Low-loss high-reliability X7F type anti-reduction ceramic dielectric material and preparation method thereof

By adding specific elements and SiO2 sintering aids to BaTiO3-based ceramics, low loss, high reliability X7F type anti-reduction ceramic dielectric material sintered under a reducing atmosphere was prepared, and the low high-temperature insulation resistivity and dielectricity in the prior art were solved. The problem of high loss achieves high insulation resistance and low dielectric loss ceramic dielectric materials, satisfying the X7F characteristics and reducing production costs.

CN118955121APending Publication Date: 2024-11-15BEIJING YUAN LIU HONG YUAN ELECTRONIC TECHNOLOGY CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411024375.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing X7R and X7F type anti-reducing ceramic dielectric materials have low insulation resistivity and high dielectric loss at high temperatures, making it difficult to meet the requirements of high reliability and low cost, especially when the base metal inner electrode and dielectric materials are sintered under reduced atmosphere. The problem of increased oxygen vacancy and electron conductivity caused by oxidation.

Method used

By adding oxides or carbonates of elements such as Mn, Cr, Co, Fe, etc. to BaTiO3-based ceramics, combining rare earth elements such as Ho, Y, Er, Dy, and oxides of Mo and V, and introducing SiO2 as sintering aid The agent was prepared to produce a low loss and high reliability X7F type anti-reduction ceramic dielectric material sintered under a reducing atmosphere, inhibiting the reduction of barium titanate and grain growth, and improving insulation resistance and temperature characteristics.

Benefits of technology

It achieves high insulation resistivity (≥1013Ω·cm) and low dielectric loss (≤0.7%) in the range of -55℃~125℃, meets the X7F characteristics, and improves the temperature stability and reliability of ceramic dielectric materials. Reduces production costs and is suitable for thin-layer and multi-layer processes of MLCC.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955121A_ABST
    Figure CN118955121A_ABST
Patent Text Reader

Abstract

The invention discloses a low-loss high-reliability X7F type anti-reduction ceramic dielectric material and a preparation method thereof, and particularly relates to the technical field of dielectric materials. The dielectric material is composed of a main material BaTiO3, auxiliary materials and a sintering aid, the auxiliary materials comprise R1, R2, R3 and R4, R1 comprises an oxide or carbonate of at least one element of Mn, Cr, Co and Fe, and R4 comprises an oxide or carbonate of at least one element of Mn, Cr, Co and Fe; r2 comprises an oxide or carbonate of at least one element of Ba, Mg, Zr, Ca and Sr; r3 comprises an oxide of at least one element of Ho, Y, Er, Dy and Sm; and R4 comprises an oxide of at least one element of Mo and V. The obtained BME ceramic dielectric material has low dielectric loss, and the dielectric loss at room temperature does not exceed 0.7%. The material system is simple in formula, low in cost, free of lead, environmentally friendly and good in application prospect; and the preparation process is simple and controllable, and is easy for industrial batch production and preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of dielectric materials, and in particular to a low-loss and high-reliability X7F type anti-reduction ceramic dielectric material and a preparation method thereof. Background Art

[0002] Multilayer ceramic capacitors, referred to as MLCC, are one of the fastest growing and most widely used SMD components in the 21st century. They are mainly composed of three parts: dielectric materials, internal electrodes, and terminal electrodes. The ceramic dielectric material and the internal electrode are stacked in a certain way and connected to the terminal electrode in parallel. With the rapid development of electronic information technology, various electronic components involved in the fields of automobiles, oil drilling, aerospace, military industry, etc. need to work at high temperatures for a long time. Long-term use of MLCC at high temperatures will seriously reduce the performance and life of the capacitor. At the same time, the development trend of MLCC thin film and multilayer has increased the consumption of internal electrode materials and greatly increased the production cost. Replacing traditional silver-palladium electrode materials with base metal internal electrode materials such as copper and nickel can greatly reduce production costs. In order to prevent oxidation of base metals and dielectric materials during high-temperature co-firing, sintering needs to be carried out in a reducing atmosphere. The oxygen element in the ceramic material is easy to escape from the lattice to form oxygen vacancies, which causes the material to be partially reduced, resulting in increased loss and decreased insulation resistance. Therefore, the preparation of low-loss and high-reliability dielectric ceramics that can be sintered with base metal electrodes in a reducing atmosphere is one of the important research directions in recent years.

