Non-oriented silicon steel plate and processing method thereof

By introducing asynchronous rolling and process control in the hot rolling and finishing process of non-oriented silicon steel, the problems of cold rolling easy to break and poor magnetic properties are solved, and the processing of silicon steel plates with low iron loss and high magnetic induction strength is realized.

CN118996087AActive Publication Date: 2024-11-22ZHANGJIAGANG YANGTZE RIVER COLD ROLLED PLATE CO LTD +2

Patent Information

Application Number
CN202411118990.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Non-oriented silicon steel with high silicon aluminum alloy content is prone to breaking the tape during cold rolling process and has poor magnetic performance. It is difficult for the prior art to simultaneously reduce iron losses and improve magnetic induction strength.

Method used

The asynchronous rolling technology is used to introduce the circumferential velocity difference between the upper and lower working rollers during hot rolling and finishing process. Combined with the normalization and annealing process, the grain size and distribution of the steel plate surface layer and intermediate layer are controlled, and crack expansion during cold rolling is hindered. ,并提高磁性能。

Benefits of technology

It effectively reduces the risk of cold-rolled edge cracks and strip breaks, improves the processability and magnetic properties of non-oriented silicon steel, and obtains silicon steel plates with low iron loss and high magnetic induction strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004994773740000121
    Figure BDA0004994773740000121
Patent Text Reader

Abstract

The invention provides a non-oriented silicon steel plate and a processing method thereof, and the processing method comprises the following steps: heating a continuous casting billet to 1080-1180 DEG C, carrying out heat preservation for 200-300 min, carrying out rough rolling and seven passes of finish rolling to obtain a hot rolled plate, and introducing asymmetrical rolling into the sixth and seventh passes of finish rolling; fine grains are obtained on the surface layer of the hot-rolled plate through normalizing, the normalizing temperature is T1 = 15 * [6.7-([Si] + 0.72 * [Al]) * 100] 2 + 760 * [1-v7up / v7down <-1 >] DEG C, the heating rate is 50-80 DEG C / s, and the heat preservation time is 20-50 s; the non-oriented silicon steel plate is obtained through cold rolling and annealing, the annealing temperature T2 is equal to T1 + 120 DEG C, and the heat preservation time is 200-400 s; through control of hot rolling and normalizing processes, a normalized plate with fine grains on the surface layer and large grains in the middle is obtained, expansion of cracks in the cold rolling process is hindered, smooth rolling is completed, and non-oriented silicon steel with good magnetic performance is obtained through long-time heat preservation annealing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of steel processing, and in particular to a non-oriented silicon steel plate and a processing method thereof. Background Art

[0002] Non-oriented silicon steel is an important metallic soft magnetic material, which is widely used in the preparation of iron core materials such as motors, compressors, and power transformers. With the rapid development of high efficiency, miniaturization, and lightweight of electromechanical products, the requirements for motor performance are getting higher and higher, and an important measure to improve motor performance is to select iron core materials with better magnetic properties. Therefore, non-oriented silicon steel is required to have the characteristics of low iron loss and high magnetic induction. In order to reduce the iron loss of non-oriented silicon steel, a higher content of silicon and a certain content of aluminum are usually added to increase the resistivity of non-oriented silicon steel, especially high-grade non-oriented silicon steel. However, with the increase of silicon and aluminum alloy element content, lattice distortion increases, the brittleness of non-oriented silicon steel increases, and the toughness decreases. Cold rolling is easy to break the strip, and it is difficult to pass the plate.

[0003] In order to solve this problem, the existing technology increases the temperature of the steel plate by preheating before rolling to make the steel plate in toughness rolling, but it will increase the production cost; by lowering the normalizing temperature, fine recrystallized grains or partially unrecrystallized mixed structures are obtained to avoid cold rolling brittle fracture caused by excessive grain size, but it will affect the growth of the finished product grains and make the magnetic properties of the finished product worse. Summary of the invention

[0004] The purpose of the present application is to provide a non-oriented silicon steel sheet and a processing method thereof. The processing method of the non-oriented silicon steel sheet introduces asynchronous rolling into hot rolling and combines the process control of normalization, so that the surface layer of the normalized steel sheet obtains fine grains, hinders the crack propagation during cold rolling, solves the problem of cold-rolled breakage of non-oriented silicon steel with high silicon-aluminum alloy content in the prior art, and obtains better magnetic properties.

[0005] In order to achieve the above application purpose, an embodiment of the present application provides a method for processing a non-oriented silicon steel sheet, comprising sequentially performing heating, hot rolling, normalizing, cold rolling, annealing and coating steps on a continuous casting billet, wherein:

[0006] In the heating process, the continuous casting billet is heated to a temperature of 1080-1180°C and the holding time is 200-300 minutes;

[0007] In the hot rolling process, the heated continuous casting billet is sent to the rolling mill for rough rolling and 7 passes of finishing rolling to obtain hot rolled plates, wherein the 6th and 7th passes of finishing rolling are asynchronous rolling;

[0008] In the normalizing process, the hot rolled sheet is sent to the normalizing furnace for normalizing treatment, and the normalizing temperature is T1 = 15 × [6.7-([Si] + 0.72 × [Al]) × 100]2 +760×[1-|v7 up / v7 down -1|]℃, heating rate is 50~80℃ / s, holding time is 20~50s, where [Si], [Al] are the mass percentages of Si and Al in the continuous casting billet, v7 up v7 is the circumferential speed of the working roll in the seventh pass of finishing rolling. down is the circumferential speed of the lower working roll in the 7th pass of finishing rolling;

[0009] In the cold rolling process, the normalized hot-rolled sheet is cold-rolled to obtain a cold-rolled sheet;

[0010] In the annealing process, the cold-rolled sheet is continuously annealed, the annealing temperature is T2=T1+120°C, and the holding time is 200-400s.

