Polypropylene composite material as well as preparation method and application thereof
By adding submicron amorphous silicon oxide and β nucleating agent to the polypropylene composite material, combined with the extrusion mechanism preparation method, the problem of poor thermal oxygen aging performance of polypropylene composite material after high temperature thermal retention is solved, and a long time has been achieved Thermal oxygen stability and low TVOC are suitable for automotive parts applications.
Patent Information
- Application Number
- CN202310616661.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
AI Technical Summary
The existing polypropylene composite materials have poor thermal oxygen aging performance after high temperature thermal retention, short powdering time, and high TVOC after thermal retention, making it difficult to meet the long-term thermal oxygen aging requirements of automotive parts.
By adding submicron amorphous silicon oxide, beta nucleating agent and antioxidant to the polypropylene composite material, and using an extruder melt extrusion preparation method, the high-temperature thermal retention stability and thermal oxygen aging performance of the material are improved, and the thermal oxygen aging performance is reduced. TVOC after thermal retention.
It significantly improves the powdering time of polypropylene composite materials after high temperature thermal retention, and reduces the TVOC after thermal retention, making it suitable for the preparation of automotive interior and exterior parts.
Smart Images

Figure BDA0004254065710000011 
Figure BDA0004254065710000021 
Figure BDA0004254065710000041
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and more specifically to a polypropylene composite material and a preparation method and application thereof. Background Art
[0002] Polypropylene material has the characteristics of low density, chemical resistance and excellent cost performance, and has been widely used in all parts of automotive interior and exterior.
[0003] In addition to the common mechanical properties, the most important requirements for polypropylene materials in automobile applications are also relatively strict requirements for thermal and oxygen aging resistance. However, since PP contains tertiary carbon groups, it is easily attacked by heat and oxygen, causing surface cracking and powdering, and the mechanical properties are greatly reduced. Therefore, many products have long-term thermal and oxygen aging resistance requirements for polypropylene.
[0004] The prior art generally improves the thermal oxidation aging resistance of polypropylene by adding antioxidants into the system. However, when polypropylene is further injection molded into parts, the problem of thermal oxidation aging failure of parts still occurs.
[0005] The prior art discloses a polypropylene composite material with long-term heat-oxidative aging resistance, low odor and anti-stickiness, which improves the heat-oxidative aging resistance of the polypropylene composite material by adding octa-epoxy cage-shaped polysilsesquioxane into the system. The embrittlement time of a 1 mm sample in a 150°C forced convection environment is only 869 to 1653 hours. However, the injection molding temperature of polypropylene is generally around 180°C, and the octa-epoxy cage-shaped polysilsesquioxane used therein is still very easy to cause powdering of polypropylene after long-term injection molding at a temperature above 200°C. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the existing polypropylene composite materials, such as poor thermal oxidation aging performance after high-temperature heat retention and short pulverization time after high-temperature heat retention, and to provide a polypropylene composite material, which improves the pulverization time after high-temperature heat retention and can also reduce TVOC after heat retention.
[0007] Another object of the present invention is to provide a method for preparing a polypropylene composite material.
[0008] Another object of the present invention is to provide an application of a polypropylene composite material in the preparation of automobile interiors or automobile exteriors.
[0009] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0010] A polypropylene composite material, comprising the following components by weight:
[0011]
[0012]
[0013] The submicron amorphous silicon oxide has an average particle size of 150 to 300 nm.
[0014] The test method for average particle size of silica is ASTM C721-20.
[0015] The submicron amorphous silicon oxide in the polypropylene composite material of the present invention effectively improves the stability of the polypropylene composite material under high-temperature thermal retention and improves the pulverization time after high-temperature thermal retention. This is because the submicron amorphous silicon oxide can be better dispersed in the matrix to improve the ability of the antioxidant to capture active free radicals, thereby improving the high-temperature thermal retention stability.
[0016] The average particle size of submicron amorphous silicon oxide is too small, and the submicron amorphous silicon oxide itself is easy to agglomerate, making it difficult to achieve better dispersion on the substrate, thereby reducing high-temperature thermal retention stability.
[0017] The average particle size of submicron amorphous silicon oxide is too large and the specific surface area is too small, and it is difficult to improve the high-temperature thermal retention stability.