[0003] For a type of ceramic dielectric material that meets the X7R temperature characteristics of the EIA standard, it is usually obtained by doping and modification with BaTiO3 as the base material. The so-called X7R means that the capacitance change rate does not exceed ±15% in the temperature range of -55℃ to +125℃, based on the capacitance at 25℃. The X7F characteristics of the EIA standard, which have higher requirements for capacitance temperature stability, means that the capacitance change rate does not exceed ±7.5% in the temperature range of -55℃ to +125℃.

[0004] BaTiO3 is a ferroelectric perovskite material with a high room temperature dielectric constant (2000-3000) and a moderate Curie temperature (120°C). Currently, BaTiO3-based ceramics constitute the cornerstone of high-dielectric multilayer ceramic capacitors, and their anti-reduction mechanism is relatively mature. Usually, when BaTiO3 is sintered in a reducing atmosphere, Ti 4+ Reduction to Ti 3+, eventually forming oxygen vacancies and weakly bound electrons. As weakly bound electrons participate in the conduction, the conductivity of the dielectric porcelain increases and the resistivity decreases. By adding amphoteric elements such as rare earth elements such as Dy, Y, Ho, and Er to inhibit the reduction of Ti and improve the insulation resistance, while adding acceptor elements such as Mn, Zn, and Mg to inhibit electronic conductivity, the oxygen vacancy compensation mechanism introduced by other defect chemical reactions makes the material anti-reduction.

[0005] However, due to the different barium-titanium ratios, grain sizes and impurity contents in the raw materials of a certain BaTiO3 substrate, the technical difficulty is to select the types of additives and optimize the respective contents to achieve the goal of anti-reduction while maintaining better temperature characteristics and better insulation performance, thereby ensuring the high reliability of the product.

[0006] For MLCC, the insulation resistivity directly affects its performance and stability in the circuit. High insulation resistivity means high reliability. Generally speaking, the higher the temperature, the lower the MLCC insulation resistivity, because high temperature will accelerate the movement of charges in the dielectric ceramic, resulting in increased leakage current, thereby reducing insulation resistivity and reliability.

[0007] Patent CN116462500A discloses a thin-layer BME ceramic material with X7R characteristics and a preparation method thereof. The invention uses barium titanate as a matrix and introduces a variety of additives for compounding. It has good temperature stability and meets the X7R standard, but the loss is greater than 1% and the insulation resistance at room temperature is low.

[0008] Patent CN111410530A discloses a BaTiO3-based dielectric ceramic that resists reduction. The dielectric ceramic uses BaTiO3 as the matrix material and Co2O3 and CaCO3 as auxiliary agents, but the insulation resistivity at room temperature is only 10 11 ~10 12 Ω·cm, and the high temperature insulation resistivity is even lower, only 10 10 ~10 11 Ω·cm.

[0009] There are many documents and patents related to the anti-reduction ceramic dielectric materials that meet the X7R characteristics, but it is difficult to achieve a room temperature insulation resistivity of 10 13 Ω·cm is rare, but the insulation resistivity at 125℃ can reach 10 13 There are few reports on anti-reduction X7F ceramic dielectric materials with Ω·cm.

[0010] With the rapid development of electronic information technology, MLCC is moving towards thin film and multi-layer. The existing technology has the following problems and shortcomings:

[0011] (1) The multi-layering of MLCC leads to an increase in the consumption of precious metal internal electrode materials, which greatly increases the production cost.

