Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal display element
By using a polyimide liquid crystal alignment agent with high imidation rate, the problem of excessive pretilt angle in the liquid crystal display element is solved, and a liquid crystal alignment film with a low pretilt angle is realized, and the viewing angle characteristics of the liquid crystal display element are optimized.
Patent Information
- Application Number
- CN201980081826.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-10
- Filing Date
- 2019-12-06
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2039-12-06
AI Technical Summary
In the field of on-board applications of liquid crystal display elements, the frictional orientation film requires a low pretilt angle to reduce the viewing angle dependence of the tone, and it is difficult for the prior art to achieve a pretilt angle of less than 1 degree.
The polyimide produced by reacting aliphatic tetracarboxylic dianhydride and alicyclic tetracarboxylic dianhydride derivative with a specific diamine is used to prepare liquid crystals. Orientation membrane.
It is realized that a low pretilt angle liquid crystal orientation film with a low pretilt angle of less than 1 degree is provided to meet various characteristic needs of liquid crystal display elements and optimize the viewing angle characteristics.
Smart Images

Figure CN113227890B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a liquid crystal alignment agent, a liquid crystal alignment film and a liquid crystal display element. Background Art
[0002] The liquid crystal display element is composed of a pair of transparent substrates with electrodes sandwiching a liquid crystal layer. In addition, in the liquid crystal display element, an organic film composed of an organic material is used as a liquid crystal alignment film to make the liquid crystal in a desired orientation state between the substrates. That is, the liquid crystal alignment film is a constituent member of the liquid crystal display element, formed on the surface of the substrate that sandwiches the liquid crystal and contacts the liquid crystal, and plays the role of orienting the liquid crystal in a certain direction between the substrates. Furthermore, according to the liquid crystal alignment film, the pretilt angle of the liquid crystal can be controlled. It is known that the method of reducing the pretilt angle is mainly through the selection of the structure of polyimide (refer to patent documents 1, 2) and the like.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 9-188761
[0006] Patent Document 2: Japanese Patent Application Laid-Open No. 10-123532 Summary of the invention
[0007] Problems to be solved by the invention
[0008] On the other hand, with the improvement in performance of liquid crystal display elements in recent years, in addition to uses such as large-screen and high-definition LCD televisions, liquid crystal display elements are also used in vehicles, such as car navigation systems, instrument panels, surveillance cameras, monitors for medical cameras, etc. Considering the requirements for viewing angle characteristics, the rubbed orientation film also requires a lower pretilt angle than before.
[0009] Furthermore, viewing angle dependency of color tone caused by the pretilt angle, so-called color shift, has been pointed out as a problem. In order to solve this problem, an alignment film having a pretilt angle of 1 degree or less is specifically required.
[0010] The inventors have conducted various intensive studies to achieve the above-mentioned object, and as a result, have found that a liquid crystal aligning agent having the following constitution is most suitable for achieving the above-mentioned object, thereby completing the present invention.
[0011] Solutions for solving problems
[0012] Thus, the present invention has been completed based on the above-mentioned findings and has the following gist.
[0013] A liquid crystal alignment agent, comprising: a polyimide, which is a reaction product of a tetracarboxylic dianhydride derivative component composed of at least one selected from aliphatic tetracarboxylic dianhydride and alicyclic tetracarboxylic dianhydride and a diamine component, wherein the diamine component contains at least one diamine selected from a structure having the following formula [A], and the imidization rate of the polyimide is 70% or more.
[0014]
[0015] In the formula, X1 and X2 are independently oxygen atoms or sulfur atoms, and R is [-((CH2)2O) p (CH2)2-], p is an integer from 1 to 3.
[0016] Effects of the Invention
[0017] By using the liquid crystal aligning agent of the present invention, it is possible to obtain a liquid crystal aligning film which provides a low pretilt angle of 1 degree or less while satisfying various characteristics required for the liquid crystal aligning film. DETAILED DESCRIPTION
[0018] <Aliphatic and alicyclic tetracarboxylic acid derivatives>
[0019] The polyimide contained in the liquid crystal aligning agent of the present invention is obtained by imidizing a polyimide precursor (hereinafter also referred to as a specific polymer), wherein the polyimide precursor is obtained by a tetracarboxylic dianhydride derivative component composed of at least one selected from aliphatic tetracarboxylic dianhydride and alicyclic tetracarboxylic dianhydride and a diamine component containing a specific diamine. Specific examples of the materials used and the manufacturing method are described in detail below.
[0020] As the tetracarboxylic acid derivative used for producing the polyimide precursor, not only tetracarboxylic dianhydride but also tetracarboxylic acid, a dihalogenated tetracarboxylic acid compound, a tetracarboxylic acid dialkyl ester, and a dihalogenated tetracarboxylic acid dialkyl ester which are derivatives thereof can be mentioned.
[0021] As aliphatic or alicyclic tetracarboxylic dianhydride or its derivative, the thing represented by following formula (4) is especially preferable.
[0022]
[0023] In the formula (4), preferred structures of X1 include the following formulae (X1-1) to (X1-24).
[0024]
[0025] In formulas (X1-1) to (X1-4), R3 to R 23Each of R3 to R4 is independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a monovalent organic group having 1 to 6 carbon atoms and containing a fluorine atom, or a phenyl group. 23 It is preferably a hydrogen atom, a halogen atom, a methyl group or an ethyl group, and more preferably a hydrogen atom or a methyl group.
[0026] As a specific example of formula (X1-1), the following formula (X1-1-1) - (X1-1-6) are mentioned. From a viewpoint of improving liquid crystal orientation, (X1-1-1) is especially preferable.
[0027]
[0028] From the viewpoint of obtaining the effects of the present invention, X1 is more preferably the above-mentioned formula (X1-1-1), (X1-1-2), (X1-9), (X1-10), (X1-21), or (X1-24).
[0029] The compound represented by the formula (4) may be two or more, and may contain the formula (4) in which X1 is the formula (X1-1) and the formula (4) in which X1 is any one of the formulas (X1-2) to (X1-24).
