A method for manufacturing a submicron color filter layer of a silicon-based OLED device
Through deep ultraviolet photoresist and dry glue removal technology, a submicron-level color filter layer was gradually produced, solving the problem of insufficient resolution in the existing technology and improving the resolution of silicon-based OLED microdisplay devices.
Patent Information
- Application Number
- CN202110468448.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-04-28
AI Technical Summary
The prior art is difficult to produce color filter layers with a resolution of less than 1um through normal exposure development processes, which limits the improvement of resolution of silicon-based OLED microdisplay devices.
Using deep ultraviolet photoresist and ash dry glue removal technology, a submicron-level color filter layer is gradually produced. Through multi-layer coating and exposure development steps, combined with the dry glue removal process, the submicron-level color filter layer is retained. Graphics, reducing line width distance.
The line width distance of the color filter layer is effectively reduced, the resolution of color OLED microdisplay devices is improved, and the production of submicron-level color filter layer is realized.
Smart Images

Figure CN113140690B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical devices, and in particular relates to a method for manufacturing a submicron color filter layer of a silicon-based OLED device. Background Art
[0002] Silicon-based OLED (Organic Light Emitting Diode) microdisplay is a new display technology that manufactures active light-emitting devices OLED on a silicon-based CMOS drive circuit substrate.
[0003] In the conventional silicon-based OLED microdisplay preparation process, a submicron (0.1um~1um) anode pixel layer can be produced through normal photolithography process. However, due to the limitation of color glue materials, the existing color filter layer can only produce line width patterns of 1um and above. It is difficult to produce resolution patterns below 1um through normal exposure and development processes, which restricts the research and development and production of higher resolution color OLED microdisplay devices. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for manufacturing a submicron color filter layer of a silicon-based OLED device, which greatly reduces the line width of the color filter layer and improves the resolution of the color OLED micro display device.
[0005] To achieve the above object, the technical solution of the present invention is: a method for manufacturing a submicron color filter layer of a silicon-based OLED device, characterized in that: the manufacturing method comprises the following steps:
[0006] Step 1. Apply a layer of red filter layer color glue on a silicon-based OLED substrate or a glass substrate and then solidify it to obtain substrate ①;
[0007] Step 2. Coat a layer of deep ultraviolet photoresist I on the red filter layer color glue, and then expose and develop to obtain substrate ②;
[0008] Step 3. Remove the deep ultraviolet photoresist I on the surface and the red filter layer colored glue exposed on the surface by ashing dry method, retain the red filter layer colored glue under the deep ultraviolet photoresist I to obtain substrate ③, and the retained red filter layer colored glue forms a red filter layer;
[0009] Step 4. Coat a layer of green filter layer color glue on substrate ③ and solidify it, coat a layer of deep ultraviolet photoresist II on the green filter layer color glue, and then expose and develop it to obtain substrate ④;
[0010] Step 5. Remove the deep ultraviolet photoresist II on the surface of substrate ④ and the green filter layer colored glue exposed on the surface by ashing dry method, retain the green filter layer colored glue under the deep ultraviolet photoresist II and the previously prepared red filter layer colored glue to obtain substrate ⑤, and the retained green filter layer colored glue forms a green filter layer;
[0011] Step 6. Coat a layer of blue filter layer color glue on substrate ⑤ and solidify it, coat a layer of deep ultraviolet photoresist III on the blue filter layer color glue, and then expose and develop it to obtain substrate ⑥;
[0012] Step 7. Remove the deep ultraviolet photoresist III on the surface of substrate ⑥ and the blue filter layer colored glue exposed on the surface by ashing dry method, retain the blue filter layer colored glue under the deep ultraviolet photoresist III and the previously made red filter layer colored glue and green filter layer colored glue to obtain substrate ⑦, and the retained blue filter layer colored glue forms a blue filter layer.
[0013] Furthermore, in the step 1, the thickness of the red filter layer color glue is 0.5um~2um, and the substrate ① is baked and cured, the baking temperature is 90℃~270℃, and the baking time is 20min~120min; the baking method is a proximity hot plate, a contact hot plate or an oven.
