Fine blanking steel rolling control method and device and fine blanking steel rolling system
By using a cover annealing furnace in the fine-rolled steel rolling system to regulate the yield strength, the problem of large thickness deviation of cold-rolled fine-rolled steel is solved, the accuracy requirements of high-end products are achieved, and the application scope of the product is expanded.
Patent Information
- Application Number
- CN202411231622.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-26
AI Technical Summary
The thickness deviation of cold-rolled fine-brushed steel in the length direction is large and cannot meet the accuracy requirements of high-end products.
By using a cover annealing and softening treatment in the fine-brushed steel rolling system, the operating parameters of the annealing furnace are adjusted to reduce the yield strength of the fine-brushed steel to the preset range, ensuring that the yield strength distribution in the length direction is evenly distributed. , thereby reducing the thickness deviation of cold-rolled fine-pulled steel.
It effectively reduces the thickness deviation of cold-rolled fine-brushed steel in the length direction, ensures that it meets the dimensional accuracy requirements of high-end products, and expands the use range of cold-rolled fine-brushed steel.
Smart Images

Figure CN119016518A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of steel rolling, and in particular to a rolling control method and device for fine blanking steel and a fine blanking steel rolling system. Background Art
[0002] Fine blanking steel mainly includes carbon structural steel, carbon tool steel, alloy structural steel, alloy tool steel, spring steel, etc. Fine blanking steel raw materials are cold rolled to obtain cold rolled fine blanking steel. Some high-end products have relatively high requirements for the dimensional accuracy of cold rolled fine blanking steel, requiring the thickness deviation of cold rolled fine blanking steel in the length direction to be ≤10um. At present, in order to make cold rolled fine blanking steel meet the requirements of high-end products, fine blanking steel will be annealed and softened before cold rolling. However, even if the fine blanking steel is annealed and softened, the rolled fine blanking steel strip will still have serious thickness fluctuations, that is, the thickness difference of the cold rolled fine blanking steel strip has a large amplitude, a short wavelength, and a steep peak, which exceeds the deviation requirements of the corresponding thickness specifications (such as Figure 1 As shown in the figure, the thickness deviation of the cold-rolled fine-blanking steel at the leading position is basically ≥10um), which does not meet the requirements of high-end products.
[0003] Based on this, how to reduce the thickness deviation of cold-rolled fine-blanking steel in the length direction is a technical problem that needs to be solved urgently. Summary of the invention
[0004] The embodiments of the present application provide a rolling control method, device, storage medium and electronic device for fine blanking steel. The technical solution provided in the present application can effectively reduce the thickness deviation of cold-rolled fine blanking steel in the length direction.
[0005] Other features and advantages of the present application will become apparent from the following detailed description, or may be learned in part by the practice of the present application.
[0006] According to a first aspect of an embodiment of the present application, a rolling control method for fine blanking steel is provided, which is applied to a central processing unit, and the central processing unit is configured in a fine blanking steel rolling system. The fine blanking steel rolling system also includes a hood annealing furnace and a cold rolling mill. The method includes: controlling the hood annealing furnace with a fine blanking steel raw material coil built in to operate according to preset operating parameters to reduce the yield strength at each position in the length direction of the fine blanking steel raw material coil to within a preset yield strength range, so as to obtain a fine blanking steel coil to be rolled, and the difference between the upper limit value and the lower limit value of the preset yield strength range is less than or equal to 20MPa; controlling the cold rolling mill to roll the fine blanking steel coil to be rolled to obtain a target fine blanking steel coil.
[0007] In some embodiments of the present application, based on the aforementioned scheme, the preset operating parameters include a first preset duration, a first rotational speed, a second rotational speed, and set working parameters. The hood annealing furnace includes a heating device, an air cooling device and a water cooling device. The air cooling device includes a circulating fan. The hood annealing furnace with a built-in fine blanking steel raw material coil is controlled to operate according to the preset operating parameters, including: controlling the heating device to heat the fine blanking steel raw material coil; when it is detected that the temperature of the fine blanking steel raw material coil reaches the preset annealing temperature, controlling the hood annealing furnace to enter the first insulation stage; when the duration of the first insulation stage reaches the first preset duration, controlling the hood annealing furnace to enter the hood cooling stage, wherein, in the hood cooling stage, the circulating fan of the air cooling device is controlled to operate at a first rotational speed, so that the fine blanking steel raw material coil is cooled at a first cooling rate, and the value range of the first cooling rate is 15℃ / h~25℃ / h. ℃ / h; when it is detected that the temperature of the fine blanking steel raw material coil reaches the first cooling temperature, the hood annealing furnace is controlled to enter the air cooling stage, wherein the first cooling temperature is lower than the preset annealing temperature, and the value range of the first cooling temperature is 550℃~650℃. In the air cooling stage, the circulating fan of the air cooling device is controlled to operate at the second speed, so that the fine blanking steel raw material coil is cooled at the second cooling rate, and the second speed is greater than the first speed; when it is detected that the temperature of the fine blanking steel raw material coil reaches the second cooling temperature, the hood annealing furnace is controlled to enter the water cooling stage, wherein the second cooling temperature is lower than the first cooling temperature. In the water cooling stage, the water cooling device is controlled to operate with the set working parameters, so that the fine blanking steel raw material coil is cooled at the third cooling rate; when it is detected that the temperature of the fine blanking steel raw material coil reaches the third cooling temperature, the hood annealing furnace is controlled to be closed, and the third cooling temperature is lower than the second cooling temperature.