[0030] <Specific diamine>
[0031] The diamine component for producing the polyimide contained in the liquid crystal aligning agent of this invention contains at least one kind selected from the diamines which have the structure of following formula [A].
[0032]
[0033] In the formula, X1 and X2 are independently oxygen atoms or sulfur atoms, and R is [-((CH2)2O) p (CH2)2-], p is an integer from 1 to 3.
[0034] Preferred specific examples of [A] include diamines of the following formulas [A-1] to [A-4]. These may be used alone or in combination of two or more.
[0035]
[0036] The content of the diamine having the structure of the above formula [A] is preferably 40% to 80% of all diamine components, more preferably 40% to 70%, and even more preferably 40% to 60%.
[0037] <Other diamines>
[0038] As the diamine component for producing the polyimide contained in the liquid crystal aligning agent of the present invention, various diamines can be used in accordance with the characteristics of the desired liquid crystal aligning agent, in addition to the diamine having the structure of the above formula [A].
[0039] The other diamine is represented by the following formula (5).
[0040]
[0041] In the above formula (5), A1 and A2 are each independently a hydrogen atom, or an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, or an alkynyl group having 2 to 5 carbon atoms.
[0042] The structure of Y1 is not particularly limited, but preferred structures include the following (Y-1) to (Y-182).
[0043]
[0044]
[0045]
[0046]
[0047]
[0048]
[0049] In the above formula, Me represents a methyl group, R 1 It represents a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms.
[0050]
[0051] From the viewpoint of improving the solubility of the polymer, it is preferred that any structure of Y1 includes a structure represented by the following formula (6).
[0052]
[0053] In the above formula (6), D is a thermally detachable group which is preferably detached at 150° C. to 230° C., more preferably 180° C. to 230° C. and is substituted with a hydrogen atom. Specific examples of Y including the structure represented by the above formula (6) include (Y-124), (Y-131), (Y-158) to (Y-163).
[0054] <Polyamic acid>
[0055] The polyamic acid used as the polyimide precursor of the present invention is obtained from a tetracarboxylic dianhydride derivative component consisting of at least one selected from aliphatic tetracarboxylic dianhydride and alicyclic tetracarboxylic dianhydride and a diamine component containing a specific diamine, and can be produced by the method shown below.
[0056] Specifically, it can be synthesized by reacting a tetracarboxylic dianhydride derivative component composed of at least one selected from aliphatic tetracarboxylic dianhydride and alicyclic tetracarboxylic dianhydride with a diamine component containing a specific diamine in the presence of an organic solvent at -20°C to 150°C, preferably 0°C to 50°C, for 30 minutes to 24 hours, preferably 1 hour to 12 hours.
[0057] From the solubility of monomers and polymers, the organic solvent used for the above reaction is preferably N, N-dimethylformamide, N-methyl-2-pyrrolidone or γ-butyrolactone, which can be used alone or in combination of two or more. From the viewpoint of not easily producing polymer precipitation and easily obtaining high molecular weight substances, the concentration of the polymer is preferably 1% to 30% by mass, more preferably 5% to 20% by mass.
[0058] As for the polyamic acid obtained as described above, the reaction solution can be fully stirred while being injected into a poor solvent to precipitate the polymer and recover it. In addition, by precipitating several times, after cleaning with a poor solvent, a powder of the purified polyamic acid can be obtained at room temperature or by heating and drying. The poor solvent is not particularly limited, and water, methanol, ethanol, hexane, butyl cellosolve, acetone, toluene, etc. can be listed.
[0059] <Polyamic acid ester>
[0060] Polyamic acid ester which is one of the polyimide precursors used for this invention can be manufactured by the method (I), (II) or (III) shown below.
[0061] (I) When made from polyamic acid
[0062] Polyamic acid ester can be synthesized by esterifying polyamic acid obtained from tetracarboxylic dianhydride and diamine. Specifically, it can be synthesized by reacting polyamic acid and an esterifying agent in the presence of an organic solvent at -20°C to 150°C, preferably 0°C to 50°C, for 30 minutes to 24 hours, preferably 1 hour to 4 hours.
[0063] As the esterifying agent, an esterifying agent that can be easily removed by purification is preferred, and examples thereof include: N,N-dimethylformamide dimethyl acetal, N,N-dimethylformamide diethyl acetal, N,N-dimethylformamide dipropyl acetal, N,N-dimethylformamide dineopentyl butyl acetal, N,N-dimethylformamide di-tert-butyl acetal, 1-methyl-3-p-tolyl triazene, 1-ethyl-3-p-tolyl triazene, 1-propyl-3-p-tolyl triazene, 4-(4,6-dimethoxy-1,3,5-triazine-2-yl)-4-methylmorpholine chloride, etc. The amount of the esterifying agent used is preferably 2 to 6 mol equivalents relative to 1 mol of the repeating unit of the polyamic acid.
[0064] From the solubility of the polymer, the solvent used in the above reaction is preferably N, N-dimethylformamide, N-methyl-2-pyrrolidone or γ-butyrolactone, which can be used alone or in combination of two or more. From the viewpoint of not easily producing the precipitation of the polymer and easily obtaining a high molecular weight substance, the concentration of the polymer in the reaction solution is preferably 1% to 30% by mass, more preferably 5% to 20% by mass.
[0065] (II) When produced by reaction of a dichlorotetracarboxylic acid diester with a diamine
[0066] Polyamic acid ester can be produced from dichlorotetracarboxylic acid diester and diamine. Specifically, it can be synthesized by reacting dichlorotetracarboxylic acid diester and diamine in the presence of a base and an organic solvent at -20°C to 150°C, preferably 0°C to 50°C, for 30 minutes to 24 hours, preferably 1 hour to 4 hours.
[0067] The base may be pyridine, triethylamine, 4-dimethylaminopyridine, etc., but pyridine is preferred for mild reaction. The base is preferably used in an amount that is easily removed and a high molecular weight substance is easily obtained in an amount that is 2 to 4 times the molar amount of the dichlorotetracarboxylic acid diester.
