Niobium hafnium zirconium potassium sodium lithium bismuth copper lead-free piezoelectric ceramic material and preparation method thereof, and lead-free piezoelectric ceramic and preparation method thereof

By adjusting the chemical formula of niobium hafnium ferrozirconate potassium sodium lithium bismuth copper lead-free piezoelectric ceramic materials with Zr and Li content, the problem of low mechanical quality factor in high-frequency devices in the prior art is solved, and the problem of low mechanical quality factor in high-frequency devices is realized. It has a combination of high Curie temperature and high voltage electrical performance, suitable for a wider temperature range.

CN118973364APending Publication Date: 2024-11-15SOLOMON (CHANGZHOU) ALLOY NEW MATERIAL CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410948299.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing potassium sodium niobium ferrozirconate lithium bismuth copper lead-free piezoelectric ceramic materials are low in high-power and high-frequency devices, resulting in large mechanical energy loss during vibration, and failing to achieve high Curie temperature at the same time. Both high voltage electrical constant and high mechanical quality factor.

Method used

The chemical formula is [(K0.45Na0.55)0.955(1-y)Li0.955y(Bi0.5Na0.5)0.045Cu0.01][Nb0.955(Hf1-xZrx)0.045Fe0.005]O3 Potassium, sodium, lithium, bismuth, copper lead-free piezoelectric ceramic material is prepared by solid phase method to adjust the content of Zr and Li to optimize the microstructure and performance of the ceramic.

Benefits of technology

It improves the Curie temperature and mechanical quality factor of ceramics, maintains high piezoelectric activity and low loss, and is suitable for a wider temperature range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973364A_ABST
    Figure CN118973364A_ABST
Patent Text Reader

Abstract

The invention discloses a niobium hafnium zirconium potassium sodium lithium bismuth copper leadless piezoelectric ceramic material and a preparation method thereof, and a leadless piezoelectric ceramic and a preparation method thereof, the chemical general formula of the niobium hafnium zirconium potassium sodium lithium bismuth copper leadless piezoelectric ceramic material is [(K < 0.45 > Na < 0.55 >) < 0.955 > (1-y) Li < 0.955 > y (Bi < 0.5 > Na < 0.5 >) < 0.045 > Cu < 0.01 >] [Nb < 0.955 > (Hf < 1-x > Zrx) < 0.045 > Fe < 0.005 >] O3, 0 < x < = 0.4, and 0 < = y < = 0.04. The niobium hafnium zirconium potassium sodium lithium bismuth copper lead-free piezoelectric ceramic obtained by the preparation method disclosed by the invention has relatively high piezoelectric activity and also keeps a relatively high mechanical quality factor; and the Curie temperature can be effectively increased while the high piezoelectric property is achieved, and the material can be applied in a larger temperature range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material science and engineering technology, and in particular to a lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite and a preparation method thereof, and to a lead-free piezoelectric ceramic and a preparation method thereof. Background Art

[0002] The piezoelectric effect is an inherent property of materials that lack a symmetry center (except for the 432 family). Piezoelectric ceramics have been widely used in many electronic components such as transducers, drivers, sensors and actuators due to their unique ability to convert mechanical vibrations into electrical energy, as well as their simple preparation process and low cost. Lead can cause harm to the human body and the environment and is not conducive to sustainable development, so the preparation of high-performance lead-free piezoelectric ceramic systems is imminent.

[0003] Potassium sodium niobate (K,Na)NbO3 (KNN) based lead-free piezoelectric ceramics have been widely studied by researchers at home and abroad due to their good piezoelectric activity and high Curie temperature. They are currently the most promising lead-free piezoelectric ceramic materials to replace lead-based piezoelectric ceramics. In recent years, researchers have improved the piezoelectric constant d of KNN-based ceramics prepared by solid phase method through element doping, phase boundary regulation and process improvement. 33 The KNN-based ceramics have a great breakthrough in the field of piezoelectricity, which has broad application prospects. 33 The mechanical quality factor (Q m ) is mostly less than 100, which is not conducive to the actual device application. Therefore, it is necessary to improve the Q of piezoelectric ceramics in high-power and high-frequency devices. m , it is very important to reduce the mechanical energy loss during vibration and avoid excessive heat or thermal runaway. On the other hand, in order for piezoelectric devices to achieve the expected performance, piezoelectric ceramics need to have sufficient piezoelectric activity and maintain a high Curie temperature. However, there is no report on lead-free piezoelectric ceramic materials of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper with high Curie temperature, high piezoelectric constant, and high mechanical quality factor.

[0004] Therefore, in view of the shortcomings of the prior art, it is necessary to provide a niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper lead-free piezoelectric ceramic material and a preparation method thereof, as well as a lead-free piezoelectric ceramic and a preparation method thereof to solve the shortcomings of the prior art. Summary of the invention

[0005] The first object of the present invention is to avoid the shortcomings of the prior art and provide a lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and niobium hafnium zirconium ferrite. The lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite can effectively increase the Curie temperature of the ceramic and maintain high piezoelectric activity, high mechanical quality factor, and low loss.

[0006] The above-mentioned purpose of the present invention is achieved by the following technical measures:

[0007] Provided is a lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where 0<x≤0.4, 0≤y≤0.04.

[0008] The optimal x is 0.2 and y is 0.01.

[0009] The niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material of the present invention is prepared from raw materials including Na2CO3, K2CO3, Nb2O5, Bi2O3, CuO, Fe2O3, and HfO2, and optionally including Li2CO3.

[0010] The piezoelectric constant d of the lead-free piezoelectric ceramic material of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper is 33 180pC / N~318pC / N; Mechanical quality factor Q m The plane electromechanical coupling coefficient k is 180~286; p 0.35~0.52; dielectric loss tanδ is 1.4%~2.0%; Curie temperature T C 314℃~361℃; residual polarization intensity P r 13μC / cm 2 ~20μC / cm 2 , coercive field E c It is 12kV / cm~22kV / cm.