[0012] (2) When base metal is used for the inner electrode, the manufacturing cost can be significantly reduced, but it needs to be sintered in a reducing atmosphere. The release of oxygen in the oxide in the dielectric material will produce oxygen vacancies and electrons, resulting in the degradation of MLCC reliability and a decrease in insulation resistance (IR). Therefore, additives should be added to the barium titanate substrate to improve the anti-reduction performance of BaTiO3-based ceramic dielectric materials, and finally obtain multilayer ceramic capacitors with high insulation resistance and high reliability.

[0013] (3) Although there are many types of X7R anti-reduction ceramic dielectric materials reported so far, these ceramic materials have problems such as high dielectric loss, too low insulation resistivity, and reliability degradation. Therefore, the preparation of low-loss and high-reliability dielectric ceramics that can be sintered with base metal electrodes in a reducing atmosphere has become one of the important research directions in recent years. Summary of the invention

[0014] To this end, the present invention provides a low-loss, high-reliability X7F type anti-reduction ceramic dielectric material and a preparation method thereof to solve the above-mentioned problems. The purpose of the present invention is to provide a method for preparing a thin-layer BME ceramic dielectric capacitor ceramic material suitable for MLCC thinning, with low loss, excellent insulation resistance, high reliability and long life, and sintered in a reducing atmosphere, with a stable capacity and temperature, using BaTiO3, which is mature in the market, as a matrix material, by adding various modified materials and sintering aids.

[0015] In order to achieve the above object, the present invention provides the following technical solutions:

[0016] According to one aspect of the present invention, a low-loss, high-reliability X7F type anti-reduction ceramic dielectric material is provided, wherein the dielectric material is composed of a main material BaTiO3 and auxiliary materials and a sintering aid, wherein the auxiliary materials include: R1, R2, R3 and R4, wherein R1 includes an oxide or carbonate of at least one element selected from the group consisting of Mn, Cr, Co and Fe; R2 includes an oxide or carbonate of at least one element selected from the group consisting of Ba, Mg, Zr, Ca and Sr; R3 includes an oxide of at least one element selected from the group consisting of Ho, Y, Er, Dy and Sm; and R4 includes an oxide of at least one element selected from the group consisting of Mo and V.

[0017] Furthermore, the sintering aid is SiO 2; The added amount is 0.1 to 0.4 parts by weight.

[0018] Furthermore, the auxiliary material R1 is added in an amount of 0.01 to 0.15 parts by weight; R2 is added in an amount of 0.5 to 1.5 parts by weight; R3 is added in an amount of 0.3 to 1.1 parts by weight; and R4 is added in an amount of 0.01 to 0.06 parts by weight.

[0019] When barium titanate is sintered in a nitrogen-hydrogen reducing atmosphere, its tetravalent titanium will be reduced to trivalent titanium, and the weakly bound electrons generated will migrate under the action of the electric field, causing the insulation resistance to decrease by an order of magnitude, forming a semiconductor or conductor and losing insulation. By adding the above R1 to R4 auxiliary components, it is possible to inhibit grain growth, improve temperature characteristics, improve dielectric loss and insulation resistance, and effectively prevent barium titanate from being reduced when sintered in a nitrogen-hydrogen reducing atmosphere.

[0020] The ceramic forming temperature of the barium titanate of the present invention is above 1350°C. By adding the sintering aid SiO2 in the above proportion, the ceramic forming temperature of the dielectric material can be reduced, so that the sintering temperature is moderate, which is more conducive to matching with the internal electrode sintering to realize MLCC production.

[0021] Furthermore, the R1 contains at least one of Mn3O4 and MnCO3.

[0022] According to another aspect of the present invention, a method for preparing a low-loss and high-reliability X7F type anti-reduction ceramic dielectric material is provided, the method comprising:

[0023] Step 1: firstly, the auxiliary materials R1, R2, R3 and R4 are mixed with the main material and the sintering aid, and then the mixture is wet dispersed and dried to form granules;

[0024] Step 2: Press the granulated powder into green discs, and remove the binder in a binder removal furnace to remove organic matter;

[0025] Step three, sintering the debinded green wafer in a nitrogen-hydrogen atmosphere furnace, cooling it down, keeping it warm, and then cooling it down to obtain a low-loss, high-reliability, anti-reduction ceramic dielectric material for X7R / X7F.

