A method for preparing a support grid
Through the combination of photosensitive polymer materials and patterned metal grilles, self-alignment exposure and curing of the supporting grid plate is achieved by using ultraviolet light, solving the screen crease and fitting problems of foldable and retractable products, and improving the product's Durability and environmental protection.
Patent Information
- Application Number
- CN202210119214.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-02-08
AI Technical Summary
The screens of existing foldable and retractable electronic products have poor crease and durability due to the hinge structure and material properties, and the uneven film surface of the retractable products makes it impossible to fit closely with the display screen during assembly, which affects the printing process.
Photosensitive polymer materials are combined with patterned metal grids to achieve self-alignment exposure and curing of the supporting grid plate through ultraviolet light irradiation to ensure uniform thickness and high fit. At the same time, the water and acid and alkali resistance of polymer materials are utilized. Perform thorough cleaning.
The degree of fit between the support grid and the display screen is improved, chemical pollution is reduced, environmentally friendly technical process optimization is achieved, and support grids without organic residues on the surface are produced without chemical pollution.
Smart Images

Figure CN116603700B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electronic product accessories, and in particular to a method for preparing a supporting grid plate. Background Art
[0002] As full-screen technology matures, foldable, retractable and rollable products in mobile terminals have received widespread market attention. For foldable products, the hinge structure and the viscoelastic properties of the screen's own materials lead to problems such as screen creases and poor durability, which greatly limits their market promotion. Retractable products can solve the above problems well, but the film surface of retractable products in related technologies is uneven, resulting in the film being unable to fit tightly with the display screen during assembly, affecting the subsequent molding process, and thus affecting its further promotion and use. Summary of the invention
[0003] The present application aims to solve one of the technical problems in the related art at least to some extent.
[0004] To this end, the embodiment of the present application proposes a method for preparing a support grid, so that a support grid with uniform thickness can be obtained, thereby improving the degree of fit between the support grid and the display screen, which is beneficial to the subsequent molding process. At the same time, since the preparation method provided in the embodiment of the present application uses a metal grid, it can itself be used as a mask, so there is no need to selectively adjust the alignment accuracy during the curing process, and the process is convenient and simple. In addition, the preparation method provided in the embodiment of the present application is based on a photosensitive polymer coating. The cured photosensitive material has a high degree of cross-linking between molecules and has the characteristics of water resistance, acid and alkali resistance, and chemical solvent resistance. Therefore, in subsequent processing, the uncured material can be thoroughly cleaned without affecting the cured material. Therefore, the preparation method can produce a support grid with no organic residue and no chemical pollution on the surface, thereby effectively reducing chemical pollution, being environmentally friendly, and achieving optimization of technical processes.
[0005] In an embodiment of the present application, the method for preparing a support grid comprises the following steps:
[0006] Provide lining;
[0007] Disposing a patterned metal grid on the liner;
[0008] coating a photosensitive polymer material on the patterned metal grid;
[0009] The photosensitive polymer material is irradiated with ultraviolet light to solidify the photosensitive polymer material to form the supporting grid plate.
[0010] In the method for preparing a supporting grid plate in an embodiment of the present application, after providing a backing plate, a patterned metal grid is arranged on the backing plate, a photosensitive polymer material is coated on the patterned metal grid, and then the photosensitive polymer material is irradiated with ultraviolet light to cure the photosensitive polymer material to form the supporting grid plate, thereby allowing the photosensitive polymer material to be cured in a "self-aligned exposure" manner, thereby achieving highly controllable gap filling depth of the supporting grid plate and improving its degree of adhesion to the display screen, thereby optimizing the technical process.
[0011] In some embodiments, before coating the photosensitive polymer material on the patterned metal grid, the patterned metal grid and the backing plate are subjected to surface treatment. Preferably, the surface treatment is surface plasma treatment or surface sandblasting treatment.