[0011] When x is 0.2 and y is 0.01, it is the best lead-free piezoelectric ceramic material of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper. 33 310pC / N; mechanical quality factor Q m is 228; the plane electromechanical coupling coefficient k p is 0.51; dielectric loss tanδ is 1.4%; Curie temperature T C is 322℃; the residual polarization intensity P r 19μC / cm 2 ; Coercive field E cIt is 13kV / cm.

[0012] The lead-free piezoelectric ceramic material of the present invention has a general chemical formula of [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where 0<x≤0.4, 0≤y≤0.04. The lead-free piezoelectric ceramic material has high piezoelectric activity while maintaining a high mechanical quality factor; and while having high piezoelectric performance, it can also effectively increase the Curie temperature and can be used in a wider temperature range.

[0013] The second object of the present invention is to avoid the shortcomings of the prior art and provide a method for preparing a lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite. The lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite obtained by the method can effectively increase the Curie temperature of the ceramic and maintain high piezoelectric activity, high mechanical quality factor and low loss.

[0014] The above-mentioned purpose of the present invention is achieved by the following technical measures:

[0015] Provided is a method for preparing a lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, comprising the following steps: preparing the lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite by a solid phase method according to the stoichiometric ratio of Na2CO3, K2CO3, Nb2O5, Bi2O3, ZrO2, CuO, Fe2O3, HfO2 and Li2CO3 according to the general chemical formula.

[0016] The preparation method of the potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite lead-free piezoelectric ceramic material of the present invention comprises the following steps:

[0017] Step 1, adding Na2CO3, K2CO3, Nb2O5, Bi2O3, ZrO2, CuO, Fe2O3, HfO2 and Li2CO3 into a ball mill according to the stoichiometric ratio of the chemical formula;

[0018] Step 2: Using zirconium oxide balls as grinding media and anhydrous ethanol as solvent, milling in a ball mill at a speed of 200 rpm to 300 rpm for 10 h to 20 h;

[0019] Step 3: Discharge the material, dry it, put it into a furnace and heat it to 800°C to 900°C, and keep it warm for 4h to 8h to obtain niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper lead-free piezoelectric ceramic material.

[0020] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite is prepared from the lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, wherein the chemical formula of the lead-free piezoelectric ceramic material is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, wherein 0<x≤0.4, 0≤y≤0.04. The niobium hafnium zirconium potassium sodium ferrite lithium bismuth copper lead-free piezoelectric ceramic material obtained by the preparation method has high piezoelectric activity while maintaining a high mechanical quality factor; and while having high piezoelectric performance, it can also effectively increase the Curie temperature and can be used in a wider temperature range.

[0021] The third object of the present invention is to avoid the shortcomings of the prior art and provide a lead-free piezoelectric ceramic of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite. The lead-free piezoelectric ceramic of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite can effectively increase the Curie temperature of the ceramic and maintain high piezoelectric activity, high mechanical quality factor and low loss.

[0022] The above-mentioned purpose of the present invention is achieved by the following technical measures:

[0023] Provided is a niobium hafnium zirconium potassium sodium lithium bismuth copper lead-free piezoelectric ceramic, which is prepared using the above-mentioned niobium hafnium zirconium potassium sodium lithium bismuth copper lead-free piezoelectric ceramic material as a raw material.

[0024] The potassium sodium niobium hafnium zirconium ferrite lithium bismuth copper lead-free piezoelectric ceramic of the present invention is prepared from potassium sodium niobium hafnium zirconium ferrite lithium bismuth copper lead-free piezoelectric ceramic materials. The potassium sodium niobium hafnium zirconium ferrite lithium bismuth copper lead-free piezoelectric ceramic has high piezoelectric activity while maintaining a high mechanical quality factor; and while having high piezoelectric performance, it can also effectively improve the Curie temperature and can be used in a wider temperature range.

[0025] The fourth object of the present invention is to avoid the shortcomings of the prior art and provide a method for preparing lead-free piezoelectric ceramics from niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic materials. The lead-free piezoelectric ceramics prepared by the method can effectively increase the Curie temperature of the ceramics and maintain high piezoelectric activity, high mechanical quality factor, and low loss.

[0026] The above-mentioned purpose of the present invention is achieved by the following technical measures:

[0027] Provided is a method for preparing a lead-free piezoelectric ceramic from potassium sodium niobium hafnium zirconium ferrite lithium bismuth copper lead-free piezoelectric ceramic material, comprising the following steps:

[0028] S1, adding the niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material to a polyvinyl alcohol solution, mixing, granulating, and tableting to obtain a green disc;

[0029] S2, debinding and sintering the green disc obtained in S1 to obtain a lead-free piezoelectric ceramic disc;

[0030] S3, silver polarizing the lead-free piezoelectric ceramic disc obtained in S2 to obtain niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramics.

[0031] The lead-free piezoelectric ceramic of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite of the present invention is prepared by the following steps:

[0032] S1, adding 5wt% to 10wt% polyvinyl alcohol aqueous solution to the lead-free piezoelectric ceramic powder, mixing and granulating, and then loading into a mold and pressing at 10MPa to 20MPa to obtain a green disc;

[0033] S2, debinding the green disc obtained in S1 at a temperature of 700° C. to 900° C., and then sintering at a temperature of 1000° C. to 1100° C. for 3 h to 15 h to obtain a lead-free piezoelectric ceramic disc;

[0034] S3. Coat the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keep it at 700°C to 800°C for 10min to 20min, and cool it to room temperature; polarize it in silicone oil with a polarization field strength of 2kV / mm to 4kV / mm and a holding time of 15min to 40min to obtain the niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic.