[0026] Furthermore, in the step 1, the wet dispersion uses zirconium oxide balls as ball milling media, and the wet ball milling time is 4 to 8 hours.

[0027] Furthermore, in the step 2, the binder removal condition is to keep the temperature at 400-500° C. for 3-5 hours.

[0028] Furthermore, in the step three, the sintering temperature is 1240° C. to 1280° C., and the temperature is kept for 2 to 3 hours.

[0029] Furthermore, in step three, the temperature is lowered to 1010° C. and kept warm for 3 to 5 hours.

[0030] The present invention has the following advantages:

[0031] 1. The BME ceramic dielectric material obtained by the present invention has excellent anti-reduction performance. By adding Mn and V elements to BaTiO3-based ceramic powder, Mn and V ions play an acceptor role during the sintering process of the ceramic dielectric material, and the oxygen vacancy concentration caused is greater than the oxygen vacancy concentration formed by oxygen volatilization, which can inhibit the occurrence of electronic conductivity to a certain extent, thereby hindering the semiconducting of barium titanate ceramic materials, improving the anti-reduction property of BaTiO3, and making Ti 4+ It is not easy to be reduced to Ti in a high temperature reducing atmosphere. 3+ As a result, barium titanate can maintain high insulation resistance even when sintered in a reducing atmosphere, greatly improving the insulation resistance of BaTiO3 ceramic dielectric materials at room and high temperatures, ensuring the high reliability of the ceramic material, which plays an important role in increasing the life of MLCC.

[0032] 2. The present invention successfully improves the temperature stability of BaTiO3 ceramic dielectric materials by introducing doping of elements such as Y, Dy, and Ho to play the role of zwitterions and form a "core-shell" structure. The material described in the present invention satisfies the capacitance temperature change rate of ≤±15% in the range of -55°C to 125°C, and satisfies the X7R characteristic. The optimal group satisfies the capacitance temperature change rate of ≤±7.5%, satisfies the X7F characteristic, and has extremely high temperature stability.

[0033] 3. The present invention uses doping Si as a sintering aid to reduce and widen the sintering temperature and prevent the grain growth of ceramic particles during the sintering process. Doping Mg is used to refine the grains, prevent the grain growth of ceramic particles during the sintering process, and promote the mass transfer process of BaTiO3 to improve the density of ceramics.

[0034] 4. The BME ceramic dielectric material obtained by the present invention has low dielectric loss: the dielectric loss does not exceed 0.7% at room temperature.

[0035] 5. The BME ceramic material obtained by the present invention has extremely high insulation resistivity ≥10 at both 25℃ and 125℃. 13 Ω·cm.

[0036] 6. The material system described in the present invention has a simple formula and low cost, is lead-free, is environmentally friendly, and has good application prospects; and the preparation process is simple and controllable, and is easy to prepare for industrial mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. Obviously, the drawings in the following description are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0038] The structures, proportions, sizes, etc. illustrated in this specification are only used to match the contents disclosed in the specification so as to facilitate understanding and reading by persons familiar with the technology. They are not used to limit the conditions under which the present invention can be implemented, and therefore have no substantial technical significance. Any structural modification, change in proportion or adjustment of size shall still fall within the scope of the technical contents disclosed in the present invention without affecting the effects and purposes that can be achieved by the present invention.

[0039] Figure 1 A cross-sectional morphology diagram of the MLCC No. 9 provided in an embodiment of the present invention;

[0040] Figure 2 This is a surface morphology diagram of the MLCC No. 9 provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0041] The following is a description of the implementation of the present invention by specific embodiments. People familiar with the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Unless otherwise specified, the raw materials selected in the present invention can be purchased through commercial channels.

