Multi-band ultraviolet photoelectric detector and preparation method thereof

By using stacked structures and two-dimensional functional layer load quantum dots in photodetectors, the problems of limited and flexible requirements for existing photodetectors in far-infrared applications are solved, and the wide spectrum and high responsiveness are achieved UV photodetection effect in band.

CN116314424BActive Publication Date: 2024-11-29SHENZHEN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211650322.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-11-29
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

Existing photodetectors are limited in the range of far infrared and terahertz. The preparation of III-V semiconductor materials is complex and requires a low temperature environment. The three-dimensional block lattice of traditional semiconductor materials is difficult to meet the flexibility requirements, and the plane structure performance is poor. .

Method used

Using a sequentially laminated substrate, ultraviolet detection layer and two-dimensional functional layer, the two-dimensional functional layer is loaded with quantum dots and simultaneously forms ohmic contact with the ultraviolet detection layer to achieve wide-spectrum photoelectric detection, by changing the two-dimensional material and voltage modulation device bands, combining the strong light absorption and charge transfer characteristics of quantum dots, improve responsiveness and sensitivity.

Benefits of technology

It realizes wide-spectral photoelectric detection from ultraviolet light to near infrared, reduces dark current, improves operating temperature and threshold sensitivity, and is suitable for multi-band ultraviolet photodetectors, simplifies the preparation process, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116314424B_ABST
    Figure CN116314424B_ABST
Patent Text Reader

Abstract

The present application belongs to the field of optoelectronic technology, and in particular, relates to a multi-band ultraviolet photodetector and a method for preparing the same. Among them, the multi-band ultraviolet photodetector includes a substrate, an ultraviolet light detection layer and a two-dimensional functional layer which are laminated and bonded in sequence, and a first electrode and a second electrode which simultaneously form an ohmic contact with the ultraviolet light detection layer and the two-dimensional functional layer; the two-dimensional functional layer is loaded with quantum dots. The multi-band ultraviolet photodetector provided by the present application makes full use of the photoelectric detection capability of the ultraviolet light detection layer in the day-blind band, the photoelectric detection capability of the two-dimensional material from visible light to near-infrared light, the strong light absorption capability and strong carrier absorption capability of quantum dots. Through the combination of various functional layers, the device has the characteristics of wide spectrum, high responsiveness, fast response, etc. It can be widely used in the fields of microelectronic technology such as integrated optoelectronic device design, manufacturing and process technology, as well as new electronic components such as semiconductor light-emitting technology and flat panel display devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of optoelectronic technology, and in particular relates to a multi-band ultraviolet photoelectric detector and a preparation method thereof. Background Art

[0002] Photodetectors are an important type of optoelectronic devices that can convert optical signals into electrical signals. They are widely used in various fields of national production and life and national defense and military, such as optical communications, industrial control, environmental monitoring, infrared imaging, space remote sensing, night vision, etc. At present, commercial photodetectors are designed based on bulk silicon materials and III-V semiconductor alloy materials. Although they have excellent performance and perfect manufacturing technology, they still face many challenges. For example: (1) Silicon-based photodetectors cannot be used in the mid-infrared and terahertz range due to the band gap limitation of silicon 1.1eV. (2) The preparation of InGaAs and HgCdTe materials usually requires complex molecular beam epitaxy technology, and their corresponding infrared photodetectors must work in harsh low-temperature environments. (3) The three-dimensional bulk lattice of traditional semiconductor materials is difficult to meet some applications with high ductility and flexibility requirements. Therefore, there is an urgent need to find a new material with a suitable band gap, high light absorption rate, good flexibility and transparency, and can be processed using simple and low-cost processes for application in photodetection.

[0003] Gallium oxide is an ideal solar-blind detection material with a solar-blind band of 200-280nm. The structures used by solar-blind photodetectors based on gallium oxide reported so far can be divided into vertical structures and planar structures. In the vertical structure, the electrodes are grown on the upper and lower sides of the gallium oxide layer respectively; in the planar structure, the electrodes are grown on the same side of the gallium oxide layer. The preparation process of vertical structure devices is relatively complicated, which increases the production cost. The preparation of the planar structure is simple, but the electric field generated by the electrode is concentrated on the surface of the gallium oxide, and there is almost no electric field distribution inside the gallium oxide, which causes the effective light absorption area of ​​the device to exist on the surface of the gallium oxide, and the photocurrent of the device also flows mainly in the surface area. However, there are often a large number of defects on the semiconductor surface caused by dangling bonds, adsorbates, etc., which leads to poor performance of planar structure photodetectors. Summary of the invention

[0004] The purpose of the present application is to provide a multi-band ultraviolet photoelectric detector and a method for preparing the same, which aims to solve to a certain extent the problem that if the existing detectors want to achieve spectral tunability, they need to add filters for filtering photons of different wavelengths or replace semiconductor materials with different bandgap widths, which makes the structure complex and the implementation difficult.

[0005] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:

[0006] In a first aspect, the present application provides a multi-band ultraviolet photodetector, which includes a substrate, an ultraviolet light detection layer and a two-dimensional functional layer stacked and bonded in sequence, and a first electrode and a second electrode that simultaneously form ohmic contact with the ultraviolet light detection layer and the two-dimensional functional layer; the two-dimensional functional layer is loaded with quantum dots.

[0007] The multi-band ultraviolet photodetector provided in the first aspect of the present application comprises a substrate, an ultraviolet light detection layer and a two-dimensional functional layer which are laminated and bonded in sequence, and a first electrode and a second electrode which simultaneously form an ohmic contact with the ultraviolet light detection layer and the two-dimensional functional layer. On the one hand, by forming an ohmic contact with the ultraviolet light detection layer and the two-dimensional functional layer and the electrode at the same time, the absorption capacity of the ultraviolet light detection layer in the ultraviolet band (in the solar blind band of 200-280nm) is fully utilized, and at the same time, the photoelectric detection ability of the two-dimensional material in the visible light to near infrared band is fully utilized, and the advantages of the two functional layer materials are fully utilized to realize wide-spectrum photoelectric detection from ultraviolet light to near infrared. And the ultraviolet light detection layer and the two-dimensional functional layer form a heterojunction, which is not only conducive to improving the responsiveness of the photoelectric detection device; and without the need for a filter, by changing the two-dimensional material on the surface of the device, or by modulating the ultraviolet light detection layer and the two-dimensional functional layer simultaneously by voltage, the detection band of the photoelectric detection device can be flexibly controlled, and a wide-spectrum high-performance photoelectric detection performance is obtained, which helps to improve the detection ability and applicability of the multi-band ultraviolet photodetector for weak light signals. In addition, the two-dimensional functional layer is loaded with quantum dots, which have strong light absorption capabilities and strong carrier absorption capabilities. By combining quantum dots with two-dimensional materials, quantum dots can fully absorb external photon radiation and generate photogenerated carriers. At the same time, quantum dots have strong and excellent charge transfer characteristics, which can effectively improve the overall photoelectric conversion capability of ultraviolet photodetectors, so that multi-band ultraviolet photodetectors have lower dark current and higher operating temperature and threshold sensitivity.