[0035] The method for preparing lead-free piezoelectric ceramics from niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic materials of the present invention can prepare lead-free piezoelectric ceramics having high piezoelectric activity while maintaining a high mechanical quality factor; and while having high piezoelectric performance, it can also effectively increase the Curie temperature and can be used in a wider temperature range. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 is 1 # to 4 # X-ray diffraction patterns of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite lead-free piezoelectric ceramics with different Zr contents.

[0037] Figure 2 For 2 # and 5 # to 8 # X-ray diffraction patterns of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite lead-free piezoelectric ceramics with different Li contents.

[0038] Figure 3 is 1 # to 4 # d of lead-free piezoelectric ceramics containing potassium sodium, lithium bismuth, and copper niobium hafnium zirconate ferrite with different Zr contents 33 , Q m and k p value.

[0039] Figure 4 For 2 # and 5 # to 8 # d of KNO3HZrFeO3 / NaLiBiCu lead-free piezoelectric ceramics with different Li contents 33 , Q m and k p value.

[0040] Figure 5 This is a scanning electron microscope (SEM) photograph of 2# niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper lead-free piezoelectric ceramic after thermal corrosion.

[0041] Figure 6 For 5 # X-ray diffraction pattern of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0042] Figure 7 is 1 # to 4 # High temperature dielectric curves of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite lead-free piezoelectric ceramics with different Zr contents.

[0043] Figure 8 For 2 # , 5 # to 6 # High temperature dielectric curve of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper lead-free piezoelectric ceramics.

[0044] Fig. 9 is 1 # to 4 # Hysteresis loops of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite lead-free piezoelectric ceramics with different Zr contents.

[0045] Fig.10 For 2 # , 5 # to 6 # Hysteresis loop diagram of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics. DETAILED DESCRIPTION

[0046] The technical scheme of the present invention is further described in conjunction with the following examples. The experimental methods in the following examples are conventional methods unless otherwise specified. The raw materials, reagent materials, etc. used in the following examples can be purchased from conventional biochemical reagent stores or pharmaceutical companies unless otherwise specified.

[0047] Example 1

[0048] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0.1, y=0.00.

[0049] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0050] Step 1: Add 2.9089 g of analytically pure sodium carbonate (Na2CO3), 2.9939 g of potassium carbonate (K2CO3), 12.7311 g of niobium pentoxide (Nb2O5), 0.5232 g of bismuth trioxide (Bi2O3), 0.0559 g of zirconium oxide (ZrO2), 0.080 g of copper oxide (CuO), 0.0402 g of iron oxide (Fe2O3), 0.8509 g of hafnium oxide (HfO2), and 0.0000 g of lithium carbonate (Li2CO3) into a ball mill according to the stoichiometric ratio of the general chemical formula;

[0051] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the zirconium oxide balls are 100 g and the anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 250 rpm for 15 h;

[0052] Step 3: Discharge the material, dry it under a baking lamp, and then heat it in a furnace to 850° C. and keep it warm for 6 hours to obtain niobium, hafnium zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material.

[0053] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0054] S1, niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material is added with 5wt% polyvinyl alcohol aqueous solution to mix and granulate, then loaded into a mold and pressed into a tablet at 20MPa, wherein the diameter is 15mm and the thickness is 1.2mm to obtain a green disc;

[0055] S2, debinding the green disc obtained in S1 at a temperature of 850° C., and then sintering at a temperature of 1060° C. for 15 hours to obtain a lead-free piezoelectric ceramic disc;

[0056] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 750°C for 15 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 3 kV / mm and a holding time of 30 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and record it as 1 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0057] Example 2

[0058] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0.2, y=0.00.

[0059] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0060] Step 1: Add 2.9086 g of analytically pure sodium carbonate (Na2CO3), 2.9997 g of potassium carbonate (K2CO3), 12.7560 g of niobium pentoxide (Nb2O5), 0.5242 g of bismuth trioxide (Bi2O3), 0.1120 g of zirconium oxide (ZrO2), 0.080 g of copper oxide (CuO), 0.0403 g of iron oxide (Fe2O3), 0.7578 g of hafnium oxide (HfO2), and 0.0000 g of lithium carbonate (Li2CO3) into a ball mill according to the stoichiometric ratio of the general chemical formula;

[0061] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the zirconium oxide balls are 100 g and the anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 250 rpm for 15 h;

[0062] Step 3: Discharge the material, dry it under a baking lamp, and then heat it in a furnace to 850° C. and keep it warm for 6 hours to obtain niobium, hafnium zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material.

[0063] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0064] S1, niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material is added with 5wt% polyvinyl alcohol aqueous solution to mix and granulate, then loaded into a mold and pressed into a tablet at 20MPa, wherein the diameter is 15mm and the thickness is 1.2mm to obtain a green disc;

[0065] S2, debinding the green disc obtained in S1 at a temperature of 850° C., and then sintering at a temperature of 1060° C. for 15 hours to obtain a lead-free piezoelectric ceramic disc;

[0066] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 750°C for 15 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 3 kV / mm and a holding time of 30 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and record it as 2 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0067] Example 3

[0068] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0.3, y=0.00.