[0043] The present invention provides a low-loss and high-reliability X7F type anti-reduction ceramic dielectric material, which is composed of a main material BaTiO3 and auxiliary materials and a sintering aid:

[0044] The main material BaTiO3 is a mature product sold in the market, with a particle size of 250-350nm and good crystallinity, which ensures that the material has good electrical properties.

[0045] The auxiliary material is one or more of R1, R2, R3 and R4, and the sintering aid R5 is SiO2, wherein:

[0046] Taking the main material BaTiO3 as 100 parts by weight, the added amount of R1 is 0.01-0.15 parts by weight; the added amount of R2 is 0.5-1.5 parts by weight; the added amount of R3 is 0.3-1.1 parts by weight; the added amount of R4 is 0.01-0.06 parts by weight; and the added amount of sintering aid R5 is 0.1-0.4 parts by weight.

[0047] Example

[0048] This embodiment provides a method for preparing a low-loss and high-reliability X7F type anti-reduction ceramic dielectric material, comprising the following steps:

[0049] Weigh the main material, auxiliary material and sintering aid in a ball mill according to the weight ratio designed in Table 1; use deionized water as the medium to mix and ball mill for 4 to 8 hours, dry at 120°C for 6 hours, take out the ceramic powder, grind it into particles with an agate mortar, pass it through a 40-mesh sieve, and store it in a sealed container for later use.

[0050] Table 1 Example related formula

[0051]

[0052] The granulated powder is pressed into a round green sheet with a diameter of 10 mm, and kept at a temperature of 400-500° C. for 3-5 hours in a debinding furnace to discharge organic matter.

[0053] The debinded green disc is sintered in a nitrogen-hydrogen atmosphere furnace at a sintering temperature of 1240°C to 1280°C for 2 to 3 hours, then cooled to 1010°C for 3 to 5 hours, and then cooled in the furnace to obtain low-loss and high-reliability anti-reduction ceramics for X7R / X7F.

[0054] Through the SEM electron microscope, we can see that the cross-sectional morphology of MLCC No. 9 is as follows Figure 1 As shown, the surface morphology of MLCC is as follows Figure 2 As shown, the cross-sectional morphology shows that the ceramic material is sintered densely and co-fired with the inner electrode. The surface morphology shows that there is no abnormal growth of grains and the particle size distribution is uniform. Therefore, the low-loss and high-reliability X7F anti-reduction ceramic dielectric material provided by the present invention has a small dielectric loss on the basis of meeting the temperature characteristics of X7F; it can meet the production needs of the highest-end models of chip capacitors.

[0055] Then the ceramic disc is surface treated, and the electrodes are coated and sintered. After the disc capacitor is made, the capacitance, loss, insulation resistance and temperature characteristics are tested, and the relative dielectric constant, insulation resistivity and temperature coefficient are calculated. The performance parameters are shown in Table 2.

[0056] Table 2 Related properties of the embodiment formula

[0057]

[0058] From the comparison of product performance obtained in Table 2, we can see that:

[0059] Among them, the low-loss and high-reliability anti-reduction ceramic dielectric materials for X7F prepared by the optimal group of formula 13 and formula 14 can form a dielectric constant between 1600 and 2100 in the temperature range of 1240℃ to 1280℃ by adjusting the ratio of the main material BaTiO3 and the auxiliary material, and the loss is less than 0.7%, and the insulation resistivity at 25℃ and 125℃ is both within 10 13 The ceramic dielectric material with a system-adjustable dielectric constant of more than Ω·cm has the overall performance of high dielectric constant, low dielectric loss, high insulation resistance, excellent temperature characteristics, and even better temperature stability in the temperature range of -55 to 125°C, meeting the X7F type (ΔC / C 25℃ ≤±7.5%) Temperature stability requirements for dielectric materials.