[0011] As a further improvement of one embodiment of the present application, in the hot rolling process, the circumferential speed ratio of the upper and lower working rolls in the 6th pass is 1:1.01 to 1:1.04, and the circumferential speed ratio of the upper and lower working rolls in the 7th pass is opposite to that of the 6th pass.

[0012] As a further improvement of one embodiment of the present application, in the hot rolling process, the final rolling temperature is 720-800°C, the coiling temperature is 600-660°C, the coiling holding time is 60-90 minutes, and after holding, the coil is unrolled and air-cooled to room temperature.

[0013] As a further improvement of one embodiment of the present application, the recrystallized grain size of the hot-rolled plate surface is 2-18 μm, wherein the surface layer includes an upper surface layer and a lower surface layer of the same thickness, and the sum of the thicknesses of the upper surface layer and the lower surface layer accounts for 20-35% of the thickness of the hot-rolled plate.

[0014] As a further improvement of one embodiment of the present application, the average recrystallized grain size of the surface layer of the hot-rolled plate after normalization is 20 to 45 μm, and the average recrystallized grain size of the middle layer is 80 to 110 μm.

[0015] As a further improvement of an embodiment of the present application, the recrystallized grain size of the cold-rolled sheet after annealing is 120 to 150 μm on average.

[0016] As a further improvement of one embodiment of the present application, the thickness of the hot-rolled plate obtained after hot rolling is 2.10 to 2.30 mm, and the thickness of the cold-rolled plate obtained after cold rolling is 0.25 to 0.35 mm.

[0017] As a further improvement of an embodiment of the present application, in the normalizing process, the atmosphere in the normalizing furnace is pure N2, and the temperature fluctuation range of the normalizing temperature is 5°C above and below the temperature T1;

[0018] In the annealing process, the protective atmosphere is a mixed atmosphere of H2 and N2, wherein the volume percentage of H2 is 30-70%.

[0019] One embodiment of the present application also provides a non-oriented silicon steel sheet, which is prepared by the aforementioned processing method. The chemical composition of the non-oriented silicon steel sheet includes, by mass percentage: C≤0.0025%, S≤0.0015%, N≤0.002%, Si: 3.25-3.65%, Al: 0.85-1.25%, Mn: 0.27-0.47%, Sn: 0.05-0.08%, P≤0.02%, Nb+V≤0.006%, Ti≤0.002%, Cu≤0.03%, Mo≤0.006%, Ni+Cr≤0.06%, and the rest is Fe and unavoidable impurities.

[0020] As a further improvement of an embodiment of the present application, when the thickness of the non-oriented silicon steel sheet is 0.25 mm, the iron loss P 1.0 / 400 ≤12W / kg, magnetic induction intensity B 5000 ≥1.64T; when the thickness of the non-oriented silicon steel sheet is 0.30mm, the iron loss P 1.0 / 400 ≤14W / kg, magnetic induction intensity B 5000 ≥1.65T; when the thickness of the non-oriented silicon steel sheet is 0.35mm, the iron loss P 1.0 / 400 ≤17W / kg, magnetic induction intensity B 5000 ≥1.68T.

[0021] As a further improvement of one embodiment of the present application, when the thickness of the non-oriented silicon steel plate is 0.25 mm, the thickness of the hot-rolled plate is 2.10 mm; when the thickness of the non-oriented silicon steel is 0.30 mm, the thickness of the hot-rolled plate is 2.20 mm; when the thickness of the non-oriented silicon steel is 0.35 mm, the thickness of the hot-rolled plate is 2.30 mm.

[0022] One or more technical solutions provided by this application have at least the following technical effects or advantages:

[0023] The processing method of the non-oriented silicon steel plate provided by the present application introduces asynchronous rolling in the 6th to 7th passes of hot rolling finishing rolling, increases the shear deformation of the surface layer of the hot-rolled plate by the circumferential speed difference between the upper and lower working rolls, and combines the process control of the hot rolling process and the normalizing process, so that the surface layer of the hot-rolled plate obtains fine recrystallized grains, and finally the size and distribution of the recrystallized grains of the normalized plate are accurately controlled, and the surface layer of the normalized plate obtains fine grains, which can hinder the crack propagation in the cold rolling process, so that the normalized plate has better machinability, reduces the risk of cold rolling edge cracks and belt breaks, and improves rolling efficiency;

[0024] Based on the improvement of the machinability of normalized plates, the content of silicon and aluminum elements in non-oriented silicon steel can be increased, and the resistivity can be further improved, thereby obtaining non-oriented silicon steel with lower iron loss;

[0025] The introduction of asynchronous rolling mill can obtain more shear deformation structures, provide nucleation sites for Goss and Cube grains, and obtain more space for grain growth, thereby enhancing Goss and Cube textures and improving the magnetic properties of the finished product. DETAILED DESCRIPTION

[0026] The present invention will be described in detail below in conjunction with specific embodiments, but these embodiments do not limit the present invention, and changes in reaction conditions, reactants or raw material amounts made by ordinary technicians in the field according to these embodiments are all included in the protection scope of the present invention.

