High-molecular polymer film-forming agent and preparation method thereof
Through the cross-linking structure of polymer film forming agent, combined with polyester-5 and hydroxypropyl starch, the stability of the cosmetic spray and liquid foundation film forming agent in high temperature and humid environments is solved, and the makeup is maintained , refreshing and comfort, providing excellent water resistance and safety.
Patent Information
- Application Number
- CN202411122877.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing makeup spray and liquid foundation film-forming agents are difficult to meet the needs of makeup holding, refreshing, comfort and safety at the same time, especially in the case of high temperatures and sweating during exercise.
The polymer film forming agent is formed by cross-linking reaction, combining polyester-5, hydroxypropyl starch and polyethylene glycol-8 to form a specific cross-linking structure, providing long-lasting makeup, refreshing, non-stick and water-resistant Performance, and the safety and performance of the film forming agent are ensured by controlling the reaction conditions and crosslinking agent selection during the preparation process.
It achieves the effect of long-lasting makeup, high comfort, refreshing and non-stick, and can maintain the perfect state of makeup in high temperature and humid environments, improves the user experience and delicate and smooth skin feeling, and avoids the sticky feeling of traditional products. and tension and discomfort.
Smart Images

Figure CN119019820A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of film-forming agents for cosmetics, and more specifically, to a high molecular polymer film-forming agent and a preparation method thereof. Background Art
[0002] In the cosmetics industry, setting spray and liquid foundation are important makeup products, and their performance is directly related to consumers' usage experience and makeup performance. As consumers' demands for cosmetics become increasingly diversified and personalized, their requirements for the setting power, experience, efficacy and makeup effect of setting spray and liquid foundation are also increasing. Especially in terms of setting power, consumers pay more and more attention to the durability and stability of makeup, and require products to maintain perfect makeup in various environments (such as high temperature, sweating during exercise, etc.).
[0003] However, there are some common problems with the film-forming agents used in the setting sprays and foundations on the current market. These film-forming agents often fail to meet consumers' demands for setting power, freshness, comfort and safety at the same time. Although some film-forming agents on the market can provide strong setting power, they are prone to produce a sticky feeling after use, affecting the user experience; or some film-forming agents are refreshing and non-sticky, but lack the ability to hold makeup, making it difficult to meet the demand for long-term makeup maintenance. In addition, some film-forming agents may cause skin tightness and discomfort during the film-forming process.
[0004] Therefore, it is necessary to develop a film-forming agent that has long-lasting makeup effect, high comfort, and maintains good effects under various conditions. Summary of the invention
[0005] The present application provides a high molecular polymer film-forming agent and a preparation method thereof. The film-forming agent is formed by a cross-linking reaction, has excellent fixing properties, can form a long-lasting continuous film layer on the skin surface, and effectively helps cosmetics achieve long-lasting makeup. At the same time, the film-forming agent also has a good smooth texture, making the setting spray and liquid foundation easier to apply evenly, improving the user experience. In addition, the film-forming agent also has a certain water resistance, can maintain the stability of cosmetics in the face of sweat and high temperature, and further prolong the durability of makeup. While providing strong makeup setting power, the film-forming agent maintains the characteristics of being refreshing and non-greasy, reduces the tightness of the skin, and meets the multi-faceted needs of consumers for setting spray and liquid foundation.
[0006] In the first aspect, the present application provides a polymer film-forming agent, which adopts the following technical solution: A high molecular polymer film-forming agent comprises the following raw materials in terms of mass percentage: 25-35% polyester-5, 0.1-1% hydroxypropyl starch and water.
[0007] Preferably, the high molecular polymer film former comprises the following raw materials in terms of mass percentage: 30% polyester-5, 0.8% hydroxypropyl starch and water.
[0008] Preferably, polyethylene glycol-8 is used in the preparation of the high molecular polymer film-forming agent.