[0008] In a second aspect, the present application provides a method for preparing a multi-band ultraviolet photodetector, comprising the following steps:

[0009] Obtaining a clean substrate, and preparing an ultraviolet light detection layer on a surface of the substrate;

[0010] Prepare a first electrode and a second electrode disposed opposite to each other on a surface of the ultraviolet light detection layer facing away from the substrate;

[0011] A two-dimensional functional layer is prepared between the first electrode and the second electrode of the ultraviolet light detection layer, and quantum dots are loaded in the two-dimensional functional layer to obtain a multi-band ultraviolet photodetector.

[0012] The second aspect of the present application provides a method for preparing a multi-band ultraviolet photodetector. After preparing a laminated ultraviolet light detection layer on the surface of a clean substrate, a first electrode and a second electrode are prepared that are relatively arranged. The electrodes can be grown on the surface of the ultraviolet light detection layer, or they can be partially grown inside the ultraviolet light detection layer. Then, a two-dimensional functional layer loaded with quantum dots is prepared between the first electrode and the second electrode of the ultraviolet light detection layer to obtain a multi-band ultraviolet photodetector. The preparation process is simple and suitable for large-scale industrial production and application. The prepared multi-band ultraviolet photodetector has the characteristics of wide spectrum, high responsiveness, and fast response through the combination of various functional layers. It can be widely used in the fields of microelectronics technology such as integrated optoelectronic device design, manufacturing and process technology, as well as new electronic components such as semiconductor light-emitting technology and flat panel display devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0014] Figure 1 This is a schematic diagram of the structure of the multi-band ultraviolet photodetector provided in the embodiment of the present application. Figure 1 ;

[0015] Figure 2 This is a schematic diagram of the structure of the multi-band ultraviolet photodetector provided in the embodiment of the present application. Figure 2 ;

[0016] Figure 3 This is a schematic diagram of the structure of the electrode partially grown inside the ultraviolet light detection layer provided in the embodiment of the present application. Figure 1 ;

[0017] Figure 4 This is a schematic diagram of the structure of the electrode partially grown inside the ultraviolet light detection layer provided in the embodiment of the present application. Figure 2 ;

[0018] Figure 5 It is a schematic flow chart of a method for preparing a multi-band ultraviolet photoelectric detector provided in an embodiment of the present application. DETAILED DESCRIPTION

[0019] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0020] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0021] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0022] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0023] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0024] The weight of the relevant components mentioned in the embodiments of the present specification can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components in the embodiments of the present specification is proportionally enlarged or reduced, it is within the scope disclosed in the embodiments of the present specification. Specifically, the mass in the embodiments of the present specification can be μg, mg, g, kg and other mass units known in the chemical industry.

[0025] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0026] A first aspect of an embodiment of the present application provides a multi-band ultraviolet photodetector, which includes a substrate, an ultraviolet light detection layer and a two-dimensional functional layer stacked and bonded in sequence, and a first electrode and a second electrode that simultaneously form ohmic contact with the ultraviolet light detection layer and the two-dimensional functional layer; the two-dimensional functional layer is loaded with quantum dots.

[0027] The multi-band ultraviolet photodetector provided in the first aspect of the embodiment of the present application comprises a substrate, an ultraviolet light detection layer and a two-dimensional functional layer which are laminated and bonded in sequence, and a first electrode and a second electrode which simultaneously form an ohmic contact with the ultraviolet light detection layer and the two-dimensional functional layer. On the one hand, by forming an ohmic contact with the ultraviolet light detection layer and the two-dimensional functional layer and the electrode at the same time, the absorption capacity of the ultraviolet light detection layer in the ultraviolet band (200-280nm in the solar blind band) is fully utilized, and the photoelectric detection capacity of the two-dimensional material in the visible light to near infrared band is fully utilized, and the advantages of the two functional layer materials are fully utilized to realize wide-spectrum photoelectric detection from ultraviolet light to near infrared. And the ultraviolet light detection layer and the two-dimensional functional layer form a heterojunction, which is not only conducive to improving the responsiveness of the photoelectric detection device; and without the need for a filter, by changing the two-dimensional material on the surface of the device, or by modulating the ultraviolet light detection layer and the two-dimensional functional layer simultaneously by voltage, the detection band of the photoelectric detection device can be flexibly controlled, and a wide-spectrum high-performance photoelectric detection performance is obtained, which helps to improve the detection capability and applicability of the multi-band ultraviolet photodetector for weak light signals. In addition, the two-dimensional functional layer is loaded with quantum dots, which have strong light absorption ability and strong carrier absorption ability. By combining quantum dots with two-dimensional materials, quantum dots can fully absorb external photon radiation and generate photogenerated carriers. At the same time, quantum dots have strong and excellent charge transfer characteristics, which can effectively improve the overall photoelectric conversion ability of ultraviolet photodetectors, so that multi-band ultraviolet photodetectors have lower dark current and higher operating temperature and threshold sensitivity. The multi-band ultraviolet photodetector of this application combines various functional layers to make the device have the characteristics of wide spectrum, high responsiveness, fast response, etc. It can be widely used in the fields of microelectronic technology such as integrated optoelectronic device design, manufacturing and process technology, as well as new electronic components such as semiconductor light-emitting technology and flat panel display devices.

[0028] The multi-band ultraviolet photodetector of the embodiment of the present application is of the photoconductive type. It outputs photocurrent through photogenerated carriers, combines the light absorption sensitivity of the two-dimensional material and the ultraviolet light detection layer, and gives full play to the detection capabilities of the day-blind band of the ultraviolet light detection material and the detection capabilities of the two-dimensional material from visible light to near-infrared light.

[0029] In some embodiments, the ultraviolet detection layer includes at least one of Ga2O3, GaN, AlGaN, ZnO, GaAs, InAs, InP, CdTe, and Ge; these materials have strong absorption capabilities in the ultraviolet band, especially in the solar-blind band (200-280nm), providing the photodetector with solar-blind band photodetection capabilities. Combined with the photodetection capabilities of two-dimensional materials in the visible to near-infrared band, by giving full play to the advantages of the two functional layer materials in the multi-band ultraviolet photodetector, wide-spectrum photodetection from ultraviolet to near-infrared is achieved.