[0068] From the solubility of monomers and polymers, the solvent used in the above-mentioned reaction is preferably N-methyl-2-pyrrolidone or γ-butyrolactone, which can be used alone or in combination of two or more. From the viewpoint of not easily producing the precipitation of the polymer and easily obtaining a high molecular weight substance, the polymer concentration in the reaction solution is preferably 1% by mass to 30% by mass, more preferably 5% by mass to 20% by mass. In addition, in order to prevent the hydrolysis of the dichlorotetracarboxylic acid diester, the solvent used for the synthesis of polyamic acid ester is preferably dehydrated as much as possible, preferably in a nitrogen atmosphere to prevent the mixing of external air.
[0069] (III) When produced by reaction of a tetracarboxylic acid diester and a diamine
[0070] Polyamic acid ester can be produced by polycondensing a tetracarboxylic acid diester and a diamine. Specifically, it can be produced by reacting a tetracarboxylic acid diester and a diamine in the presence of a condensing agent, a base, and an organic solvent at 0°C to 150°C, preferably 0°C to 100°C, for 30 minutes to 24 hours, preferably 3 hours to 15 hours.
[0071] The condensing agent may be triphenyl phosphite, dicyclohexylcarbodiimide, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, N,N'-carbonyldiimidazole, dimethoxy-1,3,5-triazinylmethylmorpholinium, O-(benzotriazole-1-yl)-N,N,N',N'-tetramethyluronium tetrafluoroborate, O-(benzotriazole-1-yl)-N,N,N',N'-tetramethyluronium hexafluorophosphate, (2,3-dihydro-2-thio-3-benzoxazolyl)phosphonic acid diphenyl ester, etc. The amount of the condensing agent added is preferably 2 to 3 times the mole of the tetracarboxylic acid diester.
[0072] The base may be a tertiary amine such as pyridine or triethylamine. The base is preferably used in an amount of 2 to 4 times the molar amount of the diamine component from the viewpoint of being easily removed and easily obtaining a high molecular weight substance.
[0073] In addition, in the above reaction, by adding a Lewis acid as an additive, the reaction proceeds efficiently. As the Lewis acid, lithium halides such as lithium chloride and lithium bromide are preferred. The amount of the Lewis acid added is preferably 0 to 1.0 times the mole of the diamine component.
[0074] In order to obtain high molecular weight polyamic acid ester among the manufacturing methods of the said three types of polyamic acid ester, the manufacturing method of said (I) or said (II) is especially preferable.
[0075] The solution of polyamic acid ester obtained as described above can be injected into a poor solvent while being fully stirred to precipitate the polymer. After several precipitations, the solution is washed with a poor solvent and then dried at room temperature or by heating to obtain a purified powder of polyamic acid ester. The poor solvent is not particularly limited, and examples thereof include water, methanol, ethanol, hexane, butyl cellosolve, acetone, toluene, and the like.
[0076] <Polyimide>
[0077] The polyimide used in the present invention can be manufactured by imidizing the polyamic acid or polyamic acid ester. From the viewpoint of electrical properties, the imidization rate of the polyimide used in the present invention is preferably 70% to 99%. In the case of manufacturing polyimide from polyamic acid ester, a basic catalyst is added to the polyamic acid ester solution, or to the polyamic acid solution obtained by dissolving the polyamic acid ester resin powder in an organic solvent, and this chemical imidization is simple. As far as chemical imidization is concerned, the imidization reaction is carried out at a relatively low temperature, and it is not easy to produce a decrease in the molecular weight of the polymer during the imidization process, so it is preferred.
[0078] Chemical imidization can be carried out by stirring the polyamic acid or polyamic acid ester to be imidized in an organic solvent in the presence of a basic catalyst and an acid anhydride. As an organic solvent, the solvent used during the above-mentioned polymerization reaction can be used. As a basic catalyst, pyridine, triethylamine, trimethylamine, tributylamine, trioctylamine, etc. can be listed. Among them, pyridine has a moderate alkalinity for the reaction to proceed, so it is preferred. In addition, as an acid anhydride, acetic anhydride, trimellitic anhydride, pyromellitic anhydride, etc. can be listed, wherein, when acetic anhydride is used, purification after the reaction is completed becomes easy, so it is preferred.
[0079] The temperature during the imidization reaction is, for example, -20°C to 120°C, preferably 0°C to 100°C, and the reaction time can be carried out within 1 hour to 100 hours. The amount of the basic catalyst is 0.5 times to 30 times the mole of the amic acid group, preferably 2 times to 20 times the mole, and the amount of the acid anhydride is 1 times to 50 times the mole of the amic acid group, preferably 3 times to 30 times the mole. The imidization rate of the obtained polymer can be controlled by adjusting the catalyst amount, temperature, and reaction time.
[0080] Since the added catalyst etc. remain in the solution after the imidization reaction of polyamic acid ester or polyamic acid, it is preferable to recover the obtained imidized polymer by the method as mentioned below, and to redissolve it in an organic solvent to make it the liquid crystal aligning agent of this invention.
[0081] The solution of the polyimide obtained as described above can be poured into a poor solvent while being sufficiently stirred to precipitate a polymer. After precipitation is performed several times, washing with a poor solvent, and drying at room temperature or by heating, a powder of a purified polyamic acid ester can be obtained.
[0082] The poor solvent is not particularly limited, and examples thereof include methanol, acetone, hexane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, ethanol, toluene, and benzene.
[0083] <Liquid crystal alignment agent>
[0084] The liquid crystal aligning agent of the present invention has the form of a solution in which a polymer containing a specific polymer is dissolved in an organic solvent. The molecular weight of the polyimide precursor and the polyimide described in the present invention is preferably 2000 to 500000, more preferably 5000 to 300000, and further preferably 10000 to 100000, in terms of weight average molecular weight. In addition, the number average molecular weight is preferably 1000 to 250000, more preferably 2500 to 150000, and further preferably 5000 to 50000.
[0085] It is preferable that content of the specific polymer in the liquid crystal aligning agent of this invention is 2 mass % - 10 mass % in a liquid crystal aligning agent, and it is more preferable that it is 3 mass % - 8 mass %.