[0069] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0070] Step 1: Add 9143 g of analytically pure sodium carbonate (Na2CO3), 3.0056 g of potassium carbonate (K2CO3), 12.7810 g of niobium pentoxide (Nb2O5), 0.5232 g of bismuth trioxide (Bi2O3), 0.1684 g of zirconium oxide (ZrO2), 0.080 g of copper oxide (CuO), 0.0404 g of iron oxide (Fe2O3), 0.6644 g of hafnium oxide (HfO2), and 0.0000 g of lithium carbonate (Li2CO3) into a ball mill according to the stoichiometric ratio of the general chemical formula;

[0071] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the zirconium oxide balls are 100 g and the anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 250 rpm for 15 h;

[0072] Step 3: Discharge the material, dry it under a baking lamp, and then heat it in a furnace to 850° C. and keep it warm for 6 hours to obtain niobium, hafnium zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material.

[0073] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0074] S1, niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material is added with 5wt% polyvinyl alcohol aqueous solution to mix and granulate, then loaded into a mold and pressed into a tablet at 20MPa, wherein the diameter is 15mm and the thickness is 1.2mm to obtain a green disc;

[0075] S2, debinding the green disc obtained in S1 at a temperature of 850° C., and then sintering at a temperature of 1060° C. for 15 hours to obtain a lead-free piezoelectric ceramic disc;

[0076] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 750°C for 15 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 3 kV / mm and a holding time of 30 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and recorded as 3 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0077] Example 4

[0078] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0.4, y=0.00.

[0079] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0080] Step 1, according to the stoichiometric ratio of the chemical formula, add 2.9199 g of analytically pure sodium carbonate (Na2CO3), 3.0115 g of potassium carbonate (K2CO3), 12.8061 g of niobium pentoxide (Nb2O5), 0.5262 g of bismuth trioxide (Bi2O3), 0.2249 g of zirconium oxide (ZrO2), 0.080 g of copper oxide (CuO), 0.0404 g of iron oxide (Fe2O3), 0.5706 g of hafnium oxide (HfO2), and 0.0000 g of lithium carbonate (Li2CO3) into a ball mill;

[0081] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the zirconium oxide balls are 100 g and the anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 250 rpm for 15 h;

[0082] Step 3: Discharge the material, dry it under a baking lamp, and then heat it in a furnace to 850° C. and keep it warm for 6 hours to obtain niobium, hafnium zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material.

[0083] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0084] S1, niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material is added with 5wt% polyvinyl alcohol aqueous solution to mix and granulate, then loaded into a mold and pressed into a tablet at 20MPa, wherein the diameter is 15mm and the thickness is 1.2mm to obtain a green disc;

[0085] S2, debinding the green disc obtained in S1 at a temperature of 850° C., and then sintering at a temperature of 1060° C. for 15 hours to obtain a lead-free piezoelectric ceramic disc;

[0086] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 750°C for 15 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 3 kV / mm and a holding time of 30 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and recorded as 4 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0087] Example 5

[0088] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0.2, y=0.01.

[0089] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0090] Step 1: Add 2.8839 g of analytically pure sodium carbonate (Na2CO3), 2.9730 g of potassium carbonate (K2CO3), 12.7701 g of niobium pentoxide (Nb2O5), 0.5248 g of bismuth trioxide (Bi2O3), 0.1121 g of zirconium oxide (ZrO2), 0.080 g of copper oxide (CuO), 0.0404 g of iron oxide (Fe2O3), 0.7587 g of hafnium oxide (HfO2), and 0.0353 g of lithium carbonate (Li2CO3) into a ball mill according to the stoichiometric ratio of the general chemical formula;

[0091] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the zirconium oxide balls are 100 g and the anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 250 rpm for 15 h;

[0092] Step 3: Discharge the material, dry it under a baking lamp, and then heat it in a furnace to 850° C. and keep it warm for 6 hours to obtain niobium, hafnium zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material.

[0093] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0094] S1, niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material is added with 5wt% polyvinyl alcohol aqueous solution to mix and granulate, then loaded into a mold and pressed into a tablet at 20MPa, wherein the diameter is 15mm and the thickness is 1.2mm to obtain a green disc;

[0095] S2, debinding the green disc obtained in S1 at a temperature of 850° C., and then sintering at a temperature of 1060° C. for 15 hours to obtain a lead-free piezoelectric ceramic disc;

[0096] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 750°C for 15 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 3 kV / mm and a holding time of 30 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and recorded as 5 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0097] Example 6

[0098] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0.2, y=0.02.

[0099] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0100] Step 1: Add 2.8591 g of analytically pure sodium carbonate (Na2CO3), 2.9463 g of potassium carbonate (K2CO3), 12.7843 g of niobium pentoxide (Nb2O5), 0.5253 g of bismuth trioxide (Bi2O3), 0.1123 g of zirconium oxide (ZrO2), 0.080 g of copper oxide (CuO), 0.0404 g of iron oxide (Fe2O3), 0.7595 g of hafnium oxide (HfO2), and 0.0707 g of lithium carbonate (Li2CO3) into a ball mill according to the stoichiometric ratio of the general chemical formula;

[0101] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the zirconium oxide balls are 100 g and the anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 250 rpm for 15 h;

[0102] Step 3: Discharge the material, dry it under a baking lamp, and then heat it in a furnace to 850° C. and keep it warm for 6 hours to obtain niobium, hafnium zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material.

[0103] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0104] S1, niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material is added with 5wt% polyvinyl alcohol aqueous solution to mix and granulate, then loaded into a mold and pressed into a tablet at 20MPa, wherein the diameter is 15mm and the thickness is 1.2mm to obtain a green disc;

[0105] S2, debinding the green disc obtained in S1 at a temperature of 850° C., and then sintering at a temperature of 1060° C. for 15 hours to obtain a lead-free piezoelectric ceramic disc;

[0106] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 750°C for 15 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 3 kV / mm and a holding time of 30 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and recorded as 6 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0107] Example 7

[0108] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0.2, y=0.03.

[0109] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0110] Step 1: Add analytically pure sodium carbonate (Na2CO3) according to the stoichiometric ratio of the chemical formula.