[0012] In some embodiments, the photosensitive polymer material is selected from at least one of the following: the photosensitive polymer material is selected from at least one of the following: UV-curable polyurethane, UV-curable polyester resin, UV-curable acrylate, UV-curable modified silicone resin and a mixture thereof.
[0013] In some embodiments, the photosensitive polymer material is coated on the patterned metal grid at a spraying flow rate of 1 to 5 ml / s. Optionally, the photosensitive polymer material is coated on the patterned metal grid at a spraying speed of 200 to 1000 cm / min.
[0014] In some embodiments, after coating the photosensitive polymer material on the patterned metal grid, the photosensitive polymer material is allowed to flow for at least 10 minutes, preferably 1 to 7 minutes, preferably 1 to 5 minutes, preferably 1 to 3 minutes, and more preferably 2 minutes, and then the photosensitive polymer material is heated at a temperature below 100°C, preferably 70 to 90°C, and more preferably 80°C to dry its surface.
[0015] In some embodiments, the solid content of the photosensitive polymer material is 30% to 100%, preferably 50% to 80%, and more preferably 60%.
[0016] In some embodiments, the backing plate is a material with high ultraviolet light transmittance. Preferably, the backing plate is quartz glass, Teflon and polypropylene film.
[0017] In some embodiments, ultraviolet light is used to irradiate the photosensitive polymer material from a side of the backing plate away from the patterned metal grid to cure the photosensitive polymer material.
[0018] Optionally, 500 to 5000 mj / cm 2 , preferably 850 to 3500 mj / cm 2, more preferably 900 to 2500 mj / cm 2 , more preferably 1000 to 2000 mj / cm 2 The photosensitive polymer material is irradiated with ultraviolet light energy.
[0019] In some embodiments, the curing depth of the photosensitive polymer material is positively correlated with the energy of the ultraviolet light. Preferably, when the energy of the ultraviolet light is 500-5000 mJ / cm 2 When the curing depth is 15μm-320μm; preferably, the UV energy is 850-3500mJ / cm 2 When the curing depth is 20μm-200μm; preferably, the UV energy is 900-2500mJ / cm 2 When the curing depth is 30μm-180μm; preferably, the UV energy is 1000-2000mJ / cm 2 The curing depth is 40-150μm.
[0020] In some embodiments, the ultraviolet light is at least one of UVA and UVB, preferably UVB.
[0021] In some embodiments, after irradiating the photosensitive polymer material with ultraviolet light to solidify the photosensitive polymer material, the method further includes:
[0022] Remove uncured photosensitive polymer materials.
[0023] According to the preparation method of the support grid plate of the embodiment of the present application, the curing depth of the polymer material in the gap is controlled by the "self-aligned exposure" process, thereby improving the degree of adhesion between the support grid plate and the display screen. In addition, the preparation method of the support grid plate of the embodiment of the present application completely removes the uncured polymer material on the surface of the support grid plate on the basis of the photosensitive polymer coating, so that the support grid plate has the advantages of no organic residue on the surface and no chemical pollution.
[0024] According to one or more technical solutions provided in the embodiments of the present application, at least the following technical effects and advantages are achieved:
[0025] The method for preparing the support grid plate of the embodiment of the present application uses a photosensitive polymer coating, utilizes the light curing characteristics of the photosensitive polymer material and the patterned structure of the grid plate, and uses ultraviolet light energy to control the curing depth of the photosensitive polymer material, thereby achieving the curing of the photosensitive polymer material in a "self-aligned exposure" manner, thereby achieving a high degree of controllability of the curing depth, improving the degree of fit between the support grid plate and the display screen, and solving the mold printing problem after the support grid plate is assembled. In addition, the preparation method of the embodiment of the present application is based on the photosensitive polymer coating, and the cured photosensitive material has a high degree of intermolecular crosslinking, and has the characteristics of water resistance, acid and alkali resistance, chemical solvent resistance, etc. Therefore, in the subsequent treatment, the uncured material can be thoroughly cleaned without affecting the cured material. As a result, the production of a support grid plate with no organic residue and no chemical pollution on the surface is achieved, which is environmentally friendly and achieves the optimization of technical processes. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings, in which:
[0027] Figure 1 is a flow chart of a method for preparing a support grid plate according to an embodiment of the present application;
[0028] Figure 2 is a schematic diagram of a method for preparing a supporting grid plate according to an embodiment of the present application;
[0029] Figure 3 is another schematic diagram of a method for preparing a support grid plate according to an embodiment of the present application;
[0030] Figure 4 is another schematic diagram of the method for preparing a supporting grid plate according to an embodiment of the present application;
[0031] Figure 5 It is another schematic diagram of the method for preparing a supporting grid plate according to an embodiment of the present application.