[0008] In some embodiments of the present application, based on the aforementioned scheme, the preset operating parameters also include a first heating power, a second heating power, and a second preset duration, and the heating device is controlled to heat the fine blanking steel raw material coil, including: controlling the heating device to operate at the first heating power; when it is detected that the temperature of the fine blanking steel raw material coil reaches the preset heating temperature, controlling the hood annealing furnace to enter the second insulation stage, and the preset heating temperature is lower than the preset annealing temperature; when the duration of the second insulation stage reaches the second preset duration, controlling the heating device to operate at the second heating power, and the second heating power is lower than the first heating power.
[0009] In some embodiments of the present application, based on the above-mentioned solution, the preset heating temperature ranges from 350° C. to 450° C., and the second preset time length is greater than or equal to 120 minutes.
[0010] In some embodiments of the present application, based on the above scheme, the preset annealing temperature ranges from 700°C to 750°C.
[0011] In some embodiments of the present application, based on the aforementioned solution, the first preset duration is greater than or equal to 480 minutes.
[0012] In some embodiments of the present application, based on the aforementioned solution, the second cooling temperature ranges from 270°C to 350°C, and the second cooling rate ranges from 20°C / h to 30°C / h.
[0013] In some embodiments of the present application, based on the aforementioned scheme, the third cooling temperature ranges from 20°C to 30°C, and the third cooling rate ranges from 10°C / h to 20°C / h.
[0014] According to a second aspect of an embodiment of the present application, a rolling control device for fine blanking steel is provided, which is configured in a central processing unit, and the central processing unit is configured in a fine blanking steel rolling system. The fine blanking steel rolling system also includes a hood annealing furnace and a cold rolling mill. The device includes: a first control unit, used to control the hood annealing furnace with a built-in fine blanking steel raw material coil to operate according to preset operating parameters, so as to reduce the yield strength at each position in the length direction of the fine blanking steel raw material coil to within a preset yield strength range, and obtain a fine blanking steel coil to be rolled, wherein the difference between the upper limit value and the lower limit value of the preset yield strength range is less than or equal to 20MPa; a second control unit, used to control the cold rolling mill to roll the fine blanking steel coil to be rolled, and obtain a target fine blanking steel coil.
[0015] According to the third aspect of the embodiments of the present application, a fine blanking steel rolling system is provided, the system comprising a central processing unit, a hood annealing furnace connected to the central processing unit, and a cold rolling mill connected to the central processing unit, the central processing unit being used to execute the fine blanking steel rolling control method of any embodiment of the first aspect mentioned above.
[0016] The technical solution of the present application is to first use a hood annealing furnace to anneal and soften the raw material steel coil of fine blanking steel before rolling it, and by adjusting the operating parameters of the hood annealing furnace, the yield strength of the fine blanking steel to be rolled obtained by the hood annealing furnace at various positions in its length direction is within a preset yield strength range, thereby ensuring that the yield strength of the fine blanking steel coil to be rolled at various positions is evenly distributed with small differences, thereby achieving a target fine blanking steel coil obtained by subsequent cold rolling, the thickness deviation of which is basically ≤10um in its length direction, effectively reducing the thickness deviation of the cold-rolled fine blanking steel in its length direction, and obtaining cold-rolled fine blanking steel suitable for high-end products, thereby increasing the scope of use of the cold-rolled fine blanking steel.
[0017] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The drawings herein are incorporated into the specification and constitute a part of the specification, showing embodiments consistent with the present application, and together with the specification, are used to explain the principles of the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the drawings:
[0019] Figure 1 A schematic diagram showing the thickness deviation of the cold-rolled fine blanking steel obtained at this stage in its length direction;
[0020] Figure 2 A schematic structural diagram of a bell-type annealing furnace according to an embodiment of the present application is shown;
[0021] Figure 3 A schematic flow chart of a rolling control method for fine blanking steel according to an embodiment of the present application is shown;
[0022] Figure 4 A schematic diagram showing a first test fine blanking steel coil and a second test fine blanking steel coil according to an embodiment of the present application is shown;
[0023] Figure 5 A schematic diagram showing the yield strength of fine blanking steel SK85 to be rolled at various positions in its length direction according to an embodiment of the present application;
[0024] Figure 6 A schematic diagram of thickness deviation of cold-rolled fine-blanking steel SK85 in its length direction according to an embodiment of the present application is shown.
[0025] Figure 7 A detailed flow chart of controlling a bell-type annealing furnace containing a fine blanking steel raw material coil to operate according to preset operating parameters according to an embodiment of the present application is shown;
[0026] Figure 8 A schematic diagram showing a temperature variation curve of a fine blanking steel bell-type annealing furnace for softening annealing according to an embodiment of the present application is shown;
[0027] Fig. 9 A block diagram of a rolling control device for fine blanking steel according to an embodiment of the present application is shown. DETAILED DESCRIPTION
[0028] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the examples set forth herein; rather, these embodiments are provided so that this application will be more comprehensive and complete and fully convey the concept of the example embodiments to those skilled in the art.
