Laminated substrate, light emitting device
By using a combination of a translucent substrate and a porous layer structure in a light-emitting device, the scattering effect of the porous layer is used to suppress light reflection, and laser separation technology is used to reduce equipment damage, solving the problems of light reflection and damage during the manufacturing process in the light-emitting device. .
Patent Information
- Application Number
- CN202010465618.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2014-01-14
- Filing Date
- 2014-12-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2034-12-09
AI Technical Summary
Reflection problems in existing light-emitting devices lead to reduced visual recognition. Especially in laminated structures, reflections caused by reflection and incidence of external light are difficult to effectively suppress.
It adopts a light-transmitting substrate and a porous layer structure. The porous layer is an organic material layer with multiple pores. It is arranged on the opposite main surface of the light-transmitting substrate to scatter external light and suppress reflection. At the same time, it is irradiated by laser Separate support substrates to reduce damage to equipment components.
It effectively suppresses reflection, improves visual recognition, reduces damage to electronic equipment components when separating support substrates, and improves manufacturing efficiency.
Smart Images

Figure CN111540845B_ABST
Abstract
Description
[0001] The present application is a divisional application of an invention application with an application date of December 9, 2014 and application number of 201410746129.7, and the name of the invention of the application is a laminated substrate, a light-emitting device, and a method for manufacturing a light-emitting device. Technical Field
[0002] The present invention relates to a laminated substrate and a light-emitting device. Background Art
[0003] Display devices such as LCD (Liquid Crystal Display) and organic EL (Electroluminescence) displays generally have a structure in which various layers are stacked on a substrate such as a glass substrate or a plastic substrate, for example, an electrode layer composed of a metal thin film, a TFT (Thin Film Transistor) layer, an insulating layer, a light-emitting layer, a sealing layer for preventing the intrusion of moisture or oxygen from the outside, a color filter, a polarizing plate, and a protective layer for preventing damage due to external mechanical stress (for example, Patent Document 1).
[0004] By forming electronic device components on a plastic film (plastic substrate), electronic devices that are light, thin, not easy to break, and bendable can be realized. Such electronic devices are collectively referred to as flexible electronic devices, and they are being actively developed in recent years. Examples of electronic devices include displays, photoelectric sensors, RF tags, etc.
[0005] The manufacturing method of electronic devices using such plastic substrates can be roughly classified into three methods. The first method is a method of temporarily fixing a plastic film on a glass support substrate and separating the support substrate after forming electronic device components. The second method is a method of forming electronic device components on a plastic film without using a support substrate. The third method is a method of forming electronic device components on a support substrate and then transferring them to a plastic film.
[0006] The second method is to form directly on the film by a roll-to-roll method, etc., but since there is no supporting substrate, the size of the film is easy to change, and there are problems in the size of the pattern processing and the accuracy of the pattern overlap. The third method is that when the electronic device element manufactured on the glass supporting substrate is transferred to the plastic film, since even if it is temporary, the plastic substrate supporting the electronic device element does not exist on the base of the electronic device element, the mechanical strength of the electronic device element during transfer is weak and may be damaged. This is particularly significant in the wiring part that must be arranged on the outside of the transferred plastic film in order to obtain electrical connection. Regarding the first method, since the existing electronic device manufacturing equipment can be used, the equipment investment can be suppressed. In addition, since it is fixed to the glass supporting substrate during the manufacturing process, the processing dimensional stability is excellent, and after the glass supporting substrate is separated, the mechanical strength is maintained due to the plastic film. As a result, it has the advantage of being able to easily manufacture the equipment.
[0007] On the other hand, when manufacturing electronic devices by the first method, it is necessary to separate the glass support substrate after forming the electronic device components. However, in this case, after the plastic film is temporarily fixed to the glass support substrate at first, the adhesion between the plastic film and the glass support substrate becomes high due to the high-temperature heating process during the process of forming the electronic device components, and sometimes the separation cannot be easily performed.
[0008] To solve this problem, Patent Document 1 discloses a method of separating a glass supporting substrate by cutting a contact portion of an interface between a glass supporting substrate and a plastic film using a laser.
[0009] In addition, in order to more stably perform separation in the method of separating a glass supporting substrate using a laser disclosed in Patent Document 1, Patent Document 2 discloses a method in which amorphous silicon is inserted between a glass supporting substrate and a plastic substrate, and hydrogen is generated from the amorphous silicon by laser irradiation, thereby promoting separation.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent No. 4870156
[0013] Patent Document 2: Japanese Patent No. 3809681 Summary of the invention
[0014] Problems to be solved by the invention
[0015] In conventional light emitting devices, it is desired to suppress reflection to obtain good visual recognition.
[0016] One embodiment of the present invention provides a light emitting device that suppresses reflection to have good visual recognition.
[0017] Means of solving problems
[0018] A light-emitting device according to one embodiment of the present disclosure includes: a light-transmitting substrate; a light-emitting device element formed on one main surface of the light-transmitting substrate; and a porous layer formed on the other main surface of the light-transmitting substrate and being an organic material layer having a plurality of pores.
[0019] In addition, the comprehensive or specific implementations may be implemented by components, systems or methods, or by any combination of components, devices, systems and methods.
[0020] Effects of the Invention
[0021] A light emitting device according to one embodiment of the present invention can suppress light reflection to obtain good visibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a partial cross-sectional view schematically showing the structure of the display device according to the first embodiment of the present invention.
[0023] Figure 2 This is a microscope photograph of a cross section of a porous layer and a light-transmitting substrate in the display device according to the present embodiment.
[0024] Figure 3 (a) is a diagram schematically showing a state of light reflection when the structure of the display device according to this embodiment is applied to a bottom emission type display device. Figure 3 (b) is a diagram schematically showing a state of light reflection when the structure of the display device according to the embodiment is applied to a top emission type display device.
[0025] Figure 4 This is a partial cross-sectional view schematically showing a part of the manufacturing process of the display device according to this embodiment. Figure 4 (a) is a partial cross-sectional view of the supporting substrate. Figure 4 (b) is a partial cross-sectional view showing a state where a porous layer is formed on a supporting substrate. Figure 4 (c) is a partial cross-sectional view showing a state where a light-transmitting substrate is formed on the porous layer. Figure 4 (d) is a partial cross-sectional view showing a state where a sealing layer is formed on a light-transmitting substrate.
[0026] Figure 5 It is schematically indicated Figure 4A partial cross-sectional view of a portion of a subsequent manufacturing process of a display device. Figure 5 (a) is a partial cross-sectional view showing a state where an electrode layer is formed on a sealing layer. Figure 5 (b) is a partial cross-sectional view showing a state where a TFT main body layer is formed on the electrode layer. Figure 5 (c) is a partial cross-sectional view showing a state where an organic EL element layer is formed on the TFT main body layer.
[0027] Figure 6 It is schematically indicated Figure 5 A partial cross-sectional view of a portion of a subsequent manufacturing process of a display device. Figure 6 (a) is a partial cross-sectional view of a support substrate and a display device schematically showing a state in which the porous layer is destroyed and the support substrate is separated. Figure 6 (b) is a partial cross-sectional view schematically showing a completed state of the display device according to the embodiment.
[0028] Figure 7 It is a schematic process diagram showing the manufacturing process of the display device involved in this embodiment.
[0029] Figure 8 (a) is a partial cross-sectional view schematically showing a state in which a display device according to Modification 2 of the present embodiment is formed on a supporting substrate. Figure 8 (b) is a partial cross-sectional view schematically showing the structure of a display device according to Modification 2.
[0030] Fig. 9 This is a partial cross-sectional view schematically showing a part of the manufacturing process of the display device involved in Modification Example 2. Fig. 9 (a) is a partial cross-sectional view schematically showing a state where a first porous layer is formed on a supporting substrate. Fig. 9 (b) is a partial cross-sectional view showing a state where the second porous layer is formed on the first porous layer. Fig. 9 (c) is a partial cross-sectional view schematically showing a state where a light-transmitting substrate is formed on the second porous layer. Fig. 9 (d) is a partial cross-sectional view of the porous layer 220 and the light-transmitting substrate 30 after the support substrate is separated.
[0031] Fig.10 This is a partial cross-sectional view schematically showing a part of the manufacturing process of the display device according to Modification 8 of the present embodiment. Fig.10 (a) is a partial cross-sectional view schematically showing a state where a porous layer is formed on a supporting substrate. Fig.10 (b) is a partial cross-sectional view schematically showing a state where a thin film is formed on a porous layer.
[0032] Fig.11It is schematically indicated Fig.10 A partial cross-sectional view of a portion of a manufacturing process of a display device according to subsequent variation 8. Fig.11 (a) is a partial cross-sectional view schematically showing a state where UV light is irradiated on a thin film. Fig.11 (b) is a partial cross-sectional view schematically showing the state of the film after UV irradiation. Fig.11 (c) is a partial cross-sectional view schematically showing a state where a light-transmitting substrate is formed on the film after UV irradiation.
[0033] Fig.12 It is a partial cross-sectional view schematically showing the structure of a display device not involved in the embodiment of the present invention.
[0034] Fig.13 (a) is a diagram schematically showing a state of light reflection in a bottom emission type display device not involved in the embodiment of the present invention. Fig.13 (b) is a diagram schematically showing a state of light reflection in a top emission type display device not involved in the embodiment of the present invention.
[0035] Fig.14 (a) is a partial cross-sectional view schematically showing a state where an electronic device according to a second embodiment of the present invention is formed on a supporting substrate. Fig.14 (b) is a schematic diagram showing the laser being irradiated on Fig.14 (a) is a partial cross-sectional view of an electronic device and a supporting substrate according to an embodiment.
[0036] Fig.15 This is a microscope photograph of a cross section of a porous layer and a plastic substrate in the electronic device according to the present embodiment.
[0037] Fig.16 This is a partial cross-sectional view schematically showing a part of the manufacturing process of the electronic device according to the present embodiment. Fig.16 (a) is a partial cross-sectional view of the supporting substrate. Fig.16 (b) is a partial cross-sectional view showing a state where a porous layer is formed on a supporting substrate. Fig.16 (c) is a partial cross-sectional view showing a state where a plastic substrate is formed on the porous layer. Fig.16 (d) is a partial cross-sectional view showing a state where a sealing layer is formed on a plastic substrate.
[0038] Fig.17 It is schematically indicated Fig.16 A partial cross-sectional view of a portion of a subsequent manufacturing process of an electronic device. Fig.17 (a) is a partial cross-sectional view showing a state where an electrode layer is formed on a sealing layer. Fig.17(b) is a partial cross-sectional view showing a state where a TFT main body layer is formed on the electrode layer. Fig.17 (c) is a partial cross-sectional view showing a state where an organic EL element layer is formed on the TFT main body layer.
[0039] Fig.18 It is schematically indicated Fig.17 A partial cross-sectional view of a portion of a subsequent manufacturing process of an electronic device. Fig.18 (a) is a partial cross-sectional view schematically showing a state where the electronic device and the supporting substrate are irradiated with laser light before the supporting substrate is separated. Fig.18 (b) is a partial cross-sectional view schematically showing the support substrate and the electronic device after separation.
[0040] Fig.19 It is a schematic process diagram showing a manufacturing process of the electronic device involved in this embodiment.
[0041] Fig. 20 (a) is a partial cross-sectional view schematically showing the structure of the test body TP1. Fig. 20 Fig. 20 (b) is a partial cross-sectional view schematically showing the structure of the test body TP2. Fig. 20 (c) is a partial cross-sectional view schematically showing the structure of the test body TP3.
[0042] Fig.21 It is a diagram showing the evaluation results of the damage suppression effect of laser irradiation in the method for manufacturing the electronic device according to the present embodiment.
[0043] Fig. 22 (a) is a microscope photograph of an electrode layer after laser irradiation in an electronic device not related to this embodiment. Fig. 22 (b) is a schematic representation of Fig. 22 (a) Diagram of the surface state of the electrode layer.
[0044] Fig.23 (a) is a microscope photograph of the test piece TP1 after laser irradiation. Fig.23 (b) is a microscope photograph of the test piece TP2 after laser irradiation. Fig.23 (c) is a microscope photograph of the test piece TP3 after laser irradiation.
[0045] Fig.24 This is a graph showing the measurement results of the variation amounts of the test pieces TP1, TP2, and TP3 after laser irradiation.
[0046] Fig.25 (a) is a partial cross-sectional view schematically showing a state in which an electronic device according to Modification 1 of the present embodiment is formed on a supporting substrate. Fig.25(b) is a partial cross-sectional view schematically showing a state in which the electronic device according to Modification 2 of the present embodiment is formed on a supporting substrate.
[0047] Fig.26 This is a partial cross-sectional view schematically showing a part of the manufacturing process of the electronic device according to Modification 6 of the present embodiment. Fig.26 (a) is a partial cross-sectional view schematically showing a state where a porous layer is formed on a supporting substrate. Fig.26 (b) is a partial cross-sectional view schematically showing a state where a thin film is formed on a porous layer.
[0048] Fig. 27 It is schematically indicated Fig.26 A partial cross-sectional view of a portion of a manufacturing process of an electronic device according to a subsequent variation 6. Fig. 27 (a) is a partial cross-sectional view schematically showing a state where UV light is irradiated onto a thin film. Fig. 27 (b) is a partial cross-sectional view schematically showing the state of the film after UV irradiation. Fig. 27 (c) is a partial cross-sectional view schematically showing a state where a plastic substrate is formed on the film after UV irradiation.
[0049] Fig.28 (a) is a partial cross-sectional view schematically showing a state where an electronic device not related to the present embodiment is formed on a supporting substrate. Fig.28 (b) is a schematic diagram showing the laser being irradiated on Fig.28 (a) is a partial cross-sectional view of an electronic device and a supporting substrate not shown in this embodiment.
[0050] Description of labels:
[0051] 10 Support substrate
[0052] 20 Porous layer
[0053] 21 holes
[0054] 21c Inner surface
[0055] 30 Translucent substrate
[0056] 31 Upper surface (one main surface)
[0057] 32 Lower surface (other main surface)
[0058] 70 Display device component layer (display device component)
[0059] 100, 100a, 100b, 200 display device
[0060] 220a First porous layer (first porous layer portion)
[0061] 220b Second porous layer (second porous layer portion)
[0062] 301 Laminated
[0063] 310 Support substrate
[0064] 320 Porous layer
[0065] 321 empty hole
[0066] 321c Inner surface
[0067] 322 Thin layer coating
[0068] 323 Surface
[0069] 330 Plastic substrate (resin substrate)
[0070] 370 Electronic equipment component layer (electronic equipment components)
[0071] 390 film
[0072] 400 Electronic equipment
[0073] 3020a 1st porous layer
[0074] 3020b Second porous layer DETAILED DESCRIPTION
[0075] Knowledge underlying the present invention
[0076] In a display device, since external light (for example, light from a fluorescent lamp in the house, sunlight outside the house, etc.) is reflected on the display surface (i.e., the surface of the display) and observed as reflection, there is a problem that it becomes difficult for the user to visually recognize the display image of the display. Moreover, in a display device having a stacked structure, there is a situation where the reflection problem is caused not only by the reflection of external light on the display surface, but also by the reflection of external light incident from the display surface into the display device at the interface of the layer, the surface of one or more layers, and the back surface, and then emitted from the display surface. The ease of reflection of light depends not only on the angle of incidence, but also on the difference in refractive index of the materials on both sides of the interface. Generally speaking, the greater the difference in refractive index, the easier it is to reflect. Therefore, the interface between a solid layer and air is more easily reflected than the interface between solid layers such as a resin layer and a glass layer. Therefore, generally speaking, the light reflection on the outermost surface or back surface of the stacked body is greatly related to the problem of reflection.
