Ferroelectric film material and preparation method and application thereof
By controlling the doping amount of Bi(Mg0.5Zr0.5)O3 in ferroelectric film materials, the microstructure is improved, and the problems of low energy storage density and efficiency of capacitors are solved, and the improvement of high energy storage density and efficiency is achieved. In advanced electronic power systems.
Patent Information
- Application Number
- CN202411523748.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The energy storage density and energy storage efficiency of existing capacitors are low, making it difficult to meet the needs of advanced electronic power systems for miniaturization, lightweight, integration and low cost. In particular, the energy storage density of inorganic thin film capacitors is limited by volume, and The organic thick film has poor stability in moisture and high temperatures.
The chemical formula of the ferroelectric film material is (1-x)Na0.5Bi0.5TiO3-xBi (Mg0.5Zr0.5)O3. By controlling the range of x to 0≤0.3, the microstructure characteristics are improved and the grains are refined. , break the long-range ferroelectric domain, reduce the polarization conversion barrier and polarization lag, and improve energy storage density and energy storage efficiency.
It effectively improves the energy storage density and energy storage efficiency of ferroelectric film materials, reduces the residual polarization value and coercive electric field, improves the stability and performance of the material, and is suitable for the dielectric layer of capacitors.
Smart Images

Figure CN119038992A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of materials, and in particular to a ferroelectric film material and a preparation method and application thereof. Background Art
[0002] Capacitors have become important devices in advanced electronic power systems due to their fast charging and discharging speeds and high power density. According to the type of dielectric material, capacitors can be divided into inorganic thin film capacitors, inorganic thick film capacitors, inorganic bulk ceramic capacitors and organic thick film capacitors. Energy storage density and energy storage efficiency are key parameters for measuring the energy storage performance of capacitors, and are closely related to the properties of dielectric materials (such as dielectric constant, polarization characteristics, and breakdown field strength).
[0003] Among all types of capacitors, inorganic bulk ceramic capacitors have a relatively large total energy storage density, but the breakdown field strength of inorganic bulk ceramic materials is limited by its thickness and the presence of many defects in the material body, making it difficult to further increase the total energy storage density. Film materials are much smaller in volume than bulk ceramic materials, and can better meet the needs of today's electronic power devices to develop in a lighter, thinner and more miniaturized direction. For organic thick film capacitors, organic thick films have the advantages of high breakdown voltage, light weight and flexibility, but their dielectric constant is very low, and they need to be in extremely high electric fields to achieve a high energy storage density, and their working stability is poor under humidity, high temperature and ultraviolet radiation. For inorganic thin film capacitors, inorganic thin film materials (for example, film thickness <1μm) are limited by their volume, and the total energy storage density is small, which makes it difficult to meet the energy supply needs of the device. For inorganic thick film capacitors, inorganic thick film materials (for example, film thickness >1μm), although the thickness of the film material is appropriately increased, so that the energy storage density is increased, the increase in film thickness is prone to increase defects in the film layer and the film layer is prone to cracking.
[0004] At present, capacitors have relatively small energy storage capacity compared to electrochemical energy storage devices (such as batteries), which hinders the development of advanced electronic power systems towards miniaturization, lightness, integration and low cost. Therefore, how to improve the energy storage density and efficiency of dielectric materials has always been an urgent problem to be solved in the industry. Summary of the invention
[0005] In view of this, the embodiments of the present application provide a ferroelectric film material and a preparation method and application thereof to solve at least one problem existing in the background technology.
[0006] In a first aspect, the present invention provides a ferroelectric film material, wherein the chemical formula of the ferroelectric film material is (1-x)Na 0.5 Bi 0.5 TiO3-xBi(Mg 0.5 Zr 0.5)O3, where 0 <x≤0.3。
[0007] In conjunction with the first aspect of the present application, in an optional implementation manner, 0.15≤x≤0.3.
[0008] In combination with the first aspect of the present application, in an optional implementation manner, the thickness of the ferroelectric film material is 1.1 μm to 4 μm.
[0009] In a second aspect, an embodiment of the present application provides a method for preparing a ferroelectric film material, the method comprising the following steps: S1: Preparation of Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 ) O3 colloid; S2: The Na 0.5 Bi 0.5 TiO3 colloid and the Bi(Mg 0.5 Zr 0.5 ) O3 colloid, adding additives and stirring, and obtaining the ferroelectric film material after spin coating and heat treatment, wherein the additives include polyvinyl pyrrolidone and / or polyvinyl alcohol, the Na 0.5 Bi 0.5 TiO3 colloid and the Bi(Mg 0.5 Zr 0.5 ) The molar ratio of O3 colloid is (1-x):x, where 0 <x≤0.3。
[0010] In conjunction with the second aspect of the present application, in an optional embodiment, the preparation of the Na 0.5 Bi 0.5 TiO3 colloid methods include: A sodium source and a bismuth source are dissolved in a first solvent and stirred to form a first colloid; acetylacetone is added to the first colloid and stirred to form a second colloid; a titanium source and deionized water are added to the second colloid and stirred to form the Na 0.5 Bi 0.5 TiO3 colloid.
[0011] In conjunction with the second aspect of the present application, in an optional implementation manner, the method satisfies at least one of the following features: (1) The sodium source includes sodium acetate trihydrate and / or sodium acetate; (2) The bismuth source includes at least one of bismuth nitrate pentahydrate, bismuth acetate, and bismuth subnitrate; (3) the first solvent includes at least one of acetic acid, ethylene glycol methyl ether, and ethylene glycol; (4) The titanium source includes titanium isopropoxide and / or titanium n-propoxide; (5) The temperature for forming the first colloid is 90°C to 100°C; (6) The stirring time for forming the first colloid is 25 min to 30 min; (7) The acetylacetone and the Na 0.5 Bi 0.5 The molar concentration ratio of TiO3 colloid is 1.2:1~1.5:1; (8) The stirring time for forming the second colloid is 20 min to 30 min; (9) The volume ratio of the deionized water to the first solvent is 1:4 to 1:5; (10) Formation of the Na 0.5 Bi 0.5 The stirring time of TiO3 colloid is 20min~30min.
[0012] In conjunction with the second aspect of the present application, in an optional embodiment, the preparation of the Bi(Mg 0.5 Zr 0.5 ) O3 colloid method, comprising: A magnesium source and a bismuth source are dissolved in a second solvent and stirred to form a third colloid; acetylacetone is added to the third colloid and stirred to form a fourth colloid; a zirconium source and deionized water are added to the fourth colloid and stirred to form the Bi(Mg 0.5 Zr 0.5 )O3 colloid.
[0013] In conjunction with the second aspect of the present application, in an optional implementation manner, the method satisfies at least one of the following features: (1) The magnesium source includes magnesium acetate tetrahydrate and / or magnesium acetate; (2) The bismuth source includes at least one of bismuth nitrate pentahydrate, bismuth acetate, and bismuth subnitrate; (3) the second solvent comprises at least one of acetic acid, ethylene glycol methyl ether and ethylene glycol; (4) The zirconium source includes zirconium isopropoxide and / or zirconium n-propoxide; (5) The temperature for forming the third colloid is 90° C. to 100° C.; (6) The stirring time for forming the third colloid is 25 min to 30 min; (7) The acetylacetone and the Bi(Mg 0.5 Zr 0.5 ) The molar concentration ratio of O3 colloid is 1.2:1~1.5:1; (8) The stirring time for forming the fourth colloid is 20 min to 30 min; The volume ratio of the deionized water to the second solvent is 1:4 to 1:5; (10)To form the Bi(Mg 0.5 Zr 0.5 )O3 colloid, the stirring time is 20 min to 30 min.