[0032] Reference numerals:
[0033] 11: Lining board;
[0034] 12: Patterned metal grille;
[0035] 13: Photosensitive polymer materials;
[0036] 14: Ultraviolet light source. DETAILED DESCRIPTION
[0037] Embodiments of the present disclosure are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present disclosure, but should not be understood as limiting the present disclosure.
[0038] The present application is based on the inventors' discovery and understanding of the following facts and problems: In the related art, a thermosetting polymer material is coated on a metal grid and cured by heating and baking, so the curing process is carried out step by step from the outside to the inside (i.e., from the periphery to the center). The cured film obtained in this way usually has an uneven thickness, so it cannot fit tightly with the display screen after assembly, which has an adverse effect on the subsequent molding process. In addition, the thermal curing process by heating and baking usually requires the introduction of an organic solvent. Since the cured film formed after curing has a low degree of cross-linking and does not have the characteristics of water resistance, acid and alkali resistance, chemical solvent resistance, etc., it is impossible to thoroughly clean the surface of the cured film, resulting in serious organic solvent residues on the surface of the cured film.
[0039] Combine the following Figure 1 To describe the method for preparing the support grid provided in the embodiments of the present application.
[0040] Figure 1 1 is a flow chart of a method for preparing a support grid plate according to an embodiment of the present application. Figure 1 As shown, the method comprises the following steps:
[0041] Step 101: providing a lining plate;
[0042] Step 102: Arranging a patterned metal grid on the liner;
[0043] Step 103: coating a photosensitive polymer material on the patterned metal grid;
[0044] Step 104: irradiating the photosensitive polymer material with ultraviolet light to solidify the photosensitive polymer material to form a supporting grid.
[0045] The method for preparing the support grid provided in the embodiment of the present application uses a photosensitive polymer coating, utilizes the light curing characteristics of the photosensitive polymer material and the patterned structure of the grid plate, and uses ultraviolet light energy to control the curing depth of the photosensitive polymer material, thereby achieving the curing of the photosensitive polymer material in a "self-aligned exposure" manner, thereby achieving a high degree of controllability of the curing depth, improving the degree of fit between the support grid plate and the display screen, and solving the mold printing problem after the support grid plate is assembled. In addition, the preparation method of the embodiment of the present application is based on the photosensitive polymer coating, and the cured photosensitive material has a high degree of intermolecular crosslinking, and has the characteristics of water resistance, acid and alkali resistance, chemical solvent resistance, etc. Therefore, in the subsequent treatment, the uncured material can be thoroughly cleaned without affecting the cured material. As a result, the production of a support grid plate with no organic residue and no chemical pollution on the surface is achieved, which is environmentally friendly and achieves the optimization of technical processes.
[0046] In the embodiment of the present application, the "support grid" is a support plate for a display screen in an electronic product, which is prepared by filling a metal grid with a polymer material based on a patterned metal grid. It is understandable that any metal grid of suitable size can be selected for the production of the support grid. In some embodiments, the metal grid has a size of 50*150mm to 150*200mm, wherein the gap depth of the grid is 100μm to 200μm. With the patterned metal grid as the basic structure, it itself can be used as a mask, so there is no need to selectively adjust the alignment accuracy during the curing process, and the process is convenient and simple.
