Magnetic toner
By controlling the dispersion state and storage elastic modulus of the magnetic body, the problem of poor fixability of magnetic toner at low temperatures and difficulty in maintaining charge in high-temperature and high-humidity environments is solved, achieving excellent low-temperature fixability and image quality, suppressing Eliminates electrostatic staining and uneven melting.
Patent Information
- Application Number
- CN202110168408.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-14
- Filing Date
- 2021-02-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-02-07
AI Technical Summary
Existing magnetic toners have poor fixing properties at low temperatures and are difficult to maintain charge in high-temperature and high-humidity environments, resulting in reduced image quality and electrostatic staining. In addition, the magnetic dispersion is uneven, affecting tinting power and abrasion resistance.
By controlling the dispersion state and storage elastic modulus of the magnetic body in the magnetic toner, ensuring that the occupied area ratio of the magnetic body is between 40.0% and 80.0%, and the storage elastic modulus is within a specific range, the emulsification aggregation method is used Adjust the pH with chelating agents to optimize the aggregation and dispersion of magnetic bodies.
It achieves excellent fixability and image quality in low-temperature environments, suppresses electrostatic staining and uneven melting, and improves image abrasion resistance and stability.
Smart Images

Figure BDA0002938294650000401 
Figure BDA0002938294650000411 
Figure BDA0002938294650000421
Abstract
Description
Technical Field
[0001] The present invention relates to a magnetic toner used in a recording method utilizing an electrophotographic method, an electrostatic recording method, or a toner jet recording method. Background Art
[0002] In recent years, there has been a demand for devices that output images in a wide range of fields from offices to homes and in various environments, and in all of these cases, high image quality is required. At the same time, the image output device itself is also required to be miniaturized and energy-saving.
[0003] In order to save energy, it is important to sufficiently fix the toner at a low temperature.
[0004] As a means for improving fixability, the use of crystalline polyesters that become quickly compatible with the binder resin of the toner and promote the melting deformation of the toner particles in the toner, and the control of the viscoelasticity of the toner have been widely studied. Crystalline polyesters that have a high influence on low-temperature fixability have the property of easily becoming compatible with the binder resin near its melting point, and the toner including the crystalline polyester easily melts and quickly deforms during fixing. Therefore, the low-temperature fixability of the toner is improved by using the crystalline polyester. Japanese Patent Application Laid-Open No. 2013-137420 proposes a toner including a crystalline polyester.
[0005] Meanwhile, miniaturization of a box containing a developer is an effective means for reducing the size of an image output device. Among the developing methods, a single-component developing method is superior to a two-component developing method using a carrier, and enables the weight of the box to be reduced. In addition, in order to reduce the mechanical load on the toner, a non-contact developing method is superior to a contact developing method in which a photosensitive member and a toner carrying member contact each other. Therefore, a single-component non-contact developing method is an effective means for satisfying miniaturization and high image quality.
[0006] In the one-component non-contact developing method, a toner carrying member and an electrostatic latent image carrying member are arranged in a non-contact manner. That is, the toner including a magnetic body is conveyed by rotating a carrying member having a built-in magnet. Since the resistance value of the magnetic body is lower than the resistance value of the binder resin, the charging performance of the toner changes depending on the presence state of the magnetic body inside the toner.
[0007] Japanese Patent Application Laid-Open No. 2005-338538 proposes a toner obtained by a dry process in which a magnetic body is uniformly dispersed inside the toner by controlling the acid value and hydroxyl value of a binder resin and the oil absorption amount and true density of the magnetic body. Summary of the invention
[0008] However, it has been found that, in the toner of Japanese Patent Application Laid-Open No. 2005-338538, improvement in the dispersibility of the magnetic body causes the magnetic body to be exposed on the toner surface, and it is difficult to maintain the charge amount of the toner under a high temperature and high humidity environment.
[0009] A core-shell type toner in which a surface layer is provided on the surface of toner particles so as to suppress exposure of a magnetic body on the toner surface can be considered.
[0010] Japanese Patent Application Publication No. 2019-3129 proposes a core-shell toner including a magnetic body obtained by a suspension polymerization method. However, it has been found that the magnetic body is unevenly distributed on the toner surface, the surface fixation between the toner particles becomes insufficient when the toner is fixed at a low temperature, and the wear resistance of the image is weakened.
[0011] Furthermore, Japanese Patent Application Publication No. 2019-15957 proposes a magnetic toner in which a magnetic body is dispersed by using an emulsion aggregation method so as to maintain appropriate dispersibility while suppressing exposure of the magnetic body on the toner surface.