[0014] Combined with the second aspect of the present application, in an alternative embodiment, step S2 satisfies at least one of the following features: (1)The polyvinylpyrrolidone includes polyvinylpyrrolidone-K30; (2)0.15 ≤ x ≤ 0.3; (3)The thickness of the ferroelectric film material is 1.1 μm to 4 μm.
[0015] In a third aspect, the embodiments of the present application provide an application of the ferroelectric film material described in any item of the first aspect or the ferroelectric film material prepared by the preparation method described in any item of the second aspect in a capacitor.
[0016] Compared with the prior art, the embodiments of the present application have the following beneficial effects: For the ferroelectric film material, its preparation method and application provided by the embodiments of the present application, the chemical general formula of the ferroelectric film material is (1 - x)Na 0.5 Bi 0.5 TiO3 - xBi(Mg 0.5 Zr 0.5 )O3, where 0 < x ≤ 0.3. The ferroelectric film material in the embodiments of the present application is composed of Na 0.5 Bi 0.5 TiO3 and Bi(Mg 0.5 Zr 0.5 )O3 with a molar ratio of (1 - x):x. By controlling the range of x to be greater than 0 and less than or equal to 0.3, the microscopic structural characteristics of the ferroelectric film material are improved, the grains are disordered and refined, the domain structure in the ferroelectric film material becomes blurred, the long-range ferroelectric domains are broken, so the polarization conversion barrier is reduced and the polarization hysteresis is reduced, making the remanent polarization value and the coercive electric field of the ferroelectric film material decrease, thereby effectively improving the energy storage density and energy storage efficiency of the ferroelectric film material.
[0017] The additional aspects and advantages of the present application will be partially given in the following description, partially become obvious from the following description, or be understood through the practice of the present application. Description of the Drawings
[0018] The drawings described herein are used to provide a further understanding of the present application, and constitute a part of the present application. The schematic embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation to the present application. In the drawings: Figure 1 A schematic diagram of a process for preparing a ferroelectric film material provided in an embodiment of the present application; Figure 2 XRD diagrams of the ferroelectric film materials prepared in Example 1, Example 2 and the comparative example; Figure 3 is an atomic force microscope morphology image of the ferroelectric film material prepared in the comparative example; Figure 4 This is an atomic force microscope morphology image of the ferroelectric film material prepared in Example 1; Figure 5 This is an atomic force microscope morphology image of the ferroelectric film material prepared in Example 2; Figure 6 hysteresis loop diagram of the ferroelectric film materials prepared in Example 1, Example 2 and Comparative Example at a field strength of 1200 kV / cm; Figure 7 The diagram is a change diagram of energy storage density of the ferroelectric film materials prepared in Example 1, Example 2 and the comparative example under a field strength from 100 kV / cm to 1200 kV / cm; Figure 8 This is a graph showing the change in energy storage efficiency of the ferroelectric film materials prepared in Example 1, Example 2 and the comparative example under a field strength ranging from 100 kV / cm to 1200 kV / cm. DETAILED DESCRIPTION
[0019] In order to make the technical scheme and beneficial effects of the present invention more obvious and easy to understand, the following is described in detail by combining the accompanying drawings and listing specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on conventional experimental conditions. The reagents and raw materials used in the present invention are commercially available unless otherwise specified.
[0020] In the following description, a large number of specific details are given to provide a more thorough understanding of the present application. However, it is obvious to those skilled in the art that the present application can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present application, some technical features known in the art are not described; that is, all features of the actual embodiments are not described here, and well-known functions and steps are not described in detail.
[0021] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be limiting of the present application. When used herein, the singular forms "a", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. The terms "consisting of" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.
[0022] In order to thoroughly understand the present application, detailed steps and detailed structures will be presented in the following description to illustrate the technical solution of the present application. The preferred embodiments of the present application are described in detail below, but in addition to these detailed descriptions, the present application may also have other implementation methods.
[0023] Unless otherwise defined, technical and scientific terms used in this application have the same meanings as those in the technical field to which this application belongs.
[0024] If no specific techniques or conditions are specified in the following examples, the conventional techniques or conditions described in the literature in the art, or the conditions recommended by the product instructions and the manufacturer are generally used. The numerical ranges in the following examples all include the endpoint values.
[0025] Energy storage density of dielectric (W rec ) depends on its dielectric polarization (P) in an applied electric field (E) and is calculated as:
[0026] Among them, P max and P r are the saturation polarization value and remanent polarization value of the hysteresis loop, respectively.
[0027] The energy storage efficiency of the dielectric can be expressed by η, and the calculation formula of η is:
[0028] Among them, W loss It refers to the energy stored in the dielectric through charging but not released externally. This energy will be lost as Joule heat during the charging and discharging process.
[0029] From the above formulas (1-1) and (1-2), we can know that P r Reducing the coercive electric field can improve the η of the dielectric. Therefore, it is necessary to pursue a large P max , Xiao P r and high breakdown electric field to achieve high W rec , in Pr Low enough while reducing the coercive field to achieve high η.
[0030] In the related art, in order to improve the energy storage density of the dielectric, nonlinear ferroelectric dielectrics with large spontaneous polarization are selected, such as BiFeO3, BaTiO3 and Pb(ZrTi)O3. However, although BiFeO3 and BaTiO3 have large spontaneous polarization values, their remanent polarization values are also large, which makes their η very low. Although Pb(ZrTi)O3 has a large spontaneous polarization value and a small remanent polarization value, it is a lead-containing component, which is extremely harmful to the environment and greatly limits its application. (NaBi)TiO3, as a lead-free ferroelectric material, has both a high spontaneous polarization value and a low remanent polarization value, and is suitable for use as a dielectric material, but the energy storage density and energy storage efficiency of dielectrics containing a single (NaBi)TiO3 component still need to be further improved.
[0031] Based on this, the present invention provides a ferroelectric film material, the chemical formula of which is (1-x)Na 0.5 Bi 0.5 TiO3-xBi(Mg 0.5 Zr 0.5 )O3, where 0 <x≤0.3。
[0032] Na 0.5 Bi 0.5 TiO3 is a lead-free material with high safety. The ferroelectric film material in the embodiment of the present application is composed of Na 0.5 Bi 0.5 TiO3 and Bi (Mg 0.5 Zr 0.5 )O3 composition, by controlling the range of x to be greater than 0 and less than or equal to 0.3, that is, by adding an appropriate amount of Bi(Mg 0.5 Zr 0.5 ) O3 and Na 0.5 Bi 0.5 TiO3 composite improves the microstructural characteristics of the ferroelectric film material, makes the grains disordered and refined, blurs the domain structure in the ferroelectric film material, breaks the long-range ferroelectric domain, thereby lowering the polarization conversion barrier and polarization hysteresis, and reducing the residual polarization value and coercive electric field of the ferroelectric film material, thereby effectively improving the energy storage density and efficiency of the ferroelectric film material.
[0033] In the chemical formula of the above ferroelectric film material, the x value represents the Na 0.5 Bi 0.5 Bi (Mg doped in TiO3 0.5 Zr 0.5)O3, when x value is large, for example, greater than 0.3, Bi(Mg 0.5 Zr 0.5 ) A large amount of O3 doping is not conducive to reducing the residual polarization value and coercive electric field of the ferroelectric film material, and is not conducive to reducing the energy storage density and energy storage efficiency of the material. Therefore, in this embodiment, the value of x is controlled within 0.3, and x can be, for example, 0.1, 0.15, 0.2, 0.25, 0.3 or any value between any two of the above value ranges. In this way, the energy storage density and energy storage efficiency of the ferroelectric film material can be effectively improved.