[0111] 2.8343g, potassium carbonate (K2CO3) 2.9194g, niobium pentoxide (Nb2O5) 12.7985g, bismuth trioxide (Bi2O3) 0.5259g, zirconium oxide (ZrO2) 0.1124g, copper oxide (CuO) 0.080g, iron oxide (Fe2O3) 0.0404g, hafnium oxide (HfO2) 0.7604g, lithium carbonate (Li2CO3) 0.1062g into a ball mill;

[0112] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the zirconium oxide balls are 100 g and the anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 250 rpm for 15 h;

[0113] Step 3: Discharge the material, dry it under a baking lamp, and then heat it in a furnace to 850° C. and keep it warm for 6 hours to obtain niobium, hafnium zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material.

[0114] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0115] S1, niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material is added with 5wt% polyvinyl alcohol aqueous solution to mix and granulate, then loaded into a mold and pressed into a tablet at 20MPa, wherein the diameter is 15mm and the thickness is 1.2mm to obtain a green disc;

[0116] S2, debinding the green disc obtained in S1 at a temperature of 850° C., and then sintering at a temperature of 1060° C. for 15 hours to obtain a lead-free piezoelectric ceramic disc;

[0117] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 750°C for 15 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 3 kV / mm and a holding time of 30 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and recorded as 7 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0118] Example 8

[0119] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0.2, y=0.04.

[0120] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0121] Step 1, according to the stoichiometric ratio of the chemical formula, add 2.8095g of analytically pure sodium carbonate (Na2CO3), 2.8926g of potassium carbonate (K2CO3), 12.8128g of niobium pentoxide (Nb2O5), 0.5265g of bismuth trioxide (Bi2O3), 0.1125g of zirconium oxide (ZrO2), 0.080g of copper oxide (CuO), 0.0405g of iron oxide (Fe2O3), 0.7612g of hafnium oxide (HfO2), and 0.1418g of lithium carbonate (Li2CO3) into a ball mill;

[0122] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the zirconium oxide balls are 100 g and the anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 250 rpm for 15 h;

[0123] Step 3: Discharge the material, dry it under a baking lamp, and then heat it in a furnace to 850° C. and keep it warm for 6 hours to obtain niobium, hafnium zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material.

[0124] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0125] S1, niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material is added with 5wt% polyvinyl alcohol aqueous solution to mix and granulate, then loaded into a mold and pressed into a tablet at 20MPa, wherein the diameter is 15mm and the thickness is 1.2mm to obtain a green disc;

[0126] S2, debinding the green disc obtained in S1 at a temperature of 850° C., and then sintering at a temperature of 1060° C. for 15 hours to obtain a lead-free piezoelectric ceramic disc;

[0127] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 750°C for 15 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 3 kV / mm and a holding time of 30 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and recording it as 8 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0128] Example 9

[0129] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0.2, y=0.04.

[0130] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0131] Step 1, according to the stoichiometric ratio of the chemical formula, add 2.8095g of analytically pure sodium carbonate (Na2CO3), 2.8926g of potassium carbonate (K2CO3), 12.8128g of niobium pentoxide (Nb2O5), 0.5265g of bismuth trioxide (Bi2O3), 0.1125g of zirconium oxide (ZrO2), 0.080g of copper oxide (CuO), 0.0405g of iron oxide (Fe2O3), 0.7612g of hafnium oxide (HfO2), and 0.1418g of lithium carbonate (Li2CO3) into a ball mill;

[0132] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the amount of zirconium oxide balls is 100 g and the amount of anhydrous ethanol is 60 g, and ball mill is performed in a ball mill at a speed of 200 rpm for 10 hours;

[0133] Step 3: Discharge the material, dry it under a baking lamp, and then heat it in a furnace to 800° C. and keep it warm for 4 hours to obtain niobium, hafnium zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material.

[0134] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0135] S1, niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material is added with 10wt% polyvinyl alcohol aqueous solution to mix and granulate, then loaded into a mold and pressed into a tablet at 10MPa, wherein the diameter is 15mm and the thickness is 1.2mm to obtain a green disc;

[0136] S2, debinding the green disc obtained in S1 at a temperature of 700° C., and then sintering at a temperature of 1000° C. for 3 hours to obtain a lead-free piezoelectric ceramic disc;

[0137] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 700°C for 10 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 2 kV / mm and a holding time of 15 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and recording it as 10 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0138] Example 10

[0139] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0.2, y=0.04.

[0140] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0141] Step 1, according to the stoichiometric ratio of the chemical formula, add 2.8095g of analytically pure sodium carbonate (Na2CO3), 2.8926g of potassium carbonate (K2CO3), 12.8128g of niobium pentoxide (Nb2O5), 0.5265g of bismuth trioxide (Bi2O3), 0.1125g of zirconium oxide (ZrO2), 0.080g of copper oxide (CuO), 0.0405g of iron oxide (Fe2O3), 0.7612g of hafnium oxide (HfO2), and 0.1418g of lithium carbonate (Li2CO3) into a ball mill;

[0142] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the amount of zirconium oxide balls is 100 g and the amount of anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 300 rpm for 20 h;

[0143] Step 3: Discharge the material, dry it under a baking lamp, and then heat it in a furnace to 900° C. and keep it warm for 8 hours to obtain niobium, hafnium zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material.

[0144] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0145] S1, niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material is added with 5wt% polyvinyl alcohol aqueous solution to mix and granulate, then loaded into a mold and pressed into a tablet at 20MPa, wherein the diameter is 15mm and the thickness is 1.2mm to obtain a green disc;

[0146] S2, debinding the green disc obtained in S1 at a temperature of 900° C., and then sintering at a temperature of 1100° C. for 15 hours to obtain a lead-free piezoelectric ceramic disc;

[0147] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 800°C for 20 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 4 kV / mm and a holding time of 40 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and recording it as 10 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0148] Comparative Example 1

[0149] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0.5 and y=0.