[0029] In addition, described feature, structure or characteristic can be combined in one or more embodiments in any suitable manner. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present application. However, those skilled in the art will appreciate that the technical scheme of the present application can be put into practice without one or more of the specific details, or other methods, components, devices, steps, etc. can be adopted. In other cases, known methods, devices, realizations or operations are not shown or described in detail to avoid blurring the various aspects of the application.
[0030] The block diagrams shown in the accompanying drawings are merely functional entities and do not necessarily correspond to physically independent entities. That is, these functional entities may be implemented in software form, or in one or more hardware modules or integrated circuits, or in different networks and / or processor devices and / or microcontroller devices.
[0031] The flowcharts shown in the accompanying drawings are only exemplary and do not necessarily include all the contents and operations / steps, nor must they be executed in the order described. For example, some operations / steps can be decomposed, and some operations / steps can be combined or partially combined, so the actual execution order may change according to actual conditions.
[0032] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the objects used in this way can be interchanged where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those shown or described.
[0033] In order to make the purpose, technical solutions and advantages of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0034] Some embodiments of the present application will be described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments may be combined with each other.
[0035] According to a first aspect of an embodiment of the present application, a fine blanking steel rolling system is provided.
[0036] The fine blanking steel rolling system comprises a central processing unit, a bell-type annealing furnace connected to the central processing unit, and a cold rolling mill connected to the central processing unit.
[0037] The central processing unit controls the operation of the hood annealing furnace and the operation of the cold rolling mill to roll the target fine blanking steel coil.
[0038] It should be noted that the central processing unit is used to execute the rolling control method of fine blanking steel in any embodiment of the second aspect described below.
[0039] In some embodiments, the bell annealing furnace is structured as follows: Figure 2 shown.
[0040] See also Figure 2 , shows a schematic structural diagram of a bell-type annealing furnace according to an embodiment of the present application.
[0041] The bell-type annealing furnace includes an inner cavity, which is used to accommodate the fine blanking steel raw material steel coil 10. Generally, the inner cavity of the bell-type annealing furnace can accommodate at least 4 rolls of fine blanking steel raw material steel coil 10. Figure 2 The provided bell-type annealing furnace has 4 rolls of fine blanking steel raw material steel coils accommodated in its inner cavity.
[0042] The bell-type annealing furnace further includes a heating hood 11. When the bell-type annealing furnace enters the heating stage, the heating hood 11 is placed on the top of the bell-type annealing furnace to heat the fine blanking raw steel coil 10 in the inner cavity. In addition, the bell-type annealing furnace further includes a heat preservation hood. When the bell-type annealing furnace enters the heat preservation stage, the heating hood 11 on the top of the bell-type annealing furnace is replaced with a heat preservation hood to keep the fine blanking raw steel coil 10 in the inner cavity warm.
[0043] The hood-type annealing furnace also includes a heating device, which includes a fuel preheating device 12 and a high-speed burner 16, wherein the fuel preheating device 12 is used to preheat the fuel to be burned, and the number of high-speed burners 16 includes 4, each high-speed burner 16 is used to spray flames toward the inner hood 17 to provide heat to the fine-blanking steel raw material steel coil 10 in the inner cavity.
[0044] It is understandable that the heating power of the heating device of the bell annealing furnace is adjustable, and the heating power refers to the amount of heat provided by the heating device to the fine blanking steel raw material coil 10. When the heating power of the heating device is greater, the heat provided to the fine blanking steel raw material coil 10 is greater.
[0045] The hood annealing furnace also includes an air cooling device, which includes a circulating fan 13 and an air nozzle 18. The speed of the circulating fan 13 is adjustable, wherein the air nozzle 18 is used to provide air to the inner cavity of the hood annealing furnace, and the circulating fan 13 is used to drive the air flow in the inner cavity of the hood annealing furnace to cool the fine blanking steel raw material steel coil 10.
[0046] The bell-type annealing furnace further comprises a convection plate 19, a fully sealed furnace table 14, a diffuser 15, and a water cooling device, wherein the water cooling device is used to provide cooling water to the inner cavity of the bell-type annealing furnace to cool the fine blanking steel raw material coil 10 in the inner cavity.
[0047] According to a second aspect of an embodiment of the present application, a rolling control method for fine blanking steel is provided.
[0048] The method is applied to the central processing unit of the first aspect.
[0049] Combine the following Figure 3 For detailed description of some implementation methods of this application, see Figure 3 According to a flow chart of a rolling control method for fine blanking steel according to an embodiment of the present application, the method specifically includes the following steps 310 to 320:
[0050] Step 310, controlling the hood annealing furnace containing the fine blanking steel raw material coil to operate according to preset operating parameters, so as to reduce the yield strength at various positions in the length direction of the fine blanking steel raw material coil to within a preset yield strength range, and obtaining the fine blanking steel coil to be rolled, wherein the difference between the upper limit value and the lower limit value of the preset yield strength range is less than or equal to 20 MPa.
[0051] Step 320, controlling the cold rolling mill to roll the fine blanking steel coil to be rolled to obtain the target fine blanking steel coil.
[0052] It should be noted that, in the length direction of the fine blanking steel raw material coil, the interval between each position may be 1 m.