[0034] When the x value is small, Bi (Mg 0.5 Zr 0.5 ) The amount of O3 is small, the residual polarization value and coercive electric field of the ferroelectric film material are not significantly reduced, and the effect on improving the energy storage density and energy storage efficiency of the material is limited. Therefore, in some specific embodiments, 0.15≤x≤0.3. This can better improve the energy storage density and energy storage efficiency of the ferroelectric film material.
[0035] The thickness of the ferroelectric film material in the embodiment of the present application can be 1.1μm to 4μm. The ferroelectric film material within this thickness range can be called a ferroelectric thick film. This can make the energy storage density of the ferroelectric film material higher. At the same time, it can avoid the problem that the ferroelectric film material is too thick and prone to more defects, which in turn leads to a decrease in the quality of the film layer and affects the energy storage performance of the material.
[0036] The present application also provides a method for preparing a ferroelectric film material. Figure 1 The method for preparing the ferroelectric film material provided in the embodiment of the present application comprises the following steps: S1: Preparation of Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 ) O3 colloid; S2: Put Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 ) O3 colloid, adding additives and stirring, and obtaining a ferroelectric film material after spin coating and heat treatment, wherein the additives include polyvinyl pyrrolidone and / or polyvinyl alcohol, Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 ) The molar ratio of O3 colloid is (1-x):x, where 0 <x≤0.3。
[0037] In the present embodiment, the molar ratio of Na0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 )O3 colloid is mixed to prepare ferroelectric film materials. By controlling the range of x to be greater than 0 and less than or equal to 0.3, the microstructural characteristics of the prepared ferroelectric film materials are improved, the grains are disordered and refined, the domain structure in the ferroelectric film materials becomes blurred, and the long-range ferroelectric domains are broken, thereby reducing the polarization conversion barrier and polarization hysteresis, and reducing the residual polarization value and coercive electric field of the ferroelectric film materials, thereby effectively improving the energy storage density and energy storage efficiency of the ferroelectric film materials. In addition, in Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 ) Adding additives including polyvinyl pyrrolidone and / or polyvinyl alcohol after mixing the O3 colloid can increase the viscosity of the colloid, facilitate the preparation of a ferroelectric film material with higher density through the colloid, and can reduce the crystallization temperature and increase the breakdown electric field of the ferroelectric film material, thereby further improving the energy storage density and energy storage efficiency.
[0038] Preparation of Na in step S1 0.5 Bi 0.5 The method for preparing TiO3 colloid may include: dissolving a sodium source and a bismuth source in a first solvent and stirring to form a first colloid; adding acetylacetone to the first colloid and stirring to form a second colloid; adding a titanium source and deionized water to the second colloid and stirring to form a Na 0.5 Bi 0.5 TiO3 colloid. This can produce transparent and stable high-quality Na 0.5 Bi 0.5 TiO3 colloid.
[0039] "Sodium source" refers to a compound for providing sodium. Exemplarily, the sodium source may include sodium acetate trihydrate and / or sodium acetate.
[0040] The "bismuth source" refers to a compound for providing bismuth. For example, the bismuth source may include at least one of bismuth nitrate pentahydrate, bismuth acetate, and bismuth subnitrate.
[0041] The "titanium source" is a compound for providing titanium. For example, the titanium source may include titanium isopropoxide and / or titanium n-propoxide.
[0042] The type of the first solvent is not particularly limited and can be selected according to actual needs. For example, the first solvent can include at least one of acetic acid, ethylene glycol methyl ether, and ethylene glycol.
[0043] As a specific example, in the actual preparation of Na 0.5 Bi 0.5When preparing TiO3 colloid, first, place the sodium source and bismuth source in a container (such as a beaker). It should be noted that because metallic sodium and metallic bismuth will volatilize under high temperature environment, 5%~10% excess should be weighed to compensate for the loss. Next, add the first solvent to the container and heat it to 90℃~100℃ in a water bath, stir for 25min~30min to obtain a clear first colloid, cool to room temperature, then add acetylacetone to the container, continue stirring for 20min~30min to obtain a stable light yellow second colloid, in which acetylacetone and Na 0.5 Bi 0.5 The molar concentration ratio of TiO3 colloid is 1.2:1~1.5:1, and then the titanium source is added to the container several times, stirred for 20min~30min, and deionized water is added several times during this process to obtain Na 0.5 Bi 0.5 The TiO3 colloid is stable in light yellow, wherein the volume ratio of deionized water to the first solvent is 1:4-1:5.
[0044] Preparation of Bi(Mg) in step S1 0.5 Zr 0.5 The method for preparing Bi(Mg)O3 colloid may include: dissolving a magnesium source and a bismuth source in a second solvent and stirring to form a third colloid; adding acetylacetone to the third colloid and stirring to form a fourth colloid; adding a zirconium source and deionized water to the fourth colloid and stirring to form Bi(Mg)O3 colloid. 0.5 Zr 0.5 )O3 colloid. This can produce transparent and stable high-quality Bi(Mg 0.5 Zr 0.5 )O3 colloid.
[0045] "Magnesium source" refers to a compound for providing magnesium. Exemplarily, the magnesium source may include magnesium acetate tetrahydrate and / or magnesium acetate.
[0046] The "bismuth source" refers to a compound for providing bismuth. For example, the bismuth source may include at least one of bismuth nitrate pentahydrate, bismuth acetate, and bismuth subnitrate.
[0047] The "zirconium source" is a compound for providing zirconium. For example, the zirconium source may include zirconium isopropoxide and / or zirconium n-propoxide.
[0048] The type of the second solvent is not particularly limited and can be selected according to actual needs. For example, the second solvent can include at least one of acetic acid, ethylene glycol methyl ether, and ethylene glycol.
[0049] As a specific example, in the actual preparation of Bi(Mg 0.5 Zr 0.5When preparing the Bi(Mg 0.5 Zr 0.5 )O3 colloid, first, put the magnesium source and bismuth source into a container (such as a beaker). It should be noted that since metallic bismuth will volatilize in a high-temperature environment, 5% - 10% should be weighed in excess to compensate for the loss. Then, add the second solvent to the container and heat it to 90°C - 100°C in a water bath, and stir for 25 min - 30 min to obtain a clear third colloid. Cool it to room temperature. Next, add acetylacetone to the container and continue to stir for 20 min - 30 min to obtain a stable light yellow fourth colloid. Among them, the molar concentration ratio of acetylacetone to Bi(Mg 0.5 Zr 0.5 )O3 colloid is 1.2:1 - 1.5:1. Then, add the zirconium source to the container in multiple portions and stir for 20 min - 30 min. During this process, add deionized water in multiple portions to make the obtained Bi(Mg
[0050] 步骤S2中首先制备Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 )O3 colloid, and then mix the two colloids, and obtain the ferroelectric film material after spin coating and heat treatment. The advantage of the preparation method in this embodiment is that the components of the colloid can be controlled more precisely, it is easy to mix and dope, the equipment used is simple, and the preparation cost is low. In addition, the colloid is also suitable for preparing film layers with uniform components and thicknesses on a large area, which is suitable for industrial production and has strong practicability.