[0014] Furthermore, in the step 4, the thickness of the green filter layer color glue is 0.5um~2um, and the substrate ④ is baked and cured, the baking temperature is 90℃~270℃, and the baking time is 20min~120min; the baking method is a proximity hot plate, a contact hot plate or an oven.
[0015] Furthermore, in the step 6, the thickness of the blue filter layer color glue is 0.5um~2um, and the substrate ⑤ is baked and cured, the baking temperature is 90℃~270℃, and the baking time is 20min~120min; the baking method is a proximity hot plate, a contact hot plate or an oven.
[0016] Furthermore, a protrusion and a groove are provided on the side of the light-emitting layer in contact with the pixel layer, the protrusion is attached to the anode, and the groove is used to accommodate the protrusion of the pixel layer; a protrusion and a groove are provided on the side of the light-emitting layer in contact with the cathode, and the cathode is embedded in the light-emitting layer by contacting the protrusion and the groove.
[0017] Furthermore, the thickness of the deep ultraviolet photoresist I, deep ultraviolet photoresist II and deep ultraviolet photoresist III are all 0.5um~2um, and the deep ultraviolet photoresist I, deep ultraviolet photoresist II and deep ultraviolet photoresist III are Arf photoresist or Krf photoresist.
[0018] Furthermore, in the exposure and development, the wavelength of the exposure light source is 193nm or 248nm, the development time is 50s~120s, and the development temperature is 23°C~50°C; after development, the line width of the positive deep ultraviolet photoresist pattern is 0.1um~1um.
[0019] Furthermore, the ashing dry stripping step uses a dry etcher or a dry stripper, the ashing gas is oxygen, the oxygen flow rate is controlled at 50 sccm-200 sccm, the pressure is controlled at 20 mTorr-50 mTorr, the power is controlled at 100 W-500 W, and the etching temperature is controlled at 10° C.-50° C.
[0020] Furthermore, the length of the deep ultraviolet photoresist I is equal to the length of the red filter layer required on the silicon-based OLED device, the length of the deep ultraviolet photoresist II is equal to the length of the green filter layer required on the silicon-based OLED device, and the length of the deep ultraviolet photoresist III is equal to the length of the blue filter layer required on the silicon-based OLED device.
[0021] The advantages of adopting the technical solution of the present invention are:
[0022] The present invention separates color pixels by forming a layer of black photoresist between the color filter layers on the encapsulation layer of the silicon-based OLED device, thereby improving optical crosstalk between the color filter layers and the problem of scattered light passing through other colors when the device is lit, thereby reducing the color gamut of the product. This can effectively prevent optical crosstalk between different color filter layers from affecting the color gamut of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:
[0024] Figure 1 This is a process diagram of the method for making a submicron color filter layer of a silicon-based OLED device of the present invention.
[0025] The marks in the above figure are: 1. Silicon-based OLED substrate or glass substrate; 11. Substrate ①; 12. Substrate ②; 13. Substrate ③; 14. Substrate ④; 15. Substrate ⑤; 16. Substrate ⑥; 17. Substrate ⑦; 2. Red filter layer colored glue; 21. Red filter layer; 31. Deep ultraviolet photoresist I; 32. Deep ultraviolet photoresist II; 33. Deep ultraviolet photoresist III; 4. Green filter layer colored glue; 41. Green filter layer; 5. Blue filter layer colored glue; 51. Blue filter layer. DETAILED DESCRIPTION
[0026] In the present invention, it is necessary to understand that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "planar direction", "circumferential", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation; be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation to the present invention.
[0027] like Figure 1 As shown, a method for manufacturing a submicron color filter layer of a silicon-based OLED device is characterized in that the manufacturing method comprises the following steps:
[0028] Step 1. A layer of red filter layer color glue 2 is coated on a silicon-based OLED substrate or a glass substrate 1 and then cured to obtain a substrate ①11; the thickness of the red filter layer color glue 2 is 0.5um~2um, and the substrate ①11 is baked and cured at a baking temperature of 90℃~270℃ for 20min~120min; the baking method is a proximity hot plate, a contact hot plate or an oven;
[0029] Step 2. Coat a layer of deep ultraviolet photoresist I31 on the red filter layer color glue 2, and then expose and develop to obtain substrate ②12; the deep ultraviolet photoresist I31 is Arf photoresist or Krf photoresist, the thickness of the deep ultraviolet photoresist I31 is 0.5um~2um, the wavelength of the exposure light source is 193nm or 248nm, the development time is 50s~120s, and the development temperature is 23℃~50℃; after development, the line width of the positive deep ultraviolet photoresist pattern is between 0.1um~1um;
[0030] Preferably, the thickness of deep ultraviolet photoresist I (31), deep ultraviolet photoresist II (32) and deep ultraviolet photoresist III (33) is 0.6 um. A deep ultraviolet photoresist film thickness in the range of 0.5 um to 2 um can produce graphics with better resolution.