[0030] In some embodiments, the thickness of the ultraviolet detection layer is 10 to 100 nm; this thickness can effectively provide the photoelectric detection capability of the multi-band ultraviolet photodetector in the day-blind band. If the thickness of the ultraviolet detection layer is too thick, the photocurrent response speed will be reduced. In some specific embodiments, the thickness of the ultraviolet detection layer can be 10 to 20 nm, 20 to 30 nm, 30 to 40 nm, 50 to 60 nm, 60 to 70 nm, 70 to 80 nm, 80 to 90 nm, 90 to 100 nm, etc.

[0031] In some embodiments, the two-dimensional functional layer includes a two-dimensional material layer, and the two-dimensional material layer includes at least one of hexagonal boron nitride, two-dimensional molybdenum disulfide, two-dimensional molybdenum diselenide, two-dimensional tungsten disulfide, two-dimensional tin sulfide, two-dimensional silicene, germanene, black phosphorus, and graphene. These two-dimensional materials are nanomaterials composed of a single layer or a few atomic layers, with a longitudinal thickness generally less than 5nm, a lateral size generally greater than 100nm, and a typical layered structure. The atomic-level thickness of the two-dimensional material ensures the transparency and flexibility of the two-dimensional material, and has great application prospects in emerging fields such as flexible electronics. Secondly, the characteristics of the atomic-level thickness make the quantum confinement in the vertical direction lead to a strong exciton binding effect, which improves the light absorption efficiency. In addition, the band gap of the two-dimensional layered material changes with the change of its number of layers, which is particularly strong in transition metal chalcogenides, that is, the optical absorption can be regulated by simply controlling the number of layers, so that the corresponding photodetector can work in different spectral ranges. Therefore, these two-dimensional materials have good light transmittance and absorption response capabilities from visible light to infrared light. Combined with the absorption capacity of the ultraviolet light detection layer in the ultraviolet band (in the solar-blind band of 200-280nm), by giving full play to the advantages of the two functional layer materials in the multi-band ultraviolet photodetector, wide-spectrum photoelectric detection from ultraviolet light to near-infrared is achieved.

[0032] In some embodiments, the thickness of the two-dimensional material layer is 2 to 20 nm; two-dimensional materials of different thicknesses have different bandgap widths and corresponding photoelectric capabilities. This thickness range of the two-dimensional material layer of the present application is conducive to regulating optical absorption by simply controlling the number of layers of the two-dimensional material, so that the corresponding photodetector can work in different spectral ranges and has a wide photoelectric detection range. In some embodiments, the two-dimensional material in the two-dimensional material layer can be a single layer, two layers, or multiple layers. In some embodiments, the thickness of the two-dimensional material layer can be 2 to 5 nm, in which case the two-dimensional material layer contains a single layer of two-dimensional material; or, the thickness of the two-dimensional material layer can be 5 to 10 nm, in which case the two-dimensional material layer contains two to five layers of two-dimensional material; or, the thickness of the two-dimensional material layer can be 10 to 20 nm, in which case the two-dimensional material layer contains multiple layers of two-dimensional material.

[0033] In some embodiments, the quantum dots include at least one of PbSe, PbS, HgTe, CsPbCl3, MAPbCl3, CsPbBr3, and MAPbBr3. These quantum dots have strong light absorption and carrier absorption capabilities, as well as strong and excellent charge transfer properties. By combining quantum dots with two-dimensional materials, quantum dots can fully absorb external photon radiation and generate photogenerated carriers, effectively improving the overall photoelectric conversion capability of the ultraviolet photodetector, and enabling the multi-band ultraviolet photodetector to have a lower dark current and a higher operating temperature and threshold sensitivity.

[0034] In some embodiments, the thickness of the loaded quantum dots in the two-dimensional functional layer is 20 to 100 nm; the loading amount is related to the rotation speed and time of spin coating, and the quantum dots of this thickness loaded in the two-dimensional functional layer can fully absorb external photon radiation and generate photogenerated carriers, effectively improving the overall photoelectric conversion capability of the ultraviolet photodetector, so that the multi-band ultraviolet photodetector has a lower dark current and a higher operating temperature and threshold sensitivity.

[0035] In some embodiments, the first electrode and the second electrode are disposed on opposite sides of the two-dimensional functional layer, and the first electrode and the second electrode are grown on the surface of the ultraviolet light detection layer. In this case, the electrodes are easy to grow, and the preparation process of the multi-band ultraviolet photodetector is simple, which is suitable for the application of most photoelectric response devices.

[0036] In some specific embodiments, the schematic diagram of the structure of the multi-band ultraviolet photodetector is shown in the attached Figure 1 As shown, from bottom to top, it includes a substrate, an ultraviolet light detection layer and a two-dimensional functional layer which are laminated and bonded in sequence, and the two-dimensional functional layer is loaded with quantum dots, and a first electrode and a second electrode which simultaneously form ohmic contact with the ultraviolet light detection layer and the two-dimensional functional layer; and the first electrode and the second electrode are grown on the surface of the ultraviolet light detection layer.

[0037] In other embodiments, the first electrode and the second electrode are arranged on opposite sides of the two-dimensional functional layer, and the first electrode and the second electrode are partially grown inside the ultraviolet light detection layer. In this case, the electrode is partially grown inside the ultraviolet light detection layer, and the electric field is evenly distributed throughout the detector, which can significantly improve the quantum efficiency, responsivity, response speed, and linear response range of the multi-band ultraviolet photodetector, and is conducive to realizing a high-responsivity device.

[0038] In some other specific embodiments, the structural diagram of the multi-band ultraviolet photoelectric detector is shown in the attached figure. Figure 2 As shown, from bottom to top, it includes a substrate, an ultraviolet light detection layer and a two-dimensional functional layer which are stacked and bonded in sequence, and the two-dimensional functional layer is loaded with quantum dots. And a first electrode and a second electrode which simultaneously form ohmic contact with the ultraviolet light detection layer and the two-dimensional functional layer; and the first electrode and the second electrode are partially grown inside the ultraviolet light detection layer.

[0039] In some specific embodiments, the schematic diagram of the structure of the electrode partially grown inside the ultraviolet light detection layer can be as shown in the attached figure. Figure 3 and 4 shown.

[0040] In some embodiments, the first electrode and the second electrode are selected from Ti / Au / Ti, and the electrodes of this structure have better photocurrent collection and transmission efficiency.