[0051] The chemical general formula of the ferroelectric film material obtained in the embodiment of this application is (1 - x)Na 0.5 Bi 0.5 TiO3 - xBi(Mg 0.5 Zr 0.5 )O3, where 0 < x ≤ 0.3. In some specific embodiments, 0.15 ≤ x ≤ 0.3, for example, it can be 0.1, 0.15, 0.2, 0.25, 0.3 or any value between any two of the above numerical ranges. In this way, the energy storage density and energy storage efficiency of the ferroelectric film material can be better improved.
[0052] Adding polyvinyl pyrrolidone and / or polyvinyl alcohol in step S2 can increase the viscosity of the prepared colloid, facilitate the preparation of a ferroelectric film material with a higher density through the colloid, and can reduce the crystallization temperature, increase the breakdown electric field of the ferroelectric film material, thereby further improving the energy storage density and energy storage efficiency. Specifically, polyvinyl pyrrolidone can include polyvinyl pyrrolidone-K30, which can further improve the quality of the ferroelectric film material, thereby facilitating further improving the energy storage density and energy storage efficiency.
[0053] In step S2, Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 ) The molar concentration of the colloid formed by mixing the O3 colloid can be 0.2mol / L~0.35mol / L, for example, it can be 0.2mol / L, 0.25mol / L, 0.3mol / L, 0.35mol / L or any value between any two of the above numerical ranges. In this way, the quality of the ferroelectric film material obtained by subsequent spin coating and heat treatment can be higher, and it is suitable for making ferroelectric films with appropriate thickness and high quality, thereby better improving the energy storage density and energy storage efficiency.
[0054] The spin coating and heat treatment in step S2 may specifically include: firstly, mixing the uniformly mixed Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 ) O3 colloid is dropped onto the LaNiO3 bottom electrode and spin-coated. After the spin-coating, heat treatment is performed. The above spin-coating and heat treatment steps are repeated to prepare a ferroelectric film material of the required thickness.
[0055] As a specific example, the specific operation steps of spin coating and heat treatment in step S2 may be: 1) Place the substrate containing the LaNiO3 bottom electrode on the suction cup of the glue spreader and use a rubber dropper to absorb the mixed Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 )O3 colloid is dripped onto the LaNiO3 bottom electrode, and the bubbles are eliminated and the colloid is completely spread over the entire LaNiO3 bottom electrode before starting to coat the surface. The spin coating parameters of the coating machine are set to 3500rot / min~4000rot / min for 30s~40s.
[0056] 2) After each spin coating, heat treatment is required quickly. Place the substrate in a rapid heat treatment furnace, heat up to 150℃~180℃ for 1s and keep warm for 3min (dry the thick film to fully volatilize the organic solvent), then heat up to 450℃~480℃ for 2s and keep warm for 5min (to crystallize the thick film), then heat up to 700℃~750℃ for 4s and keep warm for 3min (to further grow the grains, fill the gaps between the grains and make the thick film denser).
[0057] 3) Repeat the spin coating and heat treatment steps in steps 1) and 2) until the thickness of the ferroelectric film material reaches 1.1 μm to 4 μm. After reaching the desired thickness, place the substrate including the bottom electrode and the ferroelectric film material in an annealing furnace and keep it at 700℃~750℃ for 8min~12min to make (1-x)Na 0.5 Bi 0.5 TiO3-xBi(Mg 0.5 Zr 0.5 ) The O3 grains grow further to fill the gaps in each film layer.
[0058] In some embodiments, the additive in step S2 further comprises formamide and / or dimethylformamide, and the stirring after adding the additive in step S2 comprises: adding the mixed Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 ) Add formamide and / or dimethylformamide to the O3 colloid, stir to form a fifth colloid; add polyvinyl pyrrolidone and / or polyvinyl alcohol to the fifth colloid, stir, spin-coat, and heat-treat to obtain a ferroelectric film material. The spin-coating and heat-treating processes here can be understood by referring to the spin-coating and heat-treating processes in the above implementation.
[0059] In this embodiment, formamide and / or dimethylformamide are also added in step S2, so that when the colloid is prepared into a ferroelectric film material by spin coating and heat treatment, the film layer can be effectively prevented from cracking during the heat treatment process, thereby further improving the quality of the prepared ferroelectric film material.
[0060] As a specific example, step S2 may include: first, Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5) O3 colloids are mixed and stirred for 5min~10min, then, formamide solution and / or dimethylformamide solution are added to the mixed colloid, and stirring is continued for 15min~20min to obtain an orange-yellow stable transparent fifth colloid, wherein the volume ratio of formamide and / or dimethylformamide to deionized water is 1:3~1:4, then, polyvinyl pyrrolidone is added to the fifth colloid in multiple times, and it should be noted that the next addition of polyvinyl pyrrolidone can be made only after all the polyvinyl pyrrolidone added once is completely dissolved, and stirring is continued for 2h~2.5h. During this process, attention should be paid to the change of the colloid volume in real time, and the third solvent and deionized water should be replenished in time until the volume of the colloid reaches the preset volume again, wherein the ratio of the third solvent to water can be 4:1~5:1, and the third solvent can, for example, include at least one of acetic acid, ethylene glycol methyl ether, and ethylene glycol.
[0061] It should be noted that before preparing the ferroelectric film material, it is usually necessary to determine the (1-x)Na 0.5 Bi 0.5 TiO3-xBi(Mg 0.5 Zr 0.5 )O3 molar concentration and volume, where (1-x)Na 0.5 Bi 0.5 TiO3-xBi(Mg 0.5 Zr 0.5 )O3 can be regarded as Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 ) The chemical composition of the mixed colloid formed by mixing O3 colloids is determined on this basis, and the addition amount of various raw materials is determined. The above-mentioned preset volume is the volume of colloid required for spin coating determined before preparation.
[0062] In some embodiments, the method for preparing the ferroelectric film material may further include: filtering the colloid before the spin coating and heat treatment steps. This can remove impurities in the colloid and further improve the quality of the colloid. Specifically, for example, a double-layer medium-speed filter paper can be used for filtration 2 to 3 times to obtain an orange-yellow transparent colloid.
[0063] In some embodiments, the method for preparing a ferroelectric film material may further include: after filtering the colloid, aging the colloid. This can further improve the stability of the colloid. Specifically, the temperature of the aging treatment can be 20°C to 24°C, for example, 20°C, 21°C, 22°C, 23°C, 24°C or any value between any two of the above numerical ranges. The humidity of the aging treatment can be 40% to 50%, for example, 40%, 45%, 50% or any value between any two of the above numerical ranges. The time of the aging treatment can be 36h to 48h, for example, 36h, 38h, 40h, 42h, 44h, 46h, 48h or any value between any two of the above numerical ranges.
[0064] The embodiments of the present application also provide the use of the ferroelectric film material described in any of the above embodiments or the ferroelectric film material prepared by the preparation method described in any of the above embodiments in a capacitor.
[0065] A capacitor usually includes a first electrode (also called a bottom electrode), a dielectric layer, and a second electrode (also called a top electrode) stacked in sequence. The ferroelectric film material described in any of the above embodiments or the ferroelectric film material obtained by the preparation method described in any of the above embodiments can be used to make the dielectric layer, so that the energy storage density and energy storage efficiency of the capacitor are relatively high.