[0086] The liquid crystal aligning agent of the present invention may contain a polyamic acid which is a reaction product of an arbitrary tetracarboxylic acid derivative component and an arbitrary diamine component in addition to the specific polymer.
[0087] Moreover, when the liquid crystal aligning agent contains the said polyamic acid, the ratio is preferably 10 mass parts - 900 mass parts with respect to 100 mass parts of polyimide, and, more preferably, 25 mass parts - 700 mass parts.
[0088] All polymer components in the liquid crystal aligning agent of the present invention may also be mixed with other polymers. As polymers other than these, cellulose polymers, acrylic polymers, methacrylic polymers, polystyrene, polyamide, polysiloxane, etc. may be cited. With respect to a total of 100 parts by mass of polyimide and polyamic acid, the content of other polymers other than these is preferably 0.5 to 15 parts by mass, and more preferably 1 to 10 parts by mass.
[0089] The concentration of the polymer of the liquid crystal aligning agent used in the present invention can be appropriately changed according to the setting of the thickness of the coating to be formed, but is preferably 1% by weight or more from the perspective of forming a uniform and defect-free coating, and is preferably 10% by weight or less from the perspective of the storage stability of the solution.
[0090] The solvent in the liquid crystal aligning agent of the present invention preferably uses a solvent (also called a good solvent) that dissolves the polyimide precursor and the polyimide, and a solvent (also called a poor solvent) that improves the coating properties and surface smoothness of the liquid crystal aligning film when the liquid crystal aligning agent is applied. Specific examples of other solvents are listed below, but are not limited to these examples.
[0091] Specific examples of good solvents include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-butyl-2-pyrrolidone, γ-butyrolactone, γ-valerolactone, 1,3-dimethylimidazolidinone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, methyl ethyl ketone, cyclohexanone, cyclopentanone, 3-methoxy-N,N-dimethylpropionamide, and 4-hydroxy-4-methyl-2-pentanone.
[0092] Specific examples of the poor solvent include 1-butoxy-2-propanol, 2-butoxy-1-propanol, 2-propoxyethanol, 2-(2-propoxyethoxy)ethanol, 1-propoxy-2-propanol, ethanol, isopropanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, isopentanol, tert-pentanol, 3-methyl-2-butanol, neopentyl alcohol, 1-hexanol, 2-methyl-1-pentanol, 2-methyl-2-pentanol, 2-ethyl-1-butanol, 1-heptanol, 2-heptanol, 3-heptanol, 1-octanol, 2-octanol, 2-ethyl-1-hexanol, cyclohexanol, 1-methylcyclohexanol, 2-methyl-2-pentanol, 2-ethyl-1-butanol, cyclohexanol, 1-methylcyclohexanol, 2-methyl-1-pentanol, 2-methyl-2-pentanol, 2-ethyl-1-but ...1-pentanol, 2-methyl-2-pentanol, 2-ethyl-1-butanol, cyclohexanol, 1-methylcyclohexanol, 2-methyl-1-pentanol, 2 1,2-ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 2,3-butylene glycol, 1,5-pentanediol, 2-methyl-2,4-pentanediol, 2-ethyl-1,3-hexanediol, dipropyl ether, dibutyl ether, dihexyl ether, dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, 1,2-butoxyethane, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol dibutyl ether, 2-pentanone, 3-pentanone, 2-hexanone, 2-heptanone, 4-heptanone, 3-ethoxybutyl acetate, 1-methylpentyl ethyl Acid ester, 2-ethylbutyl acetate, 2-ethylhexyl acetate, propylene carbonate, ethylene carbonate, 2-(methoxymethoxy)ethanol, butyl cellosolve, ethylene glycol monoisoamyl ether, ethylene glycol monohexyl ether, 2-(hexyloxy)ethanol, furfuryl alcohol, diethylene glycol, propylene glycol, 1-(butoxyethoxy)propanol, propylene glycol monomethyl ether acetate, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, tripropylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, ethylene glycol monoacetate, ethylene glycol diacetate, diethylene glycol monoethyl ether acetate, propylene glycol diacetate, diisoamyl ether, diethylene glycol 2-(2-ethoxyethoxy)ethyl acetate, diethylene glycol acetate, triethylene glycol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol acetate monoethyl ether, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, methyl ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isoamyl lactate, diisobutyl ketone, ethyl carbitol.
[0093] As the poor solvent, a solvent represented by the following formula is preferably used, and if a specific example is given, diisobutylcarbinol is preferably used.
[0094]
[0095] R 24 , R 25 are each independently a linear or branched alkyl group having 1 to 8 carbon atoms. 24 and R 25 The total number of carbon atoms is an integer greater than 3.
[0096] Moreover, as a poor solvent, when the solubility in the solvent of the polyimide precursor and the polyimide contained in the liquid crystal aligning agent is high, the solvent represented by the following formula [D-1] - formula [D-3] is preferable.
[0097]
[0098] In formula [D-1], D 1 represents an alkyl group having 1 to 3 carbon atoms, wherein D 2 represents an alkyl group having 1 to 3 carbon atoms, wherein D 3 It represents an alkyl group having 1 to 4 carbon atoms.
[0099] As a combination of a good solvent and a poor solvent, from the aspect of good printability, the following can be cited: N-methyl-2-pyrrolidone and ethylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone and ethylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone and propylene glycol monobutyl ether; N-ethyl-2-pyrrolidone and propylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone and diethylene glycol diethyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and 2,6-diethyl ether. Methyl-4-heptanone; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and diisopropyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and 2,6-dimethyl-4-heptanol; N-methyl-2-pyrrolidone, γ-butyrolactone and dipropylene glycol dimethyl ether; N-methyl-2-pyrrolidone, propylene glycol monobutyl ether and dipropylene glycol dimethyl ether; N-ethyl-2-pyrrolidone, propylene glycol monobutyl ether and dipropylene glycol dimethyl ether; N-methyl-2-pyrrolidone, propylene glycol monobutyl ether and dipropylene glycol dimethyl ether; combinations of N-methyl-2-pyrrolidone, propylene glycol monobutyl ether and dipropylene glycol monomethyl ether, etc. These poor solvents are preferably 1 to 80% by weight of the total solvent contained in the liquid crystal aligning agent, more preferably 10 to 80% by weight, and particularly preferably 20 to 70% by weight. The type and content of the solvent are appropriately selected depending on a coating device, coating conditions, coating environment, and the like of the liquid crystal aligning agent.