[0041] In the multi-band ultraviolet photodetector of the embodiment of the present application, the energy transfer between quantum dots and two-dimensional materials (i.e., 2D semiconductor materials) may be driven by two interaction mechanisms: non-radiative energy transfer (NRET) and / or photoinduced charge transfer (CT). First, under luminescence, the sensitizing layer of the quantum dots and the two-dimensional material film absorb photons to generate electron-hole pairs. In the quantum dot layer, photoexcited carriers are efficiently generated and separated in the van der Waals heterostructure between the quantum dots and the two-dimensional material. The photogenerated electrons in the quantum dot layer are transferred to the two-dimensional material through the tunnel between the quantum dots and the two-dimensional material, and are cyclically transferred under the drive of the external electric field. The external bias electric field contributes more carriers to increase the photocurrent. At the same time, excitons can be transferred from quantum dots to the two-dimensional functional layer, and the electron-hole pairs in the two-dimensional material are increased through the non-radiative energy transfer process. At the same time, due to the nanometer-level thickness of the two-dimensional material, the thin film geometry of the two-dimensional material enhances the process of non-radiative energy transfer. Therefore, it is more effective to transfer from the sensitive layer of the quantum dot to the two-dimensional material than to the bulk material, making full use of the advantages of the two-dimensional material structure. At the same time, due to the huge difference in the band gap of the two-dimensional material and gallium oxide, a strong built-in electric field region will be formed at the junction of the two-dimensional material and gallium oxide. When the device is exposed to deep ultraviolet light, the absorption of the incident light will lead to the generation of electron-hole pairs, which will be quickly separated by the strong built-in electric field and then transferred to the electrode, resulting in increased photocurrent and fast response speed. In addition, the strong built-in electric field ensures that the device can operate under zero bias voltage and natural passivation surface, while the two-dimensional material film can prevent the device from suffering from surface leakage current.

[0042] As attached Figure 5 As shown, the second aspect of the embodiment of the present application provides a method for preparing a multi-band ultraviolet photoelectric detector, comprising the following steps:

[0043] S10. Obtain a clean substrate and prepare an ultraviolet light detection layer on a surface of the substrate;

[0044] S20. Preparing a first electrode and a second electrode disposed opposite to each other on a surface of the ultraviolet light detection layer facing away from the substrate;

[0045] S30. Prepare a two-dimensional functional layer between the first electrode and the second electrode of the ultraviolet light detection layer, wherein quantum dots are loaded in the two-dimensional functional layer to obtain a multi-band ultraviolet photodetector.

[0046] The second aspect of the embodiment of the present application provides a method for preparing a multi-band ultraviolet photodetector. After preparing a laminated ultraviolet light detection layer on the surface of a clean substrate, prepare a first electrode and a second electrode that are relatively arranged. The electrodes can be grown on the surface of the ultraviolet light detection layer, or they can be partially grown inside the ultraviolet light detection layer. Then, a two-dimensional functional layer loaded with quantum dots is prepared between the first electrode and the second electrode of the ultraviolet light detection layer to obtain a multi-band ultraviolet photodetector. The preparation process is simple and suitable for large-scale industrial production and application. The prepared multi-band ultraviolet photodetector combines various functional layers so that the device has the characteristics of wide spectrum, high responsiveness, and fast response. It can be widely used in the fields of microelectronics technology such as integrated optoelectronic device design, manufacturing and process technology, as well as new electronic components such as semiconductor light-emitting technology and flat panel display devices.

[0047] In the above step S10, a clean substrate is obtained. Specifically, after obtaining the substrate, the substrate may be pre-treated by cleaning, polishing, etc. to remove stains on the surface of the substrate and make the surface of the substrate clean and smooth.

[0048] In some embodiments, the step of preparing the ultraviolet detection layer includes: depositing ultraviolet detection material on a surface of a substrate by metal organic compound chemical vapor deposition to form an ultraviolet detection layer. The ultraviolet detection layer grown by metal organic compound chemical vapor deposition has a flat film layer, good density, and uniform thickness. In some specific embodiments, the conditions for growing the ultraviolet detection material layer on a surface of a substrate by metal organic compound chemical vapor deposition include: the back vacuum is (1-3)×10 -5 Torr, substrate temperature is 600-900°C, metal source temperature is 900-1100°C, RF power input power is 200-500W, RF power reflected power is 4-8W, and oxygen flow rate is 0.5-2sccm.

[0049] In some embodiments, the ultraviolet light detection layer includes at least one ultraviolet light detection material selected from Ga2O3, GaN, AlGaN, ZnO, GaAs, InAs, InP, CdTe, and Ge; these materials have strong absorption capabilities in the ultraviolet band, especially in the solar-blind band (200-280nm), and have excellent photoelectric detection capabilities, providing the photodetector with photoelectric detection capabilities in the solar-blind band.

[0050] In some embodiments, the thickness of the ultraviolet light detection layer is 10-100 nm, which can effectively provide the photoelectric detection capability of the multi-band ultraviolet photodetector in the solar-blind band. If the thickness of the ultraviolet light detection layer is too thick, the photocurrent response speed will be reduced.

[0051] In the above step S20, a first electrode and a second electrode are prepared opposite to each other on the surface of the ultraviolet detection layer facing away from the substrate. The electrodes can be grown on the surface of the ultraviolet detection layer or partially grown inside the ultraviolet detection layer.

[0052] In some embodiments, the first electrode and the second electrode are grown on the surface of the ultraviolet detection layer, and the steps of preparing the first electrode and the second electrode include: using an electron beam to photolithographically pattern the electrode on the surface of the ultraviolet detection layer, depositing electrode materials in the electrode pattern area, and forming the first electrode and the second electrode arranged oppositely on the surface of the ultraviolet detection layer. In this case, the electrode preparation process is simple, the device preparation process is simplified, and the device efficiency is improved.

[0053] In other embodiments, the first electrode and the second electrode are partially grown inside the ultraviolet light detection layer, and the steps of preparing the first electrode and the second electrode include: depositing photoresist on the surface of the ultraviolet light detection layer, exposing the electrode pattern and performing etching treatment, so that the surface and the interior of the ultraviolet light detection layer can be the electrode deposition area, and then depositing electrode materials to form relatively arranged first electrodes and second electrodes that are partially embedded in the ultraviolet light detection layer, and parts of the first electrodes and the second electrodes are higher than the surface of the ultraviolet light detection layer, so as to form ohmic contact with the two-dimensional functional layer at the same time.

[0054] In some embodiments, the etching treatment conditions include: etching for 5 to 20 minutes under the conditions of a radio frequency power of 150 to 600 W, a pressure of 1 to 3 Pa, and a flow ratio of etching gas to carrier of (5 to 20): (20 to 5); in this case, effective etching can be formed on the surface of the ultraviolet light detection layer and the shallow layer inside, so as to facilitate the formation of a first electrode and a second electrode partially embedded in the ultraviolet light detection layer and partially higher than the ultraviolet light detection layer after the subsequent deposition of electrode materials.