[0012] However, it has been found that in order to improve low-temperature fixability to meet the above-mentioned demand for energy saving, a large amount of a crystalline polyester having a rapid melting property needs to be included in the binder resin.
[0013] In the toner disclosed in the above document, when a large amount of crystalline resin is added in order to improve low-temperature fixability, the dispersibility of the magnetic body decreases, and the magnetic body gathers inside the toner, thereby reducing the coloring power. It is also found that the affinity between the low-polarity crystalline resin and the magnetic body is low, and thus the possibility of the magnetic body being exposed on the toner surface and charge leakage occurring is high. As a result, it is found that the toner is likely to deteriorate under severe environments such as a high-temperature and high-humidity environment and a low-temperature and low-humidity environment.
[0014] Depending on the composition of the crystalline polyester added in a large amount, the composition of the binder resin, and the combination of the surface shape and surface polarity of the magnetic body, the dispersion state of the magnetic body inside the toner may become uneven and the amount of the magnetic body contained in the toner particles may become uneven. Such a dispersion state of the magnetic body reduces the charging performance of the toner, reduces the developability, and reduces the uniformity of the image density. In addition, when the toner is fixed under a low temperature and low humidity environment, it is found that the above-mentioned method is not sufficient to suppress the melting unevenness and electrostatic offset caused by the magnetic body.
[0015] The present disclosure provides a magnetic toner that is resistant to environmental changes, has excellent low-temperature fixability, and enables toner melting unevenness and electrostatic offset to be suppressed even under severe environments.
[0016] The inventors of the present invention have found that the above-mentioned problems can be solved by controlling the dispersion state of the magnetic body in the magnetic toner and the storage elastic modulus of the magnetic toner.
[0017] The present disclosure relates to a magnetic toner comprising magnetic toner particles containing a binder resin, a magnetic body and a crystalline polyester, wherein
[0018] In cross-sectional observation of magnetic toner particles using a transmission electron microscope,
[0019] When the cross section of the magnetic toner particle is divided by a square grid having a side length of 0.8 μm, the coefficient of variation CV3 of the occupied area ratio of the magnetic body is 40.0% to 80.0%, and
[0020] Assuming that the storage elastic modulus at 40°C is defined as E'(40) [Pa] and the storage elastic modulus at 85°C is defined as E'(85) [Pa], and the storage elastic modulus is the storage elastic modulus obtained in the powder dynamic viscoelasticity measurement of the magnetic toner, the following equations (1) and (2) are satisfied.
[0021] E'(85)≤2.0×10 9 (1)
[0022] [E'(40)-E'(85)]×100 / E'(40)≥70 (2)
[0023] The present disclosure can provide a magnetic toner that is resistant to environmental changes, has excellent low-temperature fixability, and enables toner melting unevenness and electrostatic offset to be suppressed even under severe environments.
[0024] Further features of the present invention will become apparent from the following description of exemplary embodiments. DETAILED DESCRIPTION
[0025] In the present invention, unless otherwise specified, the description of "from XX to YY" or "XX to YY" expressing a numerical range means the numerical range including the lower limit and the upper limit as endpoints.
[0026] Furthermore, monomeric unit refers to the reacted form of a monomeric species in a polymer.
[0027] When describing numerical ranges step by step, the upper and lower limits of each numerical range can be arbitrarily combined.
[0028] Hereinafter, the magnetic toner will be described in more detail, but the present invention is not limited thereto.
[0029] The present disclosure relates to a magnetic toner comprising magnetic toner particles containing a binder resin, a magnetic body and a crystalline polyester, wherein
[0030] In cross-sectional observation of magnetic toner particles using a transmission electron microscope,
[0031] When the cross section of the magnetic toner particle is divided by a square grid having a side length of 0.8 μm, the coefficient of variation CV3 of the occupied area ratio of the magnetic body is 40.0% to 80.0%, and
[0032] Assuming that the storage elastic modulus at 40°C is defined as E'(40) [Pa] and the storage elastic modulus at 85°C is defined as E'(85) [Pa], and the storage elastic modulus is the storage elastic modulus obtained in the powder dynamic viscoelasticity measurement of the magnetic toner, the following equations (1) and (2) are satisfied.
[0033] E'(85)≤2.0×10 9 (1)
[0034] [E'(40)-E'(85)]×100 / E'(40)≥70 (2)
[0035] In the magnetic toner, the dispersion state of the magnetic body in the magnetic toner particles (hereinafter, also simply referred to as toner particles) is controlled to control the storage elastic modulus of the magnetic toner.