[0031] Preferably, the wavelength of the exposure light source is 193nm; the development time is 50s~120s, if the development time is less than 50s, there is a risk of incomplete development, and if it is more than 120s, it affects the production capacity; preferably, the process development time is 60S, and the development temperature is 23°C. If the temperature is too low, the development rate is slow, and if the temperature is too high, the development rate is too fast.
[0032] Step 3. Remove the surface deep ultraviolet photoresist Ⅰ31 and the red filter layer color glue exposed on the surface by ashing dry stripping, and retain the red filter layer color glue under the deep ultraviolet photoresist Ⅰ31 to obtain substrate ③13; the retained red filter layer color glue 2 forms a red filter layer 21, so that a submicron red filter layer is made on the silicon-based OLED substrate or the glass substrate 1; the dry stripping ashing equipment uses a dry etcher or a dry stripping machine, the ashing gas is oxygen, the oxygen flow rate is controlled at 50sccm~200sccm, the pressure is controlled at 20mTorr~50mTorr, the Power is controlled at 100W~500WW, and the etching temperature is controlled at 10℃~50℃;
[0033] Step 4. Coat a layer of green filter layer color glue 4 on substrate ③13 and then cure it, coat a layer of deep ultraviolet photoresist Ⅱ32 on the green filter layer color glue 4, and then expose and develop to obtain substrate ④14; the thickness of the green filter layer color glue is 0.5um~2um, and the substrate ④14 is baked and cured, the baking temperature is 90℃~270℃, and the baking time is 20min~120min; the baking method is a proximity, contact hot plate or oven; the deep ultraviolet photoresist Ⅱ32 is Arf photoresist or Krf photoresist, the thickness of the deep ultraviolet photoresist Ⅱ32 is 0.5um~2um, the exposure light source wavelength is 193nm or 248nm, the development time is 50s~120s, and the development temperature is 23℃~50℃; after development, the line width of the positive deep ultraviolet photoresist pattern is between 0.1um~1um.
[0034] The deep ultraviolet photoresist II 32 is located on the green filter layer color glue 4, and one end of the deep ultraviolet photoresist II 32 close to the red filter layer 21 is aligned with the tail of the red filter layer 21; the length of the deep ultraviolet photoresist I 31 is equal to the length of the red filter layer required on the silicon-based OLED device, and the length of the deep ultraviolet photoresist II 32 is equal to the length of the green filter layer required on the silicon-based OLED device.
[0035] Step 5. Remove the deep ultraviolet photoresist II 32 on the surface of substrate ④14 and the green filter layer color glue exposed on the surface by ashing dry stripping, retain the green filter layer color glue under the deep ultraviolet photoresist II 32 and the previously made red filter layer color glue to obtain substrate ⑤15, and the retained green filter layer color glue 4 forms a green filter layer 41, so that the submicron red filter layer 21 and the green filter layer 41 are made on the silicon-based OLED substrate or the glass substrate 1. The dry stripping ashing equipment uses a dry etcher or a dry stripping machine, the ashing gas is oxygen, the oxygen flow rate is controlled at 50sccm~200sccm, the pressure is controlled at 20mTorr~50mTorr, the power is controlled at 100W~500WW, and the etching temperature is controlled at 10℃~50℃.