[0055] In some embodiments, the electrode material includes at least one metal selected from the group consisting of Ti, Au, and Ag, which have good photocurrent collection and transmission efficiency.

[0056] In the above step S30, a two-dimensional functional layer loaded with quantum dots is prepared between the first electrode and the second electrode of the ultraviolet light detection layer, and the quantum dots and the two-dimensional material are combined. The quantum dots have strong light absorption ability, strong carrier absorption ability, and strong and excellent charge transfer characteristics. The quantum dots can fully absorb external photon radiation and generate photogenerated carriers, which can effectively improve the overall photoelectric conversion capability of the ultraviolet photodetector, so that the multi-band ultraviolet photodetector has a lower dark current and a higher operating temperature and threshold sensitivity.

[0057] In some embodiments, the steps of preparing a two-dimensional functional layer include: using a dry transfer method to transfer the two-dimensional material between the first electrode and the second electrode of the ultraviolet light detection layer, annealing to prevent the electrode from falling off during the process of spin coating quantum dots, and further strengthening the electrode by using an annealing process in a rapid annealing furnace for the device, and then depositing a quantum dot solution on the surface of the two-dimensional material, and drying to form a two-dimensional functional layer.

[0058] In some embodiments, the step of dry transfer of the two-dimensional material to the ultraviolet detection layer includes: first prepare a glass slide, stick polydimethylsiloxane PDMS on one end of the glass slide, and fix it with tape. Then stick the tape with the two-dimensional material after mechanical peeling on the PDMS, and quickly tear off the tape. At this time, a part of the two-dimensional material will remain on the PDMS. This step utilizes the adhesion of PDMS itself to the two-dimensional material. Observe the PDMS under an ultra-depth microscope, find the peeled two-dimensional material with good quality and smooth surface, and mark it. Next, observe under the ultra-depth microscope, find the position of the two-dimensional material to be transferred, align it with the electrode position, and then fit the PDMS and the sample. After fitting, remove the PDMS. Due to the van der Waals force, the two-dimensional material will naturally fit between the first electrode and the second electrode of the ultraviolet detection layer, completing the stacking process, and the transfer of the two-dimensional material is completed.

[0059] In some embodiments, the annealing conditions include: in an inert atmosphere such as nitrogen or argon, heating at a rate of 5 to 10°C / min, heating to an annealing temperature of 300 to 500°C, and keeping the temperature for 20 to 60 minutes to complete the annealing of the device.

[0060] In some embodiments, the method of depositing quantum dot solution on the surface of two-dimensional material is spin coating. In some specific embodiments, the device is placed in a glue spreader, and the forward rotation speed is set to 300-400rpm, and the rotation time is 4-8 seconds; the rear rotation speed is set to 2000-3000rpm, and the rotation time is 30-120s. Use a dropper to take an appropriate amount of solvent as quantum dot solution, and drip it on the surface of the two-dimensional material prepared by the device until the droplets wrap the surface of the sample, and then start spin coating. After spin coating, the surface of the sample is cleaned with methanol, ethanol and other solutions, and the solution is also dripped onto the surface of the two-dimensional material and then spin coated. After the end, it is dried to accelerate the evaporation of the methanol and ethanol solutions remaining on the surface of the sample after cleaning; a two-dimensional functional layer is obtained.

[0061] In some embodiments, the concentration of the quantum dot solution is 30-50 mg / ml; this concentration of the quantum dot solution is conducive to both spin coating and loading the quantum dot material in the two-dimensional material. In some specific embodiments, the concentration of the quantum dot solution can be 30-35 mg / ml, 35-40 mg / ml, 40-45 mg / ml, 45-50 mg / ml, etc.

[0062] In some embodiments, the deposition thickness of the quantum dot solution on the surface of the two-dimensional material is 100 to 200 nm; the quantum dot solution of this thickness fully ensures the loading amount of the quantum dot material in the two-dimensional material.

[0063] In some embodiments, the two-dimensional material includes a two-dimensional material layer, which is at least one of hexagonal boron nitride, two-dimensional molybdenum disulfide, two-dimensional molybdenum diselenide, two-dimensional tungsten disulfide, two-dimensional tin sulfide, two-dimensional silicene, germanene, black phosphorus, and graphene; these two-dimensional materials all have good light transmittance and absorption response capabilities from visible light to infrared light.

[0064] In some embodiments, the quantum dot solution includes at least one quantum dot selected from the group consisting of PbSe, PbS, HgTe, CsPbCl3, MAPbCl3, CsPbBr3, and MAPbBr3; these quantum dots all have strong light absorption capabilities and strong carrier absorption capabilities, as well as strong and excellent charge transfer properties. By combining quantum dots with two-dimensional materials, quantum dots can fully absorb external photon radiation and generate photogenerated carriers, effectively improving the overall photoelectric conversion capability of the ultraviolet photodetector, and enabling the multi-band ultraviolet photodetector to have a lower dark current and a higher operating temperature and threshold sensitivity.

[0065] In some embodiments, in the two-dimensional functional layer, the thickness of the two-dimensional material layer is 2 to 20 nm. This thickness range of the two-dimensional functional layer of the present application is conducive to regulating optical absorption by simply controlling the number of layers of the two-dimensional material, so that the corresponding photodetector can work in different spectral ranges and has a wide photoelectric detection range.

[0066] In some embodiments, the thickness of the loaded quantum dots in the two-dimensional functional layer is 20 to 100 nm. Quantum dots of this thickness can fully absorb external photon radiation and generate photogenerated carriers, effectively improving the overall photoelectric conversion capability of the ultraviolet photodetector, so that the multi-band ultraviolet photodetector has a lower dark current and a higher operating temperature and threshold sensitivity.

[0067] In order to enable the above implementation details and operations of the present application to be clearly understood by those skilled in the art, as well as to demonstrate the significant improvement in performance of the multi-band ultraviolet photodetector and its preparation method in the embodiment of the present application, the above technical solution is illustrated by means of multiple embodiments below.

[0068] Example 1

[0069] A multi-band ultraviolet photodetector based on gallium oxide heterojunction, the structural diagram of which is shown in the attached figure. Figure 2As shown; from bottom to top are a substrate, a gallium oxide ultraviolet light detection layer and a two-dimensional functional layer, in which quantum dots are loaded, and a first electrode and a second electrode that simultaneously form ohmic contact with the ultraviolet light detection layer and the two-dimensional functional layer; and the first electrode and the second electrode are partially embedded in the gallium oxide ultraviolet light detection layer.