[0047] In the embodiments of the present application, "polymer material" is a material based on polymer compounds. In some embodiments, the "polymer material" may be a polymer material, which is a material composed of a polymer compound as a matrix and other additives (auxiliaries). In some embodiments, the "polymer material" is a material without added solvent. According to its fixing method, polymer materials can be divided into thermosetting polymer materials and photosensitive polymer materials. In some embodiments, photosensitive polymer materials are used. It can be understood that the photosensitive polymer material can be any photosensitive curing material and its composition. In some embodiments, the photosensitive polymer material is selected from at least one of the following: UV curing polyurethane, UV curing polyester resin, UV curing acrylate, UV curing modified silicone resin and mixtures thereof. In the preparation method of the support grid in the embodiments of the present application, the photocuring properties of the photosensitive polymer material enable it to adjust the curing depth according to the exposure amount, thereby adjusting the curing filling depth in the gap of the metal grid, thereby improving the degree of fit between the prepared support grid and the display screen, and solving the mold printing problem after the support grid is assembled.
[0048] In some embodiments, the "liner" in step 101 is a material with high ultraviolet light transmittance. Preferably, the liner is quartz glass, Teflon and polypropylene film. It is understood that by using a material with high ultraviolet light transmittance as the liner, the ultraviolet light can efficiently pass through the liner and transfer the ultraviolet light energy to the photosensitive polymer material to be cured, thereby improving the utilization rate of the ultraviolet light.
[0049] In some embodiments, before coating the photosensitive polymer material on the patterned metal grid in step 103, the method further includes: performing surface treatment on the patterned metal grid and the backing plate.
[0050] Specifically, the surface treatment can be any treatment form for surface pretreatment. Preferably, the surface treatment is surface plasma treatment or surface sandblasting, and more preferably, the surface treatment is surface plasma treatment. In some embodiments, the water drop angle on the surface of the treated metal grid is 0 to 5°. Thus, the surface-treated metal grid is conducive to the subsequent coating and curing of polymer materials.
[0051] In step 103 , a photosensitive polymer material is coated on the patterned metal grid.
[0052] Specifically, when the photosensitive polymer material is coated on the patterned metal grid, the solid content of the polymer material, the spray flow rate and the spray speed are adjusted and determined according to the metal grid gap and the film thickness. In some embodiments, the photosensitive polymer material is coated on the patterned metal grid at a spray flow rate of 1 to 5 ml / s, and optionally, the photosensitive polymer material is coated on the patterned metal grid at a spray speed of 200 to 1000 cm / min. The solid content of the photosensitive polymer material is 30% to 100%, preferably 50% to 80%, and more preferably 60%. Thus, by adjusting the solid content of the polymer material, the spray flow rate and the spray speed, the uniformity of the polymer material coating is achieved, which is beneficial to the subsequent leveling and curing.
[0053] In some embodiments, after coating the photosensitive polymer material on the patterned metal grid in step 103, the method further includes: allowing the photosensitive polymer material to flow for at least 10 minutes, preferably 1 to 7 minutes, preferably 1 to 5 minutes, preferably 1 to 3 minutes, and more preferably 2 minutes, and then heating the photosensitive polymer material at a temperature below 100°C, preferably 70 to 90°C, and more preferably 80°C to dry its surface.
[0054] "Leveling" refers to the process in which the coating gradually shrinks to the smallest area due to surface tension after it is applied but before it forms a film. In some embodiments, after the photosensitive polymer material is coated on the patterned metal grid as described in step 103, the photosensitive polymer material is subjected to leveling treatment. The leveling time is selected according to the properties of the photosensitive polymer material. In some embodiments, the leveling takes at least 10 minutes, preferably 1 to 3 minutes, and more preferably 2 minutes. In this way, the photosensitive polymer material is spread on the patterned metal grid. The support grid prepared by this process has a uniform thickness and a high degree of fit with the display screen.