[0066] In some embodiments, the thickness of the ferroelectric film material described in any of the above embodiments or the ferroelectric film material prepared by the preparation method described in any of the above embodiments can be 1.1μm~4μm, and the dielectric within this thickness range can be called a dielectric thick film, which can make the energy storage density of the capacitor higher and avoid the problem of reduced film quality due to more defects caused by excessive thickness of the dielectric layer.
[0067] It can be understood that, in the ferroelectric film material described in any of the above embodiments or the ferroelectric film material prepared by the preparation method described in any of the above embodiments, by 0.5 Bi 0.5 TiO3 is doped with an appropriate amount of Bi (Mg 0.5 Zr 0.5 )O3, which improves the microstructure of the ferroelectric film material, makes the grains disordered and refined, the domain structure in the ferroelectric film material becomes blurred, and breaks the long-range ferroelectric domain. Therefore, the above-mentioned dielectric thick film can also be called a high-entropy bismuth-based dielectric thick film.
[0068] Taking the preparation of capacitors as an example, the application of the ferroelectric film material described in any of the above embodiments or the ferroelectric film material prepared by the preparation method described in any of the above embodiments in capacitors is further described below.
[0069] The steps of preparing the capacitor include cutting and cleaning the substrate, preparing the LaNiO3 bottom electrode, preparing the dielectric layer and preparing the top electrode. Specifically: The cutting and cleaning of the substrate includes: selecting a substrate (for example, a Pt-plated silicon oxide wafer), cutting the substrate into a certain size (for example, 0.9 cm×0.9 cm) for standby use. During the cutting process, the substrate is exposed to the air and is easily attached with impurities such as oil stains, dust, and organic matter. In the initial crystallization growth and film formation stage of the subsequent colloid, the cleanliness of the surface provided by the substrate is very important. In order to ensure that the colloid is further spin-coated on the initial film to increase the film thickness and ensure the film quality, the substrate cleaning process is inevitable, wherein the cleaning process can be: 1) placing the cut substrate in an ultrasonic cleaning machine filled with acetone for ultrasonic cleaning for 25min~30min; 2) draining the acetone in the ultrasonic cleaning machine, adding ethanol, and then ultrasonic cleaning for 25min~30min; 3) draining the ethanol in the ultrasonic cleaning machine, adding deionized water, and continuing ultrasonic cleaning for 25min~30min; 4) using a nitrogen gun to blow dry the deionized water, and placing the substrate in a rapid thermal treatment furnace to heat up to a certain temperature (for example, 500°C) to further dry the substrate and remove residual organic matter.
[0070] The preparation of LaNiO3 bottom electrode includes: preparing LaNiO3 colloid, using a coating machine to spin-coat the colloid onto a clean substrate, and then performing heat treatment to crystallize the colloid into a film. The specific operation steps are as follows:
[0071] 1) Weigh lanthanum nitrate and nickel acetate in a molar ratio of 1:1, weigh acetic acid and deionized water in a mass ratio of 5:1~5:2, and add them to a beaker to make the concentration of the mixed solution reach 0.2mol / L~0.4mol / L. Place the beaker in a magnetic stirring water bath and stir at 90℃~110℃ for 20min~30min.
[0072] 2) Take out the beaker, wait for the mixed solution to cool to room temperature, add formamide to the mixed solution at a molar ratio of 1:25-1:30, continue stirring for 20 minutes, and obtain a transparent green colloid.
[0073] 3) After the colloid obtained in the previous step is aged for 36 h to 48 h, it is filtered into a narrow-mouthed bottle by stacking 4 layers of medium-speed filter paper to complete the preparation of LaNiO3 colloid.
[0074] 4) The LaNiO3 bottom electrode is prepared by spin coating, for example, the cleaned substrate is placed on the suction cup of a coating machine, and the LaNiO3 colloid is sucked and dropped onto the substrate using a rubber-tipped dropper, and the coating is started after all bubbles are eliminated and the colloid is completely spread over the entire substrate. The spin coating parameters of the coating machine are set to 3500 rot / min~4000 rot / min for 30s~40s.
[0075] 5) After each spin coating, heat treatment is required quickly, for example, the substrate is placed in a rapid heat treatment furnace, the temperature is raised to 150℃~180℃ for 1s and kept for 3min (to dry the thick film and fully volatilize the organic solvent), then the temperature is raised to 450℃~480℃ for 2s and kept for 5min (to crystallize the thick film), and then the temperature is raised to 700℃~750℃ for 4s and kept for 3min (to further grow the grains, fill the gaps between the grains and make the thick film denser).
[0076] 6) Repeat the spin coating and heat treatment steps in steps 4) and 5) until the thickness of the LaNiO3 bottom electrode reaches 120nm~200nm. After reaching the required thickness, place the substrate including the bottom electrode into an annealing furnace and keep it at 700℃~750℃ for 8min~12min to allow the LaNiO3 grains to grow further to fill the gaps in each layer of the film.
[0077] The preparation steps of the dielectric layer can refer to the above embodiment, wherein the mixed Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 ) The steps of making O3 colloid into ferroelectric film material will not be repeated here.
[0078] The preparation of the top electrode includes: using an ion sputtering device to spray electrode material Au on the dielectric layer to form the top electrode.
[0079] The technical solution of the present application is further described below in combination with a plurality of embodiments and comparative examples. Example 1
[0080] In this embodiment, the chemical composition is 0.85Na 0.5 Bi 0.5 TiO3-0.15Bi(Mg 0.5 Zr 0.5 ) O3 ferroelectric film material, and determine the 0.85Na 0.5 Bi 0.5 TiO3-0.15Bi(Mg 0.5 Zr 0.5 ) The volume of O3 colloid is 30mL and the molar concentration is 0.35mol / L.
[0081] Step S101: Prepare Na 0.5 Bi 0.5 TiO3 colloid, the specific preparation steps are: a) according to 0.85Na 0.5 Bi 0.5 TiO3-0.15Bi(Mg 0.5 Zr0.5 ) Calculate the molar concentration and volume of O3 colloid and weigh the chemicals required for preparing the colloid to four decimal places; b) Put the weighed sodium acetate trihydrate and bismuth nitrate pentahydrate into a beaker (because metallic sodium and metallic bismuth will volatilize under high temperature environment, so it is necessary to weigh 5% in excess to compensate for the loss), pour in acetic acid and heat to 95℃ in a water bath, stir for about 30 minutes to obtain a clear colloid, and cool to room temperature for use; c) Pour acetylacetone into the beaker and continue stirring for 20 minutes until the colloid is stable light yellow, and the molar concentration ratio of acetylacetone to solution is 1.5:1; d) Add the weighed titanium isopropoxide in multiple times, and add deionized water in this process to make the colloid stable and light yellow (the volume ratio of deionized water to acetic acid is 1:4). This process requires continuous stirring for 20 minutes.
[0082] Step S102: Prepare Bi(Mg 0.5 Zr 0.5 ) O3 colloid, the specific preparation steps are: a) according to 0.85Na 0.5 Bi 0.5 TiO3-0.15Bi(Mg 0.5 Zr 0.5 ) Calculate the molar concentration and volume of O3 colloid and weigh the required chemicals to four decimal places; b) Put the weighed magnesium acetate tetrahydrate and bismuth nitrate pentahydrate into the same beaker (because metallic bismuth will volatilize under high temperature environment, it is necessary to overweigh 5% to compensate for the loss), pour in acetic acid and heat to 95℃ in a water bath, stir for 30 minutes to obtain a clear colloid, and cool to room temperature for use; c) Pour acetylacetone into the beaker and continue stirring for 20 minutes until the colloid is stable light yellow, and the molar concentration ratio of acetylacetone to solution is 1.5:1; d) Add the weighed zirconium n-propoxide in multiple times, and add deionized water in this process to make the colloid transparent light yellow (the volume ratio of deionized water to acetic acid is 1:4). This process requires continuous stirring for 20 minutes.