[0070] Its preparation comprises the steps of:

[0071] 1. Use Si substrate as the base and clean the surface of the base: ultrasonically clean the base with a diameter of 4 inches and a thickness of 0.5 mm in acetone, anhydrous ethanol and deionized water for 10 minutes, blow dry with nitrogen, and bake on a hot plate at 80°C for 5 minutes to remove the adsorbent on the base surface, ensure that the surface of the substrate is clean and dry, and obtain a clean base.

[0072] 2. Preparation of β-Ga2O3 UV detection layer: A β-Ga2O3 film with a thickness of about 20 nm was grown on the cleaned substrate in step 1 by molecular beam epitaxy. The growth conditions were: the back vacuum was 1.5×10 -5 Torr, the substrate temperature is 760℃, the Ga source temperature is 920℃, the RF power input power is 300W, the RF power reflected power is 6W, and the flow rate of oxygen is 1sccm to form a β-Ga2O3 ultraviolet light detection layer.

[0073] 3. Preparation of electrodes: The conditions for spin coating with PMMA are: PMMA950K, 4000r / min, 1min, thickness is about 180nm; then use a dryer to dry, the drying time is 90℃, time is 2min; PMMA photoresist layer is formed; then electron beam exposure is performed to expose the electrode pattern; after exposure, development is performed, the parameters are: soak in deionized water for 1min, developer (4-methyl-2-pentanone MIBK / isopropyl alcohol IPA) for 70s; nitrogen gun blow dry. Then, the sample is etched using a dry etching process, sulfur hexafluoride (SF6) and argon (Ar) are selected as etching gases, the total etching gas flow rate into the chamber is fixed at 20sccm, and multiple groups of samples are etched under the condition of SF6 and Ar flow ratio of 1:1. The RF power is 600W, the chamber pressure is 1.5Pa, the etching time is 10 minutes, and the electrode pattern is engraved inside the gallium oxide layer. Electron beam evaporation is performed to form electrodes of Ti / Au / Ti with thicknesses of 20nm / 50nm / 20nm respectively; the electrodes are higher than the surface of gallium oxide to facilitate ohmic contact of the two-dimensional material, thereby obtaining a first electrode and a second electrode arranged oppositely.

[0074] 4. Dry transfer of two-dimensional materials: Use dry transfer to transfer the two-dimensional material between the first electrode and the second electrode of the ultraviolet detection layer. The specific operations include: first prepare a glass slide, stick polydimethylsiloxane PDMS on one end of the glass slide, and fix it with tape. Then stick the tape with the two-dimensional material after mechanical peeling on the PDMS, and quickly tear off the tape. At this time, a part of the two-dimensional material will remain on the PDMS. This step uses the adhesion of PDMS itself to the two-dimensional material. Observe the PDMS under an ultra-depth microscope, find the two-dimensional material with good quality and smooth surface, and mark it. Next, observe under the ultra-depth microscope, find the position of the two-dimensional material to be transferred, align it with the electrode position, and then make the PDMS and the sample fit together. After fitting, remove the PDMS. Due to the van der Waals force, the two-dimensional material will naturally fit between the first electrode and the second electrode of the ultraviolet detection layer, completing the stacking process, and the transfer of the two-dimensional material is completed.

[0075] 5. Perform annealing treatment. In order to prevent the electrode from falling off during the spin coating of quantum dots, the device needs to be further reinforced by using an annealing process in a rapid annealing furnace. The annealing treatment is carried out in a nitrogen or argon atmosphere, where the annealing temperature is set to 300°C, the heating rate is 5°C / min, and the holding time is 20min.

[0076] 6. Spin coating quantum dots on the surface of two-dimensional materials: Place the device in a glue spreader, set the forward rotation speed to 350rpm, and the rotation time to 6 seconds; the rear rotation speed to 2500rpm, and the rotation time to 60s. Use a dropper to take an appropriate amount of PbSe quantum dot solution with a concentration of 40mg / ml (the solvent is n-octane), and drip it on the surface of the prepared device two-dimensional material until the droplets wrap the surface of the two-dimensional material, and then start spin coating. After spin coating, use a 1:1 methanol and ethanol mixed solution to clean the surface of the sample, and also drip it onto the surface of the two-dimensional material and spin coat it. After the end, dry it on a drying plate at 50°C for 1 minute to accelerate the evaporation of the methanol and ethanol solutions remaining on the surface of the sample after cleaning, forming a two-dimensional functional layer loaded with quantum dots. Thus, a multi-band ultraviolet photodetector based on gallium oxide heterojunction is prepared.

[0077] Example 2

[0078] A multi-band ultraviolet photodetector based on gallium oxide heterojunction, the structural diagram of which is shown in the attached figure. Figure 1 As shown; from bottom to top are a substrate, a gallium oxide ultraviolet light detection layer and a two-dimensional functional layer, in which quantum dots are loaded, and a first electrode and a second electrode that simultaneously form ohmic contact with the ultraviolet light detection layer and the two-dimensional functional layer; and the first electrode and the second electrode are grown on the surface of the gallium oxide ultraviolet light detection layer.

[0079] Its preparation comprises the steps of:

[0080] 1. Use Si substrate as the base and clean the surface of the base: ultrasonically clean the base with a diameter of 4 inches and a thickness of 0.5 mm in acetone, anhydrous ethanol and deionized water for 10 minutes, blow dry with nitrogen, and bake on a hot plate at 80°C for 5 minutes to remove the adsorbent on the base surface, ensure that the surface of the substrate is clean and dry, and obtain a clean base.

[0081] 2. Preparation of β-Ga2O3 UV detection layer: A β-Ga2O3 film with a thickness of about 20 nm was grown on the cleaned substrate in step 1 by molecular beam epitaxy. The growth conditions were: the back vacuum was 1.5×10 -5 Torr, the substrate temperature is 760℃, the Ga source temperature is 920℃, the RF power input power is 300W, the RF power reflected power is 6W, and the flow rate of oxygen is 1sccm to form a β-Ga2O3 ultraviolet light detection layer.

[0082] 3. Preparation of electrodes: The conditions for spin coating with PMMA are: PMMA950K, 4000r / min, 1min, thickness is about 180nm; then dry it with a dryer, the drying time is 90℃, time is 2min; form a PMMA photoresist layer; then perform electron beam exposure to expose the electrode pattern; after exposure, perform development, the parameters are: soak in deionized water for 1min, developer (4-methyl-2-pentanone MIBK / isopropyl alcohol IPA) for 70s; blow dry with a nitrogen gun. Perform electron beam evaporation to form the first and second electrodes oppositely arranged on the surface of the ultraviolet detection layer, the electrodes are Ti / Au / Ti, and the thicknesses are 20nm / 50nm / 20nm respectively.