[0053] It should also be noted that the preset yield strength range needs to be set according to the type of the fine blanking steel raw material coil. For example, if the fine blanking raw material coil is fine blanking steel SK85, then the corresponding preset yield strength range is [440MPa, 460MPa].
[0054] In order to achieve the purpose of reducing the thickness deviation of cold-rolled fine blanking steel in its length direction, the inventor of the present application conducted a reversal test in the early stage and studied the cause of the severe thickness fluctuation of cold-rolled fine blanking steel.
[0055] During the reversal test, the inventor used two identical test fine blanking steel coils for cold rolling test, wherein the test fine blanking steel coils were fine blanking steel coils obtained through the current annealing and softening treatment.
[0056] The two test rolls of fine blanking steel coils are as follows Figure 4 As shown, including Figure 4 (a) shows a first test fine blanking steel coil, and Figure 4In the second test fine blanking steel coil shown in (b), the leading and trailing ends of the first test fine blanking steel coil and the second test fine blanking steel coil are swapped, that is, the leading end of the first test fine blanking steel coil is the trailing end of the second test fine blanking steel coil.
[0057] By controlling the cold rolling mill to roll the first test fine blanking steel coil and the second test fine blanking steel coil respectively, the fine blanking steel coil obtained after rolling still has serious thickness deviation at the head of the strip. The thickness deviation of the fine blanking steel coil obtained by cold rolling the second test fine blanking steel at its head position is still ≥10um. Figure 1 shown.
[0058] Therefore, it can be determined that the reason why the cold-rolled fine-blanking steel has serious thickness deviation in its length direction has nothing to do with the process parameters of the cold rolling mill. The inventors determined that the reason is: due to improper handling of the fine-blanking steel during the annealing and softening process, it will cause serious thickness deviation of the fine-blanking steel during the rolling process.
[0059] Subsequently, the inventors conducted a large number of experimental tests and found that as long as the yield strength of the fine-blanking steel coil to be rolled at each position in its length direction is controlled within a preset yield strength range, and the yield strength of the fine-blanking steel coil to be rolled is evenly distributed and has small differences, the thickness deviation of the cold-rolled fine-blanking steel in its length direction can be greatly reduced.
[0060] The inventors tested the fine blanking steel SK85, the raw material specification is 2.1*1012mm, and the bell-type annealing furnace is controlled to operate according to the preset operating parameters. The yield strength of the fine blanking steel coil to be rolled at various positions in its length direction is as follows: Figure 5 shown.
[0061] from Figure 5 It can be seen that the yield strength of each position of the obtained fine blanking steel coil to be rolled is within the yield strength range of [440 MPa, 460 MPa], and the deviation of the yield strength at each position is small.
[0062] Further, with the target cold rolling thickness of 1.0 mm, the cold rolling mill is controlled to cold roll the fine blanking steel coil to be rolled, and the target fine blanking steel coil of fine blanking steel SK85 is obtained, and the thickness fluctuation in the length direction is as follows: Figure 6 shown.
[0063] See also Figure 6 , shows a schematic diagram of thickness deviation of cold-rolled fine-blanking steel SK85 in its length direction according to an embodiment of the present application.
[0064] from Figure 6It can be seen that the hit rate of the thickness deviation of cold-rolled fine blanking steel SK85 in its length direction of ≤10um reaches 99.2%, which greatly reduces the thickness deviation of cold-rolled fine blanking steel in its length direction.
[0065] In step 310 of the present application, the specific implementation method of controlling the hood annealing furnace containing the fine blanking steel raw material coil to operate according to the preset operating parameters is not limited in the present application. Specifically, a pre-test can be performed in advance according to the type and structure of the hood annealing furnace to obtain matching preset operating parameters to ensure that the yield strength of the fine blanking steel coil to be rolled obtained after being processed by the hood annealing furnace at each position in its length direction is within the corresponding preset yield strength range.
[0066] In some embodiments, in step 310, the specific implementation of controlling the bell annealing furnace containing the fine blanking steel raw material coil to operate according to the preset operating parameters can be as follows: Figure 7 Follow the steps shown.
[0067] It should be noted that, in this embodiment, the preset operating parameters include a first preset duration, a first rotation speed, a second rotation speed, and set working parameters.
[0068] See also Figure 7 , shows a detailed flow chart of controlling a bell annealing furnace containing a fine blanking steel raw material coil to operate according to preset operating parameters according to an embodiment of the present application, specifically including the following steps 311 to 316:
[0069] Step 311, controlling the heating device to heat the fine blanking steel raw material coil.
[0070] In some embodiments, the preset operating parameters further include a first heating power, a second heating power, and a second preset duration. The specific implementation of step 311 may be as follows: steps 3111 to 3113:
[0071] Step 3111, controlling the heating device to operate at a first heating power.
[0072] Step 3112, when it is detected that the temperature of the fine blanking steel raw material coil reaches the preset heating temperature, the bell-type annealing furnace is controlled to enter the second insulation stage, and the preset heating temperature is lower than the preset annealing temperature.
[0073] Step 3113, when the duration of the second insulation stage reaches a second preset duration, the heating device is controlled to operate at a second heating power, and the second heating power is less than the first heating power.
[0074] Combine the following Figure 8 The implementation details of this embodiment are described in detail. Figure 8, showing a schematic diagram of a softening annealing temperature variation curve of a fine blanking steel hood annealing furnace according to an embodiment of the present application.