[0077] Fig.12It is a partial cross-sectional view schematically showing the structure of a display device 500 which is an organic EL display device as an example of a display device not involved in the embodiment of the present invention. Fig.13 (a) is a diagram schematically showing how light reflection occurs when the structure of the display device 500 is applied to a bottom emission type display device 500a. Fig.13 (b) is a diagram schematically showing how light reflection occurs when the structure of the display device 500 is applied to a top emission type display device 500b.
[0078] like Fig.12 As shown, the display device 500 is formed by stacking a sealing layer 540, a TFT layer 550, and an organic EL element layer 560 in sequence on a light-transmitting resin such as acrylic resin or glass. In addition, an interlayer insulating layer or a protective layer may be formed between the layers, and a color filter, a sealing layer, a protective layer, etc. may be formed on the organic EL element layer 560. In addition, the TFT layer 550 and the organic EL element layer 560 constitute a display device element layer 570.
[0079] like Fig.13 As shown in (a), in the case of a bottom-emitting display device 500a not involved in the embodiment of the present invention, external light is reflected by the surface of the light-transmitting substrate 530 and enters the user's eyes together with the light representing the image information, generating reflected light. Fig.13As shown in (b), in the case of a top-emitting display device 500b not involved in the embodiment of the present invention, a portion of the external light incident from the organic EL element layer 560 to the inside of the display device 500b passes through the organic EL element layer 560, the TFT layer 550, the sealing layer 540 and the light-transmitting substrate 530 and reaches the back side of the light-transmitting substrate 530, and is reflected by the back side. Then, the reflected external light passes through the light-transmitting substrate 530, the sealing layer 540, the TFT layer 550 and the organic EL element layer 560 again, and enters the user's eyes together with the light representing the image information, generating reflected light. In addition, the main surface on the user side is set as the front surface, and the main surface on the opposite side to the user is set as the back surface. In the case of the display device 500b, a portion of the external light incident on the inside of the display device 500b is reflected by the interface of the organic EL element layer 560, the TFT layer 550, the sealing layer 540 and the translucent substrate 530, and another portion is reflected and absorbed by the electrodes (not shown) and wiring (not shown) of the organic EL element layer 560 and the TFT layer 550. In addition, since the reflection and absorption occur back and forth, the reflected light causing the reflection is generally weaker than that in the case of the display device 500a. However, in the display device 500b, sometimes, depending on the incident angle of the external light and the area of the display surface from which the external light is incident, strong reflection is caused without almost any reflection and absorption. Such reflection becomes a problem in light-emitting devices.
[0080] Therefore, the present inventors have conducted intensive studies to provide a light emitting device that suppresses reflection and has good visibility.
[0081] A light-emitting device according to one embodiment of the present invention comprises: a light-transmitting substrate; a light-emitting device element formed on one main surface of the light-transmitting substrate; and a porous layer formed on the other main surface of the light-transmitting substrate and being an organic material layer having a plurality of pores.
[0082] By disposing a porous layer on the main surface of the light-transmitting substrate on the opposite side to the side where the light-emitting device element is disposed, when the light-emitting device is a bottom-emitting type, external light incident from the front surface of the display, that is, the main surface side of the light-transmitting substrate on the opposite side to the side where the light-emitting device element is disposed, can be scattered by the porous layer to suppress reflection. In addition, in the case of a top-emitting type, external light incident from the front surface of the display into the light-emitting device is scattered by the porous layer on the main surface of the light-transmitting substrate on the opposite side to the side where the light-emitting device element is disposed, that is, the back surface. Thus, it is possible to suppress the situation where the external light incident into the light-emitting device is reflected by the back surface of the light-transmitting substrate and emitted again from the front surface of the display to generate reflection.
[0083] In addition, by making the porous layer an organic material layer, the following effects can be obtained, which are different from porous inorganic materials or inorganic particles. That is, by making the porous layer an organic material layer, the softness (flexibility) is excellent. Since the load required to bend the organic material layer is small, it is easy to bend. Therefore, the stress on the device element is small when the bending load is applied, and it is difficult to cause damage to the device element. In addition, by making the porous layer an organic material layer, the impact from the outside can be alleviated to prevent damage to the device. In addition, since the porous layer is an organic material layer, for example, when it is peeled off from the supporting substrate by laser irradiation during manufacturing, the heat diffusion to the surrounding caused by laser irradiation will be small. Therefore, the influence of heat on the device element can be suppressed, and the energy of the laser can be efficiently used for the processing of the inorganic material layer. Moreover, by making the porous layer an organic material layer, it can have a heat insulation effect, and the influence on the device element caused by heat from the outside can be reduced. As the organic material layer, a porous polyimide film can be used.
[0084] Furthermore, the porous layer may not contain inorganic particles.
[0085] Furthermore, on the main surface of the porous layer on the opposite side to the light-transmitting substrate, inner surfaces of some of the plurality of pores are exposed, and gas may exist in the pores whose inner surfaces are exposed.
[0086] Thus, in the case where the light emitting device is a bottom emission type, since the main surface of the porous layer on the opposite side to the light-transmitting substrate is the display surface, the inner surface of a part of the pores of the porous layer is exposed, and the resulting concavo-convexity exists on the display surface. Thus, since the external light is scattered by the display surface, the reflection is suppressed. In addition, since the external light is scattered by the display surface, the incidence of the external light into the inside of the light emitting device is suppressed, and as a result, the reflection caused by the external light incident into the inside of the light emitting device being reflected by the inside of the light emitting device and emitted from the display surface again can be suppressed, and the reflection suppression effect is further improved.
[0087] Furthermore, an average diameter of the pores in a portion of the porous layer on the light-transmitting substrate side may be smaller than an average diameter of the pores in a portion of the porous layer on the opposite side to the light-transmitting substrate.
[0088] Thus, when the light emitting device is a top emission type, more incident light is scattered in a region farther from the display surface, thereby making it possible to suppress the influence of scattered light on the displayed image.
[0089] In addition, in the porous layer, the average diameter of the pores in the first porous layer portion including the main surface on the opposite side of the translucent substrate can be smaller than the average diameter of the pores in the second porous layer portion which is located closer to the translucent substrate side than the first porous layer portion.
[0090] In the case of a bottom-emitting light-emitting device, although the inner surface of a part of the pores of the porous layer is exposed on the display surface to form unevenness, the unevenness can be reduced because the average diameter of the pores in the first porous layer portion is smaller. This can suppress the deterioration of the visual impression or the displayed image quality. In addition, even in the case of a touch screen type light-emitting device, since the unevenness on the touch screen surface is small, a smooth operating feeling can be provided.
[0091] Furthermore, the light emitting device element may emit light for image display toward the light-transmitting substrate.
[0092] The porous layer may be made of a light-transmitting material.
[0093] Therefore, when the structure of the light emitting device as one embodiment of the present invention is applied to a bottom emission type light emitting device, light of image information can pass through the porous layer to reach the user's eyes, and external light can be scattered by the porous layer to suppress reflection.
[0094] In addition, another embodiment of the present invention involves a stacked substrate comprising: a supporting substrate; a porous layer, which is formed above the supporting substrate and is an organic material layer having multiple pores in at least a portion of the area in which gas exists in the internal space; and a resin substrate, which is formed above the porous layer.
[0095] According to the structure of the laminated substrate involved in another embodiment of the present invention, since at least a part of the porous layer has a plurality of pores with gaps inside, the rigidity of the porous layer is lower than that of the resin substrate. Therefore, after forming an electronic device element or a part of its structural component on the top of the resin substrate, when the support substrate is separated by irradiating a laser from the support substrate side, the pressure of the gas that may be generated from the resin substrate during the irradiation of the laser will consume energy for destroying the porous layer. Thus, the stress applied to the resin substrate can be reduced, the deformation of the resin substrate can be suppressed, and thus the damage to the electronic device element formed on the top of the resin substrate can be suppressed.
[0096] Furthermore, the porous layer may not contain inorganic particles.
[0097] In addition, another embodiment of the present invention relates to a method for manufacturing a light-emitting device, which comprises: preparing a supporting substrate, forming a porous layer on top of the supporting substrate, wherein the porous layer is an organic material layer having a plurality of pores, forming a light-transmitting substrate on top of the porous layer, forming a light-emitting device element on top of the light-transmitting substrate, destroying the porous layer within the porous layer or at the interface between the supporting substrate and the porous layer, and separating the supporting substrate from the light-transmitting substrate while at least a portion of the porous layer after the destruction is attached to the light-transmitting substrate.
[0098] According to a method for manufacturing a light-emitting device according to another embodiment of the present invention, a porous layer is formed on the main surface of a translucent substrate on the opposite side to the side where the light-emitting device element is formed. In addition, at least a portion of the porous layer is attached to the main surface of the translucent substrate on the opposite side to the side where the display element is formed. Therefore, in the case where the light-emitting device is a bottom-emitting type, external light incident from the front surface of the display, that is, the main surface side of the translucent substrate on the opposite side to the side where the light-emitting device element is arranged, can be scattered by the porous layer to suppress reflection. In addition, in the case of a top-emitting type, external light incident from the front surface of the display into the light-emitting device will be scattered by the porous layer on the main surface of the translucent substrate on the opposite side to the side where the light-emitting device element is arranged, that is, the back surface. As a result, it is possible to suppress the situation where the external light incident into the light-emitting device is reflected by the back surface of the translucent substrate and emitted again from the front surface of the display to generate reflection.
[0099] In addition, by making the porous layer an organic material layer, unlike porous inorganic materials or inorganic particles, the following effects can be obtained. That is, by making the porous layer an organic material layer, the softness (flexibility) is excellent. Since the load required to bend the organic material layer is small, it is easy to bend. Therefore, the stress on the device components is small when the bending load is applied, and it is difficult to damage the device components. In addition, by making the porous layer an organic material layer, the impact from the outside can be alleviated to prevent damage to the device. In addition, since the porous layer is an organic material layer, for example, when it is peeled off from the supporting substrate by laser irradiation during manufacturing, the heat diffusion to the surrounding caused by laser irradiation is small. Therefore, the influence of heat on the device components can be suppressed, and the energy of the laser can be efficiently used for the processing of the inorganic material layer. Moreover, by making the porous layer an organic material layer, it can have a heat insulation effect, and the influence on the device components caused by heat from the outside can be reduced. As the organic material layer, a porous polyimide film can be used.
[0100] Furthermore, the porous layer may not contain inorganic particles.
[0101] Alternatively, the porous layer may be destroyed by irradiating the porous layer with laser light from the supporting substrate side.
[0102] Thus, the support substrate can be easily separated using laser light.
[0103] Furthermore, the porous layer may be destroyed by applying mechanical stress to the porous layer. Thus, the support substrate can be easily separated using a roller or the like.
[0104] Furthermore, in the porous layer after the destruction, inner surfaces of a part of the plurality of pores are exposed on the main surface opposite to the light-transmitting substrate, and gas may exist in the pores whose inner surfaces are exposed.
[0105] Thus, in the case where the light emitting device is a bottom emission type, since the main surface of the porous layer on the opposite side to the light-transmitting substrate is the display surface, the inner surface of a part of the pores of the porous layer is exposed, and the resulting concavo-convexity exists on the display surface. Thus, since the external light is scattered by the display surface, the reflection is suppressed. In addition, since the external light is scattered by the display surface, the incidence of the external light into the inside of the light emitting device is suppressed, and as a result, the reflection caused by the external light incident into the inside of the light emitting device being reflected by the inside of the light emitting device and emitted from the display surface again can be suppressed, and the reflection suppression effect is further improved.
[0106] Furthermore, an average diameter of the pores in a portion of the porous layer on the light-transmitting substrate side may be smaller than an average diameter of the pores in a portion of the porous layer on the opposite side to the light-transmitting substrate.
[0107] Thus, when the light emitting device is a top emission type, the incident light is scattered more in a region farther from the display surface, thereby suppressing the influence of the scattered light on the displayed image.
[0108] In addition, in the porous layer, the average diameter of the pores in the first porous layer portion including the main surface on the opposite side of the translucent substrate can be smaller than the average diameter of the pores in the second porous layer portion which is located closer to the translucent substrate side than the first porous layer portion.
[0109] In the case of a bottom-emitting light-emitting device, although the inner surface of a part of the pores of the porous layer is exposed on the display surface to form unevenness, the unevenness can be reduced because the average diameter of the pores in the first porous layer portion is smaller. This can suppress the deterioration of the visual impression or the displayed image quality. In addition, even in the case of a touch screen type light-emitting device, since the unevenness on the touch screen surface is small, a smooth operating feeling can be provided.
[0110] Furthermore, the porous layer has the plurality of pores having gas in the internal spaces in at least a part of the region, the light-transmitting substrate is a resin substrate, and the resin substrate can be separated from the support substrate by irradiating laser light from the support substrate side.
[0111] In the above manufacturing method, since at least a part of the porous layer has a plurality of pores with voids inside, the porous layer has a lower rigidity than the resin substrate. Therefore, the pressure of the gas that may be generated from the resin substrate during the irradiation of the laser consumes energy for destroying the porous layer, and the stress applied to the resin substrate can be reduced. Thus, the deformation of the resin substrate can be suppressed, thereby suppressing damage to electronic device components and the like formed above the resin substrate.
[0112] Furthermore, an average diameter of the pores in a portion of the porous layer on the resin substrate side may be smaller than an average diameter of the pores in a portion of the porous layer on the support substrate side.
[0113] Since the porous layer has the above structure, when the resin substrate is formed on the porous layer, the resin material of the resin substrate is not easy to enter the inside of the pores whose inner surface is exposed on the main surface of the porous layer on the side where the resin substrate is formed. Therefore, the gaps inside the pores in the surface layer part on the main surface side can be maintained, and the rigidity of the surface layer part on the main surface side of the porous layer can be suppressed from becoming higher. Thus, it is possible to prevent the porous layer from being easily destroyed by the pressure of the gas generated during the irradiation of the laser, thereby maintaining the stress reduction effect on the resin substrate.
[0114] Here, the pressure of the gas generated by the irradiation of the laser is reduced not only because it is used to destroy the porous layer, but also because the pressure is dispersed to the gas existing in the pores of the porous layer. In particular, when a plurality of pores are connected, a higher pressure dispersion effect can be obtained. Since the porous layer has the above-mentioned structure, the voids inside the pores of the surface layer portion on the main surface side of the porous layer are maintained, so that the gas pressure dispersion effect can be maintained.