[0018] Preferably, the silicon dioxide content in the submicron amorphous silicon oxide is 95-99%.
[0019] Test method for silicon dioxide content GB / T 36655-2018.
[0020] The effective silicon dioxide content can improve the thermal stability of the amorphous silicon oxide itself.
[0021] Optionally, the submicron amorphous silicon oxide has a specific surface area of 10 to 30 m 2 / g.
[0022] The appropriate specific surface area can ensure the dispersion of submicron amorphous silica in the polypropylene resin matrix.
[0023] The testing method for specific surface area of silica is GB / T 19587-2004.
[0024] More preferably, the silicon dioxide content in the submicron amorphous silicon oxide is 97-99%.
[0025] More preferably, the submicron amorphous silicon oxide has an average particle size of 150 to 180 nm.
[0026] Preferably, the molecular sieve is a microporous zeolite molecular sieve, and the average pore size of the molecular sieve is less than or equal to 2 nm.
[0027] More preferably, the average pore size of the molecular sieve is less than or equal to 1 nm.
[0028] The average pore size was measured using DFT under Ar gas conditions.
[0029] The molecular sieve is a hydrophobic molecular sieve.
[0030] Zeolite molecular sieves have more pores and can fully adsorb small molecular emissions during the modification production process.
[0031] The pore size of the molecular sieve is less than or equal to 1nm, which is more conducive to the adsorption and emission of organic matter, thereby reducing TVOC.
[0032] More preferably, the average pore size of the molecular sieve is 0.5-1 nm.
[0033] Preferably, the beta nucleating agent is a dicarboxylate of a Group IIA metal.
[0034] The β-nucleating agent is beneficial for the polypropylene resin to form a β-crystal, thereby making the crystal size of the polypropylene smaller and the structure more uniform, thereby improving the thermal oxidative aging performance.
[0035] Preferably, the β-nucleating agent is calcium pimelate and / or calcium suberate.
[0036] Optionally, the melt mass flow rate of the polypropylene resin is 10 to 150 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 230° C. and 2.16 kg.
[0037] Preferably, the melt mass flow rate of the polypropylene resin is 30 to 100 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 230° C. and 2.16 kg.
[0038] Optionally, the polypropylene resin is homopolypropylene and / or copolymer polypropylene.
[0039] Preferably, the polypropylene resin is copolymer polypropylene.
[0040] Preferably, the filler is one or more of talc, calcium carbonate, barium sulfate or alkali-free glass fiber.
[0041] More preferably, the filler is talc and / or alkali-free glass fiber.
[0042] Still more preferably, the filler is alkali-free glass fiber.
[0043] Preferably, the antioxidant is one or more of a hindered phenol antioxidant, a phosphite antioxidant or a thioester antioxidant.
[0044] Optionally, the hindered phenol antioxidant is one or more of antioxidants 1010, 3114 or 1076.
[0045] Optionally, the phosphite antioxidant is one or more of antioxidants 168, 626 or 627.
[0046] Optionally, the weight ratio of the hindered phenol antioxidant to the phosphite antioxidant is 1:1.
[0047] Antioxidants can improve the antioxidant effect of polypropylene composites.
[0048] The invention also protects a preparation method of a polypropylene composite material, comprising the following steps: mixing the components, melting and extruding through an extruder, granulating, and drying to obtain the polypropylene composite material.
[0049] The extruder is a twin-screw extruder.
[0050] The polypropylene composite material prepared by the present invention has high thermal oxidative aging performance, a long thermal oxidative aging powdering time after heat retention, and can be widely used in the preparation of plastic products. The present invention particularly protects the use of the polypropylene composite material in the preparation of automobile parts, especially automobile interiors and / or automobile exteriors.
[0051] An automobile component is made by injection molding any one of the above-mentioned polypropylene composite materials.
[0052] Preferably, the automotive component is an automotive interior and / or an automotive exterior.
[0053] The automobile interior is a dashboard frame, a central channel or a door substrate.
[0054] The automobile exterior is a bumper, a spoiler or a door sill.
[0055] Compared with the prior art, the present invention has the following beneficial effects:
[0056] The polypropylene composite material of the present invention comprises polypropylene resin, submicron amorphous silicon oxide, beta nucleating agent and antioxidant. By adding submicron amorphous silicon oxide, the thermal oxidation aging performance of the polypropylene composite material after high-temperature heat retention is effectively improved, the pulverization time after high-temperature heat retention is increased, and TVOC after heat retention can be reduced.