[0009] By adopting the above technical solution, the carboxyl group in polyester-5 and the hydroxyl group in hydroxypropyl starch undergo esterification reaction to form a stable cross-linked structure. This innovative structural design significantly optimizes the performance of the film-forming agent, not only giving it excellent heat resistance and chemical resistance, but also greatly improving the mechanical strength of the film. When this improved film-forming agent is used in the cosmetics field, such as makeup setting spray and liquid foundation, its advantages are particularly prominent.
[0010] It can bring a good refreshing experience to the skin, and can keep the makeup lasting and fresh even in hot or humid environments, avoiding the sticky feeling that traditional products may bring. At the same time, the strong makeup holding ability allows the makeup to fit the skin closely without any tightness or discomfort, truly achieving a perfect balance between naturalness and durability. The special cross-linking structure also gives downstream cosmetics a soft film-forming effect, making the skin feel more delicate and smooth, and the skin feel is significantly improved. Even in the face of challenges from external factors such as high temperature and sweat, it can easily resist and keep the makeup flawless.
[0011] In a second aspect, the present application provides a method for preparing a polymer film-forming agent, using the following technical solution: A method for preparing a high molecular polymer film-forming agent comprises the following steps: Step 1: The water is heated to 75-85° C., and the polyester-5 is mixed with the water until the polyester-5 is completely dissolved to obtain a first mixture; Step 2: Cool the first mixture to 55-65° C., add polyethylene glycol-8, and mix until completely dissolved to obtain a second mixture; Step 3: continuously stirring the hydroxypropyl starch and the second mixture to allow a cross-linking reaction to occur, and heat-retaining the mixture for 40-60 minutes to obtain a third mixture; Step 4: heating the third mixture to 95-105° C. for 30-90 min to obtain a high molecular polymer film-forming agent.
[0012] The timing of heating in step 4 is particularly important. If the polyester-5 and hydroxypropyl starch are heated before they are fully cross-linked, especially when the water content is so high, the hydroxypropyl starch will age and harden, resulting in a poor film-forming effect of the final film-forming agent.
[0013] Dissolving polyester-5 in advance in step 1 is conducive to speeding up subsequent reactions, reducing energy consumption and saving time. If the order of adding polyester-5 and hydroxypropyl starch is swapped, the following problems exist: First, the hydroxypropyl starch that has not yet undergone cross-linking is at risk of aging and hardening at 75-85°C, resulting in poor film-forming effect of the film-forming agent; second, if polyester-5 is not dissolved at 75-85°C in advance, the subsequent response speed is very slow, resulting in a serious extension of the reaction time and low efficiency. Therefore, it is necessary to further define the reaction sequence and reaction conditions.
[0014] Preferably, the usage amount of polyethylene glycol-8 is 0.03-0.8% of the total mass of the high molecular polymer film-forming agent.
[0015] Preferably, the usage amount of polyethylene glycol-8 is 0.2-0.5% of the total mass of the high molecular polymer film-forming agent.
[0016] The amount of polyethylene glycol-8 used can be any value such as 0.03%, 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8% of the total mass of the high molecular weight polymer film-forming agent.
[0017] In the cross-linking process of polyester-5 and hydroxypropyl starch, commonly used cross-linking agents can be divided into two categories: chemical cross-linking agents and physical cross-linking agents. The following are several potential cross-linking agents used in actual research and development: 1,2-Propylene oxide (propylene oxide): As an efficient chemical cross-linking agent, propylene oxide can react specifically with the hydroxyl groups in hydroxypropyl starch through its active epoxy groups to form a stable cross-linked network. However, its use needs to consider its potential irritating odor, which may affect the operating environment and human health, especially in a confined working space environment.
[0018] Polyethylene glycol diglycol (PEGDGE): This physical crosslinker interacts with the hydroxyl groups in hydroxypropyl starch through hydrogen bonding to promote the formation of crosslinked structures within the material. It is a milder choice. Its advantage is that it reduces the side effects that may be caused by chemical crosslinking, but the crosslinking strength may fluctuate due to environmental conditions such as temperature and humidity, and the crosslinking strength is insufficient.