[0027] The embodiment of the present application provides a method for processing a non-oriented silicon steel sheet, comprising sequentially performing heating, hot rolling, normalizing, cold rolling, annealing and coating steps on a continuous casting billet, wherein:

[0028] In the heating process, the continuous casting billet is heated to a temperature of 1080-1180°C and the holding time is 200-300 minutes;

[0029] In the hot rolling process, the heated continuous casting billet is sent to the rolling mill for rough rolling and 7 passes of finishing rolling to obtain hot rolled plates, wherein the 6th and 7th passes of finishing rolling are asynchronous rolling;

[0030] In the normalizing process, the hot rolled sheet is sent to the normalizing furnace for normalizing treatment, and the normalizing temperature is T1 = 15 × [6.7-([Si] + 0.72 × [Al]) × 100] 2 +760×[1-|v7 up / v7 down -1|]℃, heating rate is 50~80℃ / s, holding time is 20~50s, where [Si], [Al] are the mass percentages of Si and Al in the continuous casting billet, v7 up v7 is the circumferential speed of the working roll in the seventh pass of finishing rolling. down is the circumferential speed of the lower working roll in the 7th pass of finishing rolling;

[0031] In the cold rolling process, the normalized hot-rolled sheet is cold-rolled to obtain a cold-rolled sheet;

[0032] In the annealing process, the cold-rolled sheet is continuously annealed, the annealing temperature is T2=T1+120°C, and the holding time is 200-400s.

[0033] The processing method of non-oriented silicon steel plate provided in the present application not only avoids the deterioration of the magnetic properties of the steel plate by the solid solution of inclusions such as MnS, AlN and carbon and nitrogen compounds in the steel when heating the continuous casting billet, but also does not affect the rolling force during hot rolling and the plate shape control of the hot-rolled plate. During the finishing rolling, the 6th and 7th rolling passes, which are the two last rolling passes, adopt asynchronous rolling, which increases the shear deformation of the surface layer of the hot-rolled plate, so that the surface layer of the hot-rolled plate is nucleated and grown under the drive of thermal energy and deformation energy, and finally forms a layer of fine grains on the surface; cooperate with the faster heating rate in the normalizing process to avoid the recovery process time being too long, ensure enough grain nucleation points, and adopt short-time insulation to avoid the growth of small surface grains and the annexation of grains in the middle layer, obtain the required normalized structure, reduce the crack propagation during the cold rolling process, and avoid cold rolling breakage. The annealing process causes the fiber structure of the cold-rolled plate to recrystallize, promote the nucleation and growth of grains, and improve the texture of the steel plate. By keeping the temperature for a long time, the grains can be fully grown and homogenized, and low-temperature continuous annealing can be achieved to obtain a higher magnetic induction while ensuring excellent iron loss.

[0034] In some embodiments, in the hot rolling process, the circumferential speed ratio of the upper and lower working rolls in the 6th pass is 1:1.01 to 1:1.04, and the circumferential speed ratio of the upper and lower working rolls in the 7th pass is opposite to that in the 6th pass. The circumferential speed ratio of the upper and lower working rolls is controlled to be smaller to avoid severe deformation of the hot-rolled plate, and the circumferential speed ratio of the upper and lower working rolls in the 7th pass is controlled to be opposite to that in the 6th pass to offset the warping of the hot-rolled plate caused by asynchronous rolling and better control the plate shape.

[0035] In some embodiments, in the hot rolling process, the final rolling temperature is 720-800°C, the coiling temperature is 600-660°C, the coiling holding time is 60-90 minutes, and the coiling is unrolled and air-cooled to room temperature after holding. By controlling the final rolling temperature, coiling temperature and coiling time of hot rolling, the growth of fine grains on the surface of the hot-rolled plate can be avoided.

[0036] In some embodiments, the recrystallized grain size of the surface layer of the hot-rolled plate is 2 to 18 μm, wherein the surface layer includes an upper surface layer and a lower surface layer of the same thickness, and the sum of the thickness of the upper surface layer and the lower surface layer accounts for 20-35% of the thickness of the hot-rolled plate. The upper surface layer is a certain depth from the upper surface of the hot-rolled plate to the inside of the hot-rolled plate in the thickness direction of the hot-rolled plate; the lower surface is a certain depth from the lower surface of the hot-rolled plate to the inside of the hot-rolled plate in the thickness direction of the hot-rolled plate. The upper surface layer and the lower surface layer have the same thickness and have fine grains with a grain size of 2 to 18 μm. Among them, the method for obtaining the grain size refers to GB / T 6394-2017 "Method for Determination of Average Grain Size of Metals".

[0037] In some embodiments, the average recrystallized grain size of the surface layer of the hot-rolled plate after normalization is 20-45 μm, and the average recrystallized grain size of the middle layer is 80-110 μm. After normalization, the grains are recrystallized, and the surface grain size increases from 2-18 μm to 20-45 μm, and the grain size of the middle layer is larger than that of the surface layer.