[0100] In addition, the liquid crystal alignment agent of the present invention may also include: a cross-linking compound having an epoxy group, an isocyanate group, an oxetane group or a cyclocarbonate group; a cross-linking compound having at least one substituent selected from the group consisting of a hydroxyl group, a hydroxyalkyl group and a lower alkoxyalkyl group; or a cross-linking compound having a polymerizable unsaturated bond.
[0101] As such a crosslinking compound, various known compounds can be used according to the purpose. The compounds preferably used are the following compounds.
[0102]
[0103] The content of the crosslinking compound is preferably 0.1 to 150 parts by mass, and more preferably 1 to 50 parts by mass, for the crosslinking reaction to proceed and achieve the desired effect.
[0104] The liquid crystal aligning agent of this invention can contain the compound which improves the uniformity of the film thickness of the liquid crystal aligning film when applying a liquid crystal aligning agent, and surface smoothness.
[0105] As a compound which improves the uniformity of the film thickness of a liquid crystal aligning film and surface smoothness, a fluorine-based surfactant, a silicone-based surfactant, a nonionic surfactant, etc. are mentioned.
[0106] As for the usage-amount of a surfactant, it is preferable that it is 0.01-2 mass parts with respect to 100 mass parts of all polymer components which the liquid crystal aligning agent contains, and, as for it, it is more preferable that it is 0.01-1 mass part.
[0107] Moreover, a silane coupling agent for the purpose of improving the adhesion between the liquid crystal alignment film and the substrate, an imidization accelerator for the purpose of efficiently advancing the imidization by heating the polyimide precursor when the coating film is fired, and the like may be contained.
[0108] Examples of the silane coupling agent include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyldiethoxymethylsilane, 2-aminopropyltrimethoxysilane, 2-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, N-ethoxycarbonyl-3-aminopropyltrimethoxysilane, N-ethoxycarbonyl-3-aminopropyltriethoxysilane, N-triethoxysilylpropyltriethylenetriamine, N-trimethoxysilylpropyltriethylenetriamine, N-bis(ethylene oxide)-3-aminopropyltrimethoxysilane, and N-bis(ethylene oxide)-3-aminopropyltriethoxysilane. Silane coupling agents such as vinyl trimethoxysilane, vinyl triethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, 3-glycidoxypropyl methyl dimethoxysilane, 3-glycidoxypropyl trimethoxysilane, 3-glycidoxypropyl methyl diethoxysilane, 3-glycidoxypropyl triethoxysilane, p-phenylenediyl trimethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl methyl diethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-acryloxypropyl trimethoxysilane, tris-(trimethoxysilylpropyl) isocyanurate, 3-mercaptopropyl methyl dimethoxysilane, 3-mercaptopropyl trimethoxysilane, and 3-isocyanate propyl triethoxysilane. The usage-amount of these silane coupling agents is preferably 0.1-30 mass parts, more preferably 0.1-20 mass parts, with respect to 100 mass parts of polymer components contained in the liquid crystal aligning agent from the viewpoint of improving the liquid-crystal orientation.
[0109] <Liquid crystal alignment film, liquid crystal display element>
[0110] The liquid crystal alignment film of the present invention is a film obtained by applying the above-mentioned liquid crystal alignment agent to a substrate, drying and firing. As a substrate for applying the liquid crystal alignment agent of the present invention, as long as it is a substrate with high transparency, there is no particular limitation, and a plastic substrate such as a glass substrate, a silicon nitride substrate, an acrylic substrate, a polycarbonate substrate, etc. can also be used. At this time, if a substrate having an ITO electrode for driving a liquid crystal is used, it is preferred from the perspective of simplifying the process. In addition, in a reflective liquid crystal display element, if only a single-sided substrate is used, an opaque object such as a silicon wafer can also be used, and the electrode in this case can also use a material that reflects light such as aluminum.
[0111] The liquid crystal aligning agent is generally applied industrially by screen printing, gravure printing, flexographic printing or inkjet. Other known coating methods include dipping, roll coating, slit coating, spin coating or spray coating.
[0112] After the liquid crystal orientation agent is applied to the substrate, the solvent can be evaporated by a heating unit such as a heating plate, a thermal circulation oven or an IR (infrared) oven to form a liquid crystal orientation film. The drying and firing processes after the liquid crystal orientation agent is applied can select any temperature and time. In order to fully remove the contained solvent, the conditions of firing at 50°C to 120°C for 1 minute to 10 minutes and then firing at 150°C to 300°C for 5 minutes to 120 minutes are generally listed. If the thickness of the liquid crystal orientation film after firing is too thin, the reliability of the liquid crystal display element is sometimes reduced, so it is preferably 5nm to 300nm, and more preferably 10nm to 200nm.
[0113] The liquid crystal alignment agent of the present invention is coated on a substrate, calcined, and then oriented by brushing, photo-alignment, etc., and can be used as a liquid crystal alignment film without being oriented in vertical alignment applications. In the orientation treatment such as brushing, photo-alignment, etc., known methods and devices can be used.
[0114] As an example of a method for manufacturing a liquid crystal unit, a passive matrix liquid crystal display element is described as an example. It should be noted that an active matrix liquid crystal display element in which a conversion element such as a TFT (Thin Film Transistor) is provided in each pixel portion constituting an image display may also be used.
[0115] Specifically, a transparent glass substrate is prepared, a common electrode is provided on one substrate, and a segment electrode is provided on the other substrate. These electrodes can be provided, for example, as ITO electrodes, and patterned in a manner that enables a desired image display. Next, an insulating film is provided on each substrate in a manner that covers the common electrode and the segment electrode. The insulating film can be provided, for example, as a SiO2-TiO2 film formed by a sol-gel method.