[0019] 1,4-Butanedialdehyde (commonly known as glutaraldehyde): Glutaraldehyde is another effective chemical cross-linking agent, which can react with the hydroxyl groups in hydroxypropyl starch to enhance the cross-linking degree of the material. However, it is also necessary to pay attention to the irritating odor and toxicity that it may bring, and long-term exposure may pose a threat to human health.
[0020] Taking all factors into consideration, the above cross-linking agents have the following defects: Odor and health effects: Some cross-linking agents have strong or irritating odors, which not only affect the working environment but may also have adverse effects on the respiratory system of operators.
[0021] Toxicity risks: Long-term exposure or inhalation of toxic cross-linking agents may cause health problems, including but not limited to respiratory irritation, skin sensitivity and potential long-term toxic effects.
[0022] Cross-linking stability: The cross-linking effect is unstable, and downstream products cannot effectively resist the effects of sweat and heat, nor can they last long.
[0023] Environmental impact: Harmful substances may be released during the production and use of cross-linking agents, posing a threat to the ecological environment and not in line with the principle of sustainable development.
[0024] Safety issues: The above-mentioned cross-linking agents are not disclosed in the "Catalogue of Used Cosmetic Raw Materials (2021 Edition)" and there are risk factors.
[0025] Based on the above reasons, this application specifically selects low molecular weight polyethylene glycol-8. Polyethylene glycol-8 acts as a crosslinking agent, which can not only make polyester-5 and hydroxypropyl starch undergo crosslinking reaction in the water medium, but also effectively enhance the crosslinking effect. In addition, polyethylene glycol-8 can be volatilized by heating during preparation, so that no polyethylene glycol-8 remains in the film-forming agent, which is safe and non-toxic, and perfectly overcomes the above defects.
[0026] Specifically, an esterification reaction occurs between the carboxyl group in the polyester-5 molecule and the hydroxyl group in the polyethylene glycol-8 molecule. This chemical reaction facilitates the formation of ester bonds. At the same time, the carboxyl group in polyester-5 also actively undergoes a similar esterification reaction with the hydroxyl group in hydroxypropyl starch. This dual reaction mechanism helps the cross-linking to proceed fully and form a specific cross-linking structure. The construction of this special cross-linking structure can effectively improve the performance of the film-forming agent. This further enhances the film-forming effect of the cosmetics, allowing the film to remain long-lasting in high heat and high humidity environments.
[0027] If the amount of polyethylene glycol-8 is too much (more than 0.03-0.8% of the total mass of the polymer film-forming agent), it will lead to an increase in costs, and the energy consumption required for the subsequent decomposition of polyethylene glycol is large, and it takes a long time or a high temperature to completely remove the polyethylene glycol-8. However, the advantage of polyethylene glycol-8 is that it is highly safe, and even if a small amount remains in the film-forming agent, it will not harm the human body. Therefore, this product is very suitable for promotion and use in the cosmetics industry.
[0028] Preferably, in step 1, polyester-5 is added in multiple times and mixed with water.
[0029] Preferably, in step 2, step 3 and step 4, the rotation speed is 1500-2000r / min.
[0030] The temperature and rotation speed control when adding polyethylene glycol-8 is very important. The present application further defines specific conditions to ensure that polyester-5 and hydroxypropyl starch undergo sufficient cross-linking reaction to ensure the film-forming effect.
[0031] In summary, this application has the following beneficial effects: 1. The film-forming agent provided in this application is used in cosmetics such as makeup setting products and liquid foundation, which can bring a good refreshing experience to the skin. Even in high temperature or humid environment, it can keep the makeup lasting and fresh, avoiding the sticky feeling that traditional products may bring. At the same time, the strong makeup holding ability allows the makeup to fit the skin closely without any tightness or discomfort, truly achieving a perfect balance between naturalness and durability. The special cross-linked structure also gives the downstream cosmetics a soft film-forming effect, making the skin feel more delicate and smooth, and the skin feel is significantly improved. Even in the face of challenges from external factors such as high temperature and sweat, it can easily resist and keep the makeup flawless.
