Smelting method of tin-containing steel with uniformly distributed components
By using vacuum heating, refining and degassing and alloying technology during the tin-containing steel smelting process, combined with argon pressure control and metal zirconium addition, the problem of uneven distribution of tin elements is solved, and the composition uniformity and high melting point compound generation are achieved , improves the uniformity and welding performance of the steel liquid.
Patent Information
- Application Number
- CN202411050353.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-01
AI Technical Summary
During the smelting of tin-containing steel, due to the surfactivity and grain boundary segregation characteristics of tin elements, their distribution in the steel is uneven, affecting the quality and welding performance of the steel, making it difficult to accurately detect through direct reading spectroscopy.
Using vacuum heating, refining and degassing, alloying and steel casting, the uniform distribution of tin elements and high melting point compounds are ensured through high vacuum degassing, adding carbon powder and metal aluminum, controlling argon pressure, adding metal zirconium and other means. Generate, combining low superheat pouring and high power stirring to achieve component uniformity control.
The uniform distribution of tin elements and fine grain size are achieved, the composition control accuracy and welding performance of the steel liquid are improved, and it is suitable for smelting of tin-containing steel with Sn≤0.1 wt%, ensuring the smelting quality of steel for direct reading spectroscopy standard.
Smart Images

Figure BDA0004974733650000031 
Figure BDA0004974733650000032 
Figure BDA0004974733650000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tin-containing steel smelting, and in particular relates to a smelting method of tin-containing steel with uniform component distribution. Background Art
[0002] In the steel industry, tin has always been a harmful impurity element in steel. It affects the quality of steel, especially the quality of continuous casting billets, causing hot brittleness and temper brittleness, cracks and fractures in steel, and affecting the welding performance of steel. It is one of the "five harms" of steel. However, tin plays an important role in electrical steel, cast iron, and free-cutting steel. It needs to be added during the smelting process. Therefore, in the smelting process of such steel, the tin element needs to be quickly detected. The direct reading spectrometer is a rapid detection device for elements in steel. In order to accurately detect the tin content in steel, a matching tin-containing steel standard must be available.
[0003] In the smelting process of tin-containing steel, since tin is a surface-active element with typical grain boundary segregation characteristics, it has low solubility in the matrix, high density and low melting point. The low-melting-point eutectic is enriched in the grain boundary area. Although its content in the entire steel and alloy is low, the concentration at the grain boundary is several times or even dozens of times the average content, resulting in uneven distribution of tin in the ingot. Therefore, the key to the smelting of tin-containing steel, especially tin-containing direct-reading spectroscopy standard steel, lies in the uniformity control of various elements including tin. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for smelting tin-containing steel with uniform component distribution, thereby smelting tin-containing steel with uniform component, which can be used as standard steel for direct reading spectrum.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0006] A smelting method for tin-containing steel with uniform component distribution, comprising furnace charging, vacuum heating, refining and degassing, alloying and steel pouring processes;
[0007] Refining and degassing process: high vacuum degassing is carried out at a vacuum degree of ≤1Pa, and carbon powder is added in the later stage of refining to give full play to the deoxidation capacity of vacuum carbon. Before the end of refining, metal aluminum and metal tin are added in sequence;
[0008] Alloying process: stop the vacuum pump, fill the furnace with high-purity argon, and then add the required alloy into the molten steel;
[0009] Steel tapping and pouring process: Control the tapping temperature to 30℃~50℃ above the liquidus, add metal zirconium before tapping, and then stir at high power to prepare for tapping;
[0010] The casting ingot mold is a round ingot mold with a wall thickness of 0.4 to 0.5 of the inner diameter of the ingot mold.
[0011] Furthermore, in the alloying process of the present invention, 10000Pa to 20000Pa of high-purity argon gas is filled into the furnace.
[0012] Furthermore, in the alloying process of the present invention, after adding the alloy, the temperature of the molten steel is controlled to be 80° C. to 100° C. above the liquidus line, and the time is controlled to be 5 to 15 minutes.
[0013] Furthermore, in the pouring and tapping process of the present invention, metal zirconium is added according to 10% to 15% of the target tin content before tapping, and then high-power stirring is performed for 3 minutes to 5 minutes to prepare for tapping.
[0014] Furthermore, the smelting method of the present invention is suitable for smelting tin-containing steel with Sn≤0.1wt%.
[0015] Furthermore, the smelting method of the present invention is applicable to vacuum furnace induction furnace equipment with a furnace capacity of ≤500kg.