[0116] Next, a liquid crystal alignment film is formed on each substrate, and the substrate of one side is superimposed with the substrate of the other side in a manner that the liquid crystal alignment film faces face each other, and the periphery is bonded with a sealant. In order to control the gap between the substrates, spacers are usually mixed in the sealant. In addition, it is preferred to also spread spacers for controlling the gap between the substrates in the surface where the sealant is not provided. In a part of the sealant, an opening that can be filled with liquid crystal from the outside is pre-set. Next, through the opening provided in the sealant, a liquid crystal material is injected into the space surrounded by the two substrates and the sealant, and then the opening is sealed with an adhesive. The injection can use a vacuum injection method or a method that utilizes capillary phenomena in the atmosphere. The liquid crystal material can be any one of a positive liquid crystal material and a negative liquid crystal material, preferably a negative liquid crystal material. Next, a polarizing plate is set. Specifically, a pair of polarizing plates are bonded to the surface opposite to the liquid crystal layer of the two substrates.
[0117] Example
[0118] The present invention will be described in detail below with reference to Examples, etc., but the present invention is not limited to these Examples. The abbreviations of compounds and solvents are as follows.
[0119] NMP: N-methyl-2-pyrrolidone.
[0120] GBL: gamma-butyrolactone.
[0121] BCS: Butyl Cellosolve.
[0122] DA-1: A compound represented by the following structural formula. (Compound of formula (1))
[0123] DA-2: A compound represented by the following structural formula. (Compound of formula (2))
[0124] DA-3: A compound represented by the following structural formula.
[0125] DA-4: A compound represented by the following structural formula.
[0126] CA-1: A compound represented by the following structural formula.
[0127] (BDA: 1,2,3,4-butanetetracarboxylic dianhydride)
[0128] CA-2: A compound represented by the following structural formula.
[0129] (CBDA: 1,2,3,4-cyclobutanetetracarboxylic dianhydride)
[0130] AD-1: 3-Glycidoxypropyltriethoxysilane.
[0131]
[0132] <Viscosity>
[0133] In the synthesis example, the viscosity of the polymer solution was measured at 25° C. using an E-type viscometer TVE-22H (manufactured by Toki Sangyo Co., Ltd.) with a sample amount of 1.1 mL and a conical rotor TE-1 (1°34′, R24).
[0134] <Measurement of Imidization Ratio of Polyimide>
[0135] The imidization rate of the polyimide in the synthesis example is determined as described below. 30 mg of polyimide powder is added to an NMR (nuclear magnetic resonance) sample tube (NMR standard sampling tube, φ5 (manufactured by Kusano Scientific Co., Ltd.)), deuterated dimethyl sulfoxide (DMSO-d6, 0.05 mass% TMS (tetramethylsilane) mixture) (0.53 ml) is added, and ultrasonic waves are applied to completely dissolve it. The solution is measured by 500 MHz proton NMR in an NMR measuring machine (JNW-ECA500) (manufactured by JEOL DATUM Co., Ltd.). The imidization rate is calculated as follows: the proton derived from the structure that does not change before and after imidization is determined as the reference proton, and the peak integral value of the proton derived from the NH group of the amic acid appearing near 9.5 ppm to 10.0 ppm is used to calculate it using the following formula.
[0136] Imidization rate (%) = (1-α·x / y) × 100
[0137] In the above formula, x is the peak integral value of protons derived from NH groups of amic acid, y is the peak integral value of reference protons, and α is the ratio of the number of reference protons to protons of one NH group of amic acid in the case of polyamic acid (imidation ratio 0%).
[0138] (Synthesis example 1)
[0139] According to the following reaction formula, compound [DA-1] was synthesized via compound [1] and compound [2].
[0140]
[0141] Synthesis of compound [1]
[0142] 4-Fluoronitrobenzene (50.0 g, 354 mmol), hydroquinone (78.0 g), and potassium carbonate (73.4 g) were added to dimethylformamide (400 g), and stirred at 80°C for 2 hours. After cooling to room temperature, the reaction solution was poured into pure water (800 g) while stirring to precipitate crystals. After filtering out the crystals, methanol (1200 g) was added to the filtrate, stirred, and filtered, and the filtrate was concentrated to obtain a crude product (40 g). Ethanol (320 g) was added to the crude product, heated and stirred at 80°C, and pure water (400 g) was added and stirred to precipitate crystals. The crystals were filtered and the filtrate was dried to obtain compound [1] (yield: 34.5 g, yield: 42%, yellow earth-colored crystals).
[0143] 1H-NMR (400MHz, DMSO-d6, δppm): 9.60 (br, 1H), 8.22 (d, 2H, J=9.6Hz), 7.04 (d, 2H, J=9.6Hz), 7.02 (d, 2H, J=9.0Hz), 6.85 (d, 2H, J=9.0Hz).
[0144] Synthesis of compound [2]
[0145] Diethylene glycol di-p-toluenesulfonate (30.2 g, 72.8 mmol), compound [1] (34.5 g), and potassium carbonate (30.2 g) were added to dimethylformamide (276 g), and stirred at 80°C for 15 hours. After cooling to room temperature, pure water (552 g) was added and stirred, resulting in a viscous substance at the bottom of the flask. After removing the supernatant by decantation, methanol (100 g) was added and stirred, and the supernatant was removed by decantation again. Methanol (100 g) was added to the remaining viscous substance and stirred, and the viscous substance gradually solidified. The block was crushed, stirred, filtered, and the filtrate was dried to obtain a crude body (35.5 g). Dimethylformamide (71 g) was added to the crude body, and after heating and stirring at 80°C, methanol (142 g) was added to precipitate crystals. Cool to room temperature, filter, and dry the filtrate. The obtained crystals were recrystallized again using dimethylformamide-methanol, and the filtrate was slurry-washed with methanol (100 g), filtered, and the filtrate was dried to obtain compound [2] (yield: 24.9 g, yield: 64%, light brown crystals).