[0075] exist Figure 8 In the process, the time when the fine blanking steel raw material coil begins to be placed in the inner cavity of the bell-type annealing furnace is taken as the starting time t0. After that, the bell-type annealing furnace enters the first heating stage. In the first heating stage, the bell-type annealing furnace operates at the first heating power under the action of the heating hood and the flame spraying action of the high-speed burner. When it is detected that the temperature of the fine blanking steel raw material coil in the inner cavity reaches the preset heating temperature T1, the bell-type annealing furnace ends the first heating stage. Figure 8 In the figure, the time interval corresponding to the first heating stage is [t0, t1].
[0076] It should be noted that, because the internal structure of the fine blanking steel raw material coil has no significant change before the temperature is raised to the preset heating temperature T1, the grains elongated during the rolling process have just been restored and have not yet been recrystallized, the preset heating temperature range can be set to 350°C to 450°C, and the fine blanking steel raw material coil is controlled to heat up at a larger heating rate in the first heating stage, wherein the preset heating temperature can be 350°C, 400°C, or 450°C, etc.
[0077] Furthermore, after the bell-type annealing furnace finishes the first heating stage, the bell-type annealing furnace is controlled to enter the second insulation stage. In the second insulation stage, the temperature of the fine blanking steel raw material coil is controlled to be maintained at the preset heating temperature T1. Figure 8 The second heat preservation stage starts at time t1. In the second heat preservation stage, the heating hood on the top of the bell-type annealing furnace is replaced with a heat preservation hood.
[0078] Furthermore, when the duration of the second heat preservation stage reaches a second preset duration, the second heat preservation stage is ended, and the hood annealing furnace is controlled to enter the second heating stage.
[0079] In some embodiments, the second preset duration is greater than or equal to 120 minutes. Figure 8 In the embodiment, the time interval corresponding to the second insulation stage is [t1, t2], wherein the second preset time length can be 120 min, 150 min, or 180 min, etc.
[0080] It can be understood that, since the hood annealing furnace uses a high-speed burner to perform flame spraying treatment on four points in the first heating stage, there are usually 4 or more fine blanking steel raw material coils placed in the inner cavity, and the thickness is relatively large. In order to fully heat the fine blanking steel raw material coils in the inner cavity, a second insulation stage is set during the heating process to ensure that the fine blanking steel raw material coils are heated evenly.
[0081] Furthermore, in the second heating stage of the bell-type annealing furnace, the heating device is controlled to operate at the second heating power, and the heat preservation cover on the top of the bell-type annealing furnace is replaced by the heating cover. Figure 8 In the embodiment, the second heating stage starts at time t2.
[0082] In some embodiments, in the second heating stage, the heating device is controlled to operate at a second heating power so that the temperature of the fine blanking steel raw material coil is heated at a target heating rate, and the target heating rate ranges from 30°C / h to 60°C / h, wherein the target heating rate can be 30°C / h, 35°C / h, 40°C / h, 45°C / h, 50°C / h, or 60°C / h.
[0083] It can be understood that the second heating stage is the recrystallization formation stage of the fine blanking steel raw material coil. Therefore, the heating rate of the fine blanking steel raw material coil needs to be strictly controlled within 30℃ / h~60℃ / h, so that the yield strength of the fine blanking steel raw material coil at various positions in the length direction is uniformly reduced.
[0084] Continue to see Figure 7 , step 312, when it is detected that the temperature of the fine blanking steel raw material steel coil reaches the preset annealing temperature, the bell-type annealing furnace is controlled to enter the first insulation stage.
[0085] It is understandable that when it is detected that the temperature of the fine blanking steel raw material coil reaches the preset annealing temperature, the bell annealing furnace ends the second heating stage. Figure 8 In the figure, the time interval corresponding to the second heating stage is [t2, t3], the preset annealing temperature is T2, and the first insulation stage starts at time t3.
[0086] In some embodiments, the preset annealing temperature may range from 700°C to 750°C, wherein the preset annealing temperature may be 700°C, 710°C, 720°C, 730°C, 740°C, or 750°C.
[0087] Continue to see Figure 7 , step 313, when the duration of the first insulation stage reaches the first preset duration, the hood annealing furnace is controlled to enter the hood cooling stage, wherein in the hood cooling stage, the circulating fan of the air cooling device is controlled to run at a first speed, so that the fine blanking steel raw material steel coil is cooled at a first cooling rate, the value range of the first cooling rate is 15℃ / h~25℃ / h, and the value of the first cooling rate can be 15℃ / h, 18℃ / h, 21℃ / h, 23℃ / h, or 25℃ / h.
[0088] In some embodiments, the first preset time is greater than or equal to 480 minutes. In the first heat preservation stage, the temperature in the bell-type annealing furnace is controlled to be maintained at the preset annealing temperature. Figure 8 In the figure, the time interval corresponding to the first insulation stage is [t3, t4], and the moment t4 is the starting moment of the hood cooling stage, wherein the value of the first preset time length can be 480min, 500min, or 550min.
[0089] In this embodiment, it should be noted that the hood cooling stage refers to the stage in which the air cooling device cools down the fine blanking steel raw material coil by conveying air to the inner cavity of the hood annealing furnace when there is a heat preservation hood on the top of the hood annealing furnace.