[0036] Step 6. Coat a layer of blue filter layer color glue 5 on the substrate ⑤15 and then solidify it, coat a layer of deep ultraviolet photoresist III33 on the blue filter layer color glue 5, and then expose and develop to obtain substrate ⑥16; the thickness of the blue filter layer color glue is 0.5um~2um, and the substrate ⑤15 is baked and cured, the baking temperature is 90℃~270℃, and the baking time is 20min~120min; the baking method is a proximity type, contact type hot plate or oven; the thickness of the deep ultraviolet photoresist III33 is 0.5um~2um, the wavelength of the exposure light source is 193nm or 248nm, the development time is 50s~120s, and the development temperature is 23℃~50℃; after development, the line width of the positive deep ultraviolet photoresist pattern is between 0.1um~1um;
[0037] The deep ultraviolet photoresist III33 is located on the blue filter layer color glue 5, and the end of the deep ultraviolet photoresist III33 close to the green filter layer 41 is aligned with the tail of the green filter layer 41; the length of the deep ultraviolet photoresist I31 is equal to the length of the red filter layer required on the silicon-based OLED device, the length of the deep ultraviolet photoresist II32 is equal to the length of the green filter layer required on the silicon-based OLED device, and the length of the deep ultraviolet photoresist III33 is equal to the length of the blue filter layer required on the silicon-based OLED device.
[0038] Step 7. Remove the deep ultraviolet photoresist III33 on the surface of substrate ⑥16 and the blue filter layer colored glue 5 exposed on the surface by ashing dry stripping, retain the blue filter layer colored glue 5 under the deep ultraviolet photoresist III33 and the previously made red filter layer colored glue and green filter layer colored glue to obtain substrate ⑦17, the dry stripping ashing equipment uses a dry etcher or a dry stripper, the ashing gas is oxygen, the oxygen flow rate is controlled at 50sccm~200sccm, the pressure is controlled at 20mTorr~50mTorr, the Power (RF power) is controlled at 100W~500WW, and the etching temperature is controlled at 10℃~50℃; the retained blue filter layer colored glue 5 forms a blue filter layer 51, so that the submicron red filter layer 21, the green filter layer 41 and the blue filter layer 51 are made on the silicon-based OLED substrate or the glass substrate 1.
[0039] The basic components of photoresist are hydrocarbon organic matter. Under the action of radio frequency, oxygen is ionized into oxygen atoms and reacts chemically with the photoresist to produce carbon monoxide, carbon dioxide and water, which are then pumped away by a vacuum pump.
[0040] The oxygen flow rate affects the degumming rate. If the flow rate is less than 50sccm, the degumming rate is slow, affecting the production capacity. If the flow rate is greater than 200sccm, the degumming rate is too fast and the process is difficult to control. Pressure refers to the vacuum pressure in the reaction chamber. The greater the pressure, the greater the mean free path of electron movement, which is more conducive to ionization. However, when the oxygen flow rate and power are constant, to increase the pressure, it is necessary to replace the pump with a faster pumping speed. This process parameter is mainly determined by the equipment performance. Replacing a higher-power pump will cause the oxygen ion density to decrease, affecting the degumming effect.
[0041] The size of Power (RF power) will affect the active ion density in the chamber and the degumming rate. If it is lower than 100W, the power is too low, and the slow degumming rate affects the production capacity. The larger the Power, the greater the active ion density, which increases the degumming rate. However, the active ions required in the chamber are certain. When the Power reaches a certain value, the degumming rate reaches saturation and the degumming rate no longer increases. If the Power is too large, the product temperature will increase, affecting the product yield. Therefore, the Power size is adjusted according to the process.
[0042] The higher the etching temperature, the more active the oxygen ions in the reaction chamber, the more intense the chemical reaction, and the better the degumming rate and effect. If the temperature is lower than 10°C, the oxygen ion activity is low, the degumming rate is slow and affects the production capacity. If the temperature is higher than 50°C, the temperature of the product itself will increase, causing damage and affecting the product quality.
[0043] The present invention first uses deep ultraviolet photoresist to make submicron-level (0.1um~1um) graphics on the cured color filter layer, and then removes the deep ultraviolet photoresist and the underlying color filter layer without deep ultraviolet photoresist protection by dry degumming and ashing, thereby obtaining a submicron-level (0.1um~1um) color graphic, greatly reducing the line width of the color filter layer and improving the resolution of the color OLED micro-display device.