[0146] 1H-NMR (400MHz, DMSO-d6, δppm): 8.23 (d, 4H, J=9.6Hz), 7.14 (d, 4H, J=9.2Hz), 7.16-7.04 (m, 8H), 4.17-4.14 (m, 4H), 3.86-3.83 (m, 4H).
[0147] Synthesis of [DA-1]
[0148] Compound [2] (24.9 g, 46.8 mmol) and 5% palladium on carbon (2.5 g) were added to tetrahydrofuran (200 g), and the mixture was allowed to stand at room temperature for 18 hours under a hydrogen atmosphere, and then stirred at 40°C for 6 hours. After nitrogen substitution, the catalyst was filtered and the filtrate was concentrated to obtain a crude product (22.3 g). Ethyl acetate (23 g) was added to the crude product, and after heating and dissolving it at 70°C, hexane (45 g) was added and cooled to room temperature. As a result, the crude product solidified after oil out. The block was crushed, stirred, filtered, and the filtrate was dried to obtain compound [DA-1] (yield: 21.2 g, yield: 96%, white crystals).
[0149] 1H-NMR (400MHz, DMSO-d6, δppm): 6.88 (d, 4H, J=9.2Hz), 6.80 (d, 4H, J=9.2Hz), 6.70 (d, 4 H, J=9.2Hz), 6.55 (d, 4H, J=9.2Hz), 4.91 (br, 4H), 4.06-4.03 (m, 4H), 3.79-3.76 (m, 4H).
[0150] (Synthesis example 2)
[0151] (Example)
[0152] In a 50 mL eggplant flask equipped with a stirrer and a nitrogen inlet tube, 3.90 g (8.3 mmol) of DA-1, 1.79 g (4.5 mmol) of DA-3, and 1.25 g (2.3 mmol) of DA-4 were weighed, and 27.3 g of NMP was added, and the mixture was dissolved while nitrogen was supplied. While stirring the diamine solution under water cooling, 1.93 g (9.8 mmol) of CA-1 was added, and 7.7 g of NMP was further added, and the mixture was stirred at 50° C. for 6 hours under a nitrogen atmosphere. Furthermore, 1.0 g (5.1 mmol) of CA-2 was added, and 3.8 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere to obtain a polyamic acid solution (viscosity: 440 mPa·s) PAA-B1.
[0153] Into a 100mL conical flask with a stirrer, 20g of the polyamic acid solution was taken out, 13.3g of NMP, 1.86g of acetic anhydride, and 0.48g of pyridine were added, and after stirring at room temperature for 30 minutes, it was reacted at 55°C for 3 hours. The reaction solution was put into 125g of methanol, and the resulting precipitate was filtered out. After the precipitate was washed with methanol, it was dried under reduced pressure at a temperature of 80°C to obtain a polyimide powder (imidization rate: 85%).
[0154] Furthermore, 2.4 g of a polyimide powder was taken out in a 50 mL eggplant-shaped flask containing a stirring bar, 17.6 g of NMP was added, and the mixture was stirred at 50° C. for 24 hours to dissolve the mixture, thereby obtaining a polyimide solution SPI-A1.
[0155] (Synthesis example 3)
[0156] (Example)
[0157] In a 100 mL eggplant flask equipped with a stirrer and a nitrogen inlet tube, 5.55 g (19.3 mmol) of DA-2, 4.18 g (10.5 mmol) of DA-3, and 2.92 g (5.3 mmol) of DA-4 were weighed, and 50.6 g of NMP was added, and the mixture was stirred and dissolved while nitrogen was supplied. While stirring the diamine solution under water cooling, 4.51 g (22.8 mmol) of CA-1 was added, and 18.0 g of NMP was further added, and the mixture was stirred at 50° C. for 6 hours under a nitrogen atmosphere. Furthermore, 2.26 g (11.5 mmol) of CA-2 was added, and 8.8 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere to obtain a polyamic acid solution (viscosity: 1230 mPa·s) PAA-B2.
[0158] Into a 100mL conical flask with a stirrer, 30.0g of the polyamic acid solution was taken out, 20.0g of NMP, 3.31g of acetic anhydride, and 0.86g of pyridine were added, and after stirring at room temperature for 30 minutes, it was reacted at 55°C for 3 hours. The reaction solution was put into 190g of methanol, and the resulting precipitate was filtered out. After the precipitate was washed with methanol, it was dried under reduced pressure at a temperature of 80°C to obtain a polyimide powder (imidization rate: 84%).
[0159] Furthermore, 3.0 g of a polyimide powder was taken out in a 50 mL eggplant-shaped flask containing a stirring bar, 22.0 g of NMP was added, and the mixture was stirred at 50° C. for 24 hours to dissolve the mixture, thereby obtaining a polyimide solution SPI-A2.
[0160] (Synthesis Example 4)
[0161] (Comparative Example)
[0162] 20.0 g of the polyamic acid solution PAA-B1 obtained in Synthesis Example 2 was taken out, 13.3 g of NMP, 1.86 g of acetic anhydride, and 0.48 g of pyridine were added, and after stirring at room temperature for 30 minutes, it was reacted at 55°C for 1 hour and 30 minutes. The reaction solution was put into 125 g of methanol, and the obtained precipitate was filtered out. After the precipitate was washed with methanol, it was dried under reduced pressure at a temperature of 80°C to obtain a polyimide powder (imidization rate: 55%).
[0163] Furthermore, 2.4 g of the polyimide powder was taken out in a 50 mL eggplant flask containing a stirring bar, 17.6 g of NMP was added, and the mixture was stirred at 50° C. for 24 hours to dissolve the mixture, thereby obtaining a polyimide solution SPI-B1.
[0164] (Synthesis Example 5)
[0165] (Comparative Example)
[0166] 30.0 g of the polyamic acid solution PAA-B1 obtained in Synthesis Example 2 was taken out, 20.0 g of NMP, 3.31 g of acetic anhydride, and 0.86 g of pyridine were added, and after stirring at room temperature for 30 minutes, it was reacted at 55°C for 1 hour and 30 minutes. The reaction solution was put into 190 g of methanol, and the obtained precipitate was filtered out. After the precipitate was washed with methanol, it was dried under reduced pressure at a temperature of 80°C to obtain a polyimide powder (imidization rate: 54%).