[0038] Furthermore, the average recrystallized grain size of the cold-rolled sheet after annealing is 120-150 μm. Due to the long annealing holding time and the annealing temperature T2, the cold-rolled sheet has sufficient time to allow the grains to grow and become uniform, eliminating the difference in grain size between the surface and middle layers of the steel plate caused by asynchronous rolling during finishing rolling, and obtaining a higher magnetic induction while ensuring excellent iron loss.

[0039] In some embodiments, the thickness of the hot-rolled plate obtained after hot rolling is 2.10 to 2.30 mm, and the thickness of the cold-rolled plate obtained after cold rolling is 0.25 to 0.35 mm. In addition, the thickness of the continuous casting billet is 210 to 240 mm; in the cold rolling process, the first pass reduction rate is 38 to 42%. The target thickness of the hot-rolled plate is set according to the thickness of the silicon steel plate finally formed, and the rolling load pressure of the cold rolling process is reduced, which is convenient for controlling the shape of the cold-rolled plate. At the same time, in the cold rolling process, an ultra-large reduction rate is used in the first pass, so that a large deformation is obtained in the thickness direction, the flexibility of the steel plate is improved, and the occurrence of edge cracks in the subsequent cold rolling passes and the probability of strip breakage are reduced.

[0040] In some embodiments, during the normalizing process, the atmosphere in the normalizing furnace is pure N2, and the temperature fluctuation range of the normalizing temperature is 5°C above and below the temperature T1; during the annealing process, the protective atmosphere is a mixed atmosphere of H2 and N2, in which the volume percentage of H2 is 30-70%.

[0041] The embodiment of the present application also provides a non-oriented silicon steel sheet prepared by the aforementioned processing method, whose chemical composition, in mass percentage, includes: C≤0.0025%, S≤0.0015%, N≤0.002%, Si: 3.25~3.65%, Al: 0.85~1.25%, Mn: 0.27~0.47%, Sn: 0.05~0.08%, P≤0.02%, Nb+V≤0.006%, Ti≤0.002%, Cu≤0.03%, Mo≤0.006%, Ni+Cr≤0.06%, and the rest are Fe and unavoidable impurities.

[0042] On the basis of the above processing methods, the Si and Al contents are controlled to be relatively high to improve the resistivity of the steel sheet and reduce the iron loss. A certain amount of Mn is added to improve the punching and cutting properties of silicon steel, and the resistivity can be further improved. A certain amount of Sn is added to prevent nitrogen addition and the formation of an inner oxide layer during annealing, improve the magnetic properties of the silicon steel sheet, and P enhances the solid solution strengthening effect and improves the strength of the steel sheet. The deterioration of magnetic properties is avoided by controlling the contents of impurity elements such as C, S, N, Nb, V, Ti, Cu, Mo, Ni, and Cr.

[0043] The effects of each chemical component have the following characteristics:

[0044] C, S, N: For non-oriented silicon steel, C, S, and N are all harmful elements. An increase in C content will lead to increased iron loss, reduced magnetic induction intensity, and will also cause magnetic aging. S and Mn easily form MnS. The fine MnS plays a pinning role, hindering the grain growth during annealing, resulting in increased iron loss. In addition, S will increase the brittleness of non-oriented silicon steel. N easily forms AlN and TiN inclusions with Al and Ti, which is not conducive to grain growth during annealing and the magnetic properties of the steel plate. Therefore, in this application, the C content is controlled below 0.0025%, the S content is controlled below 0.0015%, and the N content is controlled below 0.002%.

[0045] Si, Al: Si and Al are the main functional elements to increase resistivity and reduce iron loss. Therefore, the Si content in the present application is controlled at 3.25-3.65%, and the Al content is controlled at 0.85-1.25%.

[0046] Mn: If the Si and Al contents are too high, the punching property of silicon steel sheet will be deteriorated. Adding an appropriate amount of Mn can improve the punching property and cutting property. Mn can increase the resistivity and inhibit the hot brittleness caused by S. However, if too much Mn is added, the strength and hardness of the steel sheet will increase, making it inconvenient to roll and coil. Therefore, the Mn content in this application is controlled at 0.27-0.47%.

[0047] Sn: Sn is an element that easily segregates at grain boundaries. During annealing, it can prevent {111} grains from nucleating at the original grain boundaries, creating space for {100} and {110} grains to nucleate and grow, thereby improving the magnetic induction intensity. In addition, Sn can prevent nitrogen addition and the formation of an inner oxide layer during annealing, which can improve the magnetic properties. However, too high a Sn content will lead to grain boundary embrittlement of the steel plate, which is not conducive to cold rolling and will also increase production costs. Therefore, the Sn content in this application is controlled at 0.05-0.08%.

[0048] P: P has a solid solution strengthening effect in non-oriented silicon steel and can improve the strength of the steel plate, but P will segregate along the grain boundaries. An increase in its content will deteriorate the cold ductility and increase the risk of strip breakage during rolling. Therefore, the P content in this application is controlled below 0.02%.