[0032] 2. During the preparation process, an esterification reaction occurs between the carboxyl group in the polyester-5 molecule and the hydroxyl group in the polyethylene glycol-8 molecule. This chemical reaction promotes the formation of ester bonds. At the same time, the carboxyl group of polyester-5 also actively undergoes a similar esterification reaction with the hydroxyl group in hydroxypropyl starch. This dual reaction mechanism helps to fully crosslink and form a specific crosslinking structure. The construction of this special crosslinking structure can effectively improve the performance of the film-forming agent. Thereby further enhancing the film-forming effect of the cosmetics, so that the film can still be long-lasting in high heat and high humidity environments.
[0033] 3. Polyethylene glycol-8 acts as a cross-linking agent, which can not only make polyester-5 and hydroxypropyl starch undergo cross-linking reaction in water medium and enhance the cross-linking effect, but also can volatilize polyethylene glycol-8 by heating during preparation, so that no polyethylene glycol-8 remains in the film-forming agent, which is safe and non-toxic. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The facial condition pictures of volunteer A who used the sample of Example 1 to test were taken by VISIA skin detector, and from left to right they are respectively the initial state at the start of timing, the state of timing 2h, the state of timing 4h (during which outdoor activities lasted 20min), the state of timing 6h and the state of timing 8h.
[0035] Figure 2 These are facial pictures of volunteer B who used the sample tested in Example 1, taken with a VISIA skin detector, which, from left to right, are the initial state at the start of timing, the state of timing 2h, the state of timing 4h (during which he spent 20 minutes outdoors), the state of timing 6h, and the state of timing 8h.
[0036] Figure 3 2. The test result diagram of anti-scratch test [1], the left side is the competitor's product, and the right side is the test sample of Example 1.
[0037] Figure 4 2. The test result diagram of anti-scratch test [2], the left side is the competitor's product, and the right side is the test sample of Example 1. DETAILED DESCRIPTION
[0038] The present application is further described in detail below with reference to the accompanying drawings and embodiments.
[0039] The raw materials used in the following examples and comparative examples are all commercially available products. Example
[0040] Example 1 A high molecular polymer film-forming agent comprises polyester-5, hydroxypropyl starch and the balance is supplemented by water.
[0041] The present application also provides a method for preparing a high molecular polymer film-forming agent, comprising the following steps: Step 1: Add 69.2 kg of water into the reactor and heat to 80°C.
[0042] Step 2: Add 30 kg of polyester-5 multiple times (three times in this example) into the reactor and stir until it is completely dissolved to obtain a first mixture.
[0043] Step 3: After the first mixture is completely dissolved, keep warm for 35 minutes while stirring.
[0044] Step 4: Set the temperature of the reactor to 60°C, set the speed to 1800 r / min, add 0.5 kg of polyethylene glycol-8 into the reactor, and stir until it is completely dissolved to obtain a second mixture.
[0045] Step 5: Keep the rotation speed at 1800 r / min, add 0.8 kg of hydroxypropyl starch into the reactor, continue stirring to allow it to undergo a cross-linking reaction, and keep warm for 50 minutes to obtain a third mixture.
[0046] Step 6: Set the temperature of the reactor to 100°C, maintain the speed at 1800 r / min, and continue stirring for 60 minutes.
[0047] Then the temperature is lowered to 42° C., a preservative is added according to actual needs, the mixture is stirred until uniform, and the mixture is discharged to obtain a high molecular polymer film-forming agent.
[0048] During the preparation, water was added appropriately to maintain the total amount of polyester-5, hydroxypropyl starch and water at 100 kg.
[0049] The final high molecular polymer film-forming agent was sent for sample testing, and polyethylene glycol-8 was not detected, indicating that there was no residue.
[0050] Example 2 A high molecular polymer film-forming agent, which is different from Example 1 in that it comprises polyester-5, hydroxypropyl starch, and the balance is supplemented by water.
[0051] A method for preparing a high molecular polymer film-forming agent, which is different from Example 1 in that: Step 1: Add 74.9 kg of water into the reactor and heat to 80°C.