[0090] It should also be noted that in the hood cooling stage, the specific parameters of the first speed of the circulating fan of the air cooling device controlled need to be set according to the specific structure of the hood annealing furnace and the specific structure of the air cooling device.
[0091] In this embodiment, by strictly controlling the operating parameters of the air cooling device, the first cooling rate of the fine blanking steel raw material coil in the hood cooling stage is 15°C / h to 25°C / h, which can keep the microstructure of the material uniform. If the first cooling rate is too large, it will cause a large difference in the yield strength of the fine blanking steel raw material coil in the length direction, and thickness fluctuations will easily occur during cold rolling. The value of the first cooling rate can be 15°C / h, 20°C / h, or 25°C / h.
[0092] Continue to see Figure 7 , step 314, when it is detected that the temperature of the fine blanking steel raw material coil reaches the first cooling temperature, the bell-type annealing furnace is controlled to enter the air cooling stage, wherein the first cooling temperature is less than the preset annealing temperature, and the value range of the first cooling temperature is 550°C to 650°C. In the air cooling stage, the circulating fan of the air cooling device is controlled to operate at a second speed, so that the fine blanking steel raw material coil is cooled at a second cooling rate, the second speed is greater than the first speed, and the value of the first cooling temperature can be 550°C, 600°C, or 650°C.
[0093] exist Figure 8 In the figure, T3 is the first cooling temperature. The time interval corresponding to the hood cooling stage is [t4, t5].
[0094] It should be noted that the air cooling stage refers to the stage in which the air cooling device cools down the fine blanking steel raw material coil by delivering air to the inner cavity of the hood-type annealing furnace when there is no insulation hood on the top of the hood-type annealing furnace.
[0095] In some embodiments, the second speed is associated with the specific structure of the bell annealing furnace. Figure 2 In the bell-type annealing furnace, the second rotation speed may be 1900-2100 n / h.
[0096] In some embodiments, the second cooling rate ranges from 20°C / h to 30°C / h, wherein the second cooling rate may be 20°C / h, 25°C / h, or 30°C / h.
[0097] It can be understood that by controlling the cooling of the fine blanking steel raw material coil at a smaller first cooling rate, the microstructure inside the fine blanking steel raw material coil is not destroyed during the cooling process. However, when the temperature of the fine blanking steel raw material coil is reduced to the first cooling temperature, it means that the microstructure inside the fine blanking steel raw material coil has basically been finalized. Therefore, thereafter, a slightly larger second cooling rate can be used to cool the fine blanking steel raw material coil to improve the cooling efficiency, that is, it is necessary to ensure that the second cooling rate is greater than the first cooling rate.
[0098] Continue to see Figure 7 In step 315, when it is detected that the temperature of the fine blanking steel raw material coil reaches the second cooling temperature, the bell-type annealing furnace is controlled to enter the water cooling stage, wherein the second cooling temperature is lower than the first cooling temperature. In the water cooling stage, the water cooling device is controlled to operate with the set working parameters so that the fine blanking steel raw material coil is cooled at a third cooling rate.
[0099] In some embodiments, the second cooling temperature ranges from 270°C to 350°C, wherein the second cooling temperature may be 270°C, 280°C, 300°C, 320°C, 340°C, or 350°C.
[0100] exist Figure 8 In the figure, T4 is the second cooling temperature, the time interval corresponding to the air cooling stage is [t5, t6], and the water cooling stage starts at t6.
[0101] In this embodiment, it should be noted that the set working parameters of the water cooling device are associated with the specific structure of the bell-type annealing furnace. Figure 2 In the bell-type annealing furnace shown in the figure, the set working parameter of the water cooling device can be a water flow parameter, and the value range of the water flow parameter is 20m 3 / h~30m 3 / h.
[0102] In some embodiments, the third cooling rate ranges from 10°C / h to 20°C / h, wherein the third cooling rate may be 10°C / h, 15°C / h, or 20°C / h.
[0103] Continue to see Figure 7 , step 316, when it is detected that the temperature of the fine blanking steel raw material coil reaches the third cooling temperature, the bell-type annealing furnace is controlled to be closed, and the third cooling temperature is lower than the second cooling temperature.
[0104] In some embodiments, the third cooling temperature ranges from 20°C to 30°C, wherein the third cooling temperature may be 20°C, 25°C, 26°C, or 30°C.
[0105] exist Figure 8 In the figure, T5 is the third cooling temperature, and the time interval corresponding to the water cooling stage is [t6, t7].
[0106] It is understandable that when time t7 is reached, the bell-type annealing furnace needs to be closed to complete the rolling of the fine blanking steel raw material coil and obtain the fine blanking steel coil to be rolled.
[0107] In the technical solutions provided in some embodiments of the present application, before rolling the raw material steel coils of fine blanking steel, a hood annealing furnace is first used to anneal and soften the raw material steel coils of fine blanking steel. By adjusting the operating parameters of the hood annealing furnace, the yield strength of the fine blanking steel to be rolled obtained after the treatment of the hood annealing furnace is within the preset yield strength range at each position in its length direction, ensuring that the yield strength of the fine blanking steel coil to be rolled at each position is uniformly distributed with small differences, so that the target fine blanking steel coil obtained by subsequent cold rolling has a thickness deviation of ≤10um in its length direction, effectively reducing the thickness deviation of the cold-rolled fine blanking steel in its length direction, and obtaining cold-rolled fine blanking steel suitable for high-end products, thereby increasing the scope of use of cold-rolled fine blanking steel.