[0115] In addition, the porous layer includes: a first porous layer formed above the supporting substrate; and a second porous layer formed above the first porous layer, and the average diameter of the pores in the second porous layer may be smaller than the average diameter of the pores in the first porous layer.
[0116] Thus, since the resin material of the resin substrate is difficult to enter the pores of the second porous layer located on one side of the resin substrate, the voids inside the pores are maintained, and the stress reduction effect on the resin substrate can be maintained. In addition, the dispersion effect of the gas pressure generated during the irradiation of the laser can be maintained. Moreover, since the first porous layer having the highest average diameter larger than the second porous layer is formed on the supporting substrate side of the second porous layer, the rigidity of the porous layer as a whole can be reduced, thereby suppressing the deformation of the resin substrate.
[0117] In addition, the second porous layer can be formed by a dry method or thermal deposition.
[0118] When the second porous layer is formed by a wet method, water or solvent will remain, which may cause gas generation during heating or laser irradiation in the subsequent manufacturing process. Since the second porous layer is formed by a dry method or thermal evaporation, water or solvent will not remain, and gas generation can be suppressed.
[0119] Furthermore, the first porous layer may be formed by coating a first resin material, and the second porous layer may be formed by coating a second resin material. The viscosity of the second resin material may be higher than that of the first resin material.
[0120] Thus, when the second porous layer is formed on the first porous layer, it is difficult for the second resin material to enter the pores exposed on the main surface of the first porous layer on the side where the second porous layer is formed, and the voids in the pores of the first porous layer are maintained. Therefore, the rigidity of the porous layer as a whole can be kept lower than that of the resin substrate.
[0121] In addition, after the porous layer is formed and before the resin substrate is formed, the inner surfaces of a part of the plurality of pores may be exposed on the main surface, i.e., the surface, of the porous layer on the side where the resin substrate is formed. Furthermore, after the porous layer is formed and before the resin substrate is formed, the porous layer may be subjected to affinity treatment so that the affinity of the surface of the porous layer to the resin material used to form the resin substrate is higher than the affinity of the portion other than the surface of the porous layer.
[0122] Thus, when a resin material is applied to a porous layer to form a resin substrate, it is difficult for the resin material to enter the pores exposed on the main surface of the porous layer on the side where the resin substrate is formed. Therefore, the gaps in the pores of the porous layer can be maintained, and the stress reduction effect on the resin substrate can be maintained. In addition, the dispersion effect of the gas pressure generated during laser irradiation can be maintained.
[0123] In addition, the affinity treatment is the following treatment, namely: after forming a thin film on the surface of the porous layer and the exposed inner surface using the following material, the UV light irradiation or plasma treatment is performed from the resin substrate forming side, wherein the material is a material having a lower affinity than that of the material forming the porous layer and having a property that the affinity after the UV light irradiation or plasma treatment is higher than that before the UV light irradiation or plasma treatment.
[0124] In addition, the film can be formed by applying a solution containing the following material on the surface of the porous layer and the exposed inner surface and drying it, wherein the material is a material having a lower affinity than that of the material forming the porous layer and having a property that the affinity after irradiation with UV light or plasma treatment is higher than that before irradiation with UV light or plasma treatment.
[0125] This makes it possible to easily perform the above-mentioned affinity treatment.
[0126] Furthermore, the average diameter of the pores in the portion of the porous layer on the resin substrate side may be 1 μm or less.
[0127] Thus, when the resin substrate is formed on the porous layer, it is difficult for the resin material to enter the pores exposed on the main surface of the porous layer on the side where the resin substrate is formed, and the part of the porous layer on the resin substrate side can maintain the space in the pores, and the stress reduction effect on the resin substrate can be maintained. In addition, the dispersion effect of the gas pressure generated during laser irradiation can be maintained.
[0128] Furthermore, the average diameter of the pores in the second porous layer may be 1 μm or less.
[0129] Thus, when the resin substrate is formed on the second porous layer, it is difficult for the resin material to enter the pores exposed on the main surface of the second porous layer on the side where the resin substrate is formed. Therefore, the space in the pores can be maintained in the portion of the second porous layer on the resin substrate side, and the stress reduction effect on the resin substrate can be maintained. In addition, the dispersion effect of the gas pressure generated during laser irradiation can be maintained.
[0130] Furthermore, the porous layer may have a thin-layer coating portion without the pores on the main surface or surface on the side where the resin substrate is formed, and the thin-layer coating portion may be formed of the same material as that of the porous layer other than the thin-layer coating portion.
[0131] Thus, when the resin substrate is formed on the porous layer, the resin material will not enter the pores of the porous layer because it is blocked by the coated thin layer portion, so the gaps in the pores of the porous layer can be maintained, and the stress reduction effect on the resin substrate can be maintained. In addition, the dispersion effect of the gas pressure generated during laser irradiation can be maintained. Moreover, since the coated thin layer portion is formed of the same material as the porous layer portion, the increase in the types of materials and processes can be suppressed, which is conducive to suppressing the manufacturing cost.
[0132] In addition, the porous layer does not need to contain inorganic particles.
[0133] Hereinafter, specific examples of the embodiments and modifications of the present invention will be shown, and the structures, operations, and effects will be described.
[0134] In addition, the embodiments and modified examples used in the following description are examples used to easily explain the structure and action / effect related to one embodiment of the present invention, and the present invention is not limited to the following embodiments and modified examples except for its essential parts.
[0135] 《First Implementation Method》
[0136] [1. Structure of display device]
[0137] The structure of the display device according to the first embodiment of the present invention is described with reference to the case where the display device is applied to an active matrix organic EL display device as an example. Figure 1 , Figure 2 To explain.
[0138] Figure 1 1 is a partial cross-sectional view schematically showing the structure of a display device 100 according to the present embodiment. In the present embodiment, the display device 100 is an active matrix organic EL display device.
[0139] like Figure 1 As shown, the display device 100 is formed by stacking a porous layer 20, a light-transmitting substrate 30, a sealing layer 40, a TFT layer 50, and an organic EL element layer 60 in this order. The TFT layer 50 is composed of an electrode layer 51 and a TFT main layer 52. The TFT layer 50 and the organic EL element layer 60 constitute a display device element layer (or display device element) 70. The display device 100 has a display device element layer 70 above the upper surface (or one main surface) 31 of the light-transmitting substrate 30, and has a porous layer 20 on the lower surface (or the other main surface) 32 of the light-transmitting substrate 30.
[0140] In addition, Figure 1In the figure, within the solid circle, there is an enlarged cross-sectional view schematically showing the structure of the portion surrounded by the dotted circle in the cross-sectional view of the display device 100 (i.e., the main surface of the porous layer 20 on the opposite side to the translucent substrate 30 and its vicinity).
[0141] (Porous layer)
[0142] like Figure 1 The solid circle of Figure 2 As shown, the porous layer 20 has a plurality of pores 21 inside. Figure 2 : is a scanning microscope photograph of a cross section of a portion near the interface between the porous layer 20 and the light-transmitting substrate 30. Figure 1 As shown in the solid circle, on the main surface 24 of the porous layer 20 opposite to the light-transmitting substrate 30 , the inner surfaces 21 c of some of the pores 21 are exposed, and air exists in the internal space of the pores 21 where the inner surfaces 21 c are exposed.
[0143] Here, in the present embodiment, no matter whether the inner surface of the pore is exposed or the inner surface is not exposed, any gas such as air or gas vaporized from a solvent exists inside the pore 21. In addition, in addition to gas, liquids such as water or solvents, solid foreign matter such as dust, etc. may also exist in the internal space of the pore 21. In addition, for example, a substance having a different light refractive index from the material of the porous layer 20 may also be filled. In this case, the difference between the refractive index of the substance filled in the internal space of the pore and the refractive index of the material of the porous layer 20 is preferably large.
[0144] In addition, the term "pore" here is not limited to unit-shaped pores having a completely closed internal space, but is also used as a concept to include pores in which a part of the wall defining the unit is missing, pores in which the missing part of the wall is exposed on the outside of the layer, and pores in which a plurality of units are connected in a state where the internal spaces of each other are connected.
[0145] Here, the so-called pores refer to pores having a diameter of, for example, 10 nm to 10 μm, more preferably 100 nm to 5 μm. When a plurality of pores are connected, the diameter of each pore may be within the above range.
[0146] Here, the diameter of a hole refers to the length of the internal space of the hole in the direction of expansion of the layer (a direction perpendicular to the thickness direction of the layer).
[0147] Here, the porosity of the porous layer 20 is preferably, for example, 10% or more and 90% or less.
[0148] In addition, the porosity of the porous layer 20 may also be more preferably not less than 50% and not more than 90%. By setting the porosity to not less than 50%, the proportion of the porous layer being destroyed when the supporting substrate is separated by laser can be increased, and as a result, the pressure applied to the light-transmitting substrate 30 can be further reduced. In addition, by setting the porosity to not more than 90%, a certain degree of mechanical strength can be ensured in the porous layer 20, for example, the breakage caused by mechanical stress caused by decompression / pressurization during vacuum film formation in the manufacturing process can be suppressed. The so-called breakage caused by the mechanical stress refers to the peeling of the film, etc., more specifically. In addition, if the porosity is too high, when a resin material (for example, polyimide) is used to form the light-transmitting substrate 30, the resin material will enter the pores, and as a result, the strength of the porous layer 20 will be increased, so the porosity of the porous layer 20 is preferably not more than about 90%.
[0149] In addition, the measuring method of the porosity of porous layer 20, for example, has the following method.After obtaining the cross section of porous layer 20 by mechanical cutting or convergent ion beam processing, observe the cross section by scanning electron microscope, and calculate the ratio of the void in the cross section to the porous partition wall.Because it can be easily assumed that the ratio is also the same in other cross sections, the ratio can be set as the porosity as the volume ratio.In addition, by carrying out the above-mentioned measurement of multiple points in the plane, and taking it on average, the accuracy can be further improved.
[0150] As the material of the porous layer 20 , an organic material can be used.
[0151] Although not particularly limited, the method for forming the porous layer 20 may be a wet forming method or a dry forming method. The temperature in the forming process of the porous layer 20 or the heating temperature after the formation is preferably higher than the temperature in the forming process of each layer formed thereon. The reason is that when the forming process of the upper layer is performed at a higher temperature than the forming temperature of the porous layer 20, the porous layer 20 may change, which is not preferred. For example, water, solvents, and other gases adsorbed in the pores or solid parts of the porous layer 20 may be desorbed during the forming process of the upper layer, and there is a possibility that a failure such as separation may occur between the upper layer and the porous layer 20.
[0152] The thickness of the porous layer 20 is not particularly limited, but is preferably about 1 μm to 1000 μm.
[0153] (Light-transmitting substrate)
[0154] As the material of the light-transmitting substrate 30, although not particularly limited, for example, there are: alkali-free glass (borosilicate glass), alkali glass, soda glass, non-fluorescent glass, phosphoric acid glass, boric acid glass, quartz and other glass materials, insulating materials such as aluminum, etc. In addition, resin materials such as polyethylene, polypropylene, ethylene polymer, polyvinylidene chloride, polyethylene terephthalate, polyethylene naphthalate, polycarbonate, polyethylene sulfonic acid, silicon, acrylic resin, epoxy resin, phenolic resin, polyamide, polyimide, and aramid resin can also be used. Moreover, two or more of these materials can also be mixed and used, and these materials can also be chemically modified. In addition, two or more of the above materials can also be combined to form a multilayer structure.
[0155] When the display device 100 is a flexible display, the light-transmitting substrate 30 needs to have the property of being difficult to crack or break when bent. Without this property, a display device with high flexibility cannot be obtained.
[0156] In addition, when the display device 100 is a flexible display, the film thickness of the light-transmitting substrate 30 is preferably in the range of 1 μm to 1000 μm. If it is thinner, mechanical strength cannot be obtained. If it is thicker, it is difficult to bend, and a display device with high flexibility cannot be obtained.
[0157] The method for forming the translucent substrate 30, when the translucent substrate is made of a resin material, can also be formed by applying a liquid resin material. When the translucent substrate 30 is made of a material such as resin or glass, a substrate that has been formed into a plate or sheet shape can also be bonded to the porous layer 20, without particular limitation. In the case of bonding a substrate that has been formed into a plate or sheet shape, in addition to bonding using an adhesive material, a method of bonding by pressing can also be used. As an adhesive material, any material that can obtain the desired adhesive force, such as a silicone-based material or an acrylic-based material, can be used, without particular limitation. The translucent substrate 30 can also be a plastic substrate 330 described later.
[0158] (Sealing layer)
[0159] As the sealing layer 40 , for example, a silicon nitride film can be used.
[0160] (TFT layer)
[0161] TFTs for driving organic EL elements are formed in the TFT layer 50. The TFT layer 50 is composed of an electrode layer 51 composed of a gate electrode as a part of the TFT and a TFT main body layer 52 which is a part other than the gate electrode of the TFT.
[0162] The electrode layer 51 is formed by forming a metal material film by vacuum evaporation or sputtering, and selectively removing the metal material film by etching, etc. Examples of the material of the electrode layer 51 include: silver; aluminum; an alloy of silver, palladium, and copper; an alloy of silver, rubidium, and gold.
[0163] The TFT main body layer 52 includes a gate insulating film, source-drain electrodes, a bank, a semiconductor layer, a passivation film, etc. The TFT may be a device using silicon as a channel material, a device using an oxide semiconductor such as indium gallium zinc oxide, or a device using an organic semiconductor such as pentacene.
[0164] (Organic EL element layer)
[0165] The organic EL element layer 60 includes: an upper electrode, a lower electrode, and an organic functional layer sandwiched between the upper electrode and the lower electrode. The organic functional layer includes a light-emitting layer. In addition to the light-emitting layer, the organic functional layer may also appropriately include an electron injection layer, an electron transport layer, an electron hole injection layer, an electron hole transport layer, etc. In addition to the upper electrode, the lower electrode, and the organic functional layer, the organic EL element layer 60 may also include a partition layer, a sealing layer, etc., and may also include a color filter, a protective layer, etc.
[0166] The TFT layer 50 and the organic EL element layer 60 constitute a display device element layer 70 .
[0167] In this embodiment, the TFT layer 50 has a multilayer structure including the electrode layer 51 and the TFT main body layer 52 , but the present invention is not limited thereto. For example, when the display device 100 is a passive organic EL display device, the wiring layer corresponds to the TFT layer 50 .
[0168] In addition, when the display device 100 is a liquid crystal display device, an LCD element is formed in the display device element layer 70 .
[0169] [2. Reflection suppression]
[0170] Figure 3 (a) is a partial cross-sectional view schematically showing how light reflection is suppressed when the structure of the display device 100 according to the present embodiment is applied to a bottom emission type display device 100 a . Figure 3 (b) is a partial cross-sectional view schematically showing how light reflection is suppressed when the structure of the display device 100 is applied to a top-emission type display device 100 b .