[0083] Step S103: Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 )O3 colloid is fully mixed to obtain 0.85Na 0.5 Bi 0.5 TiO3-0.15Bi(Mg 0.5 Zr 0.5 ) O3 colloid, the specific steps are: a) the Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5) After mixing the O3 colloid, stir for 5 minutes, add formamide solution to the mixed colloid, and continue stirring for 15 minutes to obtain an orange-yellow stable transparent colloid, the volume ratio of formamide to deionized water is 4:1; b) Add polyvinyl pyrrolidone-K30 to the colloid in multiple times, and add the next time only after the polyvinyl pyrrolidone-K30 added once is completely dissolved, and continue stirring for 2 hours. During this process, pay attention to the change of the colloid volume in real time, and add acetic acid and water in time until the colloid reaches 30ml again, and the ratio of acetic acid to water is 4:1; c) After the stirring is completed, use double-layer medium-speed filter paper to filter the solution twice to obtain an orange-yellow transparent colloid, and then store it at a temperature of 22°C and a humidity of 45°C for aging for 36 hours.
[0084] Step S104: a) Prepare 0.85Na by spin coating 0.5 Bi 0.5 TiO3-0.15Bi(Mg 0.5 Zr 0.5 ) O3 dielectric layer, place the prepared LaNiO3 bottom electrode on the suction cup of the glue spreader, and use a glue-tipped dropper to absorb the 0.85Na prepared in step S104 0.5 Bi 0.5 TiO3-0.15Bi(Mg 0.5 Zr 0.5 ) O3 colloid is dripped onto the LaNiO3 bottom electrode, and the bubbles are eliminated and the colloid is completely spread over the entire LaNiO3 bottom electrode before the coating is started. The spin coating parameters of the coating machine are set to 4000 rot / min for 30 seconds; b) After each spin coating, heat treatment is required to be performed quickly. Spin-coated 0.85Na 0.5 Bi 0.5 TiO3-0.15Bi(Mg 0.5 Zr 0.5 ) Place the LaNiO3 bottom electrode of O3 colloid in a rapid thermal treatment furnace, heat it to 150℃ for 1s and keep it for 3min, then heat it to 450℃ for 2s and keep it for 5min, then heat it to 750℃ for 4s and keep it for 3min; c) Repeat the spin coating and heat treatment steps in steps a) and b) until 0.85Na 0.5 Bi 0.5 TiO3-0.15Bi(Mg 0.5 Zr 0.5 ) The thickness of the O3 dielectric layer reaches 1.4μm. The dielectric layer is placed in an annealing furnace and kept at 750℃ for 10min to make 0.85Na 0.5 Bi 0.5 TiO3-0.15Bi(Mg 0.5 Zr 0.5 ) The O3 grains grow further to fill the gaps in each film layer.
[0085] Step S105: Use an ion sputtering device to spray electrode material Au on the dielectric layer prepared in step S104 to form a top electrode. In this step, a complete capacitor is prepared to facilitate performance testing. Example 2
[0086] In this embodiment, the chemical composition of the preparation is 0.7Na 0.5 Bi 0.5 TiO3-0.3Bi(Mg 0.5 Zr 0.5 ) O3 ferroelectric film material, and determine the 0.7Na 0.5 Bi 0.5 TiO3-0.3Bi(Mg 0.5 Zr 0.5 ) The volume of O3 colloid is 30mL and the molar concentration is 0.35mol / L.
[0087] Step S101: Prepare Na 0.5 Bi 0.5 TiO3 colloid, the specific preparation steps are: a) according to 0.7Na 0.5 Bi 0.5 TiO3-0.3Bi(Mg 0.5 Zr 0.5 ) Calculate the molar concentration and volume of O3 colloid and weigh the chemicals required for preparing the colloid to four decimal places; b) Put the weighed sodium acetate trihydrate and bismuth nitrate pentahydrate into a beaker (because metallic sodium and metallic bismuth will volatilize under high temperature environment, so it is necessary to weigh 5% in excess to compensate for the loss), pour in acetic acid and heat to 95℃ in a water bath, stir for about 30 minutes to obtain a clear colloid, and cool to room temperature for use; c) Pour acetylacetone into the beaker and continue stirring for 20 minutes until the colloid is stable light yellow, and the molar concentration ratio of acetylacetone to solution is 1.5:1; d) Add the weighed titanium isopropoxide in multiple times, and add deionized water in this process to make the colloid stable and light yellow (the volume ratio of deionized water to acetic acid is 1:4). This process requires continuous stirring for 20 minutes.
[0088] Step S102: Prepare Bi(Mg 0.5 Zr 0.5 ) O3 colloid, the specific preparation steps are: a) according to 0.7Na 0.5 Bi 0.5 TiO3-0.3Bi(Mg 0.5 Zr 0.5) Calculate the molar concentration and volume of O3 colloid and weigh the required chemicals to four decimal places; b) Put the weighed magnesium acetate tetrahydrate and bismuth nitrate pentahydrate into the same beaker (because metallic bismuth will volatilize under high temperature environment, it is necessary to overweigh 5% to compensate for the loss), pour in acetic acid and heat to 95℃ in a water bath, stir for 30 minutes to obtain a clear colloid, and cool to room temperature for use; c) Pour acetylacetone into the beaker and continue stirring for 20 minutes until the colloid is stable light yellow, and the molar concentration ratio of acetylacetone to solution is 1.5:1; d) Add the weighed zirconium n-propoxide in multiple times, and add deionized water in this process to make the colloid transparent light yellow (the volume ratio of deionized water to acetic acid is 1:4). This process requires continuous stirring for 20 minutes.
[0089] Step S103: Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 )O3 colloid is fully mixed to obtain 0.7Na 0.5 Bi 0.5 TiO3-0.3Bi(Mg 0.5 Zr 0.5 ) O3 colloid, the specific steps are: a) the Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 ) After mixing the O3 colloid, stir for 5 minutes, add formamide solution to the mixed colloid, and continue stirring for 15 minutes to obtain an orange-yellow stable transparent colloid, the volume ratio of formamide to deionized water is 4:1; b) Add polyvinyl pyrrolidone-K30 to the colloid in multiple times, and add the next time only after the polyvinyl pyrrolidone-K30 added once is completely dissolved, and continue stirring for 2 hours. During this process, pay attention to the change of the colloid volume in real time, and add acetic acid and water in time until the colloid reaches 30ml again, and the ratio of acetic acid to water is 4:1; c) After the stirring is completed, use double-layer medium-speed filter paper to filter the solution twice to obtain an orange-yellow transparent colloid, and then store it at a temperature of 22°C and a humidity of 45°C for aging for 36 hours.