[0167] Furthermore, 3.0 g of the polyimide powder was taken out in a 50 mL eggplant-shaped flask containing a stirring bar, 22.0 g of NMP was added, and the mixture was stirred at 50° C. for 24 hours to dissolve the mixture, thereby obtaining a polyimide solution SPI-B2.
[0168] (Examples 1 and 2)
[0169] To the polyimide solutions obtained in Synthesis Examples 2 and 3, NMP, GBL, BCS, and an NMP solution containing 1 wt % of AD-1 were added with stirring so as to have the compositions shown in Table 1 below, and further stirred at room temperature for 2 hours to obtain liquid crystal aligning agents of Examples 1 and 2.
[0170] (Comparative Examples 1 to 4)
[0171] To the polyamic acid solutions obtained in Synthesis Examples 2 and 3 and the polyimide solutions obtained in Synthesis Examples 4 and 5, NMP, GBL, BCS, and an NMP solution containing 1% by weight of AD-1 were added with stirring so as to have the compositions shown in Table 2 below, and further stirred at room temperature for 2 hours, thereby obtaining liquid crystal aligning agents of Comparative Examples 1 to 4.
[0172] [Table 1]
[0173]
[0174] [Table 2]
[0175]
[0176] A method for producing a liquid crystal cell for evaluating a pretilt angle is described below.
[0177] [Fabrication of Liquid Crystal Cell]
[0178] First, a substrate with electrodes was prepared. The substrate was a glass substrate with a size of 30 mm×40 mm and a thickness of 1.1 mm. An ITO electrode with a film thickness of 35 nm was formed on the substrate in a stripe pattern of 40 mm in length and 10 mm in width.
[0179] Next, after filtering out the liquid crystal alignment agent through a filter with a pore size of 1.0 μm, it was applied to the prepared substrate with electrodes by spin coating. After drying on a hot plate at 80°C for 2 minutes, it was calcined in an IR oven at 230°C for 20 minutes to form a coating with a film thickness of 100 nm, and a substrate with a liquid crystal alignment film was obtained. The liquid crystal alignment film was rubbed with rayon cloth (roller diameter: 120 mm, roller speed: 1000 rpm, moving speed: 20 mm / sec, pressing length: 0.4 mm), and then irradiated with ultrasonic waves in pure water for 1 minute for cleaning. After removing water droplets by air blowing, it was dried at 80°C for 10 minutes to obtain a substrate with a liquid crystal alignment film. Two substrates with liquid crystal alignment films were prepared, and after 4 μm spacers were spread on the surface of one of the liquid crystal alignment films, a sealant was printed from above it, and the other substrate was bonded in the opposite direction of the rubbing direction and the film surfaces were facing each other, and the sealant was cured to make an empty unit. Liquid crystal MLC-3019 (Merck Co., Ltd.) was injected into the empty cell by reduced pressure injection, and the injection port was sealed to obtain a liquid crystal cell. The obtained liquid crystal cell was then heated at 120°C for 1 hour, left overnight at 23°C, and used for various evaluations.
[0180] <Pretilt Angle>
[0181] The pretilt angle in the liquid crystal cell 1 was evaluated using an AxoScan Mueller matrix polarimeter manufactured by Optometrics.
[0182] The results of the pretilt angles performed as described above about the liquid crystal display elements using the respective liquid crystal aligning agents of Examples 1 and 2 and Comparative Examples 1 to 4 are shown in Table 3 below.
[0183] [Table 3]
[0184] Polymer 1 Pretilt Angle(°) Example 1 SPI-A1 0.6 Example 2 SPI-A2 0.7 Comparative Example 1 PAA-B1 1.6 Comparative Example 2 PAA-B2 1.9 Comparative Example 3 SPI-B1 1.4 Comparative Example 4 SPI-B2 1.7
[0185] It was found that the liquid crystal display element using the liquid crystal aligning agent of Example of the present invention had a low pretilt angle and was excellent in viewing angle characteristics.
[0186] Industrial Applicability
[0187] By using the liquid crystal aligning agent of the present invention, it is possible to obtain a liquid crystal aligning film that satisfies various properties required for a liquid crystal aligning film and provides a liquid crystal aligning film having a low pretilt angle of 1 degree or less.
Claims
1. A liquid crystal alignment agent, wherein: contain: A polyimide is a reaction product of a tetracarboxylic dianhydride derivative component consisting of at least one selected from aliphatic tetracarboxylic dianhydride and alicyclic tetracarboxylic dianhydride represented by the following formula (4) and a diamine component, In the formula, X1 is selected from the following (X1-1-1), (X1-1-2), (X1-21) and (X1-24) The structure in The diamine component contains at least one selected from the following formula [A-1] to formula [A-3], and the imidization rate of the polyimide is 70% or more.
2. The liquid crystal alignment agent according to claim 1, wherein The total content of the diamines of the formula [A-1] to [A-3] is 40% to 80% of all diamine components.
3. The liquid crystal aligning agent according to claim 1 or 2, wherein: The diamine component further includes a diamine having the following formula (6) in its structure, In the above formula (6), D is a thermally desorbable group which is desorbed at 150°C to 230°C and replaced by a hydrogen atom.
4. The liquid crystal alignment agent according to claim 3, wherein: The diamine having the structure of the formula (6) is at least one selected from the following diamines, In the formula, n is an integer from 1 to 12.
5. The liquid crystal aligning agent according to claim 1 or 2, wherein The liquid crystal alignment agent further contains: polyamic acid, which is a reaction product of a tetracarboxylic dianhydride derivative and a diamine. 6 . A liquid crystal alignment film, obtained from the liquid crystal alignment agent according to claim 1 . 7 . A liquid crystal display element comprising the liquid crystal alignment film according to claim 6 .