[0171] exist Figure 3In the case of the bottom emission type display device 100a shown in (a), the light of the image information emitted from the light emitting layer of the organic EL element layer 60 passes through the TFT layer 50, the sealing layer 40, the light-transmitting substrate 30, and the porous layer 20 and enters the user's eyes. In this case, the porous layer 20 is made of a light-transmitting material.
[0172] On the other hand, the external light is reflected by the surface of the porous layer 20 (here, the main surface on the opposite side to the light-transmitting substrate 30) and enters the user's eyes together with the light of the image information. This causes the user to recognize it as reflected light, which reduces the visual recognition of the image information. Figure 1 As shown in the circle of the solid line, on the surface of the porous layer 20, the inner surface 21c of a part of the pores 21 of the porous layer 20 is exposed to form a concave-convex. As a result, since the external light is scattered on the surface of the porous layer 20, the amount of reflected light entering the user's eyes can be reduced, thereby suppressing the reflection. In addition, the external light that passes through the surface of the porous layer 20 and enters the inside of the porous layer 20 will also be scattered by refraction or reflection when passing through the boundary between the solid part of the porous layer 20 and the gas part inside the pores 21 inside the porous layer 20. Therefore, the external light that passes through the porous layer 20 and enters the translucent substrate 30 is reduced, and as a result, the reflection at the interface between the translucent substrate 30 and the sealing layer 40, the reflection at the interface between the sealing layer 40 and the display device element layer 70, and the reflection at the interface of each layer constituting the display device element layer 70 or the surface of the constituent parts such as electrodes are reduced. As a result, the reflection is further suppressed.
[0173] In addition, if Figure 2 As shown, the porous layer 20 forms a layer without pores with a thickness of about 1 μm on the surface of the light-transmitting substrate 30, that is, the covering thin layer portion 22. Therefore, when a resin material is coated on the porous layer 20 to form the light-transmitting substrate 30, there is no situation where the resin material enters the inside of the pores and fills the internal space of the pores with the resin material. Therefore, since the space inside the pores of the porous layer 20 can be maintained, there is an advantage that the amount of light scattering can be maintained to a large extent.
[0174] In the case of the top-emitting display device 100b, the light generated from the organic functional layer of the organic EL element layer 60 is emitted from the upper surface side of the organic EL element layer 60, that is, through the upper electrode to the outside of the display device. Therefore, a light-transmitting material (transparent conductive film) is used for the upper electrode. In addition, in recent years, as a transparent display, there are many cases where materials with good light transmittance are used in the lower electrode and the TFT layer 50. Therefore, the external light incident into the display device 100b from the light emission side of the organic EL element layer 60, that is, the user side, passes through the organic EL element layer 60, the TFT layer 50, the sealing layer 40, and the light-transmitting substrate 30 and enters the inside of the porous layer 20. The light incident into the inside of the porous layer 20 reaches the back side of the porous layer 20 (the main surface on the opposite side to the user, here, the main surface on the opposite side to the light-transmitting substrate 30). Since there is air as a gas outside the porous layer 20 as a solid, it is considered that the external light is easily reflected on the back side of the porous layer 20 as their interface. However, on the back side of the porous layer 20, Figure 1 As shown in the circle of the solid line, the inside 21c of the pores 21 of a part of the porous layer 20 is exposed to form a concavoconvex shape, so that the external light that passes through the layers of the display device 100b and reaches the back side of the porous layer 20 is scattered on the back side of the porous layer 20, and the reflection of the external light on the back side is reduced. As a result, the external light that is reflected by the back side of the porous layer 20 and passes through the layers of the display device 100b again to enter the user's eyes can be reduced, and the reflection of light can be suppressed.
[0175] In addition, Fig.13 In the case of the top-emitting display device 500b not covered by the present embodiment shown in (b), light incident from the outside at an angle relative to the display device is easily reflected by the structural components in the display device element layer 570, and is difficult to reach the back side of the light-transmitting substrate 530. Similarly, light reflected by the back side of the light-transmitting substrate 530 is also reflected by the structural components in the display device element layer 570, and is difficult to be emitted to the user side. Therefore, in the case of using a top-emitting display device, the amount of light reflected by the back side of the light-transmitting substrate 530 and emitted to the user side is small.
[0176] However, light incident perpendicularly to the display surface of the display device (in the display device 500b, the main surface of the organic EL element layer 60 on the user side), specifically, light incident on a light-transmitting area such as between pixels, is reflected. As a result, reflected light may be emitted to the user side, which may have a negative impact on the visual recognition of the image, similar to the bottom emission type.
[0177] In this case as well, the top emission type display device 100 b to which the structure of the display device 100 according to the embodiment is applied can suppress the reflection of light as described above.
[0178] In addition, in the case of a display device using a flat glass substrate other than that of the present embodiment, the condition of light reflection can be avoided by slightly tilting the angle of the display device, and thus it is relatively easy to improve visibility.
[0179] In contrast, in a flexible display device that uses a flexible material such as a resin substrate as a substrate and can be used in a curved manner, the reflection angle of the display surface is continuous for the user. Therefore, even if the angle is adjusted, the position of the angle at which the reflection occurs will move, and it is difficult to set an angle that can completely avoid the reflection. Therefore, in a flexible display device having a curved display, it is particularly important to suppress the reflection of light on the back side of the light-transmitting substrate.
[0180] In this case as well, the top emission type display device 100 b to which the structure of the display device 100 according to the embodiment is applied can effectively suppress light reflection as described above.
[0181] Here, if Figure 2 As shown in FIG. 1 , the diameter of the pores 21a of the porous layer 20 according to the present embodiment, which are close to the light-transmitting substrate 30, is generally smaller than the diameter of the pores 21b of the portion far from the light-transmitting substrate 30. That is, it can be said that the average diameter of the pores 21a is smaller than the average diameter of the pores 21b. In addition, the so-called average diameter can be expressed by the area 10×10μm 2 The average diameter of the region can be represented by observing 2 to 3 points of the cross section of the porous layer 20 using a focused ion beam (FIB) scanning electron microscope (SEM), for example.
[0182] In the case of a top emission type display device, incident light at an angle that would not be reflected in a direction to enter the user's eyes if the porous layer 20 is not provided may be scattered by the porous layer 20 and enter the user's eyes.
[0183] Here, when the average diameter of the pores 21 in the portion close to the light-transmitting substrate 30 is large, the number of pores 21 per unit volume is small in the portion close to the light-transmitting substrate 30, so the number of times the incident light is refracted and reflected in this portion becomes small. Therefore, the incident light may be hardly dispersed and enter the user side with a high light intensity.
[0184] However, in the display device 100 involved in the present embodiment, as described above, the average diameter of the pores 21a in the portion of the porous layer 20 closer to the light-transmitting substrate 30 is smaller than the average diameter of the pores 21b in the portion farther away. Therefore, the number of pores 21 per unit volume in the portion closer to the light-transmitting substrate 30 is greater than that in the portion farther away. Therefore, in the portion closer to the light-transmitting substrate 30, the number of times the incident light is refracted and reflected increases, and the incident light is dispersed more evenly. As a result, in the case where the incident light is reflected to the user side in the portion closer to the light-transmitting substrate 30, since the reflected light is dispersed and weakened, the influence of the reflected light caused by the porous layer 20 can be suppressed.
[0185] In the case of a bottom-emitting display device, since the average diameter of the pores 21a in the porous layer 20 closer to the light-transmitting substrate 30 is small and the porous layer 20 has pores with different average diameters, light in a wider wavelength range can be scattered. Thus, a scattering effect can be effectively obtained for the entire visible light region.
[0186] [3. Method for manufacturing display device]
[0187] Below, refer to Figure 4 , Figure 5 , Figure 6 , Figure 7 A method for manufacturing the display device 100 according to this embodiment will be described. Figure 4 , Figure 5 , Figure 6 It is a partial cross-sectional view schematically showing a part of the manufacturing process of the display device 100 according to the present embodiment. Figure 7 Schematic process diagram showing a manufacturing process of the display device 100 according to the present embodiment.
[0188] First, if Figure 4 As shown in (a), a supporting substrate 10 ( Figure 7 The support substrate 10 is a member on which the display device 100 is formed and serves as a base when the display device 100 is formed.
[0189] As the material of the support substrate 10, for example, there are glass materials such as alkali-free glass (borosilicate glass), alkali glass, soda glass, non-fluorescent glass, phosphate glass, boric acid glass, quartz, and insulating materials such as aluminum, but it is not particularly limited thereto. In this embodiment, specifically, EAzLE2000 manufactured by Corning is used as the support substrate 10.
[0190] In order to form thin film device elements such as display device elements, the surface of the support substrate 10 (the main surface forming the display device 100 side) is preferably highly flat after temporarily fixing the light-transmitting substrate 30. Specifically, the maximum height difference is preferably 10 μm or less, more preferably 1 μm or less.
[0191] In addition, in order to achieve good adhesion with the next layer to be formed, the surface of the support substrate 10 is preferably kept clean. As a surface cleaning method, UV light irradiation, ozone treatment, plasma treatment, hydrofluoric acid treatment, etc. can be used. In this embodiment, specifically, for example, the surface of the support substrate 10 is cleaned by performing excimer UV (wavelength 172nm) treatment on the surface.
[0192] Furthermore, a layer for improving adhesion with a layer formed thereon may be provided on the surface of the support substrate 10. As the layer for improving adhesion, for example, a silicon oxide film may be used.
[0193] Next, if Figure 4 As shown in (b), a porous layer 20 ( Figure 7 In the present embodiment, specifically, for example, polyimide is applied on the support substrate 10 by spin coating, and heated at a heating temperature of 400° C. for 8 hours to form a porous polyimide layer with a film thickness of 18 μm, i.e., the porous layer 20. Specifically, the polyimide used as the material of the porous layer 20 is, for example, U-imide varnish type BP manufactured by UNITIKA.
[0194] Then, if Figure 4 As shown in FIG. 2( c ), a light-transmitting substrate 30 ( Figure 7 In the present embodiment, for example, a polyimide layer having a thickness of 30 μm is formed by spin coating on the porous layer 20 to form a light-transmitting substrate 30 as a substrate of a flexible display. Specifically, the polyimide used as a material of the light-transmitting substrate 30 is, for example, U-Varnish manufactured by Ube Industries.
[0195] Then, if Figure 4 As shown in (d), a sealing layer 40 is formed on the light-transmitting substrate 30 ( Figure 7 In the present embodiment, the sealing layer 40 is formed by, for example, forming a silicon nitride film having a film thickness of 1 μm at 300° C. by capacitively coupled plasma CVD.
[0196] Then, if Figure 5As shown in (a), after a metal thin film is formed on the sealing layer 40, an etching process is performed to form an electrode layer 51 ( Figure 7 In the present embodiment, specifically, a layer having a thickness of 100 nm made of an alloy of molybdenum and tungsten is manufactured by sputtering, patterned by photolithography using a resist, and etched by a mixture of phosphoric acid / nitric acid / acetic acid to form the electrode layer 51.
[0197] Next, if Figure 5 As shown in (b), a TFT main body layer 52 is formed on the electrode layer 51 to complete the TFT layer 50 ( Figure 7 Step S6).
[0198] Then, if Figure 5 As shown in (c), an organic EL element layer 60 is formed on the TFT layer 50 ( Figure 7 Step S7). Thus, an electronic device body 1000 in which the display device 100 is formed on the supporting substrate 10 is obtained.
[0199] Then, if Figure 6 As shown in (a), the porous layer 20 is destroyed within the porous layer 20 to separate the light-transmitting substrate 30 from the supporting substrate 10 ( Figure 7 Step S8), such as Figure 6 As shown in (b), the display device 100 is obtained.
[0200] In order to separate the support substrate 10, for example, a method of irradiating laser light from the support substrate 10 side toward the electronic device body 1000 or a method of mechanical separation using a roller can be adopted. In the present embodiment, specifically, for example, the support substrate 10 is separated by scanning and irradiating an excimer laser having a wavelength of 305 nm, a pulse width of 20 ns per time, and an irradiation area of 20.0 mm×1.0 mm from the support substrate 10 side.
[0201] In addition, it is not limited to Figure 6 In the method shown in (a), the supporting substrate 10 is separated by destroying the porous layer 20 in the layer, and a part of the porous layer 20 is attached to the light-transmitting substrate 30. Alternatively, the supporting substrate 10 may be separated from the porous layer 20 at the interface between the porous layer 20 and the supporting substrate 10, and the entire porous layer 20 may be attached to the light-transmitting substrate 30. That is, it is sufficient as long as at least a part of the porous layer 20 is attached to the light-transmitting substrate 30 after the support substrate 10 is separated. However, in this case, it is preferred that the entire main surface of the light-transmitting substrate 30 on the opposite side to the sealing layer 40 is covered by the porous layer 20. It is preferred that at least the area corresponding to the image display area is covered by the porous layer 20, even if not the entire surface.
[0202] In addition, in the display device 100 according to this embodiment, Figure 2 As shown, the average diameter of the pores 21a of the porous layer 20 closer to the light-transmitting substrate 30 is smaller than the average diameter of the pores 21b of the porous layer 20 farther from the light-transmitting substrate 30. As a result, the unevenness of the upper surface (the main surface on the side where the light-transmitting substrate 30 is formed) of the porous layer 20 can be reduced, and the influence of the unevenness on the layers formed above the porous layer 20 is reduced, so that a higher quality display device can be obtained.
[0203] Specifically, the average diameter of the pores on the light-transmitting substrate 30 side of the porous layer 20 is preferably, for example, 10 nm or more and 100 nm or less. Specifically, the average diameter of the pores on the supporting substrate 10 side of the porous layer 20 is preferably, for example, 100 nm or more and 10 μm or less.
[0204] In order to eliminate the above-mentioned reflection problem, a method of dispersing fillers in a light-transmitting substrate to suppress the reflection of incident light is also considered. However, in this case, there is a disadvantage that the upper surface of the light-transmitting substrate is formed with unevenness due to the influence of the fillers, which reduces the sealing performance of the sealing layer 40 formed thereon. According to the structure of the display device 100 involved in this embodiment, reflection can be suppressed without reducing the sealing performance of the sealing layer 40.
[0205] In addition, in order to suppress reflection, when a polarizing film is used, especially in the case of a bottom-emitting type, the light of the image information is also changed, so there is a disadvantage that the amount of light entering the user's eyes is reduced and the brightness of the display screen is greatly reduced. According to the structure of the display device 100 involved in this embodiment, reflection can be suppressed without significantly reducing the brightness of the display screen.
[0206] 《Variation Example》
[0207] As mentioned above, although this invention was demonstrated based on embodiment, this invention is not limited to the said embodiment, and the following modification examples are possible.
[0208] (Variant 1)
[0209] In the embodiment, the porous layer 20 has the thin-layer coating portion 22 , but the present invention is not limited thereto and the porous layer 20 may have a structure without the thin-layer coating portion 22 .