[0049] Nb, V, Ti, Cu, Mo, Ni, Cr: For non-oriented silicon steel, Nb, V, Ti, Cu, Mo, Ni, Cr are all impurity elements. Although they can improve the strength, they will deteriorate the magnetic properties. Nb, V, Ti, C, and N can form carbon and nitrogen compounds, which will be dissolved in the hot rolling heating process. They will be dispersed and precipitated in the subsequent rolling and coiling process, hindering the growth of grains and causing the magnetic properties to deteriorate; the increase in Cu content is prone to cause hot brittleness. Therefore, the content of these elements should be reduced as much as possible, and controlled within Nb+V≤0.006%, Ti≤0.002%, Cu≤0.03%, Mo≤0.006%, and Ni+Cr≤0.06%.

[0050] Furthermore, when the thickness of the non-oriented silicon steel sheet is 0.25 mm, the iron loss P 1.0 / 400 ≤12W / kg, magnetic induction intensity B 5000 ≥1.64T; when the thickness of non-oriented silicon steel sheet is 0.30mm, the iron loss P 1.0 / 400 ≤14W / kg, magnetic induction intensity B 5000 ≥1.65T; when the thickness of non-oriented silicon steel sheet is 0.35mm, the iron loss P 1.0 / 400 ≤17W / kg, magnetic induction intensity B 5000 ≥1.68T.

[0051] Furthermore, when the thickness of the non-oriented silicon steel sheet is 0.25 mm, the thickness of the hot-rolled sheet is 2.10 mm; when the thickness of the non-oriented silicon steel is 0.30 mm, the thickness of the hot-rolled sheet is 2.20 mm; when the thickness of the non-oriented silicon steel is 0.35 mm, the thickness of the hot-rolled sheet is 2.30 mm.

[0052] The technical solution of the present application is further described below in conjunction with some specific embodiments.

[0053] Example 1

[0054] The chemical composition of a non-oriented silicon steel sheet provided in Example 1 includes, by mass percentage, C: 0.0015%, S: 0.0013%, N: 0.0018%, Si: 3.34%, Al: 1.21%, Mn: 0.31%, Sn: 0.06%, P: 0.018%, Nb: 0.0032%, V: 0.0024%, Ti: 0.0017%, Cu: 0.027%, Mo: 0.005%, Ni: 0.027%, Cr: 0.025%, and the rest is Fe and unavoidable impurities.

[0055] The processing method of the non-oriented silicon steel sheet comprises the following steps:

[0056] Heating process: the continuous casting billet is placed in a heating furnace for heating at a temperature of 1089°C and a holding time of 288 minutes;

[0057] Hot rolling process: the heated continuous casting billet is sent to the rolling mill for rough rolling and 7 passes of finishing rolling to obtain a hot rolled plate with a thickness of 2.3 mm, wherein the circumferential speed ratio of the upper and lower working rolls in the 6th pass of finishing rolling is 1:1.01, and the circumferential speed ratio of the upper and lower working rolls in the 7th pass of finishing rolling is 1.01:1. The final rolling temperature is controlled to be 744°C, the coiling temperature is 610°C, the coiling holding time is 65 minutes, and the coil is unrolled after holding for air cooling to room temperature.

[0058] Normalizing process: send the hot rolled plate into the normalizing furnace for normalizing treatment. The atmosphere in the normalizing furnace is pure N2, the normalizing temperature is 845℃, the heating rate is 52℃ / s, and the holding time is 23s.

[0059] Cold rolling process: the normalized hot-rolled sheet is cold rolled, and the first pass reduction rate of cold rolling is controlled to be 38.2%;

[0060] Annealing process: anneal the cold-rolled sheet in a protective atmosphere of a mixed atmosphere of H2 and N2, wherein the volume percentage of H2 is 30-70%, the annealing temperature is 965°C, and the holding time is 217s;

[0061] Coating process: An insulating layer is coated on the surface of the cold-rolled sheet after annealing to produce a non-oriented silicon steel sheet with a thickness of 0.35 mm.

[0062] Example 2

[0063] The chemical composition of a non-oriented silicon steel sheet provided in Example 2 includes, by mass percentage, C: 0.0015%, S: 0.0013%, N: 0.0018%, Si: 3.34%, Al: 1.21%, Mn: 0.31%, Sn: 0.06%, P: 0.018%, Nb: 0.0032%, V: 0.0024%, Ti: 0.0017%, Cu: 0.027%, Mo: 0.005%, Ni: 0.027%, Cr: 0.025%, and the rest is Fe and unavoidable impurities.

[0064] The processing method of the non-oriented silicon steel sheet comprises the following steps:

[0065] Heating process: the continuous casting billet is placed in a heating furnace for heating at a temperature of 1127°C and a holding time of 273 minutes;

[0066] Hot rolling process: the heated continuous casting billet is sent to the rolling mill for rough rolling and 7 passes of finishing rolling to obtain a hot rolled plate with a thickness of 2.2 mm, wherein the circumferential speed ratio of the upper and lower working rolls in the 6th pass of finishing rolling is 1:1.02, and the circumferential speed ratio of the upper and lower working rolls in the 7th pass of finishing rolling is 1.02:1. The final rolling temperature is controlled to be 782°C, the coiling temperature is 653°C, the coiling holding time is 73 minutes, and the coiling is unrolled after holding for air cooling to room temperature.