[0055] "Surface drying" is also called touch drying, which means that the wet coating has reached the stage of surface drying, and the coating has changed from a flowable liquid state to a state that is relatively difficult to flow and the surface begins to form a film. In an embodiment of the present application, after the photosensitive polymer material is subjected to leveling treatment, it is subjected to surface drying treatment. It is understandable that the corresponding surface drying time is selected according to the condition of the photosensitive polymer material coating. In some embodiments, a tunnel furnace is used to perform surface drying treatment on the photosensitive polymer material, and the surface drying temperature is set to a temperature below 100°C, preferably 70 to 90°C, and more preferably 80°C to heat the photosensitive polymer material to dry its surface. Surface drying is conducive to the coating film no longer adhering to light and small particles, and the support grid prepared by this process has a uniform thickness and a high degree of fit with the display screen.
[0056] In step 104, the photosensitive polymer material is irradiated with ultraviolet light to solidify the photosensitive polymer material to form a support grid.
[0057] In some embodiments, ultraviolet light is used to irradiate the photosensitive polymer material from the side of the backing plate away from the patterned metal grid to cure it. Figure 4 As shown, "self-aligned exposure" is achieved by illuminating from the side of the substrate away from the patterned metal grid (ie, backside illumination).
[0058] Specifically, "self-aligned exposure" means that during the curing process of the polymer coating, there is no need for deliberate alignment. Due to the obstruction of the patterned metal grid, the photosensitive polymer coating between the grids will be cured, while the coating material blocked by the grid will not be cured. In other words, self-aligned exposure is based on the far-field diffraction of light, using the pattern of the metal grid itself, and using the metal grid pattern itself as a "mask" to achieve the curing of the polymer material filling the material gap through ultraviolet exposure. It can be understood that the "mask" refers to the metal grid, and the photosensitive polymer material without the grid can be cured because it can receive ultraviolet light, while the photosensitive polymer material with the grid cannot be cured because it cannot be irradiated by ultraviolet light due to the obstruction of the metal grid. The embodiment of the present application uses a self-aligned exposure process to cure the photosensitive polymer material, thereby achieving a highly controllable depth of curing of the gap of the support grid and improving its fit with the display screen, thereby solving the mold printing problem after the support grid is assembled.
[0059] In some embodiments, 500 to 5000 mj / cm 2 , preferably 850 to 3500 mj / cm 2 , more preferably 900 to 2500 mj / cm 2 , more preferably 1000 to 2000 mj / cm 2The photosensitive polymer material is irradiated with ultraviolet light energy. It is understandable that the curing depth of the photosensitive polymer material in the gap of the patterned metal grid can be controlled by adjusting the ultraviolet light energy according to specific needs and actual conditions (such as the molecular structure of the photosensitive polymer material used, the number and position of polar groups, the number and position of double bonds, the initiation efficiency and quantity of the initiator, etc.), wherein the curing depth is positively correlated with the ultraviolet light energy, that is, the higher the ultraviolet light energy, the deeper the curing depth. In some embodiments, when the ultraviolet light energy is 500-5000mJ / cm 2 When the UV energy is 850-3500mJ / cm 2 When the curing depth is 20μm-200μm, the UV energy is 900-2500mJ / cm 2 When the curing depth is 30μm-180μm, the UV energy is 1000-2000mJ / cm 2 When the curing depth is 40-150 μm, the filling depth of the polymer material in the metal grid gap is highly controllable, the degree of fit between the support grid and the display screen is improved, and the mold printing problem after the support grid is assembled is solved.