[0052] Step 2: Add 25 kg of polyester-5 multiple times (three times in this example) into the reactor and stir until it is completely dissolved to obtain a first mixture.
[0053] Step 3: After the first mixture is completely dissolved, keep warm for 35 minutes while stirring.
[0054] Step 4: Set the temperature of the reactor to 60°C, set the speed to 1800 r / min, add 0.03 kg of polyethylene glycol-8 into the reactor, and stir until it is completely dissolved to obtain a second mixture.
[0055] Step 5: Keep the rotation speed at 1800 r / min, add 0.1 kg of hydroxypropyl starch into the reactor, continue stirring to allow it to undergo a cross-linking reaction, and keep warm for 50 minutes to obtain a third mixture.
[0056] Step 6: Set the temperature of the reactor to 100°C, maintain the speed at 1800 r / min, and continue stirring for 60 minutes.
[0057] Then the temperature is lowered to 42° C., a preservative is added according to actual needs, the mixture is stirred until uniform, and the mixture is discharged to obtain a high molecular polymer film-forming agent.
[0058] During the preparation, water was added appropriately to maintain the total amount of polyester-5, hydroxypropyl starch and water at 100 kg.
[0059] The final high molecular polymer film-forming agent was sent for sample testing, and polyethylene glycol-8 was not detected, indicating that there was no residue.
[0060] Example 3 A high molecular polymer film-forming agent, which is different from Example 1 in that it comprises polyester-5, hydroxypropyl starch, and the balance is supplemented by water.
[0061] A method for preparing a high molecular polymer film-forming agent, which is different from Example 1 in that: Step 1: Add 64 kg of water into the reactor and heat to 80°C.
[0062] Step 2: Add 35 kg of polyester-5 multiple times (three times in this example) into the reactor and stir until it is completely dissolved to obtain a first mixture.
[0063] Step 3: After the first mixture is completely dissolved, keep warm for 35 minutes while stirring.
[0064] Step 4: Set the temperature of the reactor to 60°C, set the speed to 1800 r / min, add 0.8 kg of polyethylene glycol-8 into the reactor, and stir until it is completely dissolved to obtain a second mixture.
[0065] Step 5: Keep the rotation speed at 1800 r / min, add 1 kg of hydroxypropyl starch into the reactor, continue stirring to allow it to undergo a cross-linking reaction, and keep warm for 50 minutes to obtain a third mixture.
[0066] Step 6: Set the temperature of the reactor to 100°C, maintain the speed at 1800 r / min, and continue stirring for 60 minutes.
[0067] Then the temperature is lowered to 42° C., a preservative is added according to actual needs, the mixture is stirred until uniform, and the mixture is discharged to obtain a high molecular polymer film-forming agent.
[0068] During the preparation, water was added appropriately to maintain the total amount of polyester-5, hydroxypropyl starch and water at 100 kg.
[0069] The final high molecular polymer film-forming agent was sent for sample testing, and polyethylene glycol-8 was not detected, indicating that there was no residue.
[0070] Example 4 A method for preparing a high molecular polymer film-forming agent, which is different from Example 1 in that polyethylene glycol-8 is replaced by polyethylene glycol-4000.
[0071] The performance of high molecular weight polyethylene glycol-4000 is already very stable and cannot induce cross-linking reaction between polyester-5 and hydroxypropyl starch, so high molecular weight polymer film-forming agent cannot be prepared.
[0072] Example 5 A method for preparing a high molecular polymer film-forming agent, which is different from Example 1 in that the rotation speed of step 4, step 5 and step 6 is 500 r / min.
[0073] The final high molecular polymer film-forming agent was sent for sample testing, and polyethylene glycol-8 was not detected, indicating that there was no residue.
[0074] Example 6 A method for preparing a high molecular polymer film-forming agent, which is different from Example 1 in that the amount of polyethylene glycol-8 used is 1 kg.
[0075] The final high molecular polymer film-forming agent was sent for sample testing, and polyethylene glycol-8 was detected at 0.05%, with a small amount of residue.