[0083] 4. Dry transfer of two-dimensional materials: Use dry transfer to transfer the two-dimensional material between the first electrode and the second electrode of the ultraviolet detection layer. The specific operations include: first prepare a glass slide, stick polydimethylsiloxane PDMS on one end of the glass slide, and fix it with tape. Then stick the tape with the two-dimensional material after mechanical peeling on the PDMS, and quickly tear off the tape. At this time, a part of the two-dimensional material will remain on the PDMS. This step uses the adhesion of PDMS itself to the two-dimensional material. Observe the PDMS under an ultra-depth microscope, find the two-dimensional material with good quality and smooth surface, and mark it. Next, observe under the ultra-depth microscope, find the position of the two-dimensional material to be transferred, align it with the electrode position, and then make the PDMS and the sample fit together. After fitting, remove the PDMS. Due to the van der Waals force, the two-dimensional material will naturally fit between the first electrode and the second electrode of the ultraviolet detection layer, completing the stacking process, and the transfer of the two-dimensional material is completed.

[0084] 5. Perform annealing treatment. In order to prevent the electrode from falling off during the spin coating of quantum dots, the device needs to be further reinforced by using an annealing process in a rapid annealing furnace. The annealing treatment is carried out in a nitrogen or argon atmosphere, where the annealing temperature is set to 300°C, the heating rate is 5°C / min, and the holding time is 20min.

[0085] 6. Spin coating quantum dots on the surface of two-dimensional materials: Place the device in a glue spreader, set the forward rotation speed to 350rpm, and the rotation time to 6 seconds; the rear rotation speed to 2500rpm, and the rotation time to 60s. Use a dropper to take an appropriate amount of PbSe quantum dot solution with a concentration of 40mg / ml (the solvent is n-octane), and drip it on the surface of the prepared device two-dimensional material until the droplets wrap the surface of the two-dimensional material, and then start spin coating. After spin coating, use a 1:1 methanol and ethanol mixed solution to clean the surface of the sample, and also drip it onto the surface of the two-dimensional material and spin coat it. After the end, dry it on a drying plate at 50°C for 1 minute to accelerate the evaporation of the methanol and ethanol solutions remaining on the surface of the sample after cleaning, forming a two-dimensional functional layer loaded with quantum dots. Thus, a multi-band ultraviolet photodetector based on gallium oxide heterojunction is prepared.

[0086] Comparative Example 1

[0087] A multi-band ultraviolet photodetector based on a gallium oxide heterojunction comprises, from bottom to top, a substrate, a gallium oxide ultraviolet light detection layer and a two-dimensional functional layer, and a first electrode and a second electrode that simultaneously form ohmic contacts with the ultraviolet light detection layer and the two-dimensional functional layer; and the first electrode and the second electrode are grown on the surface of the gallium oxide ultraviolet light detection layer.

[0088] The difference between this embodiment and Example 2 is that the process of spin coating quantum dots on the surface of the two-dimensional material in step 6 is not performed.

[0089] Comparative Example 2

[0090] A multi-band ultraviolet photodetector based on a gallium oxide heterojunction comprises, from bottom to top, a substrate, a gallium oxide ultraviolet light detection layer, a first electrode and a second electrode grown on the surface of the gallium oxide ultraviolet light detection layer and arranged oppositely.

[0091] The difference between this embodiment and Example 2 is that steps 4 to 6 are not performed.

[0092] Furthermore, in order to verify the progress of the embodiments of the present application, the following performance tests were performed on the embodiments and the comparative examples respectively:

[0093] 1. Spectral response range. Using lasers in different bands to test the sample’s photoelectric performance is to see if it has good light response in different bands. If it can generate photocurrent in a wider band range and show good photosensitivity, it means it has good spectral response characteristics.

[0094] 2. Light responsivity: It is the comparison between the generated photocurrent and the incident power; the unit is A / W; the incident power is compared with the photogenerated photocurrent; therefore, the light responsivity can be obtained by knowing the incident power of a given light source of different wavelengths, and then comparing the photogenerated photocurrent with the incident power of the light source to obtain the light responsivity of the device.

[0095] 3. Light response time: Usually, the output electrical signal of the photoelectric device lags behind the light signal acting on it in time, that is, the output electrical signal of the photoelectric period is equivalent to the time axis expansion of the input light signal. If the step signal acts on the photoelectric period, the time taken by the photoelectric device to rise from 10% to 90% of the steady-state value is t r It is called the rise time and fall time of the device. f It is defined as the time taken for the response to drop from 90% to 10% of the steady state.

[0096] 4. Photoelectric detection capability: mainly expressed by detection rate. Generally, the greater the detection rate, the stronger the ability of the detector to detect weak signals. The detection rate reflects the sensitivity of the photoelectric detector. A higher detection rate indicates that the detection performance of the photoelectric device is better. The detection capability generally decreases with the increase of wavelength. The embodiment of the present application mainly combines quantum dots with two-dimensional materials and gallium oxide materials, fully combining their respective advantages, enhancing the device's ability to absorb light and improving the photoelectric detection capability.

[0097] The test results are shown in Table 1 below:

[0098] Table 1

[0099]

[0100] It can be seen from the above test results that the multi-band ultraviolet photodetectors based on gallium oxide heterojunction prepared in Examples 1 and 2 of the present application have a wide spectral range from 220nm to 1050nm, and a short response time of only 0.001s and 0.02s, a high light responsivity of 0.08 and 0.02, and a high specific detection rate of 1.2×10 12 Jones and 5×10 11Jones. It is explained that the embodiment of the present application combines quantum dots, two-dimensional materials and gallium oxide, fully designs the energy band structure, and combines the three materials to improve the spectral response range. At the same time, the use of quantum dots increases the light absorption capacity and improves the responsiveness. The reasonable energy band structure design improves the response speed during the period. However, the multi-band ultraviolet photodetector based on gallium oxide heterojunction prepared in Comparative Example 1 did not spin-coat the quantum dot material on the surface of the two-dimensional material, which significantly reduced the light responsiveness and response time of the device. The multi-band ultraviolet photodetector based on gallium oxide heterojunction prepared in Comparative Example 2 did not perform steps 4 to 6, that is, the two-dimensional functional layer loaded with quantum dots was not formed, and the light responsiveness, response time and specific detection rate of the device dropped sharply.