[0210] In this case, the average diameter of the pores in the part of the porous layer 20 on the light-transmitting substrate 30 side is preferably smaller than the average diameter of the pores in the part on the supporting substrate side. If the average diameter of the pores in the part on the light-transmitting substrate 30 side is smaller, it is difficult for the coated resin material to enter the pores when the light-transmitting substrate 30 is formed by coating using a resin material, so that the voids can be maintained, and the light scattering effect of the part of the porous layer 20 closer to the light-transmitting substrate 30 can be maintained.
[0211] In the above embodiment, the porous layer 20 is formed by applying a resin material and then heating it. However, generally speaking, the closer the bubbles of the solvent are to the surface, the easier they are to escape. Therefore, the closer the bubbles are to the surface, the smaller the average diameter of the pores. The thin coating portion 22 may be prevented from being formed by adjusting the heating temperature and heating time when forming the porous layer 20, and the type and dosage of the solvent of the resin material.
[0212] (Variant 2)
[0213] In the display device 100 according to the above embodiment, the porous layer 20 has a single-layer structure, but the present invention is not limited thereto and the porous layer 20 may have a multi-layer structure composed of a plurality of sub-layers.
[0214] Figure 8 (a) is a partial cross-sectional view schematically showing the structure of an electronic device body 2000 in which a display device 200 according to Modification 2 is formed on a supporting substrate 10 . Figure 8 (b) is a partial cross-sectional view schematically showing the structure of the display device 200 .
[0215] like Figure 8 As shown in (a) and (b), the display device 200 includes a porous layer 220, and the porous layer 220 is composed of two sub-layers, namely a first porous layer 220a and a second porous layer 220b.
[0216] Fig. 9 FIG. 2 is a partial cross-sectional view schematically showing a part of the manufacturing process of the display device 200 . Fig. 9 (a) is a partial cross-sectional view schematically showing a state where the first porous layer (first porous layer portion) 220 a is formed on the supporting substrate 10 . Fig. 9 (b) is a partial cross-sectional view schematically showing a state where the second porous layer (second porous layer portion) 220b is formed on the first porous layer 220a. Fig. 9 (c) is a partial cross-sectional view schematically showing a state where the light-transmitting substrate 30 is formed on the second porous layer 220b. Fig. 9(d) is a partial cross-sectional view of the porous layer 220 and the light-transmitting substrate 30 of the display device 200 after the support substrate 10 is separated. Fig. 9 In (d), the sealing layer 40, the TFT layer 50, and the organic EL element layer 60 are omitted.
[0217] like Fig. 9 As shown in (b), (c), and (d), in the display device 200 according to the second modification, the average diameter of the pores in the first porous layer 220a is smaller than the average diameter of the pores in the second porous layer 220b.
[0218] As described in the above-mentioned modification 1, when a porous layer is formed by applying a resin material and then heating it, generally, the average diameter of the pores decreases as the distance from the surface increases.
[0219] Here, when the porous layer is formed as a single layer as in the display device 100 according to the embodiment, if the average diameter of the pores in the porous layer 20 becomes too small, a portion with a very small pore diameter and a low porosity or a portion where the pores disappear and no pores exist may be formed near the surface. Thus, in the case of being applied to a top-emitting display device in particular, a sufficient light diffusion effect may not be obtained.
[0220] On the other hand, when the average diameter of the pores in the porous layer 20 is large, especially in the case of a bottom-emitting display device, the part of the porous layer 20 that is in close contact with the support substrate 10, that is, the part of the side with a large diameter of the pores, will be exposed on the user side. At this time, if the diameter of the pores is too large, the unevenness of the display surface becomes larger, and there is a possibility that the visual impression or the image quality of the display will deteriorate. In addition, when the display functions as a touch screen, the tactile feeling when the user touches it with a finger to operate it may be not smooth, and a good operating feeling cannot be provided.
[0221] In the display device 200 involved in the second variant, the porous layer 220 is composed of a first porous layer 220a and a second porous layer 220b formed on the first porous layer 220a, and the average diameter of the pores in the first porous layer 220a is smaller than the average diameter of the pores in the second porous layer 220b. Therefore, even in the case of being applied to a top-emitting display device, since the average diameter of the pores in the second porous layer 220b on the side of the light-transmitting substrate 30 is larger, the porosity is ensured and a sufficient light diffusion effect is obtained. In addition, in the case of being applied to a bottom-emitting display device, as shown in FIG. Fig. 9As shown in (d), the first porous layer 220a having a small average diameter of pores is exposed on the user side. Therefore, the unevenness of the display surface becomes smaller, which can suppress the deterioration of the visual impression or the image quality of the display. In addition, even in the case of a touch screen type display device, since the unevenness of the touch screen surface is small, a smooth operating feeling can be provided.
[0222] In addition, as in the porous layer 220 involved in variant example 2, the average diameter of the pores in the portion on the main surface side opposite to the translucent substrate 30 (in this case, the porous layer 220a) may be smaller than the average diameter of the pores in the porous layer 220 at a specified thickness position (in this case, the portion on the first porous layer 220a side of the porous layer 220b).
[0223] In addition, although the porous layer 220 is composed of two sub-layers in the second modification, the present invention is not limited thereto and may be composed of three or more sub-layers.
[0224] (Variant 3)
[0225] In addition, in the above-mentioned modification 2, the viscosity of the second resin material used to form the second porous layer 220b is preferably higher than the viscosity of the first resin material used to form the first porous layer 220a. As a result, since the second resin material used to form the second porous layer 220b is difficult to enter the pores of the first porous layer 220a, the porosity of the first porous layer 220b can be maintained.
[0226] (Variant 4)
[0227] In the above-mentioned modification 2, the case where the average diameter of the pores of the first porous layer 220a is smaller than the average diameter of the pores of the second porous layer 220b is described. However, this is not limited to this, and the average diameter of the pores of the first porous layer 220a may also be larger than the average diameter of the pores of the second porous layer 220b.
[0228] In this case, the light scattering effect in the first porous layer 220a having a larger average diameter of pores becomes greater. Therefore, since more incident light is scattered in a region farther from the image emission surface (here, the light-emitting layer of the organic EL element layer 60), the influence of scattered light on the displayed image can be suppressed.
[0229] (Variant 5)
[0230] In the case where the porous layer 220 has the first porous layer 220a and the second porous layer 220b as in the above-mentioned variation 2, the second porous layer 220b can be formed by any dry method such as CVD method, sputtering method, and evaporation method. In the case where the second porous layer 220b is formed by a wet method, water or solvent will remain in the pores or inside the solid part of the second porous layer 220b. Therefore, in the case of a heating step in the subsequent manufacturing process or laser irradiation when separating the support substrate 10, it will become a cause of gas generation at this time. In the case where the second porous layer 220b is formed by a wet method or thermal evaporation, water or solvent will not remain, and the generation of gas can be suppressed.
[0231] (Variant 6)
[0232] When the light-transmitting substrate 30 is bonded to the porous layer 20, an adhesive layer may be provided between the porous layer 20 and the light-transmitting substrate 30. Since the adhesive layer is generally formed by coating, it is difficult for the material of the adhesive layer to penetrate into the pores with a small average diameter of the pores in the surface portion of the porous layer 20 on the side where the light-transmitting substrate 30 is formed. In addition, when bonded, the area of the surface of the porous layer 20 that is in close contact with the light-transmitting substrate 30 is larger than that in the case where the average diameter of the pores in the surface portion of the porous layer 20 on the side where the light-transmitting substrate 30 is formed is larger, and the close contact with the light-transmitting substrate 30 is higher. As a result, it is possible to prevent the light-transmitting substrate 30 from being accidentally separated from the porous layer 20 during the manufacturing process of the display device.
[0233] (Variant 7)
[0234] In addition, the resin material of the translucent substrate 30 can be filled in the pores of the part near the main surface on the translucent substrate 30 side of the porous layer 20, and the gas can be present in the pores of the part of the porous layer 20 on the opposite side of the translucent substrate 30 to form voids. When the pores are in a void state, the refractive index difference when light passes through the inside of the pores will be greater, and the scattering of light will be greater. Therefore, by filling the pores of the part on one side of the translucent substrate 30 with a resin material, the pores of the part on the opposite side of the translucent substrate 30 will be kept in a void state, so that more scattering of incident light will be generated in the area farther from the image emission surface (here, the light-emitting layer of the organic EL element layer 60). As a result, the influence of scattered light on the displayed image can be suppressed.
[0235] (Variant 8)
[0236] When the light-transmitting substrate 30 is formed by coating with a resin material, an affinity treatment may be performed after the step of forming the porous layer 20 and before the step of forming the light-transmitting substrate 30 so that the resin affinity of the inner surface 21c of the pores 21 exposed on the surface 23 is higher than that of the surface (the main surface on the side where the light-transmitting substrate 30 is formed) 23 of the porous layer 20 (see Fig.10 (a) The affinity for the resin material of the light-transmitting substrate 30 (hereinafter, simply referred to as “resin affinity”) is low.
[0237] Below, refer to Fig.10 as well as Fig.11 , to illustrate the above affinity treatment method.
[0238] Fig.10 (a) is a partial cross-sectional view showing a state where the porous layer 20 is formed on the supporting substrate 10. As shown in the figure, on the surface 23 of the porous layer 20, the inner surfaces 21c of a part of the pores 21 are exposed.
[0239] Next, if Fig.10 As shown in (b), a thin film 90 having low resin affinity is formed on the surface 23 and the inner surface 21c. The thin film 90 can be formed by, for example, applying a solution containing a material having low resin affinity to the surface 23 and the inner surface 21c and then drying the solution.
[0240] Then, if Fig.11 As shown in (a), UV light is irradiated from the film 90 side. Fig.11 As shown in (b), in the film 90, the portion formed on the surface 23 of the porous layer 20, the shallow portion of the inner surface 21c of the pore 21, and the portion formed on the region corresponding to the bottom surface of the large opening are exposed to UV light, and the resin affinity is improved, and the high resin affinity portion 90a is formed. On the other hand, even in the portion deep in the inner surface 21c of the pore 21 or the portion close to the opening, the portion inclined to be parallel to the irradiation direction of the UV light does not reach enough UV light, so it is not exposed to UV light, and the resin affinity is kept low, and the low resin affinity portion 90b is formed.
[0241] Here, in this modification, the film 90 is a part of the porous layer 20. In addition, the portion of the film 90 exposed to the UV light is included in the surface 23 of the porous layer 20, and the portion not exposed to the UV light is included in the inner surface 21c of the pore 21 of the porous layer 20.
[0242] Then, if Fig.11As shown in (c), a resin material is applied from a film 90 to form a light-transmitting substrate 30. At this time, since there is a low resin affinity portion 90b on the inner surface 21c of the pore 21, it is difficult for the resin material to enter the pore, and the porosity near the surface of the porous layer 20 can be maintained.
[0243] On the other hand, since the high resin affinity portion 90a is formed on the surface 23, the porous layer 20 and the light-transmitting substrate 30 have high adhesion, which can prevent the light-transmitting substrate 30 from being accidentally separated from the porous layer 20 in the remaining manufacturing steps of the subsequent electronic device.
[0244] In the above description, UV light is used for the resin affinity treatment, but the present invention is not limited thereto and the affinity treatment may be performed by light (visible light) irradiation or plasma treatment instead of UV light irradiation, depending on the type of the film 90 .
[0245] Other knowledge underlying the present invention
[0246] The present invention relates to a method for manufacturing an electronic device and a laminated substrate, and in particular, to a method for manufacturing an electronic device capable of reducing damage to the electronic device when a supporting substrate is separated and a laminated substrate used in the manufacturing method.
[0247] Fig.28 (a) is a cross-sectional view schematically showing a state in which an active matrix organic EL display device is formed on a supporting substrate, taking an example as an electronic device not covered by the embodiment of the present invention, and the electronic device body 9000 formed by forming an electronic device not covered by the embodiment of the present invention (here, an organic EL display device) 600 on a supporting substrate 610 is formed by stacking a supporting substrate 610 made of glass, a plastic substrate 630 mainly composed of a resin material, a sealing layer 640, a TFT (Thin Film Transistor) layer 650, and an organic EL element layer 660 in this order. In addition, the electronic device element layer 670 is composed of the TFT layer 650 and the organic EL element layer 660. In addition, the electronic device 600 is composed of a plastic substrate 630, a sealing layer 640, and an electronic device element layer 670 (TFT layer 650 and organic EL element layer 660).
[0248] Here, in the case of an amorphous silicon layer as in Patent Document 2, hydrogen gas is generated by laser irradiation as described above. However, even in the case of no amorphous silicon layer, sometimes a portion of the plastic substrate 630 in close contact with the support substrate 610 is destroyed by laser irradiation, and a relatively high-pressure gas is generated due to ablation or thermal decomposition. The generation of this gas causes mechanical traction displacement at the interface between the support substrate 610 and the plastic substrate 630, and between the closely contacted portions adjacent to the portion being separated. In addition, since the rigidity of the plastic substrate 630 is lower than that of the support substrate 610, Fig.28 As shown in (b), the plastic substrate 630 is deformed and lifted upward due to the pressure of the generated gas G. Due to the deformation of the plastic substrate 630, stress is applied to the layers or electronic device elements arranged above the plastic substrate 630, which are likely to be damaged. In particular, the sealing layer 640 composed of a silicon nitride thin film, the TFT layer 650 having an electrode layer composed of a metal thin film, etc. are easily damaged.
[0249] Therefore, the present inventors have conducted intensive studies to suppress damage to the device when separating the supporting substrate in a method for manufacturing an electronic device in which the supporting substrate is separated after forming electronic device elements on a plastic film disposed on the supporting substrate.
[0250] In a method for manufacturing an electronic device according to one embodiment of the present invention, a porous layer is formed between a support substrate and a resin substrate. The porous layer has a plurality of pores in which gas exists in the internal space in at least a portion of its region. In addition, since there is gas inside the pores, that is, there are gaps inside the pores, the rigidity of the porous layer is lower than that of the resin substrate in at least a portion of the above-mentioned region, and it is more easily deformed and damaged than the resin substrate. Therefore, since the pressure of the gas causes the above-mentioned at least a portion of the region of the porous layer to be deformed or damaged, and the pressure of the gas is relaxed, the stress on the resin substrate can be reduced, wherein the pressure of the gas is generated from the resin substrate that is destroyed by ablation caused by laser irradiation, etc. Thus, damage to electronic device components formed above the resin substrate can be suppressed.
[0251] In the laminated substrate involved in another embodiment of the present invention, the stress on the resin substrate can be reduced for the same reason as above. Thus, when electronic device components (electronic device components or part of their structural components) are formed on or above the resin substrate, damage to the electronic device components can be suppressed.