[0076] Comparative Example Comparative Example 1 A method for preparing a high molecular polymer film-forming agent, which is different from Example 1 in that: Step 1: Add 69.2 kg of water into the reactor and heat to 80°C.
[0077] Step 2: Add 30 kg of polyester-5 multiple times (three times in this comparative example) into the reactor and stir until it is completely dissolved to obtain a first mixture.
[0078] Step 3: After the first mixture is completely dissolved, keep warm for 35 minutes while stirring.
[0079] Step 4: Set the temperature of the reactor to 100° C., set the rotation speed to 1800 r / min, add 0.5 kg of polyethylene glycol-8 into the reactor, and stir until it is completely dissolved to obtain a second mixture.
[0080] Step 5: Keep the rotation speed at 1800 r / min, add 0.8 kg of hydroxypropyl starch into the reactor, continue stirring to allow it to undergo a cross-linking reaction, and keep warm for 50 minutes to obtain a third mixture.
[0081] Step 6: Maintain the temperature of the reactor at 100°C, maintain the rotation speed at 1800 r / min, and continue stirring for 60 minutes.
[0082] Then the temperature is lowered to 42° C., and the material is discharged to obtain a high molecular polymer film-forming agent.
[0083] During the preparation, water was added appropriately to maintain the total amount of polyester-5, hydroxypropyl starch and water at 100 kg.
[0084] The final high molecular polymer film-forming agent was sent for sample testing, and polyethylene glycol-8 was not detected, indicating that there was no residue.
[0085] Comparative Example 2 A method for preparing a high molecular polymer film-forming agent, which is different from Example 1 in that: Step 1: Add 69.2 kg of water into the reactor and heat to 80°C.
[0086] Step 2: Add 0.8 kg of hydroxypropyl starch into the reactor and stir until it is completely dissolved to obtain a first mixture.
[0087] Step 3: After the first mixture is completely dissolved, keep warm for 35 minutes while stirring.
[0088] Step 4: Set the temperature of the reactor to 60°C, set the speed to 1800 r / min, add 0.5 kg of polyethylene glycol-8 into the reactor, and stir until it is completely dissolved to obtain a second mixture.
[0089] Step 5: Keep the rotation speed at 1800 r / min, add 30 kg of polyester-5 (three times in this comparative example) into the reactor, continue stirring to allow it to undergo a cross-linking reaction, and keep warm for 50 minutes to obtain a third mixture.
[0090] Step 6: Set the temperature of the reactor to 100°C, maintain the speed at 1800 r / min, and continue stirring for 60 minutes.
[0091] Then the temperature is lowered to 42° C., and the material is discharged to obtain a high molecular polymer film-forming agent.
[0092] The final high molecular polymer film-forming agent was sent for sample testing, and polyethylene glycol-8 was not detected, indicating that there was no residue.
[0093] Performance testing 1. Makeup lasting effect test: (1) Preparation of test samples: The test sample is composed of the following components: 1% butylene glycol, 0.5% p-hydroxyacetophenone, 0.03% EDTA-disodium, 5.5% high molecular polymer film-forming agent, 1.5% ethanol, 0.5% hexylene glycol, and water is used to make up the balance to 100%.
[0094] The high molecular polymer film-forming agent is the high molecular polymer film-forming agent of Examples 1-3, Examples 5-6, Comparative Examples 1-2 or the commercially available aqueous film-forming agent 803.
[0095] The method for preparing the test sample comprises the following steps: Add water, butylene glycol, p-hydroxyacetophenone and disodium EDTA into an emulsifying pot, heat to 80°C, keep warm for 10 minutes, then stir and cool to below 35°C; Then continue to add high molecular polymer film-forming agent, ethanol and hexylene glycol, stir until dispersed evenly, and obtain the test sample.
[0096] (2) Selection of volunteers: 80 female volunteers aged 25-30 were selected and randomly divided into 8 groups, with 10 people in each group, and each group corresponded to one test sample.
[0097] (3) Detection method: The volunteers used the corresponding test samples with a test time of 8 hours, spending 20 minutes outdoors at noon and the rest of the time indoors.