[0060] It is understood that any wavelength of ultraviolet light or a combination thereof that can pass through the UVA and UVB bands of the liner can be used as needed. In some embodiments, the ultraviolet light is at least one of UVA and UVB, preferably UVB. That is, the wavelength of the ultraviolet light is at least one of 275-400nm. Preferably, the wavelength of the ultraviolet light is 280-320nm. As a result, the ultraviolet light can effectively pass through the liner and use its energy to cure the photosensitive polymer material, thereby realizing a process of controlling the curing depth with ultraviolet light energy.
[0061] In some embodiments, after irradiating the photosensitive polymer material with ultraviolet light to cure the photosensitive polymer material in step 104, the method further includes: removing uncured photosensitive polymer material.
[0062] In some embodiments, the uncured photosensitive polymer material is removed by physical means, such as using an organic solvent or using an air knife to remove the uncured photosensitive polymer material on the surface. Optionally, organic solvents such as alcohols and ketones are used to remove the uncured photosensitive polymer material on the surface. In some embodiments, a cleaning machine is used to clean and remove the uncured photosensitive polymer material on the surface. It can be understood that the photosensitive polymer material is cured after being irradiated with the above-mentioned ultraviolet light, and the cured photosensitive material has a high degree of cross-linking between molecules and has the characteristics of water resistance, acid and alkali resistance, and chemical solvent resistance. Therefore, the uncured material can be thoroughly cleaned by the above-mentioned physical method without affecting the cured material. Therefore, the preparation method can produce a support grid plate with no organic residue and no chemical pollution on the surface, thereby effectively reducing chemical pollution, being environmentally friendly, and achieving optimization of technical processes.
[0063] In some embodiments, after removing the uncured photosensitive polymer material, the method further includes: passing the support grid through an air knife and then sending it into a high temperature unit for drying and aging after drying.
[0064] Specifically, the support grid after removing the uncured photosensitive polymer material is passed through an air knife to preliminarily dry and remove debris on the surface of the support grid. It is understandable that the air knife and high temperature unit parameters are set and adjusted according to the specific circumstances of removing the uncured polymer material. In some embodiments, the air knife speed is 15 to 20 m / s. In some embodiments, the temperature of the high temperature unit is set to 110 to 140°C, and the processing time is set to 20 to 45 min. It is understandable that when treated by the high temperature unit, the lower the temperature setting, the longer the processing time setting time. The support grid produced in this way has a uniform thickness and a high degree of fit with the display screen; at the same time, the process is simple, and process optimization is achieved.
[0065] In some embodiments, after removing the uncured photosensitive polymer material, the method further includes: removing the supporting grid.
[0066] Specifically, after drying and aging in a high-temperature unit, a carbon dioxide laser cutting machine is used to cut along the edge of the product (i.e., the support grid) to separate it from the back lining and remove the lining. After the lining is removed, the original contact surface between the support grid and the lining (i.e., the back of the product) is covered with a protective film, and then the polymer material coating surface is covered with a protective film, and the protective film on the back of the product is turned over to remove the protective film, and then the protective film on the coating surface is turned over again to remove the protective film, and the support grid is taken out. It can be understood that during production, the protective film provided can prevent the product from being contaminated by the external environment and at the same time prevent the product from being scratched by hard objects. The support grid produced by this process has a uniform thickness and a high degree of fit with the display screen, which is conducive to the subsequent film printing process.