[0252] A method for manufacturing an electronic device according to one embodiment of the present invention comprises: preparing a support substrate, forming a porous layer having a plurality of pores in at least a portion of the support substrate, wherein a gas is present in the internal space, on top of the support substrate. Next, forming a resin substrate on top of the porous layer, and forming an electronic device element on top of the resin substrate. Then, irradiating the support substrate with laser light, thereby separating the resin substrate from the support substrate.
[0253] In the above manufacturing method, since at least a part of the porous layer has a plurality of pores with voids inside, the porous layer has a lower rigidity than the resin substrate. Therefore, the pressure of the gas that may be generated from the resin substrate during the irradiation of the laser consumes energy for destroying the porous layer, and the stress applied to the resin substrate can be reduced. Thus, the deformation of the resin substrate can be suppressed, thereby suppressing damage to electronic device components and the like formed above the resin substrate.
[0254] Furthermore, an average diameter of the pores in a portion of the porous layer on the resin substrate side may be smaller than an average diameter of the pores in a portion of the porous layer on the support substrate side.
[0255] Since the porous layer has the above structure, when the resin substrate is formed on the porous layer, the resin material of the resin substrate is difficult to enter the inside of the pores on the main surface of the porous layer on the side where the resin substrate is formed. Therefore, the gaps inside the pores in the surface layer part on the main surface side can be maintained, and the rigidity of the surface layer part on the main surface side of the porous layer can be suppressed from becoming higher. Thus, it is possible to prevent the porous layer from being easily destroyed by the pressure of the gas generated during the irradiation of the laser, thereby maintaining the stress reduction effect on the resin substrate.
[0256] Here, the pressure of the gas generated by the irradiation of the laser is reduced not only because it is used to destroy the porous layer, but also because the pressure is dispersed to the gas existing in the pores of the porous layer. In particular, when a plurality of pores are connected, a higher pressure dispersion effect can be obtained. Since the porous layer has the above-mentioned structure, the gap inside the pores of the surface layer part on the main surface side of the porous layer is maintained, the gas pressure dispersion effect can be maintained.
[0257] In addition, the porous layer includes: a first porous layer formed above the supporting substrate; and a second porous layer formed above the first porous layer, and the average diameter of the pores in the second porous layer may be smaller than the average diameter of the pores in the first porous layer.
[0258] Thus, since the resin material of the resin substrate is difficult to enter the pores of the second porous layer located on one side of the resin substrate, the voids inside the pores are maintained, and the stress reduction effect on the resin substrate can be maintained. In addition, the dispersion effect of the gas pressure generated during the irradiation of the laser can be maintained. Moreover, since the first porous layer having a maximum average diameter larger than the second porous layer is formed on the supporting substrate side of the second porous layer, the rigidity of the porous layer as a whole can be reduced, thereby suppressing the deformation of the resin substrate.
[0259] Alternatively, the second porous layer may be formed by a dry method or thermal deposition.
[0260] When the second porous layer is formed by a wet method, water or solvent will remain, which may cause gas generation during heating or laser irradiation in the subsequent manufacturing process. Since the second porous layer is formed by a dry method or thermal evaporation, water or solvent will not remain, and gas generation can be suppressed.
[0261] Furthermore, the first porous layer may be formed by coating a first resin material, and the second porous layer may be formed by coating a second resin material. The viscosity of the second resin material may be higher than that of the first resin material.
[0262] Thus, when the second porous layer is formed on the first porous layer, it is difficult for the second resin material to enter the pores exposed on the main surface of the first porous layer on the side where the second porous layer is formed, and the voids in the pores of the first porous layer are maintained. Therefore, the rigidity of the porous layer as a whole can be kept lower than that of the resin substrate.
[0263] In addition, after the porous layer is formed and before the resin substrate is formed, the inner surfaces of a part of the plurality of pores may be exposed on the main surface, i.e., the surface, of the porous layer on the side where the resin substrate is formed. Furthermore, after the porous layer is formed and before the resin substrate is formed, the porous layer may be subjected to affinity treatment so that the affinity of the surface of the porous layer to the resin material used to form the resin substrate is higher than the affinity of the portion other than the surface of the porous layer.
[0264] Thus, when a resin material is applied to a porous layer to form a resin substrate, it is difficult for the resin material to enter the pores exposed on the main surface of the porous layer on the side where the resin substrate is formed. Therefore, the gaps in the pores of the porous layer can be maintained, and the stress reduction effect on the resin substrate can be maintained. In addition, the dispersion effect of the gas pressure generated during laser irradiation can be maintained.
[0265] In addition, the affinity treatment is the following treatment, namely: after forming a thin film on the surface of the porous layer and the exposed inner surface using the following material, the UV light irradiation or plasma treatment is performed from the resin substrate forming side, wherein the material is a material having a lower affinity than that of the material forming the porous layer and having a property that the affinity after the UV light irradiation or plasma treatment is higher than that before the UV light irradiation or plasma treatment.
[0266] In addition, the film can also be formed by applying a solution containing the following material on the surface of the porous layer and the exposed interior and drying it, wherein the material is a material having a lower affinity than that of the material forming the porous layer and having a property that the affinity after irradiation with UV light or plasma treatment is higher than that before irradiation with UV light or plasma treatment.
[0267] This makes it possible to easily perform the above-mentioned affinity treatment.
[0268] Furthermore, the average diameter of the pores in the portion of the porous layer on the resin substrate side may be 1 μm or less.
[0269] Thus, when the resin substrate is formed on the porous layer, it is difficult for the resin material to enter the pores exposed on the main surface of the porous layer on the side where the resin substrate is formed, and the part of the porous layer on the resin substrate side can maintain the space in the pores, and the stress reduction effect on the resin substrate can be maintained. In addition, the dispersion effect of the gas pressure generated during laser irradiation can be maintained.
[0270] Furthermore, the average diameter of the pores in the second porous layer may be 1 μm or less.
[0271] Thus, when the resin substrate is formed on the second porous layer, it is difficult for the resin material to enter the pores exposed on the main surface of the second porous layer on the side where the resin substrate is formed. Therefore, the space in the pores can be maintained in the portion of the second porous layer on the resin substrate side, and the stress reduction effect on the resin substrate can be maintained. In addition, the dispersion effect of the gas pressure generated during laser irradiation can be maintained.
[0272] Furthermore, the porous layer may have a thin-layer coating portion without the pores on the main surface or surface on the side where the resin substrate is formed, and the thin-layer coating portion is formed of the same material as that of the porous layer other than the thin-layer coating portion.
[0273] Thus, when the resin substrate is formed on the porous layer, the resin material does not enter the pores of the porous layer because it is blocked by the coated thin layer portion, so the gaps in the pores of the porous layer can be maintained, and the stress reduction effect on the resin substrate can be maintained. In addition, the dispersion effect of the gas pressure generated during laser irradiation can be maintained. Moreover, since the coated thin layer portion is formed of the same material as the porous layer portion, the increase in the types of materials and processes can be suppressed, which is conducive to suppressing the manufacturing cost.
[0274] In addition, another embodiment of the present invention relates to a stacked substrate comprising: a supporting substrate; a porous layer formed above the supporting substrate and having a plurality of pores in at least a portion of the region in which gas exists in the internal space; and a resin substrate formed above the porous layer.
[0275] According to the structure of the laminated substrate involved in another embodiment of the present invention, since at least a part of the porous layer has a plurality of pores with gaps inside, the rigidity of the porous layer is lower than that of the resin substrate. Therefore, after forming an electronic device element or a part of its structural component on the top of the resin substrate, when the support substrate is separated by irradiating a laser from the support substrate side, the pressure of the gas that may be generated from the resin substrate during the irradiation of the laser will consume energy for destroying the porous layer. Thus, the stress applied to the resin substrate can be reduced, the deformation of the resin substrate can be suppressed, and thus the damage to the electronic device element formed on the top of the resin substrate can be suppressed.
[0276] Furthermore, an average diameter of the pores in a portion of the porous layer on the resin substrate side may be smaller than an average diameter of the pores in a portion of the porous layer on the support substrate side.
[0277] Thus, when the resin substrate is formed on the porous layer, the resin material of the resin substrate is difficult to enter the inside of the pores whose inner surface is exposed on the main surface of the porous layer on the side where the resin substrate is formed. Therefore, the voids inside the pores in the surface layer portion on the main surface side can be maintained, and the rigidity of the surface layer portion on the main surface side of the porous layer can be suppressed from becoming higher. Thus, it is possible to prevent the porous layer from being easily destroyed by the pressure of the gas generated during the irradiation of the laser, thereby maintaining the stress reduction effect on the resin substrate.
[0278] Furthermore, by maintaining the voids in the pores of the surface layer of the porous layer, the pressure of the gas generated by laser irradiation is dispersed by the gas in the voids of the pores, thereby reducing the stress applied to the resin substrate by the pressure of the gas.
[0279] Hereinafter, specific examples of the embodiments and modifications of the present invention will be shown, and the structures, operations, and effects will be described.
[0280] In addition, the embodiments and modified examples used in the following description are examples used to easily explain the structure and action / effect related to one embodiment of the present invention, and the present invention is not limited to the following embodiments and modified examples except for its essential parts.
[0281] <<Second Implementation Method>>
[0282] [1. Structure of electronic equipment]
[0283] Regarding the structure of the electronic device according to the second embodiment of the present invention, a case where the electronic device is applied to an active matrix organic EL display device is described as follows. Fig.14 , Fig.15 , Fig.16 To explain.
[0284] Fig.14 (a) is a partial cross-sectional view schematically showing the structure of an electronic device body 4000 of the electronic device 400 according to the present embodiment formed on a supporting substrate 310. In the present embodiment, the electronic device 400 is an active matrix organic EL display device. Fig.14 (b) is a partial cross-sectional view schematically showing a state where the electronic device 4000 is irradiated with laser light from the support substrate 310 side.
[0285] like Fig.14 As shown in (a), the electronic device body 4000 is formed by stacking a support substrate 310, a porous layer 320, a plastic substrate (resin substrate) 330, a sealing layer 340, a TFT layer 350, and an organic EL element layer 360 in this order. The electronic device element layer (electronic device element) 370 is formed by the TFT layer 350 and the organic EL element layer 360. The electronic device 400 involved in the embodiment is formed by the plastic substrate 330, the sealing layer 340, the TFT layer 350, and the organic EL element layer 360. In addition, the stacked substrate 301 involved in the embodiment is formed by the support substrate 310, the porous layer 320, and the plastic substrate 330.
[0286] (Supporting substrate)
[0287] Examples of the material of the support substrate 310 include, but are not limited to, alkali-free glass (borosilicate glass), alkali glass, soda glass, non-fluorescent glass, phosphate glass, boric acid glass, glass materials such as quartz, and insulating materials such as aluminum.
[0288] In order to form thin film device elements such as display device elements, the surface of the support substrate 310 (the main surface forming the electronic device 400 side) is preferably highly flat after the plastic substrate 330 is temporarily fixed. Specifically, the maximum height difference is preferably 10 μm or less, more preferably 1 μm or less.
[0289] In order to improve the adhesion with the next layer to be formed, the surface of the support substrate 310 is preferably set to a clean state. As a surface cleaning method, UV light irradiation, ozone treatment, plasma treatment, hydrofluoric acid treatment, etc. can be used. In addition, a layer for improving the adhesion with the layer formed thereon can also be provided on the surface of the support substrate 310. As the layer for improving the adhesion, for example, a silicon oxide film can be used.
[0290] (Porous layer)
[0291] like Fig.15 As shown, the porous layer 320 has a plurality of pores inside. Fig.15 This is a scanning microscope photograph of a cross section of a portion near the interface between the porous layer 320 and the plastic substrate 330 .
[0292] Here, the so-called pores refer to the internal space that is not completely filled with liquid or solid, but contains any gas such as air or gas formed by vaporization of solvent. In addition, in the internal space, in addition to gas, liquid such as water or solvent, solid foreign matter such as dust, etc. may also exist. However, even in this case, it is preferred that more than 50% of the volume of the internal space is filled with gas.
[0293] The porosity of the porous layer 320 is at least higher than the porosity of the plastic substrate 330 . In addition, the rigidity of at least a portion of the porous layer 320 is lower than the rigidity of the plastic substrate 330 .
[0294] In addition, the term "pore" here is not limited to unit-shaped pores having a completely closed internal space, but is also used as a concept to include pores in which a part of the wall defining the unit is missing, pores in which the missing part of the wall is exposed on the outside of the layer, and pores in which a plurality of units are connected in a state where the internal spaces of each other are connected.
[0295] Here, the so-called pores refer to pores having a diameter of, for example, 10 nm to 10 μm, more preferably 100 nm to 5 μm. When a plurality of pores are connected, the diameter of each pore may be within the above range.
[0296] Here, the diameter of a hole refers to the length of the internal space of the hole in the direction of expansion of the layer (a direction perpendicular to the thickness direction of the layer).
[0297] Here, the porosity of the porous layer 320 is preferably, for example, 10% or more and 90% or less.
[0298] In addition, the porosity of the porous layer 320 may also be more preferably 50% or more and 90% or less. By setting the porosity to be 50% or more, the proportion of the porous layer being destroyed when the support substrate is separated by the laser can be increased, and as a result, the pressure applied to the plastic substrate can be further reduced. In addition, by setting the porosity to be 90% or less, a certain degree of mechanical strength is ensured in the porous layer 320, for example, it is possible to suppress the breakage caused by mechanical stress caused by decompression / pressurization during vacuum film formation in the manufacturing process. The so-called breakage caused by the mechanical stress refers to the peeling of the film, etc. In addition, if the porosity is too high, when the plastic substrate 330 is formed, the resin material (for example, polyimide) will enter the pores, and as a result, the strength of the porous layer 320 will be improved, so the porosity of the porous layer 320 is preferably about 90% or less.
[0299] In addition, the measuring method of the porosity of porous layer 320, for example, has the following method.After obtaining the cross section of porous layer 320 by mechanical cutting or convergent ion beam processing, observe the cross section by scanning electron microscope, and calculate the ratio of the space in the cross section to the porous partition wall.Because it can be easily assumed that the ratio is also the same in other cross sections, its ratio can be set as the porosity as volume ratio.In addition, by carrying out the above-mentioned measurement of multiple points in the surface, and taking it on average, thereby can further improve accuracy.
[0300] As the material of the porous layer 320 , an organic material can be used.
[0301] The method for forming the porous layer 320 is not particularly limited, but a wet forming method or a dry forming method can be used, for example. The temperature in the forming process of the porous layer 320 or the heating temperature after the formation is preferably higher than the temperature in the forming process of each layer formed thereon. The reason is that when the forming process of the upper layer is performed at a higher temperature than the forming temperature of the porous layer 320, the porous layer 320 may change, which is not preferred. For example, water, solvents, and other gases adsorbed in the pores or solid parts of the porous layer 320 may be desorbed during the forming process of the upper layer, causing a malfunction such as separation between the upper layers.
[0302] The thickness of the porous layer 320 is not particularly limited, but is preferably approximately 1 μm to 1000 μm.