[0098] Indoor temperature is 29℃ and humidity is 62%; outdoor temperature is 36℃ and humidity is 55%.
[0099] Instructions for using the test sample: After cleansing with water, spray toner. After the toner is dry, apply makeup with isolation, liquid foundation, and loose powder in sequence, and then spray the test sample evenly on the entire face. The amount of test sample to be used is 5 sprays, and the timing begins after the film is completely formed.
[0100] After the experiment, the volunteers' faces were observed with the naked eye and the makeup-setting effect was scored on a scale of 0-10. The closer to 10 the score, the more complete the makeup and the less obvious the makeup coming off. The closer to 0 the score, the more mottled and incomplete the makeup and the more severe the makeup coming off.
[0101] The average score of volunteers in the same group is the result of that group.
[0102] The results are recorded in Table 1.
[0103] Table 1 According to the data in Table 1, the test samples of Examples 1-3 and 5-6 have better makeup-setting effects than the test sample using the commercially available aqueous film-forming agent 803.
[0104] Two volunteers who used the test samples of Example 1 used the VISIA skin detector to take pictures of their faces. Figure 1 , 2 , from left to right are the initial state of timing, the state of timing 2h, the state of timing 4h (during 20min of outdoor activities), the state of timing 6h and the state of timing 8h.
[0105] from Figure 1 It can be seen that the makeup has basically not fallen off and is very adherent.
[0106] Figure 2 At each moment in the experiment, the volunteers' makeup hardly changed. Due to outdoor activities during the experiment, a small amount of oil was observed on the volunteers' cheeks in the 4-hour timed state diagram, but the effect on their makeup was minor.
[0107] 2. Anti-scratch detection: (1) Preparation of test samples: The test samples consisted of the following components: Phase A: 3% BENTONEGELVS-5PCV, 6% RB 22 (containing cyclopentasiloxane and trimethylsiloxysilicate), 1% bis-hydroxyethoxypropyl dimethicone / IPDI copolymer urethane, 2% Skinsens PG-9400; Phase B: 8.4% Sensation CR-5000HD, 3.6% Caprylyl Methicone; Phase C: 10% Sensation CN-1820HD, 2% Skinsens HT-5000, 1% Cetyl PEG / PPG-10 / 1 Dimethicone, 2% Diethylhexyl Sebacate, 2% PEG-10 Dimethicone, 12% Cyclopentasiloxane; Phase D: 0.504% ALT-MTY-10 (CI 77492 and Triethoxycaprylylsilane), 0.112% ALT-MTRX-10 (CI 77491 and Triethoxycaprylylsilane), 0.03% ALT-MTB-10 (CI 77499 and Triethoxycaprylylsilane), 0.514% Caprylyl Methicone; Phase E: 5% isododecane, water, 12% polymer film former, 4% butanediol; Phase G: 1.5% 1,2-pentanediol, 0.4% phenoxyethanol, 0.03% fragrance; Phase H: 2% ethanol, 7.4% polydimethylsiloxane; The water in phase E is made up to 100%.
[0108] The high molecular polymer film-forming agent is the high molecular polymer film-forming agent of Examples 1-3, Examples 5-6, and Comparative Examples 1-2.
[0109] The method for preparing the test sample comprises the following steps: Add phase A to the emulsifier and homogenize and disperse evenly; grind phase B / C / D with three rollers to less than 10μm, add phase E to the emulsifier and homogenize and disperse evenly; Put phase F into the water phase pot and stir until it becomes transparent; Start stirring the emulsifier, pump phase F into the emulsifier for emulsification, stir and disperse evenly, and homogenize for 5-8 minutes; Add phase G and phase H into the emulsifying pot, homogenize for 3-5 minutes, and discharge the material after passing the inspection to obtain the test sample.
[0110] (2) Mark the test area on the arm, apply the test sample on the test area, wait for 3 minutes for film formation, and perform the following tests: 【1】Place the black card paper on the corresponding test area of the arm and gently rub it to observe whether the test sample adheres to the surface of the black card paper. Record the test results in Table 2.