[0044] The present invention is described above by way of example in conjunction with the accompanying drawings. It is obvious that the specific implementation of the present invention is not limited to the above-mentioned method. As long as various non-substantial improvements are made using the technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A method for manufacturing a submicron color filter layer of a silicon-based OLED device, Features: The production method comprises the following steps: Step 1. Coat a layer of red filter layer color glue (2) on a silicon-based OLED substrate or a glass substrate (1) and then cure the layer to obtain substrate ① (11); Step 2. coating a layer of deep ultraviolet photoresist I (31) on the red filter layer color glue (2), and then exposing and developing to obtain substrate ② (12); Step 3. Remove the surface deep ultraviolet photoresist I (31) and the red filter layer colored glue exposed on the surface by ashing dry method, retain the red filter layer colored glue under the deep ultraviolet photoresist I (31) to obtain substrate ③ (13), and the retained red filter layer colored glue (2) forms a red filter layer (21); Step 4. Coating a layer of green filter layer colored glue (4) on the substrate ③ (13) and then curing it, coating a layer of deep ultraviolet photoresist II (32) on the green filter layer colored glue (4), and then exposing and developing it to obtain substrate ④ (14); Step 5. Remove the deep ultraviolet photoresist II (32) on the surface of the substrate ④ (14) and the green filter layer colored glue exposed on the surface by ashing dry method, retain the green filter layer colored glue under the deep ultraviolet photoresist II (32) and the previously prepared red filter layer colored glue to obtain the substrate ⑤ (15), and the retained green filter layer colored glue (4) forms a green filter layer (41); Step 6. Coating a layer of blue filter layer colored glue (5) on the substrate ⑤ (15) and then curing it, coating a layer of deep ultraviolet photoresist III (33) on the blue filter layer colored glue (5), and then exposing and developing to obtain substrate ⑥ (16); Step 7. Remove the deep ultraviolet photoresist III (33) on the surface of the substrate ⑥ (16) and the blue filter layer colored glue (5) exposed on the surface by ashing dry method, retain the blue filter layer colored glue (5) under the deep ultraviolet photoresist III (33) and the previously prepared red filter layer colored glue and green filter layer colored glue to obtain the substrate ⑦ (17), and the retained blue filter layer colored glue (5) forms a blue filter layer (51); The thickness of the red filter layer colored glue (2) in step 1 is 0.5um~2um, and the substrate ① (11) is baked and cured at a baking temperature of 90°C~270°C for 20min~120min; the baking method is a proximity hot plate, a contact hot plate or an oven; In step 4, the thickness of the green filter layer color glue is 0.5um~2um, and the substrate ④ (14) is baked and cured at a temperature of 90℃~270℃ for 20min~120min; the baking method is a proximity hot plate, a contact hot plate or an oven; In step 6, the thickness of the blue filter layer color glue is 0.5um~2um, and the substrate ⑤ (15) is baked and cured at a temperature of 90℃~270℃ for 20min~120min; the baking method is a proximity hot plate, a contact hot plate or an oven; The thickness of the deep ultraviolet photoresist I (31), deep ultraviolet photoresist II (32) and deep ultraviolet photoresist III (33) are all 0.5um~2um, and the deep ultraviolet photoresist I (31), deep ultraviolet photoresist II (32) and deep ultraviolet photoresist III (33) are Arf photoresist or Krf photoresist; The wavelength of the exposure light source in the exposure and development is 193nm or 248nm, the development time is 50s~120s, and the development temperature is 23°C~50°C; the line width of the positive deep ultraviolet photoresist pattern after development is 0.1um~1um; The ashing dry stripping step uses a dry etcher or a dry stripping machine, the ashing gas is oxygen, the oxygen flow rate is controlled at 50sccm~200sccm, the pressure is controlled at 20mTorr~50mTorr, the power is controlled at 100W~500W, and the etching temperature is controlled at 10℃~50℃.
2. A method for manufacturing a submicron color filter layer of a silicon-based OLED device as claimed in claim 1, Features: The length of the deep ultraviolet photoresist I (31) is equal to the length of the red filter layer required on the silicon-based OLED device, the length of the deep ultraviolet photoresist II (32) is equal to the length of the green filter layer required on the silicon-based OLED device, and the length of the deep ultraviolet photoresist III (33) is equal to the length of the blue filter layer required on the silicon-based OLED device.