[0303] In addition, in this embodiment, if Fig.15As shown in FIG. 1 , the porous layer 320 forms a layer without pores having a thickness of about 1 μm on the surface of the plastic substrate 330 side, that is, a coating thin layer portion 322. By forming the coating thin layer portion 322, when the resin material for forming the plastic substrate 330 is applied to the porous layer 320, the resin material does not enter the pores and fill the internal space of the pores with the resin material. As a result, the gas pressure relaxation effect of the porous layer 320 can be well maintained.
[0304] Here, the term "resin material" is used to mean a material containing a resin polymer and a solvent. In addition, a plurality of resin polymers and solvents may be mixed and used.
[0305] Here, it is considered that during the formation process of the porous layer 320, when the resin material used to form the porous layer 320 is heated, the solvent in the resin material becomes bubbles to form pores. At this time, since the bubbles near the surface can escape from the surface to the atmosphere relatively easily, as time passes, there are no bubbles near the surface, and as a result, it is considered that the coating thin layer part 322 is formed.
[0306] (Plastic substrate)
[0307] Although not particularly limited, the material of the plastic substrate 330 includes, for example, polyethylene, polypropylene, ethylene polymer, polyvinylidene chloride, polyethylene terephthalate, polyethylene naphthalate, polycarbonate, polyethylene sulfonic acid, silicon, acrylic resin, epoxy resin, phenolic resin, polyamide, polyimide, aramid resin, etc. In addition, two or more of these materials may be mixed and used, and these materials may also be chemically modified. Moreover, two or more of these materials may be combined to form a laminated film of a multilayer structure.
[0308] The plastic substrate 330 needs to have a property that it is difficult to crack or break when bent. If it does not have this property, a display device with high flexibility cannot be obtained.
[0309] The thickness of the plastic substrate 330 is preferably in the range of 1 μm to 1000 μm. If it is thinner than this, mechanical strength cannot be obtained. If it is thicker than this, it is difficult to bend, and a display device with high flexibility cannot be obtained.
[0310] The method for forming the plastic substrate 330 is: it can be formed by applying a liquid resin material, or it can be formed by pressing a component that has been formed into a film, and there is no particular limitation. In the case of pressing a component that has been formed into a film, an adhesive layer can be formed between the film and the porous layer. As the adhesive layer, any material that can obtain the desired adhesive force, such as a silicon-based material or an acrylic-based material, is not particularly limited. The plastic substrate 330 can also be the above-mentioned light-transmitting substrate 30.
[0311] (Sealing layer)
[0312] As the sealing layer 340 , for example, a silicon nitride film can be used.
[0313] (TFT layer)
[0314] TFTs for driving organic EL elements are formed in the TFT layer 350. The TFT layer 350 is composed of an electrode layer 351 composed of a gate electrode as a part of the TFT and a TFT main body layer 352 which is a part other than the gate electrode of the TFT.
[0315] The electrode layer 351 is formed by forming a metal material film by vacuum evaporation or sputtering, and selectively removing the metal material film by etching, etc. Examples of the material of the electrode layer 351 include: silver; aluminum; an alloy of silver, palladium, and copper; an alloy of silver, rubidium, and gold, etc.
[0316] The TFT main body layer 352 includes a gate insulating film, source-drain electrodes, a bank, a semiconductor layer, a passivation film, etc. The TFT may be a device using silicon as a channel material, a device using an oxide semiconductor such as indium gallium zinc oxide, or a device using an organic semiconductor such as pentacene.
[0317] (Organic EL element layer)
[0318] The organic EL element layer 360 includes: a cathode, an anode, and a light-emitting layer sandwiched between the cathode and the anode. In addition to the above, the organic EL element layer 360 may also include an electron injection layer, an electron transport layer, an electron hole injection layer, an electron hole transport layer, a partition layer, a sealing layer, etc. The organic EL element layer 360 may further include a color filter, a protective layer, etc.
[0319] The TFT layer 350 and the organic EL element layer 360 constitute an electronic device element layer 370 .
[0320] In this embodiment, the TFT layer 350 has a multilayer structure including the electrode layer 351 and the TFT main body layer 352 , but the present invention is not limited thereto. For example, when the electronic device 400 is a passive organic EL display device, the wiring layer corresponds to the TFT layer 350 .
[0321] When the electronic device 400 is a liquid crystal display device, an LCD element is formed in the electronic device element layer 370. When the electronic device 400 is a photoelectric sensor, a photoelectric conversion element is formed in the electronic device element layer 370.
[0322] [2. Separation of electronic device and supporting substrate]
[0323] In order to separate the support substrate 310 from the electronic device 400, laser light is irradiated from the support substrate 310. Thus, the electronic device 400 can be separated from the support substrate 310 by destroying a portion of the porous layer 320 at the interface between the support substrate 310 and the porous layer 320, in the porous layer 320, or at the interface between the porous layer 320 and the plastic substrate 330.
[0324] Here, in Fig.28 In the case of the electronic device body 9000 not involved in the present embodiment shown in (a), the plastic substrate 630 is formed directly above the support substrate 610, which cannot alleviate the mechanical stress during laser irradiation. Fig.28 As shown in (b), the plastic substrate 630 is significantly deformed. Specifically, the deformation of the plastic substrate 630 is stretching. If the stretching state before laser irradiation is set to d, and the stretching state after laser irradiation is set to d+Δd, the change rate is [(d+Δd) / d] -1 For example, it is known that in the case of a plastic substrate having an inorganic film of silicon nitride, which is generally used as a sealing film, the limit change rate of barrier destruction is about 0.5% to 1.0%, and the upper layer will be damaged even by a slight change. The reason for the deformation is that the plastic substrate 630 absorbs the laser due to laser irradiation, and although high-pressure gas is generated when ablation occurs, the pressure cannot be deviated to the support substrate 610 side, so the energy is consumed by the deformation of the plastic substrate 630.
[0325] On the other hand, in the method of manufacturing an electronic device according to the present embodiment, the porous layer 320 is formed between the supporting substrate 310 and the plastic substrate 330 .
[0326] Here, the porous layer 320 has a shape including voids therein, so that its rigidity becomes lower than that of the support substrate 310 or the plastic substrate 330. Fig.14 As shown in (b), the high-pressure gas G generated by ablation or thermal decomposition during laser irradiation consumes energy by causing the porous layer 320 to be destroyed and deformed. Furthermore, the pressure is relieved by utilizing the voids in the porous layer 320, thereby suppressing the deformation of the plastic substrate 330. Furthermore, the deformation of each layer disposed above the plastic substrate 330 can be suppressed.
[0327] Furthermore, when a plurality of pores are connected to one another, the gas generated from the resin substrate is dispersed in the plurality of pores connected to one another, thereby relieving the pressure and reducing the stress on the resin substrate.
[0328] Furthermore, since the porous layer 320 is mechanically fragile and easily damaged, the bonding force between atoms or molecules in the porous layer 320 or the bonding force between the plastic substrate 330 and the porous layer 320 may be lost, thereby enabling the plastic substrate 330 to be stably and easily separated from the supporting substrate 310 .
[0329] In addition, since the efficiency of the separation process is improved by forming the porous layer 320, deformation of the plastic substrate 330 can be suppressed even when the intensity of the laser is increased. In addition, since the porous layer 320 is easily mechanically broken, the area ratio for maintaining the adhesion is small, and the separation process can be stably performed.
[0330] As described above, the structure of the embodiment as one mode of the present invention can suppress (reduce) damage to the electronic device when the support substrate is separated. In addition, the support substrate 310 can be separated stably and easily.
[0331] [3. Method for manufacturing electronic device]
[0332] Below, refer to Fig.16 , Fig.17 , Fig.18 , Fig.19 A method for manufacturing an electronic device according to an embodiment of one aspect of the present invention will be described. Fig.16 , Fig.17 , Fig.18 It is a partial cross-sectional view schematically showing a part of the manufacturing process of the electronic device 400 according to the embodiment. Fig.19 Schematic process diagram showing a manufacturing process of the electronic device 400 according to the embodiment.
[0333] First, if Fig.16 As shown in (a), a supporting substrate 310 ( Fig.19 The support substrate 310 is cleaned by performing an excimer UV (wavelength 172 nm) treatment on the surface.
[0334] Next, if Fig.16 As shown in (b), a porous layer 320 ( Fig.19 Step S12).
[0335] Then, if Fig.16 As shown in FIG. 2( c ), a plastic substrate 330 ( Fig.19 Step S13). Thus, a laminated substrate 301 is obtained.
[0336] Then, if Fig.16As shown in (d), a sealing layer 340 is formed on the plastic substrate 330 ( Fig.19 Step S14).
[0337] Then, if Fig.17 As shown in (a), on the sealing layer 340, after the metal film is formed, etching is performed to form an electrode layer 351 ( Fig.19 Step S15).
[0338] Next, if Fig.17 As shown in (b), a TFT main body layer 352 is formed on the electrode layer 351, so that the TFT layer 350 is completed ( Fig.19 In step S16). In addition, when forming a passive matrix display, it is not necessary to form a TFT layer, and only a wiring layer needs to be formed.
[0339] Then, if Fig.17 As shown in (c), an organic EL element layer 360 is formed on the TFT layer 350 ( Fig.19 Step S17). Thus, the electronic device body 4000 is obtained.
[0340] Then, if Fig.18 As shown in (a), laser light is irradiated from the support substrate 310 side toward the electronic device body 4000 ( Fig.19 Step S18).
[0341] By laser irradiation, the support substrate 310 and the porous layer 320 are separated from the plastic substrate 330 to obtain the electronic device 400 ( Fig.19 Step S19).
[0342] In addition, after the support substrate 310 and the porous layer 320 are separated, a part of the porous layer 320 may be attached to the plastic substrate 330 .
[0343] [4. Damage suppression effect]
[0344] A verification test was conducted on the damage suppression effect of the electronic device in the manufacturing method of the electronic device involved in the embodiment of one mode of the present invention. The verification test was conducted using two test bodies TP1 and TP2 with different thicknesses of the porous layer 320 and a test body TP3 without the porous layer 320 as a comparative example. The test bodies TP1, TP2, and TP3 were subjected to laser irradiation without forming the TFT main body layer 352 and the organic EL element layer 360, and the surface state of the electrode layer 351 was observed and measured to conduct the verification test.
[0345] (Test subject TP1)
[0346] Next, a specific method and conditions for producing the test piece TP1 will be described.
[0347] First, a support substrate 310 ( Fig.16 (a) Fig.19 Step S11). EAzLE2000 manufactured by Corning was used as the support substrate 310, and the surface of the support substrate 310 was subjected to excimer UV (wavelength 172 nm) treatment to clean the surface.
[0348] Next, polyimide was applied on the support substrate 310 by spin coating and heated at 400° C. for 8 hours to form a porous polyimide layer with a thickness of 18 μm, namely, the porous layer 320 ( Fig.16 (b) Fig.19 Step S12). The polyimide used as the material of the porous layer 320 is, for example, U-imide varnish type BP manufactured by UNITIKA.
[0349] Next, a polyimide layer with a thickness of 30 μm is formed on the porous layer 320 by spin coating, thereby forming a plastic substrate 330 ( Fig.16 (c) Fig.19 Step S13). The polyimide used as the material of the plastic substrate 330 is, specifically, U-Varnish manufactured by Ube Industries.
[0350] Then, on the plastic substrate 330, as the sealing layer 340, a silicon nitride film (1 μm thick) was formed at 300°C by capacitively coupled plasma CVD. Fig.16 (d) Fig.19 Step S14).
[0351] Next, a layer with a thickness of 100 nm made of an alloy of molybdenum and tungsten is formed on the sealing layer 340 by sputtering, patterned by photolithography using a resist, and etched by a mixed solution of phosphoric acid / nitric acid / acetic acid to form an electrode layer 351 ( Fig.17 (a) Fig.19 Step S15), the test body TP1 is obtained. Fig. 20 (a) is a schematic cross-sectional view of the test body TP1.
[0352] (Test subject TP2)
[0353] As the porous layer 320, the same process as that of the test piece TP1 was carried out except that the spin coating speed was reduced to form a porous polyimide with a film thickness of 117 μm, thereby obtaining a test piece TP2. Fig. 20 (b) is a schematic cross-sectional view of the test body TP2.
[0354] (Test subject TP3)
[0355] The same manufacturing process as that of the test piece TP1 was carried out except that the porous layer 320 was not formed, thereby obtaining a test piece TP3 as a comparative example. Fig. 20 (c) is a schematic cross-sectional view of the test body TP3.
[0356] At least four test bodies TP1, TP2, and TP3 were prepared, and each test body was irradiated with laser at four different laser irradiation power densities to separate the film 302 composed of the plastic substrate 330, the sealing layer 340, and the electrode layer 351 from the support substrate 310 (and the porous layer 320). Then, the following three evaluations were performed on each test body. In addition, laser irradiation was performed by scanning and irradiating with an excimer laser having a wavelength of 305 nm, a pulse width of 20 ns per time, and an irradiation area of 20.0 mm×1.0 mm from the support substrate 310 side.
[0357] (1) Whether the plastic substrate 330 can be separated from the support substrate 310 was evaluated. The case where the plastic substrate 330 can be separated with almost no resistance by hand was considered to be separable. In addition, in the case where the close contact with the support substrate 310 is high and it is difficult to separate by hand, although a method of separating by applying force using a roller or the like is considered, when a force is applied, the plastic substrate 330 will deform and the sealing layer 340 or the electrode layer 351 formed on the upper layer will be damaged, so it is not preferred.
[0358] (2) The laser was repeatedly irradiated with a power density of one laser until the parts could be separated with almost no resistance by hand, and the number of irradiations was used as an indicator of the processing speed of the process.
[0359] (3) The surface of the electrode layer 351 after the support substrate 310 is separated is checked with a microscope to confirm whether there is any abnormality such as cracking of the electrode layer 351 .
[0360] exist Fig.21 The results of the above three evaluations are shown in .
[0361] In the test piece TP3, the laser irradiation energy density was 140 mJ / cm 2 In the case of , the laser power is too low and does not reach the threshold of energy density for ablating polyimide. Therefore, even if the number of laser irradiation times is increased, separation is not possible. 2In the above case, since ablation during laser irradiation generates high-pressure gas (decomposition product of polyimide) and deforms the plastic substrate 330 , it is observed that the electrode layer 351 made of molybdenum-tungsten alloy formed on the plastic substrate 330 is damaged.
[0362] Fig. 22 (a) is a microscope photograph of the surface of the electrode layer 351 of the test body TP3 after laser irradiation. Fig. 22 (b) is a schematic representation that is easy to understand Fig. 22 (a) is a microscopic photograph of the surface of the electrode layer 351. Fig. 22 As shown in (a) and (b), on the surface of the electrode layer 351 of the test body TP3 after laser irradiation, stripe-like portions 351a like multiple leaf-vein-like cracks and cracks, or point defect portions 351b visible like through holes or recesses are observed.