[0111] 【2】Place the phone screen on the corresponding test area of the arm and gently wipe it to observe whether the test sample adheres to the surface of the phone screen. Record the test results in Table 2.
[0112] Table 2 According to the test results in Table 2, the test products of Examples 1-3 and 5-6 can form films quickly and are not easy to adhere to arms or mobile phone screens.
[0113] Reference Figure 3 , which is the test result diagram of [1], with the competitor product on the left and the test sample of Example 1 on the right.
[0114] Reference Figure 4 , which is the test result diagram of [2], with the competitor product on the left and the test sample of Example 1 on the right.
[0115] 3. Sensory evaluation: Questionnaires were distributed to volunteers who underwent makeup-lasting effect testing, and they were asked to rate the freshness and comfort on a scale of 0-10. The closer the score is to 10, the more refreshing and less greasy it is / the more comfortable, less tight and less burdensome it is.
[0116] The average score of the volunteers in the same group is taken as the group data and recorded in Table 3.
[0117] Table 3 According to the test results in Table 3, the volunteers who used the test samples of Examples 1-3 and 5 were very satisfied with the products, which were refreshing, non-greasy, highly comfortable, and had good film-forming effects.
[0118] In summary, the film-forming agent prepared in this application is used in downstream products. Its strong makeup-holding ability allows the makeup to fit closely to the skin. Even in high temperature or sweaty environments, it can keep the makeup lasting and fresh, avoiding the sticky feeling that traditional products may bring. The special cross-linking structure also gives the downstream cosmetics a soft film-forming effect, making the skin feel more delicate and smooth, and significantly improving the skin feel.
[0119] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high molecular polymer film-forming agent, characterized in that: According to mass percentage, the following raw materials are included: 25-35% polyester-5, 0.1-1% hydroxypropyl starch, and water.
2. The high molecular polymer film-forming agent according to claim 1, characterized in that: According to mass percentage, the high molecular polymer film-forming agent includes the following raw materials: 30% polyester-5, 0.8% hydroxypropyl starch, and water.
3. A method for preparing a high molecular polymer film-forming agent according to any one of claims 1 to 2, characterized in that: The following steps are involved: Step 1: The water is heated to 75-85° C., and the polyester-5 is mixed with the water until the polyester-5 is completely dissolved to obtain a first mixture; Step 2: Cool the first mixture to 55-65° C., add polyethylene glycol-8, and mix until completely dissolved to obtain a second mixture; Step 3: continuously stirring the hydroxypropyl starch and the second mixture to allow a cross-linking reaction to occur, and heat-retaining the mixture for 40-60 minutes to obtain a third mixture; Step 4: heating the third mixture to 95-105° C. for 30-90 min to obtain a high molecular polymer film-forming agent.
4. The method for preparing a high molecular polymer film-forming agent according to claim 3, characterized in that: The usage amount of the polyethylene glycol-8 is 0.03-0.8% of the total mass of the high molecular polymer film-forming agent.
5. The method for preparing a high molecular polymer film-forming agent according to claim 4, characterized in that: The usage amount of the polyethylene glycol-8 is 0.2-0.5% of the total mass of the high molecular polymer film-forming agent.
6. The method for preparing a high molecular polymer film-forming agent according to claim 3, characterized in that: In the step 1, polyester-5 is added in multiple times and mixed with water.
7. The method for preparing a high molecular polymer film-forming agent according to claim 3, characterized in that: In step 2, step 3 and step 4, the rotation speed is 1500-2000r / min.
Citation Information
Patent Citations
Preparation method of film forming agent and impregnating compound containing film forming agent
CN101831078A
Thin film mask pack having excellent wear sensation, electrical conductivity and antibacterial property, and manufacturing method therefor
CN111867422A
High-molecular polymer film-forming agent, preparation method thereof and makeup fixing spray
CN115068359A
Macromolecular gel for improving silky touch as well as preparation method and application of macromolecular gel
CN117567864A
Cited By
Film-forming composition and preparation method thereof, film-forming agent, application and cosmetics
CN121512885A