[0060] The invention protects a new type of low-loss, high-reliability, anti-reduction ceramic dielectric material for X7F. The ceramic dielectric material is composed of the main material BaTiO3 and auxiliary materials such as Mg, Mn, Y and sintering aids. The comprehensive electrical properties of the dielectric material are adjusted by controlling the components of the auxiliary materials and sintering aids. The atmosphere sintering is carried out at 1240℃~1280℃ to prepare an anti-reduction ceramic dielectric material with good performance: dielectric constant ≥1600, dielectric loss ≤0.7%; within the temperature range of -55~+125℃, the temperature characteristics meet the X7R characteristics, and the optimal temperature can be adjusted to X7F (ΔC / C 25℃ ≤±7.5%); can meet the requirements of MLCC process where ceramic dielectric is sintered with base metal electrodes in a reducing atmosphere; has extremely high insulation resistivity of ≥10 at both 25℃ and 125℃ 13 Ω·cm, providing a performance foundation for high reliability and long life.

[0061] Although the present invention has been described in detail above by general description and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.

Claims

1. A low-loss, high-reliability X7F type anti-reduction ceramic dielectric material, characterized in that: The dielectric material is composed of a main material BaTiO3 and auxiliary materials and a sintering aid, wherein the auxiliary materials include: R1, R2, R3 and R4, wherein R1 includes an oxide or carbonate of at least one element among Mn, Cr, Co, and Fe; R2 includes an oxide or carbonate of at least one element among Ba, Mg, Zr, Ca, and Sr; R3 includes an oxide of at least one element among Ho, Y, Er, Dy, and Sm; and R4 includes an oxide of at least one element among Mo and V.

2. The low-loss, high-reliability X7F type anti-reduction ceramic dielectric material according to claim 1, characterized in that: The sintering aid is SiO2.

3. The low-loss and high-reliability X7F type anti-reduction ceramic dielectric material according to claim 1, characterized in that: The auxiliary material R1 is added in an amount of 0.01 to 0.15 parts by weight; R2 is added in an amount of 0.5 to 1.5 parts by weight; R3 is added in an amount of 0.3 to 1.1 parts by weight; and R4 is added in an amount of 0.01 to 0.06 parts by weight.

4. The low-loss and high-reliability X7F type anti-reduction ceramic dielectric material according to claim 1, characterized in that: The R1 contains at least one of Mn3O4 and MnCO3.

5. A method for preparing a low-loss, high-reliability X7F type anti-reduction ceramic dielectric material, characterized in that: The method comprises: Step 1: firstly, the auxiliary materials R1, R2, R3 and R4 are mixed with the main material and the sintering aid, and then the mixture is wet dispersed and dried to form granules; Step 2: Press the granulated powder into green discs, and remove the binder in a binder removal furnace to remove organic matter; Step three, sintering the debinded green wafer in a nitrogen-hydrogen atmosphere furnace, cooling it down, keeping it warm, and then cooling it down to obtain a low-loss, high-reliability, anti-reduction ceramic dielectric material for X7R / X7F.

6. The method for preparing a low-loss and high-reliability X7F type anti-reduction ceramic dielectric material according to claim 5, characterized in that: In the step 1, the wet dispersion uses zirconium oxide balls as ball milling media, and the wet ball milling time is 4 to 8 hours.

7. The method for preparing a low-loss and high-reliability X7F type anti-reduction ceramic dielectric material according to claim 5, characterized in that: In the step 2, the binder removal condition is to keep the temperature at 400-500° C. for 3-5 hours.

8. The method for preparing a low-loss and high-reliability X7F type anti-reduction ceramic dielectric material according to claim 5, characterized in that: In the step 3, the sintering temperature is 1240° C. to 1280° C. and the temperature is kept for 2 to 3 hours.

9. The method for preparing a low-loss and high-reliability X7F type anti-reduction ceramic dielectric material according to claim 5, characterized in that: In the step 3, the temperature is lowered to 1010° C. and kept for 3 to 5 hours.

Citation Information

Patent Citations

  • Dielectric ceramic material for multilayer ceramic capacitor with high temperature insulation performance

    CN103553591A

  • Dielectric material, preparation method thereof and multilayer chip ceramic capacitor

    CN116041058A