[0363] It is believed that the sealing layer 340 on the bottom of the electrode layer 351 deforms along with the deformation of the plastic substrate 330, so the electrode layer 351 formed on the top thereof is also destroyed. 2 However, under this condition, more than 20 laser irradiations are required to stably separate by hand. For example, when considering the treatment on a large 4th generation glass substrate, it takes more than 5 hours to laser treat the entire surface, which is not realistic in terms of production efficiency.
[0364] Here, if Fig.15 As shown in FIG. 1 , the diameter of the pores 321a of the porous layer 320 of the embodiment closer to the plastic substrate 330 is generally smaller than the diameter of the pores 321b of the portion farther from the plastic substrate 330 (the portion on the support substrate 310 side). In other words, the average diameter of the pores 321a is smaller than the average diameter of the pores 321b. In addition, the so-called average diameter can be expressed by an area of 10×10μm 2 The average diameter of the porous layer 320 can be used to represent the porous layer 320 , for example, by observing 2 to 3 points of the cross section of the porous layer 320 using a focused ion beam (FIB) scanning electron microscope (SEM).
[0365] If you observe Fig.21 The laser separation results of the test pieces TP1 and TP2 shown in FIG. 1 have two characteristics compared to the test piece TP3 without the porous layer 320. The first characteristic is that in the high energy density region (180, 200 mJ / cm 2), no cracking of the electrode layer 351 was confirmed. This is because the following effect of the present invention is exerted: the energy of the gas generated by laser ablation or thermal decomposition is not used to deform the plastic substrate 330 side, but is consumed in destroying the porous layer 320. In addition, in the lower area of the porous layer 320 (the area on the support substrate 310 side), since the pore diameter of the pores is large, the porosity can be increased, and the stress of the gas generated from the plastic substrate 330 can be more easily absorbed by the porous layer 320.
[0366] exist Fig.23 (a), (b), and (c) show the energy density of 180 mJ / cm 2 Microscope photographs of the surface of the electrode layer 351 of the test bodies TP1, TP2, and TP3 after being irradiated with laser. In order to further clarify the effect of laser irradiation, these photographs were taken after irradiating the laser in a linear manner instead of the entire surface. Fig.23 In (a), (b), and (c), the range of arrows indicates the range of laser irradiation.
[0367] Fig.24 Indicates that the probe type step profiler is used to Fig.23 (a), (b), and (c) show the results of measuring the displacement of the electrode layer 351 surface in the thickness direction of the test pieces TP1, TP2, and TP3 after laser irradiation. Fig.24 In FIG. 1 , the area indicated by the arrow corresponds to the area irradiated with the laser.
[0368] like Fig.23 (a), (b), (c) and Fig.24 As shown in FIG. 1 , in the test body TP3, the separation of the electrode layer 351 was clearly confirmed. It was confirmed that the high-pressure gas generated by the ablation phenomenon based on the laser irradiation caused the plastic substrate 330 to be lifted up, and the electrode layer 351 was greatly displaced. In the test bodies TP1 and TP2, the displacement of the electrode layer 351 was smaller than that of the test body TP3. In addition, in the test body TP2, the displacement of the electrode layer 351 was smaller than that of the test body TP1. Fig.24 As shown, in the test piece TP3, the displacement of the electrode layer 351 is about 4 μm, whereas in the test piece TP1, it is about 1.5 μm or less, and in the test piece TP2, it is about 1 μm or less.
[0369] The second feature is: at an energy density of 160mJ / cm 2When compared, the number of laser irradiations until separation is possible is significantly reduced in test pieces TP1 and TP2 compared to test piece TP3. This is believed to be because the porous layer 320 has a high porosity and a small area for maintaining its adhesion, so separation is easily performed by one laser irradiation.
[0370] Through these two effects, since high energy density irradiation conditions can be used and the number of laser irradiations can be reduced, the time required for separating the supporting substrate can be shortened even when processing the entire surface of a large substrate, which has great advantages in production.
[0371] The average diameter of the pores on the plastic substrate 330 side of the porous layer 320 is preferably, for example, 10 nm or more and 1 μm or less. The average diameter of the pores on the support substrate 310 side of the porous layer 320 is preferably, for example, 100 nm or more and 10 μm or less.
[0372] 《Variation Example》
[0373] As mentioned above, although this invention was demonstrated based on embodiment, this invention is not limited to the said embodiment, and the following modification examples are possible.
[0374] (Variant 1)
[0375] In the embodiment, the porous layer 320 includes the thin-layer coating portion 322 , but the present invention is not limited thereto and the porous layer 320 may be configured not to include the thin-layer coating portion 322 .
[0376] In this case, the average diameter of the pores in the portion on the plastic substrate 330 side of the porous layer 320 is preferably smaller than the average diameter of the pores in the portion on the support substrate side. Since the average diameter of the pores in the portion on the plastic substrate 330 side is smaller, it is more difficult for the resin material applied when forming the plastic substrate 330 to enter the pores, so that the porosity of the porous layer 320 can be maintained, and the effect of relieving the pressure of the gas caused by ablation can be maintained.
[0377] In addition, although the porous layer 320 is formed by applying a resin material and then heating it, generally speaking, the closer the bubbles of the solvent are to the surface, the easier they are to escape, so the closer the bubbles are to the surface, the smaller the average diameter of the pores. The heating temperature and heating time when forming the porous layer 320, and the type and dosage of the solvent of the resin material can also be adjusted so that the thin coating portion 322 is not formed.
[0378] (Variant 2)
[0379] When the plastic substrate 330 is bonded to the porous layer 320, Fig.25As in the electronic device body 5000 according to the second modification shown in (a), an adhesive layer 380 is provided between the porous layer 320 and the plastic substrate 330. Since the adhesive layer 380 is generally formed by coating, it is difficult for the material of the adhesive layer to penetrate into the pores with a small average diameter of the pores in the surface portion of the porous layer 320 on the side where the plastic substrate 330 is formed. In addition, when the pores are bonded, the area of the surface of the porous layer 320 that is in close contact with the plastic substrate 330 is larger than that in the case where the average diameter of the pores in the surface portion of the porous layer 320 on the side where the plastic substrate 330 is formed is larger, and the bond with the plastic substrate 330 is higher. As a result, it is possible to prevent the plastic substrate 330 from being accidentally separated from the porous layer 320 during the manufacturing process of the electronic device.
[0380] Furthermore, a laminated substrate 5001 according to Modification 2 is constituted by the support substrate 310 , the porous layer 320 , the adhesive layer 380 , and the plastic substrate 330 .
[0381] (Variant 3)
[0382] Furthermore, the porous layer may be composed of two or more layers. Fig.25 (b) is a partial cross-sectional view of the electronic device body 3000 according to Modification 3. Fig.25 As shown in (b), in the electronic device body 3000, the porous layer 3020 is composed of a first porous layer 3020a formed on a supporting substrate 310 and a second porous layer 3020b formed on the first porous layer 3020a. In this case, the average diameter of the pores of the second porous layer 3020b is preferably smaller than the average diameter of the pores of the first porous layer 3020a. In the case where a plastic substrate 330 is formed on the second porous layer 3020b by coating, it is difficult for the resin material to enter the pores of the second porous layer 3020b with a small average diameter, so the porosity of the second porous layer 3020b can be maintained. As a result, the pressure of the gas caused by ablation during laser irradiation can be alleviated, the deformation of the plastic substrate can be suppressed, and the damage to the device can be suppressed.
[0383] Furthermore, even when the porous layer 320 is composed of a single layer or multiple layers, it is preferred that the resin material of the plastic substrate 330 is not filled in the pores at least at a thickness of 1 / 2 or more of the thickness of the porous layer 320 .
[0384] In addition, another layer may be further formed between the supporting substrate 310 and the first porous layer 3020 a and / or between the first porous layer 3020 a and the second porous layer 3020 b .
[0385] Furthermore, the support substrate 310 , the porous layer 3020 , and the plastic substrate 330 constitute a laminated substrate 3001 according to the third modification.
[0386] (Variant 4)
[0387] When the porous layer 3020 includes the first porous layer 3020a and the second porous layer 3020b as in the above-mentioned modification 3, the second porous layer 3020b may be formed by any dry method such as CVD, sputtering, or vapor deposition. When the second porous layer 3020b is formed by a wet method, water or solvent may remain in the pores or inside the solid part of the second porous layer 3020b, which may cause gas generation during heating or laser irradiation in the subsequent manufacturing process. When the second porous layer 3020b is formed by a dry method or thermal vapor deposition, water or solvent does not remain, and gas generation can be suppressed.
[0388] (Variant 5)
[0389] In addition, the viscosity of the second resin material used to form the second porous layer 3020b is preferably higher than the viscosity of the first resin material used to form the first porous layer 3020a. Thus, since the second resin material used to form the second porous layer 3020b is difficult to enter the pores of the first porous layer 3020a, the porosity of the first porous layer 3020a can be maintained.
[0390] (Variant 6)
[0391] After the process of forming the porous layer 320 and before the process of forming the plastic substrate 330, affinity treatment may also be performed so that the resin affinity of the inner surface 321c of the exposed pores 321 on the surface 323 is lower than the affinity of the surface 323 of the porous layer 320 (the main surface on the side where the plastic substrate 330 is formed) 323 to the resin material of the plastic substrate 330 (hereinafter referred to as "resin affinity").
[0392] Below, refer to Fig.26 as well as Fig. 27 , to illustrate the above affinity treatment method.
[0393] Fig.26 (a) is a partial cross-sectional view showing a state where a porous layer 320 is formed on a supporting substrate 310. As shown in the figure, on a surface 323 of the porous layer 320, inner surfaces 321c of a part of pores 321 are exposed.
[0394] Next, if Fig.26As shown in (b), a thin film 390 having low resin affinity is formed on the surface 323 and the inner surface 321c. The thin film 390 can be formed by, for example, applying a solution containing a material having low resin affinity on the surface 323 and the inner surface 321c and then drying it.
[0395] Then, if Fig. 27 As shown in (a), UV light is irradiated from the film 390 side. Fig. 27 As shown in (b), in the film 390, the portion formed on the surface 323 of the porous layer 320, the shallower portion of the inner surface 321c of the pore 321, and the portion formed on the region corresponding to the bottom surface of the larger opening are exposed to UV light, and the resin affinity is improved, forming a high resin affinity portion 390a. On the other hand, even in the portion deep in the inner surface 321c of the pore 321 or the portion close to the opening, the portion inclined to be nearly parallel to the irradiation direction of the UV light does not reach enough UV light, and is therefore not exposed to UV light, and the resin affinity is kept low, forming a low resin affinity portion 390b.
[0396] Here, in this modification, the film 390 is a part of the porous layer 320. In addition, the portion of the film 390 exposed to the UV light is included in the surface 323 of the porous layer 320, and the portion not exposed to the UV light is included in the inner surface 321c of the pore 321 of the porous layer 320.
[0397] Then, if Fig. 27 As shown in (c), a resin material is applied from a film 390 to form a plastic substrate 330. At this time, since there is a low resin affinity portion 390b on the inner surface 321c of the pore 321, it is difficult for the resin material to enter the pore, and the porosity near the surface of the porous layer 320 can be maintained.
[0398] On the other hand, since the high resin affinity portion 390a is formed on the surface 323, the porous layer 320 and the plastic substrate 330 have high adhesion, which can prevent the plastic substrate 330 from being accidentally separated from the porous layer 320 in the remaining manufacturing steps of the subsequent electronic device.
[0399] In the above description, UV light is used for the resin affinity treatment, but the present invention is not limited thereto and the affinity treatment may be performed by light (visible light) irradiation or plasma treatment instead of UV light irradiation, depending on the type of the film 390 .
[0400] (Variant 7)
[0401] In addition, the average diameter of the pores on the plastic substrate 330 side of the porous layer 320 may be larger than the average diameter of the pores on the support substrate 310 side. In this case, although the resin material used to form the plastic substrate 330 easily enters the pores, since the rigidity of the side closer to the plastic substrate 330 becomes lower, there is an advantage that the stress caused by the high-pressure gas generated when irradiating the laser is more easily absorbed.
[0402] The display panel device and the manufacturing method thereof according to the present invention are described above based on the embodiments and variations (hereinafter referred to as “embodiments, etc.”), but the present invention is not limited to the above-mentioned embodiments, etc. The first embodiment, the second embodiment, and these variations may be appropriately combined. The present invention also includes methods obtained by implementing various variations that a person skilled in the art may conceive of for the above-mentioned embodiments, etc., or methods achieved by arbitrarily combining the structural elements and functions in the embodiments, etc., within the scope of the main purpose of the present invention.
[0403] In addition, although the embodiment and the modified example describe the method of using the laminated substrate for the display device, this is only an example and is not limited to this method. For example, even when the laminated substrate is applied to an electronic device other than a display device, especially a light-emitting device that emits light from at least a portion (for example, a lighting device, an electronic advertisement, etc.), the reflection of external light can be suppressed. In addition, although the display device is described as a device having a display device element in the embodiment, in the case of a light-emitting device, the display device element can also be replaced with a light-emitting device element.
[0404] Industrial Applicability
[0405] The flexible display realized by the present invention can be applied to displays with excellent design that match the curved surfaces of, for example, televisions, mobile terminals such as tablets and smartphones, wearable terminals such as watch-type terminals, and car interiors.
Claims
1. A light emitting device, comprising: Light-transmitting substrate; A light-emitting device element formed on one main surface of the light-transmitting substrate, comprising an upper electrode, a light-emitting layer and a lower electrode; and a porous layer formed on the other main surface of the light-transmitting substrate and being an organic material layer having a plurality of pores, An average diameter of the pores in a portion of the porous layer on the light-transmitting substrate side is smaller than an average diameter of the pores in a portion of the porous layer on the opposite side to the light-transmitting substrate.
2. The light emitting device according to claim 1, On the main surface of the porous layer opposite to the light-transmitting substrate, inner surfaces of a part of the plurality of pores are exposed. Gas exists in the pores whose inner surfaces are exposed, and the inner surfaces of another part of the plurality of pores are not exposed.
3. The light emitting device according to claim 1, In the porous layer, the average diameter of the pores in the first porous layer portion including the main surface on the opposite side of the translucent substrate is smaller than the average diameter of the pores in the second porous layer portion located closer to the translucent substrate than the first porous layer portion.
4. The light emitting device according to claim 1, The light emitting device element emits light for image display toward the light-transmitting substrate. The porous layer is made of a light-transmitting material.
5. The light emitting device according to any one of claims 1 to 4, The porous layer does not contain inorganic particles.
6. The light emitting device according to claim 1, The porous layer has a predetermined porosity.
7. The light emitting device according to claim 6, The porosity is 10% or more and 90% or less.
8. The light emitting device according to claim 7, The porosity is 50% or more and 90% or less.
9. The light emitting device according to claim 1, further comprising: A TFT layer formed on the one main surface of the light-transmitting substrate; and A sealing layer is formed between the one main surface and the TFT layer.
10. The light emitting device according to claim 9, The sealing layer is made of silicon nitride.