[0067] Example 1
[0068] Combine the following Figures 2 to 5To explain the method for preparing the support grid plate in Example 1 of the present application. Example 1 of the present application shows a method for producing a support grid plate by spraying and curing a UV-type polymer material to form a solidified filling, comprising:
[0069] 1. Provide highly transparent quartz glass as a lining plate, and set a patterned metal grid on the lining plate. The specific structure is as follows: Figure 2 As shown;
[0070] 2. Use air plasma to treat the surface of patterned metal grille and lining plate. After treatment, the water drop angle on the surface of metal grille is less than 5°;
[0071] 3. Spray UV curing polyurethane coating (such as Figure 3 As shown), after 2 minutes of leveling time, the surface is dried in a tunnel oven at 80°C for 10 minutes;
[0072] 4. UV curing: 2000mj / cm 2 Ultraviolet light energy (ultraviolet light wavelength of 300nm) irradiates the UV curable polyurethane coating on the liner side (i.e., the back side) to cure it, and the resulting curing depth is 150μm. Figure 4 As shown;
[0073] 5. Remove the uncured UV-curable polyurethane material on the surface of the support grid: Figure 5 As shown, the support grid is passed through an air knife to remove the uncured polymer material on the surface, and the air knife speed is set to 15m / s. It is then placed in a high temperature unit for drying and aging, and the high temperature unit is set to 110°C for a treatment time of 45min.
[0074] 6. Take out the product (i.e. the supporting grid): Use a carbon dioxide laser cutting machine to separate the product from the back lining along the edge, cover the polyurethane coated surface with a protective film, flip the product over to remove the protective film on the back, then flip it over again to remove the protective film on the coated surface, and take out the product.
[0075] Meanwhile, in the above step 4, different ultraviolet light energies are used for irradiation to cure the UV-curable polyurethane coating. The specific ultraviolet light parameters and the obtained curing depth are shown in Table 1.
[0076] Example 2
[0077] Example 2 of the present application shows a method for preparing a support grid plate using a UV-curable polyester resin as a photosensitive polymer material, wherein in step 3 of the above-mentioned Example 1, a UV-curable polyester resin is used as a photosensitive polymer material, and different ultraviolet light energies are used for irradiation to cure the UV-curable polyester resin coating, and the remaining steps are the same as those of Example 1. Specific ultraviolet light parameters and the obtained curing depth are shown in Table 1.
[0078] Example 3
[0079] Example 3 of the present application shows a method for preparing a support grid plate using UV-curable acrylate as a photosensitive polymer material, wherein in step 3 of the above-mentioned Example 1, UV-curable acrylate is used as a photosensitive polymer material, and different ultraviolet light energies are used for irradiation to cure the UV-curable acrylate coating, and the remaining steps are the same as those of Example 1. Specific ultraviolet light parameters and the obtained curing depth are shown in Table 1.
[0080] Example 4
[0081] Example 4 of the present application shows a method for preparing a support grid plate using a UV-curable modified silicone resin as a photosensitive polymer material, wherein in step 3 of the above-mentioned Example 1, a UV-curable modified silicone resin is used as a photosensitive polymer material, and different ultraviolet light energies are used for irradiation to cure the UV-curable modified silicone resin coating, and the remaining steps are the same as those of Example 1. Specific ultraviolet light parameters and the obtained curing depth are shown in Table 1.
[0082] Example 5
[0083] The surface of the prepared support grid was tested for organic residues, and the display screen was attached to the support grid and the degree of adhesion was evaluated. The specific results are shown in Table 1.
[0084] Table 1
[0085]
[0086]
[0087] As can be seen from Table 1, the support grid prepared by the method of Examples 1-4 of the present application has a high degree of adhesion to the display screen, thereby solving the mold printing problem after the support grid is assembled. In addition, the method completely removes organic residues on the surface of the support grid, effectively reduces chemical pollution, and achieves optimization of the technical process.
[0088] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0089] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0090] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0091] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0092] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a support grid, characterized in that: The following steps are involved: Provide lining; Disposing a patterned metal grid on the liner; coating a photosensitive polymer material on the patterned metal grid; Irradiating the photosensitive polymer material with ultraviolet light to solidify the photosensitive polymer material to form the support grid; and Remove uncured photosensitive polymer materials. wherein ultraviolet light is used to irradiate the photosensitive polymer material from a side of the backing plate away from the patterned metal grid to cure the photosensitive polymer material, Among them, 500 to 5000mj / cm 2 The photosensitive polymer material is irradiated with ultraviolet light energy. After coating the photosensitive polymer material on the patterned metal grid, the photosensitive polymer material is leveled for at least 10 minutes, and then the photosensitive polymer material is heated at a temperature below 100° C. to dry its surface, and The photosensitive polymer material is selected from at least one of the following: UV curable polyurethane, UV curable polyester resin, UV curable acrylate, UV curable modified silicone resin and a mixture thereof.