[0150] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0151] Step 1: Add 2.9257 g of analytically pure sodium carbonate (Na2CO3), 3.0174 g of potassium carbonate (K2CO3), 12.8315 g of niobium pentoxide (Nb2O5), 0.5273 g of bismuth trioxide (Bi2O3), 0.2816 g of zirconium oxide (ZrO2), 0.0808 g of copper oxide (CuO), 0.0402 g of iron oxide (Fe2O3), 0.4764 g of hafnium oxide (HfO2), and 0.0000 g of lithium carbonate (Li2CO3) into a ball mill according to the stoichiometric ratio of the general chemical formula;

[0152] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the zirconium oxide balls are 100 g and the anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 250 rpm for 10 h;

[0153] Step 3: Discharge the material, dry it under a baking lamp, and then heat it in a furnace to 850° C. and keep it warm for 6 hours to obtain niobium, hafnium zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic powder.

[0154] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0155] S1. Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic powders are added to a 5wt% polyvinyl alcohol aqueous solution and mixed to form granules, which are then loaded into a mold and pressed into tablets at 20MPa, wherein the diameter is 15mm and the thickness is 1.2mm to obtain green discs;

[0156] S2, debinding the green disc obtained in S1 at a temperature of 850° C., and then sintering at a temperature of 1060° C. for 15 hours to obtain a lead-free piezoelectric ceramic disc;

[0157] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 750°C for 15 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 3 kV / mm and a holding time of 30 minutes to obtain the lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and recording it as comparison 1 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0158] Comparative Example 2

[0159] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0.6 and y=0.

[0160] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0161] Step 1: Add 2.9316 g of analytically pure sodium carbonate (Na2CO3), 3.0234 g of potassium carbonate (K2CO3), 12.8568 g of niobium pentoxide (Nb2O5), 0.5283 g of bismuth trioxide (Bi2O3), 0.3387 g of zirconium oxide (ZrO2), 0.0809 g of copper oxide (CuO), 0.0402 g of iron oxide (Fe2O3), 0.3819 g of hafnium oxide (HfO2), and 0.0000 g of lithium carbonate (Li2CO3) into a ball mill according to the stoichiometric ratio of the general chemical formula;

[0162] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the zirconium oxide balls are 100 g and the anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 250 rpm for 10 h;

[0163] Step 3: Discharge the material, dry it under a baking lamp, and then heat it in a furnace to 850° C. and keep it warm for 6 hours to obtain niobium, hafnium zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic powder.

[0164] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0165] S1. Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic powders are added to a 5wt% polyvinyl alcohol aqueous solution and mixed to form granules, which are then loaded into a mold and pressed into tablets at 20MPa, wherein the diameter is 15mm and the thickness is 1.2mm to obtain green discs;

[0166] S2, debinding the green disc obtained in S1 at a temperature of 850° C., and then sintering at a temperature of 1060° C. for 15 hours to obtain a lead-free piezoelectric ceramic disc;

[0167] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 750°C for 15 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 3 kV / mm and a holding time of 30 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and recording it as Comparative Example 2 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0168] Comparative Example 3

[0169] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0 and y is 0.05.

[0170] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0171] Step 1: Add 2.7736 g of analytically pure sodium carbonate (Na2CO3), 2.8544 g of potassium carbonate (K2CO3), 12.7770 g of niobium pentoxide (Nb2O5), 0.5250 g of bismuth trioxide (Bi2O3), 0.0000 g of zirconium oxide (ZrO2), 0.0804 g of copper oxide (CuO), 0.0399 g of iron oxide (Fe2O3), 0.9488 g of hafnium oxide (HfO2), and 0.1767 g of lithium carbonate (Li2CO3) into a ball mill according to the stoichiometric ratio of the general chemical formula;

[0172] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the amount of zirconium oxide balls is 100 g and the amount of anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 200 rpm for 20 hours;

[0173] Step 3: Dry under a baking lamp, then heat in a furnace to 850°C and keep warm for 6 hours to obtain niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper lead-free piezoelectric ceramic powder.

[0174] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0175] S1. Add 10 wt% polyvinyl alcohol aqueous solution to lead-free piezoelectric ceramic powder and mix to form granules, then put into a mold and press into tablets at 20 MPa, wherein the diameter is 15 mm and the thickness is 1.2 mm, to obtain green discs;

[0176] S2, debinding the green disc obtained in S1 at a temperature of 850° C., and then sintering at a temperature of 1100° C. for 3 hours to obtain a lead-free piezoelectric ceramic disc;

[0177] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 800°C for 10 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 3.5 kV / mm and a holding time of 40 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and recording it as comparative example 3 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0178] Comparative Example 4

[0179] A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, the general chemical formula of which is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955(Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where x=0 and y is 0.06.

[0180] The preparation method of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite comprises the following steps:

[0181] Step 1: Add analytically pure sodium carbonate (Na2CO3) according to the stoichiometric ratio of the chemical formula.

[0182] 2.7488g, potassium carbonate (K2CO3) 2.8275g, niobium pentoxide (Nb2O5) 12.7912g, bismuth trioxide (Bi2O3) 0.5256g, zirconium oxide (ZrO2) 0.0000g, copper oxide (CuO) 0.0805g, iron oxide (Fe2O3) 0.0400g, hafnium oxide (HfO2) 0.9499g, lithium carbonate (Li2CO3) 0.2122g are put into a ball mill;

[0183] Step 2: Use zirconium oxide balls as grinding media and anhydrous ethanol as solvent, wherein the amount of zirconium oxide balls is 100 g and the amount of anhydrous ethanol is 60 g, and the mixture is milled in a ball mill at a speed of 200 rpm for 20 hours;

[0184] Step 3: Dry under a baking lamp, then heat in a furnace to 900°C and keep warm for 8 hours to obtain niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper lead-free piezoelectric ceramic powder.