[0016] The beneficial effects of the above technical solution are as follows: During the refining and degassing period, the present invention makes full use of the vacuum carbon deoxidation capacity, adds aluminum for deep deoxidation while ensuring that the gas content in the steel is low, realizes low oxygen control of the molten steel, and then fills argon gas during the alloying process, which greatly improves the control accuracy of each component in the steel. Since the Sn element is easy to segregate along the grain boundary during the solidification process, metal zirconium is added before steelmaking to form a high melting point Zr with tin. x Sn y compounds, thereby changing its precipitation conditions and eliminating the grain boundary segregation of tin; the casting process adopts low superheat casting, and high-power stirring before pouring, and uses a round ingot mold with a wall thickness of 0.4 to 0.5 of the inner diameter of the ingot mold. In this way, while ensuring sufficient shrinkage of the molten steel, the molten steel has a more uniform composition distribution and a finer grain size during the solidification process. DETAILED DESCRIPTION
[0017] The present invention will be further described in detail below in conjunction with specific embodiments.
[0018] Embodiment 1-3: The smelting method of the tin-containing steel with uniform component distribution adopts the following specific process.
[0019] The equipment uses a 500kg vacuum induction furnace. The smelting composition is shown in Table 2, and the smelting weight is 500kg.
[0020] (1) Charging the furnace: Put pure iron into the crucible, and load aluminum particles, metallic tin, electrolytic manganese, industrial silicon, and metallic chromium into the material bin in sequence to ensure that the alloy material is dry and free of moisture.
[0021] (2) Vacuum heating: Evacuate the crucible and apply electric heating until all the pure iron in the crucible is melted.
[0022] (3) Refining and degassing: high vacuum degassing is carried out at a vacuum degree of ≤1Pa, and carbon powder is added in the later stage of refining. Before the end of refining, metallic aluminum and metallic tin are added in sequence.
[0023] (4) Alloying: After the refining period, stop the vacuum pump, fill the furnace with 10000Pa~20000Pa high-purity argon, add electrolytic manganese, industrial silicon and metallic chromium to the molten steel, and control the temperature of the molten steel to 80℃~100℃ above the liquidus for 5~15min.
[0024] (5) Steel-making and pouring process: After the steel liquid composition is tested and qualified, the steel-making temperature is controlled to be 30°C to 50°C above the liquidus line. Before steel-making, metal zirconium is added according to 10% to 15% of the target tin content. After adding, high-power stirring is performed for 3 minutes to 5 minutes to prepare for steel-making.
[0025] The parameter control at each stage of the smelting process is shown in Table 1. The steel ingot is forged after demoulding. The specification after forging is φ50mm. The edge, center and 1 / 2R of the cross section of the forged bar are taken for direct reading spectrum detection. The test results are shown in Table 2.
[0026] Table 1. Parameter control at each stage of smelting process of Examples 1-3
[0027]
[0028] Note: TL is the liquidus temperature of the steel grade.
[0029] Table 2 Chemical composition of steel grades smelted in Example 1-3 and direct reading test results after forging (wt%)
[0030]
[0031] In Table 2, the balance is Fe and unavoidable impurities.
[0032] Example 4-6: The smelting method of tin-containing steel with uniform component distribution adopts the following specific process.
[0033] The equipment uses a 200kg vacuum induction furnace. The smelting composition is shown in Table 4, and the smelting weight is 200kg.
[0034] (1) Charging the furnace: Put pure iron into the crucible, and load aluminum particles, metallic tin, electrolytic manganese, and ferrophosphorus into the sub-bin in sequence to ensure that the alloy material is dry and free of moisture.
[0035] (2) Vacuum heating: Evacuate the crucible and apply electric heating until all the pure iron in the crucible is melted.
[0036] (3) Refining and degassing: high vacuum degassing is carried out at a vacuum degree of ≤1Pa, and carbon powder is added in the later stage of refining. Before the end of refining, metallic aluminum and metallic tin are added in sequence.
[0037] (4) Alloying: After the refining period, stop the vacuum pump, fill the furnace with 10000Pa~20000Pa high-purity argon, add electrolytic manganese and ferrophosphorus to the molten steel, and control the temperature of the molten steel to 80℃~100℃ above the liquidus for 5~15min.
[0038] (5) Steel-making and pouring process: After the steel liquid composition is tested and qualified, the steel-making temperature is controlled to be 30°C to 50°C above the liquidus line. Before steel-making, metal zirconium is added according to 10% to 15% of the target tin content. After adding, high-power stirring is performed for 3 minutes to 5 minutes to prepare for steel-making.
[0039] The parameter control at each stage of the smelting process is shown in Table 3. The steel ingot is forged after demoulding. The specification after forging is φ50mm. The edge, center and 1 / 2R of the cross section of the forged bar are taken for direct reading spectrum detection. The test results are shown in Table 4.
[0040] Table 3. Parameter control at each stage of smelting process of Example 4-6
[0041]
[0042] Note: TL is the liquidus temperature of the steel grade.
[0043] Table 4. Chemical composition of steel grades smelted in Example 4-6 and direct reading test results after forging (wt%)
[0044]
[0045] In Table 4, the balance is Fe and unavoidable impurities.