[0067] Normalizing process: send the hot rolled plate into the normalizing furnace for normalizing treatment. The atmosphere in the normalizing furnace is pure N2, the normalizing temperature is 838℃, the heating rate is 78℃ / s, and the holding time is 40s;

[0068] Cold rolling process: the normalized hot-rolled sheet is cold rolled, and the first pass reduction rate of cold rolling is controlled to be 39.5%;

[0069] Annealing process: anneal the cold rolled sheet in a protective atmosphere of a mixed atmosphere of H2 and N2, wherein the volume percentage of H2 is 30-70%, the annealing temperature is 958°C, and the holding time is 307s;

[0070] Coating process: An insulating layer is coated on the surface of the cold-rolled sheet after annealing to produce a non-oriented silicon steel sheet with a thickness of 0.30 mm.

[0071] Example 3

[0072] The chemical composition of a non-oriented silicon steel sheet provided in Example 3 includes, by mass percentage, C: 0.0015%, S: 0.0013%, N: 0.0018%, Si: 3.34%, Al: 1.21%, Mn: 0.31%, Sn: 0.06%, P: 0.018%, Nb: 0.0032%, V: 0.0024%, Ti: 0.0017%, Cu: 0.027%, Mo: 0.005%, Ni: 0.027%, Cr: 0.025%, and the rest is Fe and unavoidable impurities.

[0073] The processing method of the non-oriented silicon steel sheet comprises the following steps:

[0074] Heating process: the continuous casting billet is placed in a heating furnace for heating at a temperature of 1157°C and a holding time of 232 minutes;

[0075] Hot rolling process: the heated continuous casting billet is sent to the rolling mill for rough rolling and 7 passes of finishing rolling to obtain a hot rolled plate with a thickness of 2.1 mm, wherein the circumferential speed ratio of the upper and lower working rolls in the 6th pass of finishing rolling is 1:1.04, and the circumferential speed ratio of the upper and lower working rolls in the 7th pass of finishing rolling is 1.04:1. The final rolling temperature is controlled to be 750°C, the coiling temperature is 643°C, the coiling holding time is 78 minutes, and the coiling is unrolled after holding for air cooling to room temperature.

[0076] Normalizing process: the hot rolled plate is sent into the normalizing furnace for normalizing treatment. The atmosphere in the normalizing furnace is pure N2, the normalizing temperature is 823℃, the heating rate is 68℃ / s, and the holding time is 47s;

[0077] Cold rolling process: the normalized hot-rolled sheet is cold rolled, and the first pass reduction rate of cold rolling is controlled to be 41.8%;

[0078] Annealing process: anneal the cold-rolled sheet in a protective atmosphere of a mixed atmosphere of H2 and N2, wherein the volume percentage of H2 is 30-70%, the annealing temperature is 943°C, and the holding time is 377s;

[0079] Coating process: An insulating layer is coated on the surface of the cold-rolled sheet after annealing to produce a non-oriented silicon steel sheet with a thickness of 0.25 mm.

[0080] Example 4

[0081] The chemical composition of a non-oriented silicon steel sheet provided in Example 4 includes, by mass percentage, C: 0.0020%, S: 0.0011%, N: 0.0011%, Si: 3.61%, Al: 0.89%, Mn: 0.44%, Sn: 0.08%, P: 0.016%, Nb: 0.0021%, V: 0.0027%, Ti: 0.0015%, Cu: 0.025%, Mo: 0.004%, Ni: 0.025%, Cr: 0.029%, and the rest is Fe and unavoidable impurities.

[0082] The processing method of the non-oriented silicon steel sheet comprises the following steps:

[0083] Heating process: the continuous casting billet is placed in a heating furnace for heating at a temperature of 1173°C and a holding time of 265 minutes;

[0084] Hot rolling process: the heated continuous casting billet is sent to the rolling mill for rough rolling and 7 passes of finishing rolling to obtain a hot rolled plate with a thickness of 2.3 mm, wherein the circumferential speed ratio of the upper and lower working rolls in the 6th pass of finishing rolling is 1:1.02, and the circumferential speed ratio of the upper and lower working rolls in the 7th pass of finishing rolling is 1.02:1. The final rolling temperature is controlled to be 723°C, the coiling temperature is 631°C, the coiling holding time is 86 minutes, and the coiling is unrolled after holding for air cooling to room temperature.

[0085] Normalizing process: send the hot rolled plate into the normalizing furnace for normalizing treatment. The atmosphere in the normalizing furnace is pure N2, the normalizing temperature is 835℃, the heating rate is 70℃ / s, and the holding time is 28s.

[0086] Cold rolling process: the normalized hot-rolled sheet is cold rolled, and the first pass reduction rate of cold rolling is controlled to be 40.7%;

[0087] Annealing process: anneal the cold-rolled sheet in a protective atmosphere of a mixed atmosphere of H2 and N2, wherein the volume percentage of H2 is 30-70%, the annealing temperature is 955°C, and the holding time is 389s;

[0088] Coating process: An insulating layer is coated on the surface of the cold-rolled sheet after annealing to produce a non-oriented silicon steel sheet with a thickness of 0.35 mm.