[0185] A lead-free piezoelectric ceramic of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, is prepared from the above-mentioned lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite, lithium bismuth copper, and comprises the following steps:

[0186] S1. Add 10 wt% polyvinyl alcohol aqueous solution to lead-free piezoelectric ceramic powder and mix to form granules, then put into a mold and press into tablets at 20 MPa, wherein the diameter is 15 mm and the thickness is 1.2 mm, to obtain green discs;

[0187] S2, debinding the green disc obtained in S1 at a temperature of 900° C., and then sintering at a temperature of 1100° C. for 3 hours to obtain a lead-free piezoelectric ceramic disc;

[0188] S3, coating the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keeping the temperature at 800°C for 10 minutes and cooling to room temperature; polarizing in silicone oil with a polarization field strength of 4 kV / mm and a holding time of 40 minutes to obtain a lead-free piezoelectric ceramic of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper, and recording it as Comparative Example 4 # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics.

[0189] Test Case

[0190] 1. Phase structure analysis

[0191] The X-ray diffractometer (XRD, DX-2700) was used to analyze the # to 8 # Phase structure analysis of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramic discs, such as Figure 1 and Figure 2 shown.

[0192] The results show that the potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite lead-free piezoelectric ceramic of the present invention has a single perovskite structure and presents ROT multiphase coexistence at room temperature, thereby ensuring a relatively high piezoelectric activity.

[0193] 2. Piezoelectric constant d 33 , Planar electromechanical coupling coefficient k p and mechanical quality factor Q m Detection

[0194] Utilize d 33 The piezoelectric constants d of the lead-free piezoelectric ceramic discs of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper were tested by a piezoelectric tester (ZJ-3A) and an impedance analyzer (HP 4294A). 33 , Planar electromechanical coupling coefficient k p and mechanical quality factor Q m ,like Figure 3 and Figure 4 shown.

[0195] The results show that the lead-free piezoelectric ceramics of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite of the present invention have a higher piezoelectric constant d 33 And the planar electromechanical coupling coefficient k p , and has a high mechanical quality factor Q m , where the piezoelectric constant d 33 180pC / N~318pC / N, mechanical quality factor Q m The plane electromechanical coupling coefficient k is 180~286. p It is 0.35~0.52.

[0196] 3. Surface morphology analysis

[0197] Using electron microscope (SEM, JSM-5900), thermal corrosion method was used to observe 2 # and 5 # Surface morphology of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramic discs, such as Figure 5 and Figure 6 shown.

[0198] The results show that the grain size of the lead-free piezoelectric ceramic of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite of the present invention is increased and uniform, and the grains are relatively dense, indicating that the density of the lead-free piezoelectric ceramic is further improved, thereby improving the piezoelectric performance.

[0199] 4. High temperature and dielectric temperature curve separation

[0200] The LCR analyzer (HP 4980, TH2816A) was used to test 1 # , 2 # , 3 # , 4 # , 5 # and 6 # High temperature dielectric curve of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramic discs, see Figure 7 and Figure 8 shown.

[0201] The results show that the lead-free piezoelectric ceramics of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite of the present invention have a high Curie temperature (T C ), the operating temperature range is wide, among which the Curie temperature T C It is 314℃~361℃.

[0202] 5. Hysteresis loop analysis

[0203] Tested using Radiant Precision Workstation 1 # , 2 # , 3 # , 4 # , 5 # and 6 # Hysteresis loop of niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramic disc, such as Fig. 9 and Fig.10 shown.

[0204] The results show that the lead-free piezoelectric ceramics of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite of the present invention have excellent hysteresis loops and good residual polarization strength, wherein the residual polarization strength P r 13μC / cm 2 ~20μC / cm 2 , coercive field E c It is 12kV / cm~22kV / cm.

[0205] Among them, Table 1 is 1 # to 8 # Statistical results of performance tests on niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramics.

[0206] Table 1. Performance test results of lead-free piezoelectric ceramics of potassium sodium lithium bismuth copper niobium hafnium zirconate ferrite

[0207]

[0208]

[0209] It can be seen from Table 1 that when the Zr content is used as a variable, the 1 # ~4 # The piezoelectric constant of the niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper ceramic material first decreases slightly and then decreases significantly with the increase of x; the planar electromechanical coupling coefficient and the mechanical quality factor first increase and then decrease; the dielectric loss remains at a low value (≤1.8%); and the Curie temperature increases slightly with the increase of x.

[0210] When the Zr content increases to 0.5 and 0.6, the piezoelectric constant of the potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite ceramic materials obtained in Comparative Examples 1 and 2 further decreases, the electromechanical coupling coefficient drops to about 100, the planar electromechanical coupling coefficient is about 0.36, the dielectric loss and Curie temperature do not change much, and the comprehensive performance is relatively low. # The best overall performance is obtained from ceramic materials.

[0211] When Li content is used as a variable, 2 # and 5 # ~8 # The piezoelectric constant and planar electromechanical coupling coefficient of the niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper ceramic material first decrease slightly and then decrease significantly with the increase of x, while the mechanical quality factor first decreases slightly and then increases significantly, and the Curie temperature is significantly improved.