[0046] Examples 7-9: The smelting method of tin-containing steel with uniform component distribution adopts the following specific process.
[0047] The equipment uses a 50kg vacuum induction furnace. The smelting composition is shown in Table 6, and the smelting weight is 50kg.
[0048] (1) Furnace loading: pure iron is placed in a crucible, and aluminum particles, metallic tin, electrolytic manganese, industrial silicon, and electrolytic copper are placed in the material bin in sequence to ensure that the alloy material is dry and free of moisture.
[0049] (2) Vacuum heating: Evacuate the crucible and apply electric heating until all the pure iron in the crucible is melted.
[0050] (3) Refining and degassing: high vacuum degassing is carried out at a vacuum degree of ≤1Pa, and carbon powder is added in the later stage of refining. Before the end of refining, metallic aluminum and metallic tin are added in sequence.
[0051] (4) Alloying: After the refining period, stop the vacuum pump, fill the furnace with 10000Pa~20000Pa high-purity argon, add electrolytic manganese, industrial silicon and electrolytic copper to the molten steel, and control the temperature of the molten steel to 80℃~100℃ above the liquidus for 5~15min.
[0052] (5) Steel-making and pouring process: After the steel liquid composition is tested and qualified, the steel-making temperature is controlled to be 30°C to 50°C above the liquidus line. Before steel-making, metal zirconium is added according to 10% to 15% of the target tin content. After adding, high-power stirring is performed for 3 minutes to 5 minutes to prepare for steel-making.
[0053] The parameter control at each stage of the smelting process is shown in Table 5. The steel ingot is forged after demoulding. The specification after forging is φ50mm. The edge, center and 1 / 2R of the cross section of the forged bar are taken for direct reading spectrum detection. The test results are shown in Table 6.
[0054] Table 5. Parameter control at each stage of smelting process of Examples 7-9
[0055]
[0056] Note: TL is the liquidus temperature of the steel grade.
[0057] Table 6 Chemical composition of steel grades smelted in Examples 7-9 and direct reading test results after forging (wt%)
[0058]
[0059]
[0060] In Table 6, the balance is Fe and unavoidable impurities.
[0061] It can be seen from Tables 2, 4 and 6 that the present invention achieves uniformity control of various elements in tin-containing steel.
Claims
1. A method for smelting tin-containing steel with uniform composition distribution, It is characterized in that It includes furnace charging, vacuum heating, refining and degassing, alloying and steel pouring processes; Refining and degassing process: high vacuum degassing is carried out at a vacuum degree of ≤1Pa, and carbon powder is added in the late stage of refining. Before the end of refining, metal aluminum and metal tin are added in sequence; Alloying process: stop the vacuum pump, fill the furnace with high-purity argon, and then add the required alloy into the molten steel; Steel tapping and pouring process: Control the tapping temperature to 30℃~50℃ above the liquidus, add metal zirconium before tapping, and then stir at high power to prepare for tapping; The casting ingot mold is a round ingot mold with a wall thickness of 0.4 to 0.5 of the inner diameter of the ingot mold.
2. The smelting method of tin-containing steel with uniform component distribution according to claim 1, It is characterized in that During the alloying process, 10000Pa to 20000Pa of high-purity argon gas is filled into the furnace.
3. The smelting method of tin-containing steel with uniform component distribution according to claim 2, It is characterized in that In the alloying process, after adding the alloy, the temperature of the molten steel is controlled to be 80° C. to 100° C. above the liquidus line, and the time is controlled to be 5 to 15 minutes.
4. The smelting method of tin-containing steel with uniform component distribution according to claim 3, It is characterized in that In the pouring and tapping process, metal zirconium is added according to 10% to 15% of the target tin content before tapping, and then high-power stirring is performed for 3 minutes to 5 minutes to prepare for tapping.
5. A method for smelting tin-containing steel with uniform component distribution according to any one of claims 1 to 4, It is characterized in that The smelting method is suitable for smelting tin-containing steel with Sn≤0.1wt%.
6. The smelting method of tin-containing steel with uniform component distribution according to claim 5, It is characterized in that The smelting method is applicable to vacuum furnace induction furnace equipment with a furnace capacity of ≤500kg.
Citation Information
Patent Citations
Complex additive for spheroidizing and dispersing sulfides in steel and use method thereof
CN102031441A
Production method of low-carbon sulfur series free-cutting steel continuous casting billet
CN102816979A
Abnormally segregated stanniferous low-clearance ferritic stainless steel and preparation method thereof
CN103866194A
Medium carbon free-cutting non-quenched-and-tempered steel containing sulfur and tellurium and production technological method thereof
CN107287504A
Preparation method of tin-containing free-cutting steel and tin-containing free-cutting steel
CN115747619A