[0090] Step S104: a) Prepare 0.7Na by spin coating 0.5 Bi 0.5 TiO3-0.3Bi(Mg 0.5 Zr 0.5 ) O3 dielectric layer, place the prepared LaNiO3 bottom electrode on the suction cup of the glue spreader, and use a glue-tipped dropper to absorb the 0.7Na prepared in step S104 0.5 Bi 0.5TiO3-0.3Bi(Mg 0.5 Zr 0.5 ) O3 colloid is dropped onto the LaNiO3 bottom electrode, and the bubbles are eliminated and the colloid is completely spread over the entire LaNiO3 bottom electrode before the coating is started. The spin coating parameters of the coating machine are set to 4000 rot / min for 30 seconds; b) After each spin coating, heat treatment is required to be performed quickly. Spin-coated 0.7Na 0.5 Bi 0.5 TiO3-0.3Bi(Mg 0.5 Zr 0.5 ) Place the LaNiO3 bottom electrode of O3 colloid in a rapid thermal treatment furnace, heat it to 150℃ for 1s and keep it for 3min, then heat it to 450℃ for 2s and keep it for 5min, then heat it to 750℃ for 4s and keep it for 3min; c) Repeat the spin coating and heat treatment steps in steps a) and b) until 0.7Na 0.5 Bi 0.5 TiO3-0.3Bi(Mg 0.5 Zr 0.5 ) The thickness of the O3 dielectric layer reaches 1.4μm. The dielectric layer is placed in an annealing furnace and kept at 750℃ for 10min to make 0.7Na 0.5 Bi 0.5 TiO3-0.3Bi(Mg 0.5 Zr 0.5 ) The O3 grains grow further to fill the gaps in each layer of the film.
[0091] Step S105: Use an ion sputtering device to spray electrode material Au on the dielectric layer prepared in step S104 to form a top electrode. In this step, a complete capacitor is prepared to facilitate performance testing.
[0092] Comparative Example In this comparative example, the chemical composition of the preparation is Na 0.5 Bi 0.5 TiO3 ferroelectric film material, and determine the Na 0.5 Bi 0.5 The volume of TiO3 colloid is 30mL and the molar concentration is 0.35mol / L.
[0093] Step S201: Prepare Na 0.5 Bi 0.5 TiO3 colloid, the specific preparation steps are: a) according to Na 0.5 Bi 0.5Calculate the molar concentration and volume of TiO3 colloid and weigh the chemicals required for preparing the colloid to four decimal places; b) Put the weighed sodium acetate trihydrate and bismuth nitrate pentahydrate into a beaker (because metallic sodium and metallic bismuth will volatilize under high temperature environment, 5% excess should be weighed to compensate for the loss), pour in acetic acid and heat to 95°C in a water bath, stir for about 30 minutes to obtain a clear colloid, and cool to room temperature for use; c) Pour acetylacetone into the beaker and continue stirring for 20 minutes until the colloid is stable light yellow, and the molar concentration ratio of acetylacetone to solution is 1.5:1; d) Add the weighed titanium isopropoxide in multiple times, and add deionized water in this process to make the colloid stable and light yellow (deionized water and acetic acid are 1:1). The volume ratio is 1:4), and this process needs to be stirred continuously for 20 minutes; e) Add formamide solution to the colloid and continue stirring for 15 minutes to obtain an orange-yellow stable transparent colloid. The volume ratio of formamide to deionized water is 4:1; f) Add polyvinyl pyrrolidone-K30 to the colloid in multiple times. The next addition can be made only after the polyvinyl pyrrolidone-K30 added once is completely dissolved. Continue stirring for 2 hours. During this process, pay attention to the change in the volume of the colloid in real time, and add acetic acid and water in time until the colloid reaches 30ml again. The ratio of acetic acid to water is 4:1; g) After the stirring is completed, use double-layer medium-speed filter paper to filter the solution twice to obtain an orange-yellow transparent colloid, and then store it at a temperature of 22°C and a humidity of 45°C for aging for 36 hours.
[0094] Step S202: a) Prepare Na by spin coating 0.5 Bi 0.5 TiO3 dielectric layer, place the prepared LaNiO3 bottom electrode on the suction cup of the glue spreader, and use a glue-tipped dropper to absorb the Na prepared in step S201. 0.5 Bi 0.5 TiO3 colloid is dripped onto the LaNiO3 bottom electrode, and the bubbles are eliminated and the colloid is completely spread over the entire LaNiO3 bottom electrode before the coating begins. The spin coating parameters of the coating machine are set to 4000 rot / min for 30 seconds. b) After each spin coating, heat treatment is required to be performed quickly to spin-coated Na 0.5 Bi 0.5 The LaNiO3 bottom electrode of the TiO3 colloid is placed in a rapid thermal treatment furnace, heated to 150°C for 1s and kept for 3min, then heated to 450°C for 2s and kept for 5min, and then heated to 750°C for 4s and kept for 3min; c) the spin coating and thermal treatment steps in steps a) and b) are repeated until Na 0.5 Bi 0.5 The thickness of the TiO3 dielectric layer reaches 1.4 μm. The dielectric layer is placed in an annealing furnace and kept at 750°C for 10 minutes to make the Na 0.5 Bi 0.5 The TiO3 grains further grow to fill the gaps in each film layer.
[0095] Step S203: using an ion sputtering apparatus to spray electrode material Au on the dielectric layer prepared in step S202 to form a top electrode. In this step, a complete capacitor is prepared to facilitate performance testing.
[0096] The properties of the ferroelectric film materials (dielectric layers) prepared in the above-mentioned embodiments and comparative examples were tested.
[0097] (1) XRD test Figure 2 The XRD patterns of the ferroelectric film materials prepared in Example 1, Example 2 and Comparative Example are shown in FIG. Figure 2 It can be seen that the ferroelectric film materials prepared in Example 1, Example 2 and Comparative Example 1 all present a pure perovskite phase structure. 0.5 Bi 0.5 TiO3 is doped with an appropriate amount of Bi (Mg 0.5 Zr 0.5 )O3, then Na 0.5 Bi 0.5 The TiO3-based structure had no significant effect.
[0098] (2) Atomic force microscopy (AFM) morphology test Figures 3 to 5 The atomic force microscope morphology images of the ferroelectric film materials prepared in the comparative example, embodiment 1 and embodiment 2 are shown respectively. Figure 4 and Figure 5 and Figure 3 It can be seen from the comparison that the components prepared in this application are (1-x)Na 0.5 Bi 0.5 TiO3-xBi(Mg 0.5 Zr 0.5 )O3 ferroelectric film material relative to the comparative example component Na 0.5 Bi 0.5 The TiO3 ferroelectric film material has obviously disordered grains and has been refined. The domain structure in the ferroelectric film material has become more blurred, breaking the long-range ferroelectric domain. In addition, Figure 4 and Figure 5 It can be seen that in this application, as Bi (Mg 0.5 Zr 0.5 ) With the increase of O3 addition, the domain structure in the ferroelectric film material becomes more blurred, the grains become more chaotic and further refined, and the long-range ferroelectric domains are better broken. Figure 4 and Figure 5 As shown, when x is 0.15 (corresponding to Example 1) and x is 0.3 (corresponding to Example 2), (1-x)Na 0.5 Bi 0.5TiO3-xBi(Mg 0.5 Zr 0.5 ) It is difficult to find a uniform and continuous large-area domain structure in O3 materials. The refined domain structure is conducive to polarization switching behavior and can effectively increase the energy storage density and efficiency. Therefore, it can be considered that an x value between 0.15 and 0.3 is a more preferred solution.