[0212] 5 obtained in Example 5 of the present invention # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics have the best comprehensive performance, with a high Curie temperature, while maintaining excellent piezoelectric activity and mechanical quality factor, as well as high planar electromechanical coupling coefficient and low loss. # Niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, copper, lead-free piezoelectric ceramics have a piezoelectric constant d 33 310pC / N; mechanical quality factor Q m is 228; the plane electromechanical coupling coefficient k p is 0.51; dielectric loss tanδ is 1.4%; Curie temperature T C is 322℃; the residual polarization intensity P r 19μC / cm 2 ; Coercive field E c It is 13kV / cm.

[0213] When the Li content increases to 0.05 and 0.06, the piezoelectric constant further decreases to more than 100, the electromechanical coupling coefficient continues to increase, the planar electromechanical coupling coefficient decreases to 0.24, and the dielectric loss and Curie temperature increase slightly. Although the electromechanical coupling coefficient and Curie temperature are high, the piezoelectric constant and electromechanical coupling coefficient are very low, and its comprehensive performance is low.

[0214] In summary, the niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic of the present invention has high piezoelectric activity while maintaining a high mechanical quality factor; and while having high piezoelectric performance, it can also effectively increase the Curie temperature and can be used in a wider temperature range.

[0215] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, characterized in that: The chemical formula of the lead-free piezoelectric ceramic material is [(K 0.45 Na 0.55 ) 0.955(1-y) Li 0.955y (Bi 0.5 Na 0.5 ) 0.045 Cu 0.01 ][Nb 0.955 (Hf 1-x Zr x ) 0.045 Fe 0.005 ]O3, where 0<x≤0.4, 0≤y≤0.

04.

2. The potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite lead-free piezoelectric ceramic material according to claim 2, characterized in that: x is 0.2 and y is 0.

01.

3. The lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite according to claim 1, characterized in that: The raw materials for preparing the niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material include Na2CO3, K2CO3, Nb2O5, Bi2O3, ZrO2, CuO, Fe2O3, and HfO2.

4. The lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite according to claim 1, characterized in that: The raw materials for preparing the niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic material include Na2CO3, K2CO3, Nb2O5, Bi2O3, ZrO2, CuO, Fe2O3, HfO2, and Li2CO3.

5. The potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite lead-free piezoelectric ceramic material according to any one of claims 1 to 4, characterized in that: The piezoelectric constant d of the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite 33 180pC / N~318pC / N; Mechanical quality factor Q m 180~286; Planar electromechanical coupling coefficient k p 0.35~0.52; Dielectric loss tanδ is 1.4% to 2.0%; Curie temperature T C 314℃~361℃; Remanent polarization intensity P r 13μC / cm 2 ~20μC / cm 2 , coercive field E c It is 12kV / cm~22kV / cm.

6. A method for preparing the potassium sodium lithium bismuth copper niobate hafnium zirconium ferrite lead-free piezoelectric ceramic material according to any one of claims 1 to 2, characterized in that: The following steps are involved: The lead-free piezoelectric ceramic material of potassium sodium niobium hafnium zirconium ferrite is prepared by a solid phase method using the stoichiometric ratio of Na2CO3, K2CO3, Nb2O5, Bi2O3, ZrO2, CuO, Fe2O3, HfO2 and Li2CO3 according to the general chemical formula.

7. The method for preparing the lead-free piezoelectric ceramic material of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite according to claim 6, characterized in that: The following steps are involved: Step 1, adding Na2CO3, K2CO3, Nb2O5, Bi2O3, ZrO2, CuO, Fe2O3, HfO2 and Li2CO3 into a ball mill according to the stoichiometric ratio of the chemical formula; Step 2: Using zirconium oxide balls as grinding media and anhydrous ethanol as solvent, milling in a ball mill at a speed of 200 rpm to 300 rpm for 10 h to 20 h; Step 3: Discharge the material, dry it, put it into a furnace and heat it to 800°C to 900°C, and keep it warm for 4h to 8h to obtain niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth and copper lead-free piezoelectric ceramic material.

8. A lead-free piezoelectric ceramic of potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite, characterized in that: The piezoelectric ceramic is prepared from the potassium sodium niobium hafnium zirconium ferrite lead-free piezoelectric ceramic material as described in any one of claims 1 to 4 as raw material.

9. A method for preparing lead-free piezoelectric ceramics from potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite lead-free piezoelectric ceramic materials, comprising the following steps: S1. Adding the potassium sodium lithium bismuth copper niobium hafnium zirconium ferrite lead-free piezoelectric ceramic material according to any one of claims 1 to 4 to a polyvinyl alcohol solution, mixing, granulating and tableting to obtain a green disc; S2, debinding and sintering the green disc obtained in S1 to obtain a lead-free piezoelectric ceramic disc; S3, silver polarizing the lead-free piezoelectric ceramic disc obtained in S2 to obtain niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramics.

10. The method for preparing lead-free piezoelectric ceramics according to claim 9, characterized in that: The following steps are involved: S1, adding 5wt% to 10wt% polyvinyl alcohol aqueous solution to the lead-free piezoelectric ceramic powder, mixing and granulating, and then loading into a mold and pressing at 10MPa to 20MPa to obtain a green disc; S2, debinding the green disc obtained in S1 at a temperature of 700° C. to 900° C., and then sintering at a temperature of 1000° C. to 1100° C. for 3 h to 15 h to obtain a lead-free piezoelectric ceramic disc; S3. Coat the surface of the lead-free piezoelectric ceramic disc obtained in S2 with silver paste, keep it at 700°C to 800°C for 10min to 20min, and cool it to room temperature; polarize it in silicone oil with a polarization field strength of 2kV / mm to 4kV / mm and a holding time of 15min to 40min to obtain the niobium, hafnium, zirconium, potassium, sodium, lithium, bismuth, and copper lead-free piezoelectric ceramic.

Citation Information

Cited By

  • Lead-free piezoelectric ceramic material as well as preparation method and application thereof