[0108] Based on the same inventive concept, the embodiment of the present application provides a rolling control device for fine blanking steel, which can be used to execute the rolling control method for fine blanking steel in the above embodiment of the present application. For details not disclosed in the embodiment of the present application, please refer to the embodiment of the rolling control method for fine blanking steel in the above embodiment of the present application.
[0109] See also Fig. 9 , shows a block diagram of a rolling control device for fine blanking steel according to an embodiment of the present application.
[0110] like Fig. 9 As shown, according to an embodiment of the present application, a fine blanking steel rolling control device 900 is configured in a central processing unit, and the central processing unit is configured in a fine blanking steel rolling system. The fine blanking steel rolling system also includes a hood annealing furnace and a cold rolling mill. The device 900 includes: a first control unit 901 and a second control unit 902.
[0111] Among them, the first control unit 901 is used to control the hood annealing furnace with the fine blanking steel raw material coil built in to operate according to the preset operating parameters, so as to reduce the yield strength at each position in the length direction of the fine blanking steel raw material coil to within the preset yield strength range, and obtain the fine blanking steel coil to be rolled, and the difference between the upper limit value and the lower limit value of the preset yield strength range is less than or equal to 20MPa; the second control unit 902 is used to control the cold rolling mill to roll the fine blanking steel coil to be rolled to obtain the target fine blanking steel coil.
[0112] In some embodiments of the present application, based on the aforementioned scheme, the preset operating parameters include a first preset duration, a first rotational speed, a second rotational speed, and set working parameters, the hood annealing furnace includes a heating device, an air cooling device and a water cooling device, the air cooling device includes a circulating fan, and the first control unit 901 is also used to: control the heating device to heat the fine blanking steel raw material coil; when it is detected that the temperature of the fine blanking steel raw material coil reaches the preset annealing temperature, control the hood annealing furnace to enter the first insulation stage; when the duration of the first insulation stage reaches the first preset duration, control the hood annealing furnace to enter the hood cooling stage, wherein, in the hood cooling stage, the circulating fan of the air cooling device is controlled to operate at a first rotational speed, so that the fine blanking steel raw material coil is cooled at a first cooling rate, and the value range of the first cooling rate is 15°C / h to 25°C / h ... When the temperature of the raw steel coil of the fine blanking steel reaches the first cooling temperature, the hood annealing furnace is controlled to enter the air cooling stage, wherein the first cooling temperature is lower than the preset annealing temperature, and the value range of the first cooling temperature is 550°C to 650°C. In the air cooling stage, the circulating fan of the air cooling device is controlled to operate at the second speed, so that the raw steel coil of the fine blanking steel is cooled at a second cooling rate, and the second speed is greater than the first speed; when it is detected that the temperature of the raw steel coil of the fine blanking steel reaches the second cooling temperature, the hood annealing furnace is controlled to enter the water cooling stage, wherein the second cooling temperature is lower than the first cooling temperature. In the water cooling stage, the water cooling device is controlled to operate with the set working parameters, so that the raw steel coil of the fine blanking steel is cooled at a third cooling rate; when it is detected that the temperature of the raw steel coil of the fine blanking steel reaches the third cooling temperature, the hood annealing furnace is controlled to be closed, and the third cooling temperature is lower than the second cooling temperature.
[0113] In some embodiments of the present application, based on the aforementioned scheme, the preset operating parameters also include a first heating power, a second heating power, and a second preset duration, and the first control unit 901 is also used to: control the heating device to operate at the first heating power; when it is detected that the temperature of the fine-blanking steel raw material coil reaches the preset heating temperature, control the hood-type annealing furnace to enter the second insulation stage, and the preset heating temperature is lower than the preset annealing temperature; when the duration of the second insulation stage reaches the second preset duration, control the heating device to operate at the second heating power, and the second heating power is lower than the first heating power.
[0114] In some embodiments of the present application, based on the above-mentioned solution, the preset heating temperature ranges from 350° C. to 450° C., and the second preset time length is greater than or equal to 120 minutes.
[0115] In some embodiments of the present application, based on the above scheme, the preset annealing temperature ranges from 700°C to 750°C.
[0116] In some embodiments of the present application, based on the aforementioned solution, the first preset duration is greater than or equal to 480 minutes.
[0117] In some embodiments of the present application, based on the aforementioned solution, the second cooling temperature ranges from 270°C to 350°C, and the second cooling rate ranges from 20°C / h to 30°C / h.
[0118] In some embodiments of the present application, based on the aforementioned scheme, the third cooling temperature ranges from 20°C to 30°C, and the third cooling rate ranges from 10°C / h to 20°C / h.
[0119] The above description is only an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present application shall be included in the scope of the claims of the present application.