[0099] (3) Energy storage performance test Figure 6 The hysteresis loop diagram of the ferroelectric film material prepared in Example 1, Example 2 and Comparative Example under a field strength of 1200 kV / cm. Figure 6 It can be seen that the hysteresis loops of the ferroelectric film materials prepared in Example 1, Example 2 and the comparative example all show typical ferroelectric properties. The components prepared in this application are (1-x)Na 0.5 Bi 0.5 TiO3-xBi(Mg 0.5 Zr 0.5 )O3 ferroelectric film material relative to the comparative example component Na 0.5 Bi 0.5 The hysteresis loop of the ferroelectric film material of TiO3 becomes thinner, from which it can be seen that the residual polarization value and coercive electric field of the ferroelectric film material in the present application are significantly lower than the residual polarization value and coercive electric field of the ferroelectric film material in the comparative example, and the energy storage performance of the ferroelectric film material in the present application is significantly better.
[0100] Figure 7 This is a graph showing the change in energy storage density of the ferroelectric film materials prepared in Example 1, Example 2 and the comparative example under a field strength ranging from 100 kV / cm to 1200 kV / cm. Figure 8 The figure is a graph showing the energy storage efficiency change of the ferroelectric film materials prepared in Example 1, Example 2 and the comparative example under a field strength from 100 kV / cm to 1200 kV / cm. Figure 7 and Figure 8 It can be seen that under different field strengths, the energy storage density and energy storage efficiency of the ferroelectric film materials in Examples 1 and 2 are significantly higher than those of the ferroelectric film materials in the comparative example. 0.5 Zr 0.5 ) O3 and Na 0.5 Bi 0.5 TiO3 composite improves the microstructural characteristics of the ferroelectric film material, makes the grains disordered and refined, blurs the domain structure in the ferroelectric film material, breaks the long-range ferroelectric domain, thereby lowering the polarization conversion barrier and polarization hysteresis, and reducing the residual polarization value and coercive electric field of the ferroelectric film material, thereby effectively improving the energy storage density and efficiency of the ferroelectric film material.
[0101] It should be noted that the ferroelectric film material embodiments, ferroelectric film material preparation method embodiments and application embodiments provided in this application belong to the same concept; the technical features in the technical solutions recorded in each embodiment can be combined arbitrarily without conflict.
[0102] It should be understood that the above embodiments are exemplary and are not intended to include all possible implementations. Various modifications and changes may be made on the basis of the above embodiments without departing from the scope of the present disclosure. Similarly, the various technical features of the above embodiments may be arbitrarily combined to form other embodiments of the present invention that may not be explicitly described. Therefore, the above embodiments only express several implementations of the present invention and do not limit the scope of protection of the patent of the present invention.
Claims
1. A ferroelectric film material, characterized in that: The chemical formula of the ferroelectric film material is (1-x)Na 0.5 Bi 0.5 TiO3-xBi(Mg 0.5 Zr 0.5 )O3, where 0 <x≤0.3。 2. The ferroelectric film material according to claim 1, characterized in that: 0.15≤x≤0.3。 3. The ferroelectric film material according to claim 1 or 2, characterized in that: The thickness of the ferroelectric film material is 1.1 μm to 4 μm.
4. A method for preparing a ferroelectric film material, characterized in that: The method comprises the following steps: S1: Preparation of Na 0.5 Bi 0.5 TiO3 colloid and Bi(Mg 0.5 Zr 0.5 ) O3 colloid; S2: The Na 0.5 Bi 0.5 TiO3 colloid and the Bi(Mg 0.5 Zr 0.5 ) O3 colloid, adding additives and stirring, and obtaining the ferroelectric film material after spin coating and heat treatment, wherein the additives include polyvinyl pyrrolidone and / or polyvinyl alcohol, the Na 0.5 Bi 0.5 TiO3 colloid and the Bi(Mg 0.5 Zr 0.5 ) The molar ratio of O3 colloid is (1-x):x, where 0 <x≤0.3。 5. The method for preparing a ferroelectric film material according to claim 4, characterized in that: The preparation of the Na 0.5 Bi 0.5 TiO3 colloid methods include: A sodium source and a bismuth source are dissolved in a first solvent and stirred to form a first colloid; acetylacetone is added to the first colloid and stirred to form a second colloid; a titanium source and deionized water are added to the second colloid and stirred to form the Na 0.5 Bi 0.5 TiO3 colloid.
6. The method for preparing a ferroelectric film material according to claim 5, characterized in that: The method satisfies at least one of the following features: (1) The sodium source includes sodium acetate trihydrate and / or sodium acetate; (2) The bismuth source includes at least one of bismuth nitrate pentahydrate, bismuth acetate, and bismuth subnitrate; (3) the first solvent includes at least one of acetic acid, ethylene glycol methyl ether, and ethylene glycol; (4) The titanium source includes titanium isopropoxide and / or titanium n-propoxide; (5) The temperature for forming the first colloid is 90°C to 100°C; (6) The stirring time for forming the first colloid is 25 min to 30 min; (7) The acetylacetone and the Na 0.5 Bi 0.5 The molar concentration ratio of TiO3 colloid is 1.2:1~1.5:1; (8) The stirring time for forming the second colloid is 20 min to 30 min; (9) The volume ratio of the deionized water to the first solvent is 1:4 to 1:5; (10) Formation of the Na 0.5 Bi 0.5 The stirring time of TiO3 colloid is 20min~30min.
7. The method for preparing a ferroelectric film material according to claim 4, characterized in that: Step S1 in which the Bi(Mg) 0.5 Zr 0.5 ) O3 colloid method, comprising: A magnesium source and a bismuth source are dissolved in a second solvent and stirred to form a third colloid; acetylacetone is added to the third colloid and stirred to form a fourth colloid; a zirconium source and deionized water are added to the fourth colloid and stirred to form the Bi(Mg 0.5 Zr 0.5 )O3 colloid.
8. The method for preparing a ferroelectric film material according to claim 7, characterized in that: The method satisfies at least one of the following features: (1) The magnesium source includes magnesium acetate tetrahydrate and / or magnesium acetate; (2) The bismuth source includes at least one of bismuth nitrate pentahydrate, bismuth acetate, and bismuth subnitrate; (3) the second solvent comprises at least one of acetic acid, ethylene glycol methyl ether and ethylene glycol; (4) The zirconium source includes zirconium isopropoxide and / or zirconium n-propoxide; (5) The temperature for forming the third colloid is 90° C. to 100° C.; (6) The stirring time for forming the third colloid is 25 min to 30 min; (7) The acetylacetone and the Bi(Mg 0.5 Zr 0.5 ) The molar concentration ratio of O3 colloid is 1.2:1~1.5:1; (8) The stirring time for forming the fourth colloid is 20 min to 30 min; (9) The volume ratio of the deionized water to the second solvent is 1:4 to 1:5; (10) Forming the Bi(Mg 0.5 Zr 0.5 ) The stirring time of O3 colloid is 20min~30min.
9. The method for preparing a ferroelectric film material according to claim 4, characterized in that: Step S2 satisfies at least one of the following characteristics: (1) The polyvinyl pyrrolidone includes polyvinyl pyrrolidone-K30; (2)0.15≤x≤0.3; (3) The thickness of the ferroelectric film material is 1.1 μm to 4 μm.
10. Use of the ferroelectric film material according to any one of claims 1 to 3 or the ferroelectric film material prepared by the preparation method according to any one of claims 4 to 9 in capacitors.
Citation Information
Patent Citations
Leadless ferroelectric thick film and manufacturing method thereof
CN105931838A
Lead-free ferroelectric thick film and preparation method thereof
CN107244915A
Sodium bismuth titanate-based relaxor ferroelectric ceramic material with wide temperature range and high electrocaloric effect as well as preparation method and application of sodium bismuth titanate-based relaxor ferroelectric ceramic material
CN116813335A