[0089] Example 5

[0090] The chemical composition of a non-oriented silicon steel sheet provided in Example 5 includes, by mass percentage, C: 0.0020%, S: 0.0011%, N: 0.0011%, Si: 3.61%, Al: 0.89%, Mn: 0.44%, Sn: 0.08%, P: 0.016%, Nb: 0.0021%, V: 0.0027%, Ti: 0.0015%, Cu: 0.025%, Mo: 0.004%, Ni: 0.025%, Cr: 0.029%, and the rest is Fe and unavoidable impurities.

[0091] The processing method of the non-oriented silicon steel sheet comprises the following steps:

[0092] Heating process: the continuous casting billet is placed in a heating furnace for heating at a temperature of 1094°C and a holding time of 210 minutes;

[0093] Hot rolling process: the heated continuous casting billet is sent to the rolling mill for rough rolling and 7 passes of finishing rolling to obtain a hot rolled plate with a thickness of 2.2 mm, wherein the circumferential speed ratio of the upper and lower working rolls in the 6th pass of finishing rolling is 1:1.03, and the circumferential speed ratio of the upper and lower working rolls in the 7th pass of finishing rolling is 1.03:1. The final rolling temperature is controlled to be 766°C, the coiling temperature is 624°C, the coiling holding time is 81 minutes, and the coiling is unrolled after holding for air cooling to room temperature.

[0094] Normalizing process: the hot rolled plate is sent into the normalizing furnace for normalizing treatment. The atmosphere in the normalizing furnace is pure N2, the normalizing temperature is 827℃, the heating rate is 51℃ / s, and the holding time is 33s;

[0095] Cold rolling process: the normalized hot-rolled sheet is cold rolled, and the first pass reduction rate of cold rolling is controlled to be 38.9%;

[0096] Annealing process: anneal the cold-rolled sheet in a protective atmosphere of a mixed atmosphere of H2 and N2, wherein the volume percentage of H2 is 30-70%, the annealing temperature is 947°C, and the holding time is 268s;

[0097] Coating process: An insulating layer is coated on the surface of the cold-rolled sheet after annealing to produce a non-oriented silicon steel sheet with a thickness of 0.30 mm.

[0098] Example 6

[0099] The chemical composition of a non-oriented silicon steel sheet provided in Example 6 includes, by mass percentage, C: 0.0020%, S: 0.0011%, N: 0.0011%, Si: 3.61%, Al: 0.89%, Mn: 0.44%, Sn: 0.08%, P: 0.016%, Nb: 0.0021%, V: 0.0027%, Ti: 0.0015%, Cu: 0.025%, Mo: 0.004%, Ni: 0.025%, Cr: 0.029%, and the rest is Fe and unavoidable impurities.

[0100] The processing method of the non-oriented silicon steel sheet comprises the following steps:

[0101] Heating process: the continuous casting billet is placed in a heating furnace for heating at a temperature of 1144°C and a holding time of 225 minutes;

[0102] Hot rolling process: the heated continuous casting billet is sent to the rolling mill for rough rolling and 7 passes of finishing rolling to obtain a hot rolled plate with a thickness of 2.1 mm, wherein the circumferential speed ratio of the upper and lower working rolls in the 6th pass of finishing rolling is 1:1.01, and the circumferential speed ratio of the upper and lower working rolls in the 7th pass of finishing rolling is 1.01:1. The final rolling temperature is controlled to be 794°C, the coiling temperature is 656°C, the coiling holding time is 68 minutes, and the coiling is unrolled after holding for air cooling to room temperature.

[0103] Normalizing process: the hot rolled plate is sent into the normalizing furnace for normalizing treatment. The atmosphere in the normalizing furnace is pure N2, the normalizing temperature is 842℃, the heating rate is 63℃ / s, and the holding time is 37s;

[0104] Cold rolling process: the normalized hot-rolled sheet is cold rolled, and the first pass reduction rate of cold rolling is controlled to be 40.3%;

[0105] Annealing process: anneal the cold-rolled sheet in a protective atmosphere of a mixed atmosphere of H2 and N2, wherein the volume percentage of H2 is 30-70%, the annealing temperature is 962°C, and the holding time is 256s;

[0106] Coating process: An insulating layer is coated on the surface of the cold-rolled sheet after annealing to produce a non-oriented silicon steel sheet with a thickness of 0.25 mm.

[0107] Table 1

[0108]

[0109] It should be understood that although this specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

[0110] The series of detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present application. They are not intended to limit the scope of protection of the present application. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present application should be included in the scope of protection of the present application.

Claims

1. A method for processing a non-oriented silicon steel sheet, characterized in that: The process includes heating, hot rolling, normalizing, cold rolling, annealing and coating the continuous casting billet in sequence, wherein: In the heating process, the continuous casting billet is heated to a temperature of 1080-1180°C and the holding time is 200-300 minutes; In the hot rolling process, the heated continuous casting billet is sent to the rolling mill for rough rolling and 7 passes of finishing rolling to obtain hot rolled plates, wherein the 6th and 7th passes of finishing rolling are asynchronous rolling; In the normalizing process, the hot rolled sheet is sent to the normalizing furnace for normalizing treatment, and the normalizing temperature is T1 = 15 × [6.7-([Si] + 0.72 × [Al]) × 100] 2 +760×[1-|v7 up / v7 down -1|]℃, heating rate is 50~80℃ / s, holding time is 20~50s, where [Si], [Al] are the mass percentages of Si and Al in the continuous casting billet, v7 up v7 is the circumferential speed of the working roll in the seventh pass of finishing rolling. down is the circumferential speed of the lower working roll in the 7th pass of finishing rolling; In the cold rolling process, the normalized hot-rolled sheet is cold-rolled to obtain a cold-rolled sheet; In the annealing process, the cold-rolled sheet is continuously annealed, the annealing temperature is T2=T1+120°C, and the holding time is 200-400s.