2. The method according to claim 1, characterized in that Before coating the photosensitive polymer material on the patterned metal grid, the patterned metal grid and the lining plate are subjected to surface treatment.
3. The method according to claim 2, characterized in that The surface treatment is surface plasma treatment or surface sandblasting treatment.
4. The method according to claim 1, characterized in that: The photosensitive polymer material is coated on the patterned metal grid at a spraying flow rate of 1 to 5 ml / s.
5. The method according to claim 4, characterized in that The photosensitive polymer material is coated on the patterned metal grid at a spraying speed of 200 to 1000 cm / min.
6. The method according to claim 1, characterized in that After coating the photosensitive polymer material on the patterned metal grid, the photosensitive polymer material is leveled for 1 to 7 minutes, and then the photosensitive polymer material is heated at a temperature below 100° C. to dry its surface.
7. The method according to claim 6, characterized in that After coating the photosensitive polymer material on the patterned metal grid, the photosensitive polymer material is leveled for 1 to 5 minutes, and then the photosensitive polymer material is heated at a temperature of 70 to 90° C. to dry the surface thereof.
8. The method according to claim 7, characterized in that After coating the photosensitive polymer material on the patterned metal grid, the photosensitive polymer material is leveled for 1 to 3 minutes, and then the photosensitive polymer material is heated at a temperature of 70 to 90° C. to dry the surface thereof.
9. The method according to claim 8, characterized in that After coating the photosensitive polymer material on the patterned metal grid, the photosensitive polymer material was leveled for 2 minutes, and then the photosensitive polymer material was heated at a temperature of 80° C. to dry its surface.
10. The method according to claim 1, characterized in that The solid content of the photosensitive polymer material is 30% to 100%.
11. The method according to claim 10, characterized in that The solid content of the photosensitive polymer material is 50% to 80%.
12. The method according to claim 11, characterized in that The solid content of the photosensitive polymer material is 60%.
13. The method according to claim 1, characterized in that The lining plate is made of a material with high ultraviolet light transmittance.
14. The method according to claim 13, characterized in that The lining plate is made of quartz glass, Teflon or polypropylene film.
15. The method according to claim 1, characterized in that 850 to 3500 mj / cm 2 The photosensitive polymer material is irradiated with ultraviolet light energy.
16. The method according to claim 15, characterized in that 900 to 2500 mj / cm 2 The photosensitive polymer material is irradiated with ultraviolet light energy.
17. The method according to claim 16, characterized in that 1000 to 2000 mj / cm 2 The photosensitive polymer material is irradiated with ultraviolet light energy.
18. The method according to any one of claims 1 to 14, characterized in that The curing depth of the photosensitive polymer material is positively correlated with the energy of the ultraviolet light.
19. The method according to claim 18, characterized in that When the UV energy is 500-5000mj / cm 2 The curing depth is 15μm-320μm.
20. The method according to claim 19, characterized in that When the UV energy is 850-3500mj / cm 2 When the curing depth is 20μm-200μm.
21. The method according to claim 20, characterized in that When the UV energy is 900-2500mj / cm 2 The curing depth is 30μm-180μm.
22. The method according to claim 21, characterized in that When the UV energy is 1000-2000mj / cm 2 The curing depth is 40-150μm.
23. The method according to any one of claims 1 to 14, characterized in that The ultraviolet light is at least one of UVA and UVB.
24. The method according to claim 23, characterized in that The ultraviolet light is UVB.