Claims
1. A rolling control method for fine blanking steel, characterized in that: Applied to a central processing unit, the central processing unit is configured in a fine blanking steel rolling system, the fine blanking steel rolling system also includes a bell annealing furnace and a cold rolling mill, the method includes: Controlling the bell annealing furnace containing the fine blanking steel raw material coil to operate according to preset operating parameters, so as to reduce the yield strength at each position in the length direction of the fine blanking steel raw material coil to a preset yield strength range, and obtaining the fine blanking steel coil to be rolled, wherein the difference between the upper limit value and the lower limit value of the preset yield strength range is less than or equal to 20 MPa; The cold rolling mill is controlled to roll the fine blanking steel coil to be rolled to obtain a target fine blanking steel coil.
2. The method according to claim 1, characterized in that The preset operating parameters include a first preset duration, a first rotation speed, a second rotation speed, and set working parameters. The bell-type annealing furnace includes a heating device, an air cooling device, and a water cooling device. The air cooling device includes a circulating fan. The bell-type annealing furnace with a fine blanking steel raw material steel coil built therein is controlled to operate according to the preset operating parameters, including: Controlling the heating device to heat the fine blanking steel raw material coil; When it is detected that the temperature of the fine blanking steel raw material coil reaches the preset annealing temperature, the bell-type annealing furnace is controlled to enter the first insulation stage; When the duration of the first heat preservation stage reaches a first preset duration, the hood annealing furnace is controlled to enter a hood cooling stage, wherein in the hood cooling stage, the circulating fan of the air cooling device is controlled to run at a first speed, so that the fine blanking steel raw material steel coil is cooled at a first cooling rate, and the value range of the first cooling rate is 15°C / h to 25°C / h; When it is detected that the temperature of the fine blanking steel raw material coil reaches a first cooling temperature, the bell-type annealing furnace is controlled to enter an air cooling stage, wherein the first cooling temperature is lower than the preset annealing temperature, and the value range of the first cooling temperature is 550°C to 650°C. In the air cooling stage, the circulating fan of the air cooling device is controlled to operate at a second speed, so that the fine blanking steel raw material coil is cooled at a second cooling rate, and the second speed is greater than the first speed; When it is detected that the temperature of the fine blanking steel raw material coil reaches a second cooling temperature, the bell-type annealing furnace is controlled to enter a water cooling stage, wherein the second cooling temperature is lower than the first cooling temperature, and in the water cooling stage, the water cooling device is controlled to operate with set working parameters so that the fine blanking steel raw material coil is cooled at a third cooling rate; When it is detected that the temperature of the fine blanking steel raw material coil reaches a third cooling temperature, the bell-type annealing furnace is controlled to be closed, and the third cooling temperature is lower than the second cooling temperature.
3. The method according to claim 2, characterized in that The preset operating parameters also include a first heating power, a second heating power, and a second preset duration, and the controlling the heating device to heat the fine blanking steel raw material coil includes: Controlling the heating device to operate at a first heating power; When it is detected that the temperature of the fine blanking steel raw material coil reaches a preset heating temperature, the bell-type annealing furnace is controlled to enter a second heat preservation stage, and the preset heating temperature is lower than the preset annealing temperature; When the duration of the second heat preservation stage reaches a second preset duration, the heating device is controlled to operate at a second heating power, which is less than the first heating power.
4. The method according to claim 3, characterized in that The preset heating temperature ranges from 350° C. to 450° C., and the second preset time length is greater than or equal to 120 minutes.
5. The method according to claim 2, characterized in that: The preset annealing temperature ranges from 700°C to 750°C.
6. The method according to claim 2, characterized in that The first preset duration is greater than or equal to 480 minutes.
7. The method according to claim 2, characterized in that: The second cooling temperature ranges from 270° C. to 350° C., and the second cooling rate ranges from 20° C. / h to 30° C. / h.
8. The method according to claim 2, characterized in that: The third cooling temperature ranges from 20°C to 30°C, and the third cooling rate ranges from 10°C / h to 20°C / h.
9. A rolling control device for fine blanking steel, characterized in that: The device is configured in a central processing unit, the central processing unit is configured in a fine blanking steel rolling system, the fine blanking steel rolling system also includes a bell annealing furnace and a cold rolling mill, and the device includes: A first control unit is used to control the bell annealing furnace with the fine blanking steel raw material coil built therein to operate according to preset operating parameters, so as to reduce the yield strength at each position in the length direction of the fine blanking steel raw material coil to a preset yield strength range, thereby obtaining the fine blanking steel coil to be rolled, wherein the difference between the upper limit value and the lower limit value of the preset yield strength range is less than or equal to 20 MPa; The second control unit is used to control the cold rolling mill to roll the fine blanking steel coil to be rolled to obtain a target fine blanking steel coil.
10. A fine blanking steel rolling system, characterized in that: The system includes a central processing unit, a hood annealing furnace connected to the central processing unit, and a cold rolling mill connected to the central processing unit, and the central processing unit is used to execute the rolling control method of fine blanking steel as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Method for controlling swelling rib in central section of color coating base material
CN102226231A
Cover-type furnace annealing process
CN102994708A
350MPa-grade low-cost high-magnetic-induction cold-rolled magnetic pole steel and manufacturing method thereof
CN115261732A
Cover annealing preparation method of structural steel for automobile and structural steel for automobile
CN115537543A
Cold machining and heat treatment method of Ni-Cr electrothermal alloy hot-rolled wire rod
CN116891955A