2. The method for processing a non-oriented silicon steel sheet according to claim 1, characterized in that: In the hot rolling process, the circumferential speed ratio of the upper and lower working rolls in the 6th pass is 1:1.01 to 1:1.04, and the circumferential speed ratio of the upper and lower working rolls in the 7th pass is opposite to that of the 6th pass.

3. The method for processing a non-oriented silicon steel sheet according to claim 1, characterized in that: In the hot rolling process, the final rolling temperature is 720-800°C, the coiling temperature is 600-660°C, the coiling holding time is 60-90 minutes, and after the holding time, the coil is unrolled and air-cooled to room temperature.

4. The method for processing a non-oriented silicon steel sheet according to claim 3, characterized in that: The recrystallized grain size of the hot-rolled plate surface layer is 2-18 μm, wherein the surface layer includes an upper surface layer and a lower surface layer of the same thickness, and the sum of the thickness of the upper surface layer and the lower surface layer accounts for 20-35% of the thickness of the hot-rolled plate.

5. The method for processing a non-oriented silicon steel sheet according to claim 4, characterized in that: The average recrystallized grain size of the surface layer of the hot-rolled plate after normalization is 20-45 μm, and the average recrystallized grain size of the middle layer is 80-110 μm.

6. The method for processing a non-oriented silicon steel sheet according to claim 5, characterized in that: The recrystallized grain size of the cold-rolled sheet after annealing is 120 to 150 μm on average.

7. The method according to claim 1, characterized in that: The thickness of the hot-rolled sheet obtained after hot rolling is 2.10 to 2.30 mm, and the thickness of the cold-rolled sheet obtained after cold rolling is 0.25 to 0.35 mm.

8. The method for processing a non-oriented silicon steel sheet according to claim 1, characterized in that: In the normalizing process, the atmosphere in the normalizing furnace is pure N2, and the temperature fluctuation range of the normalizing temperature is 5°C above and below the temperature T1; In the annealing process, the protective atmosphere is a mixed atmosphere of H2 and N2, wherein the volume percentage of H2 is 30-70%.

9. A non-oriented silicon steel sheet, characterized in that: The non-oriented silicon steel sheet is prepared by the processing method according to claim 1, and the chemical composition of the non-oriented silicon steel sheet includes, by mass percentage, C≤0.0025%, S≤0.0015%, N≤0.002%, Si: 3.25-3.65%, Al: 0.85-1.25%, Mn: 0.27-0.47%, Sn: 0.05-0.08%, P≤0.02%, Nb+V≤0.006%, Ti≤0.002%, Cu≤0.03%, Mo≤0.006%, Ni+Cr≤0.06%, and the rest is Fe and unavoidable impurities.

10. The non-oriented silicon steel sheet according to claim 9, characterized in that: When the thickness of the non-oriented silicon steel sheet is 0.25 mm, the iron loss P 1.0 / 400 ≤12W / kg, magnetic induction intensity B 5000 ≥1.64T; when the thickness of the non-oriented silicon steel sheet is 0.30mm, the iron loss P 1.0 / 400 ≤14W / kg, magnetic induction intensity B 5000 ≥1.65T; when the thickness of the non-oriented silicon steel sheet is 0.35mm, the iron loss P 1.0 / 400 ≤17W / kg, magnetic induction intensity B 5000 ≥1.68T.

11. The non-oriented silicon steel sheet according to claim 10, characterized in that: When the thickness of the non-oriented silicon steel sheet is 0.25 mm, the thickness of the hot-rolled sheet is 2.10 mm; when the thickness of the non-oriented silicon steel sheet is 0.30 mm, the thickness of the hot-rolled sheet is 2.20 mm; when the thickness of the non-oriented silicon steel sheet is 0.35 mm, the thickness of the hot-rolled sheet is 2.30 mm.

Citation Information

Patent Citations

  • Oriented silicon steel preparation method by means of double roll continuous casting thin strip asymmetrical hot rolling process

    CN103111466A

  • Cold-rolled non-oriented silicon steel low in iron loss and production method

    CN105256226A

  • Asymmetrical rolling method for producing high-grade non-oriented silicon steel

    CN105772502A

  • Production method of cold-rolled non-oriented silicon steel with excellent iron loss performance in low field

    CN110616370A

  • Low-iron-loss non-oriented electrical steel adapting to high-frequency working condition and production method thereof

    CN113512635A

Cited By

  • Ultra-thin non-oriented silicon steel for motor stator and rotor iron core and production method and application of ultra-thin non-oriented silicon steel

    CN119553178A

  • High-grade non-oriented silicon steel and production method of high-grade non-oriented silicon steel

    CN122522124A