[0057] The polypropylene composite material of the invention can increase the thermal oxidation pulverization time to 1028-1480 hours after heat retention at 250°C for 30 minutes, and can reduce TVOC to 18.9-47.2 μgC / g after heat retention. DETAILED DESCRIPTION
[0058] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0059] The raw materials used in the embodiments and comparative examples of the present invention are shown in Table 1 below.
[0060] Table 1
[0061]
[0062]
[0063] The preparation method of submicron amorphous silicon oxide 2 is as follows: 10 mL of tetraethyl orthosilicate is dissolved in 120 mL (a portion) of anhydrous ethanol to prepare solution A, and 20 mL of ammonia water (volume concentration 25%) is dissolved in 80 mL (b portion) of anhydrous ethanol to prepare solution B, and the mass ratio is tetraethyl orthosilicate / (a+b portions of anhydrous ethanol+ammonia water)=5:96; solution A is placed in an ultrasonic device, the power is set to 100 W, the frequency is set to 40 KHz, and the temperature is set to 30° C., solution B is added to solution A under ultrasound, and then ultrasound is continued for 1 hour; after the ultrasound is completed, the precipitate generated in the mixed solution is separated, the precipitate is washed with water and anhydrous ethanol respectively, and then dried at 60° C. to obtain submicron amorphous silicon oxide 2;
[0064] The preparation method of submicron amorphous silicon oxide 3 is as follows: 10 mL of tetraethyl orthosilicate is dissolved in 120 mL (a portion) of anhydrous ethanol to prepare solution A, and 20 mL of ammonia water (volume concentration 25%) is dissolved in 80 mL (b portion) of anhydrous ethanol to prepare solution B, and in terms of mass ratio, tetraethyl orthosilicate / (a+b portions of anhydrous ethanol+ammonia water)=5:96; solution A is placed in an ultrasonic device, the power is set to 100 W, the frequency is set to 40 KHz, and the temperature is set to 35° C., solution B is added to solution A under ultrasound, and then ultrasound is continued for 2 hours; after the ultrasound is completed, the precipitate generated in the mixed solution is separated, the precipitate is washed with water and anhydrous ethanol respectively, and then dried at 60° C. to obtain submicron amorphous silicon oxide 3;
[0065] The preparation method of submicron amorphous silicon oxide 4 is as follows: 10 mL of tetraethyl orthosilicate is dissolved in 120 mL (a part) of anhydrous ethanol to prepare solution A, and 40 mL of ammonia water (volume concentration 28%) is dissolved in 100 mL (b part) of anhydrous ethanol to prepare solution B, in which the mass ratio is tetraethyl orthosilicate / (a+b parts of anhydrous ethanol+ammonia water)=4:100; solution A is placed in an ultrasonic device, the power is set to 95 W, the temperature is set to 35° C., and the frequency is set to 40 KHz, solution B is added to solution A under ultrasound, and then ultrasound is continued for 2 hours; after the ultrasound is completed, the precipitate generated in the mixed solution is separated, the precipitate is washed with water and anhydrous ethanol respectively, and then dried at 65° C. to obtain submicron amorphous silicon oxide 4.
[0066] Examples 1 to 15
[0067] A polypropylene composite material comprises the following components by weight: polypropylene resin; filler; submicron amorphous silicon oxide; molecular sieve; beta nucleating agent; antioxidant.
[0068] The specific content of each component is shown in Table 2 below.