[0101] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A multi-band ultraviolet photodetector, It is characterized in that The multi-band ultraviolet photodetector comprises a substrate, an ultraviolet light detection layer and a two-dimensional functional layer which are stacked and bonded in sequence, and a first electrode and a second electrode which simultaneously form ohmic contact with the ultraviolet light detection layer and the two-dimensional functional layer; the two-dimensional functional layer is loaded with quantum dots; the ultraviolet light detection layer comprises Ga 2 O 3 , at least one ultraviolet light detection material selected from GaN, AlGaN, ZnO, GaAs, InAs, InP, CdTe, and Ge, the interaction mechanism driving the energy transfer between the quantum dots and the two-dimensional material in the two-dimensional functional layer includes: non-radiative energy transfer and / or light-induced charge transfer; in the two-dimensional functional layer, the two-dimensional material is a nanomaterial with a layered structure composed of a single layer or a few atomic layers, the longitudinal thickness of the two-dimensional material is less than 5nm, and the lateral size is greater than 100nm; the thickness of the ultraviolet light detection layer is 10-100nm; in the two-dimensional functional layer, the thickness of the two-dimensional material layer is 2-20nm, and the thickness of the loaded quantum dots is 20-100nm.

2. The multi-band ultraviolet photodetector according to claim 1, It is characterized in that The two-dimensional functional layer includes a two-dimensional material layer, and the two-dimensional material layer includes at least one two-dimensional material selected from the group consisting of hexagonal boron nitride, two-dimensional molybdenum disulfide, two-dimensional molybdenum diselenide, two-dimensional tungsten disulfide, two-dimensional tin sulfide, two-dimensional silicene, germanene, black phosphorus, and graphene; And / or, the quantum dots include PbSe, PbS, HgTe, CsPbCl 3 MAPbCl 3 、CsPbBr 3 MAPbBr 3 At least one of .

3. The multi-band ultraviolet photodetector according to claim 1 or 2, It is characterized in that The first electrode and the second electrode are arranged on two opposite sides of the two-dimensional functional layer, and the first electrode and the second electrode are grown on the surface of the ultraviolet light detection layer; Alternatively, the first electrode and the second electrode are arranged on two opposite sides of the two-dimensional functional layer, and the first electrode and the second electrode are partially grown inside the ultraviolet light detection layer.

4. The multi-band ultraviolet photodetector according to claim 3, It is characterized in that The first electrode and the second electrode are selected from Ti / Au / Ti.

5. A method for preparing a multi-band ultraviolet photodetector according to any one of claims 1 to 4, It is characterized in that The following steps are involved: Obtain a clean substrate, and prepare an ultraviolet light detection layer on one surface of the substrate; the ultraviolet light detection layer includes Ga 2 O 3 At least one ultraviolet light detection material selected from GaN, AlGaN, ZnO, GaAs, InAs, InP, CdTe, and Ge; the thickness of the ultraviolet light detection layer is 10 to 100 nm; Prepare a first electrode and a second electrode disposed opposite to each other on a surface of the ultraviolet light detection layer facing away from the substrate; A two-dimensional functional layer is prepared between the first electrode and the second electrode of the ultraviolet light detection layer, and quantum dots are loaded in the two-dimensional functional layer to obtain a multi-band ultraviolet photodetector; in the two-dimensional functional layer, the two-dimensional material is a nanomaterial with a layered structure composed of a single layer or a few atomic layers, and the longitudinal thickness of the two-dimensional material is less than 5nm and the lateral size is greater than 100nm; in the two-dimensional functional layer, the thickness of the two-dimensional material layer is 2 to 20nm, and the thickness of the loaded quantum dots is 20 to 100nm.

6. The method for preparing the multi-band ultraviolet photodetector according to claim 5, It is characterized in that The step of preparing the ultraviolet detection layer includes: depositing ultraviolet detection material on a surface of the substrate by metal organic compound chemical vapor deposition method to form the ultraviolet detection layer.

7. The method for preparing the multi-band ultraviolet photodetector according to claim 5 or 6, It is characterized in that The first electrode and the second electrode are grown on the surface of the ultraviolet detection layer, and the steps of preparing the first electrode and the second electrode include: after photolithography of an electrode pattern on the surface of the ultraviolet detection layer using an electron beam, electrode materials are deposited in the electrode pattern area to form the first electrode and the second electrode arranged opposite to each other on the surface of the ultraviolet detection layer; Alternatively, the first electrode and the second electrode are partially grown inside the ultraviolet light detection layer, and the steps of preparing the first electrode and the second electrode include: depositing photoresist on the surface of the ultraviolet light detection layer, performing etching after exposing the electrode pattern, depositing electrode material, and forming the first electrode and the second electrode arranged opposite to each other; and the first electrode and the second electrode are higher than the surface of the ultraviolet light detection layer.

8. The method for preparing the multi-band ultraviolet photodetector according to claim 7, It is characterized in that The etching treatment conditions include: etching for 5 to 20 minutes under the conditions of RF power of 150 to 600 W, pressure of 1 to 3 Pa, and flow ratio of etching gas to carrier of (5 to 20): (20 to 5); And / or, the electrode material includes at least one metal of Ti, Au, and Ag.

9. The method for preparing the multi-band ultraviolet photodetector according to claim 5 or 8, It is characterized in that The steps of preparing the two-dimensional functional layer include: transferring the two-dimensional material between the first electrode and the second electrode of the ultraviolet light detection layer by dry transfer, depositing a quantum dot solution on the surface of the two-dimensional material after annealing, and drying to form the two-dimensional functional layer.

10. The method for preparing the multi-band ultraviolet photodetector according to claim 9, It is characterized in that The annealing treatment conditions include: in an inert atmosphere, heating to 300-500°C at a heating rate of 5-10°C / min, and keeping the temperature for 20-60min; and / or, the concentration of the quantum dot solution is 30 to 50 mg / ml; and / or, the deposition thickness of the quantum dot solution on the surface of the two-dimensional material is 100 to 200 nm; And / or, the two-dimensional material includes a two-dimensional material layer, and the two-dimensional material layer includes at least one of hexagonal boron nitride, two-dimensional molybdenum disulfide, two-dimensional molybdenum diselenide, two-dimensional tungsten disulfide, two-dimensional tin sulfide, two-dimensional silicene, germanene, black phosphorus, and graphene; And / or, the quantum dot solution includes PbSe, PbS, HgTe, CsPbCl 3 MAPbCl 3 、CsPbBr 3 MAPbBr 3 At least one quantum dot.

Citation Information

Patent Citations

  • Quantum dot-photodoped graphene / boron nitride / gallium nitride ultraviolet detector and manufacturing method thereof

    CN106505115A

  • Photoelectric detector with graphene sandwich structure

    CN110224041A

  • High-speed photoelectric detector based on gallium oxide / molybdenum disulfide two-dimensional heterojunction

    CN111599890A