfonyl ionic compound, pyridinium salt compound and deionized water; The polyol is selected from one of dipropylene glycol, glycerol or butylene glycol; The polyol amine is selected from one of diisopropanolamine, triisopropanolamine or triethanolamine; The mercaptosulfonyl ionic compound is selected from sodium thiazolyl dithiopropane sulfonate, sodium dimethyl dithiocarbonyl propane sulfonate, and sodium 3-(benzothiazole-2-thio)-propane sulfonate; The pyridinium salt compound is selected from 1-ethyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide, or 3-(4-tert-butyl 1-pyridyl)propanesulfonate, or 3-(1-pyridyl)propanesulfonate; Using the metal as an anode, an inert metal as a cathode, and a cleaning agent as an electrolyte, a power source is applied between the metal anode and the inert metal cathode to clean the anode metal; The cleaning process is as follows: (1) Turn on the DC power supply: current density 3-5A / cm 2 , polishing time is 5-7min, temperature is 20-25℃, inter-electrode distance is 15-20mm; (2) Turn on the millisecond pulse power supply: the forward pulse current density is 2-3mA / cm 2 , the forward pulse width is 100-150ms, the forward duty cycle is 10-15%, the number of pulses is 5-10, and the reverse pulse current density is 2-3mA / cm 2 , pulse width is 150-170ms, reverse duty cycle is 10-15%, pulse number is 1, temperature is 20-25℃, time is 2-3min; (3) Turn on the microsecond pulse power supply: the forward pulse current density is 1-2 mA / cm 2 , forward pulse width is 50-100μs, forward duty cycle is 10-15%, pulse number is 10-15, reverse pulse current density is 1-2mA / cm 2 , reverse pulse width is 50-100μs, reverse duty cycle is 10-15%, pulse number is 1, temperature is 13-15℃, time is 0.5-1min; The content of the polyol is 30-65 vol.%, the content of perchloric acid is 3-5 vol.%, the content of the polyol amine is 10-15 ml / L, the content of the mercaptosulfonyl ionic compound is 3-5 g / L, and the content of the pyridinium salt compound is 1.5-3 g / L; The metal is an aluminum alloy.
2. A method for treating metal with a cleaning agent as claimed in claim 1, Features An intermittent step is set between step (1) and step (2), and between step (2) and step (3): turn off the power, start stirring, the stirring speed is 200-300 rpm, the stirring temperature is 17-23°C, and the stirring time is 2-3 minutes.
3. A method for treating metal with a cleaning agent as claimed in claim 1, Features After step (3), post-processing is provided: turning off the power supply, washing with anhydrous ethanol, and purging and drying with an inert atmosphere.
4. A method for treating metal with a cleaning agent as claimed in claim 3, Features The inert atmosphere is nitrogen or argon, the temperature is 35-40°C, and the time is 1-2h.