[0069] Table 2 Composition of polypropylene composite materials in various embodiments (by weight)
[0070] Components Example 1 Example 2 Example 3 Polypropylene resin 1 78.5 78 68 Packing 1 20 0 0 Packing 2 0 0 0 Packing 3 0 20 30 Submicron amorphous silicon oxide 1 0.5 1 1 Molecular sieve 1 0.5 0.5 0.5 β-nucleating agent 1 0.1 0.1 0.1 Antioxidants 0.4 0.4 0.4
[0071] Table 2
[0072]
[0073]
[0074] Table 2
[0075] Components 13 14 15 Polypropylene resin 1 78.5 78.5 78.5 Filler 1 Glass fiber 20 20 0 Submicron amorphous silicon oxide 1 0.5 0.5 0.5 Molecular sieve 1 0.5 0 Molecular sieve 2 0.5 β-nucleating agent 1 0.1 0.1 β-nucleating agent 2 0.1 Antioxidants 0.4 0.4 0.4
[0076] The preparation method of the polypropylene composite material comprises the following steps:
[0077] The components were weighed in parts by weight and added to a high-speed mixer for mixing for 3 to 5 minutes, and then added to a twin-screw extruder with a length-to-diameter ratio of 48:1 for melting, mixing and dispersion. The polypropylene composite material was obtained by plasticizing in the twin-screw extruder and then stranding and pelletizing. The setting temperature of the twin-screw extruder from the feed port to the die head was 100°C, 180°C, 180°C, 200°C, 200°C, 200°C, 180°C, 200°C, 200°C, and the screw speed was 450 rpm.
[0078] Wherein, filler 1 glass fiber is fed from the side feeding port of the twin-screw extruder;
[0079] Filler 2 and filler 3 are fed into the twin-screw extruder with the remaining components from the main feed port.
[0080] Comparative Examples 1 to 7
[0081] A polypropylene composite material comprises the following components by weight: polypropylene resin; filler; submicron amorphous silicon oxide; molecular sieve; beta nucleating agent; antioxidant.
[0082] The specific content of each component is shown in Table 3 below.
[0083] Table 3 Composition of polypropylene composite materials of each comparative example (by weight)
[0084] Components 1 2 3 4 5 6 7 Polypropylene resin 1 78.5 78.5 78.5 78.5 78.5 78.5 78.5 Filler 1 Glass fiber 20 20 20 20 20 20 20 Submicron amorphous silicon oxide 1 0 2.5 0.5 0.5 0.5 0.5 Amorphous Nano-Silica 0.5 Molecular sieve 1 0.5 0.5 0.5 2.5 0.5 0.5 0.5 β-nucleating agent 1 0.1 0.1 0.1 0.1 0.001 1.5 α Nucleating Agent 0.1 Antioxidants 0.4 0.4 0.4 0.4 0.4 0.4 0.4
[0085] The preparation method of the polypropylene composite material is the same as that in the embodiment, and will not be described again here.
[0086] Results
[0087] The polypropylene composite materials of each embodiment and comparative example were tested according to the following method:
[0088] (1) Thermal oxidative aging performance:
[0089] The injection molding machine was used for injection molding at 250°C. After the material was plasticized in the barrel, it stayed at high temperature for 30 minutes before injection molding the sample; the sample size was 100*100*2.5mm.
[0090] Use the sample in an aging oven at 150°C according to ISO 188-20112 and record the time when powdering occurs.
[0091] (2) TVOC:
[0092] The injection molding machine was used for injection molding at 250°C. After the material was plasticized in the barrel, it stayed at high temperature for 30 minutes before injection molding the sample; the sample size was 100*100*2.5mm.
[0093] TVOC was tested using samples in accordance with VDA 277 standard at a test temperature of 120°C for 5 hours.
[0094] The specific test results of the polypropylene composite materials of each embodiment and comparative example are described in Table 3 below:
[0095] Table 3
[0096]
[0097]
[0098] Table 3
[0099]
[0100] Table 3
[0101]
[0102] From the above data, it can be seen that the polypropylene composite material of the present invention has improved thermal oxidation aging performance and TVOC after high-temperature thermal retention by adding submicron amorphous silicon oxide. The thermal oxidation pulverization time of the polypropylene composite material of the present invention can be increased to 1028-1480h after thermal retention at 250°C for 30min, and the TVOC can be reduced to 18.9-47.2μgC / g after thermal retention.
[0103] It can be seen from Comparative Example 1 that without the presence of submicron amorphous silica, the thermal oxidation aging powdering time after thermal retention is significantly reduced. This is because without the addition of submicron amorphous silica, the resin matrix undergoes irreversible degradation at 250°C, resulting in a significant reduction in the thermal oxidation aging powdering time after thermal retention, and the small molecular substances caused by the degradation will lead to an increase in TVOC.
[0104] It can be seen from Comparative Example 2 that when the amount of submicron amorphous silicon oxide added is too much, the thermal oxygen aging powdering time after thermal retention is significantly reduced. This is because when the amount of submicron amorphous silicon oxide added is too much, more interfaces are generated, thereby reducing the thermal oxygen aging performance after thermal retention.
[0105] It can be seen from Comparative Example 3 that replacing submicron amorphous silicon oxide with amorphous nano-silica cannot achieve the purpose of improving high-temperature thermal retention stability. This is because the particle size of amorphous nano-silica is too small, and the amorphous nano-silica itself is easier to agglomerate, which will lead to a decrease in thermal oxidation aging after thermal retention, and the small molecules produced by thermal retention will cause an increase in TVOC.
[0106] It can be seen from Comparative Example 4 that when the amount of molecular sieve added is too much, the thermal oxygen aging powdering time after heat retention is significantly reduced. This is because although the addition of too much molecular sieve is beneficial to reduce TVOC, it will cause more interfaces to be generated, thereby reducing the thermal oxygen aging performance after heat retention.
[0107] It can be seen from Comparative Example 5 that the amount of nucleating agent added is too little, and the thermal oxidation aging powdering time after heat retention is too low. This is because the amount of nucleating agent added is too little, which will cause an imperfect crystal structure and thus affect the thermal oxidation aging.
[0108] It can be seen from Comparative Example 6 that the amount of nucleating agent added is too much, and the thermal oxidation aging powdering time after heat retention is too low. This is because the excessive amount of nucleating agent added will also cause an increase in the interface and reduce the thermal oxidation aging performance.
[0109] It can be seen from Comparative Example 7 that the nucleating agent is an α-nucleating agent, which has no obvious effect on thermal oxidative aging and low emission.
[0110] It can be seen from Examples 1 and 6 to 9 that the melt mass flow rate of the polypropylene resin mainly affects the thermal oxidative aging properties of the material after high-temperature heat retention. A higher melt mass flow rate of polypropylene is more conducive to the dispersion of antioxidants and silicon oxide, and is beneficial to improving the thermal oxidative aging properties. When the melt mass flow rate of the polypropylene is higher, due to the large amount of polydisperse small molecular substances in the material, it is not conducive to the stability of the thermal retention process, thereby reducing the thermal oxidative aging properties.
[0111] It can be seen from Example 1 and Example 10 to Example 12 that the silicon dioxide content of the submicron amorphous silicon oxide mainly affects the thermal oxygen aging performance of the material after thermal retention, and a slightly higher silicon dioxide content is more conducive to improving the thermal oxygen aging performance and achieving TVOC reduction.
[0112] It can be seen from Example 1 and Example 14 that when the nucleating agent is calcium suberate, thermal oxidation aging and TVOC after high-temperature heat retention can be better achieved.
[0113] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A polypropylene composite material, characterized in that: By weight, it includes the following components: The submicron amorphous silicon oxide has an average particle size of 150 to 300 nm.
2. The polypropylene composite material according to claim 1, characterized in that: The silicon dioxide content in the submicron amorphous silicon oxide is 95-99%.
3. The polypropylene composite material according to claim 1 or 2, characterized in that: The submicron amorphous silicon oxide has a silicon dioxide content of 97-99% and an average particle size of 150-180 nm.
4. The polypropylene composite material according to claim 1, characterized in that: The molecular sieve is a microporous zeolite molecular sieve, and the average pore size of the molecular sieve is less than or equal to 2 nm.
5. The polypropylene composite material according to claim 1, characterized in that: The beta nucleating agent is a dicarboxylate of a Group IIA metal.
6. The polypropylene composite material according to claim 4, characterized in that: The β nucleating agent is calcium pimelate and / or calcium suberate.
7. The polypropylene composite material according to claim 1, characterized in that: The melt mass flow rate of the polypropylene resin is 10 to 150 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 230° C. and 2.16 kg.
8. The polypropylene composite material according to claim 1, characterized in that: The filler is one or more of talcum powder, calcium carbonate, barium sulfate or alkali-free glass fiber; the antioxidant is one or more of hindered phenol antioxidants, phosphite antioxidants or thioester antioxidants.
9. The method for preparing the polypropylene composite material according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: mixing the components, melting and extruding through an extruder, granulating, and drying to obtain the polypropylene composite material.
10. Use of the polypropylene composite material according to any one of claims 1 to 8 in the preparation of automotive interior or exterior materials.