[0036] The inventors of the present invention have found a method for solving the problems of improving low-temperature fixability and suppressing electrostatic offset by setting the storage elastic modulus of a magnetic toner within a specific range.
[0037] However, regarding durability, there are issues regarding development performance during durability.
[0038] The inventors of the present invention believe that the sharp melting property of a toner to which a large amount of a crystalline resin is added will be improved by including a segment containing no magnetic body so that the crystalline resin can easily form a domain.
[0039] Therefore, it is believed that the locations where the binder resin is unevenly distributed in the magnetic toner particles, that is, the presence of domains of the binder resin in the toner particles is an effective solution to the problem of the sharp meltability of the toner particles.
[0040] The inventors of the present invention have found means for forming a state in which a magnetic body is aggregated to some extent in each toner particle. As a result, a toner excellent in low-temperature fixability and storage stability is obtained, and the present invention is completed.
[0041] In the magnetic toner, when the cross section of the magnetic toner particle is divided by a square grid with a side length of 0.8 μm, the coefficient of variation CV3 of the occupied area ratio of the magnetic body is 40.0% to 80.0% in cross-sectional observation of the magnetic toner particle using a transmission electron microscope (TEM). CV3 is preferably 45.0% to 70.0%.
[0042] The fact that CV3 is within the above range means that the magnetic body is unevenly localized in the magnetic toner particles. That is, by making the magnetic body unevenly distributed in the magnetic toner particles, a portion where the magnetic body does not exist (i.e., the domain portion of the binder resin) can be appropriately set and the crystalline polyester can be crystallized in this portion.
[0043] As a result, rapid melting properties of toner particles are promoted, and under conditions of high process speed, adhesion of toner to a medium such as paper can be improved when a large number of images are output.
[0044] In addition, since the magnetic body is not excessively exposed on the surface of the toner particles, a satisfactory image with less electrostatic fouling can be obtained, leakage of the charge of the toner particles can be suppressed, and the development performance during the endurance period is improved. In addition, by dispersing the magnetic body in the toner particles in a properly aggregated state, it becomes possible to improve the storage elastic modulus at low temperatures and increase the value of E'(40) [Pa].
[0045] When CV3 is less than 40.0%, the difference in the occupied area ratio of the magnetic body between the grids dividing the cross section of the magnetic toner particle is small. That is, this means that there is no domain portion of the binder resin including the crystallized crystalline polyester, or the domain portion of the binder resin including the crystallized crystalline polyester exists in a small amount.
[0046] In this case, most of the crystalline polyester forms a fine network structure, and the connection between the crystalline polyester parts becomes thin. As a result, the rapid melting property of the toner particles is hindered, and the low-temperature fixability is reduced. In addition, the magnetic body becomes excessively dispersed, and it becomes difficult to maintain the elasticity of the entire toner when melted, so that the fixation separation property is reduced.
[0047] Meanwhile, when CV3 exceeds 80.0%, the magnetic body is excessively localized in the toner. In this case, when the magnetic bodies aggregate with each other and the toner becomes wet and spreads at the time of fixing, the coloring power decreases due to the decrease in shielding power, and the image density at the initial stage of image output decreases. In addition, since the magnetic body may exist near the toner surface, the magnetic body tends to migrate from the toner surface, and the image density difference before and after long-term use becomes large (the image density uniformity decreases).
[0048] As a method for adjusting CV3 within the above range, there can be mentioned controlling the hydrophilicity / hydrophobicity, BET specific surface area and oil absorption of the surface of the magnetic body, and controlling the aggregation degree of the magnetic body at the time of production of toner particles.
[0049] For example, in the case of using the emulsion aggregation method, a method of aggregating the magnetic body in advance and introducing the aggregate into the toner particles, a method of adding a chelating agent and / or adjusting pH in the aggregation step to adjust the aggregation degree of the magnetic body, and the like can be used.
[0050] Furthermore, in cross-sectional observation of the magnetic toner particles using a transmission electron microscope (TEM), when the cross-section of the magnetic toner particles is divided by a square grid with a side length of 0.8 μm, the average value of the occupied area ratio of the magnetic body is 10.0% to 40.0%, and more preferably 15.0% to 30.0%.
[0051] When the average value of the occupied area ratio of the magnetic body is within the above range, the dispersion state of the magnetic body in the toner particles becomes appropriate, and a decrease in coloring power due to an excessive aggregation state can be suppressed.
[0052] In addition, the amount of the binder resin domain present is appropriate, and the toner particles are less likely to break. As a result, electrostatic offset and reduction in fixation separation properties hardly occur, and a satisfactory image can be obtained. In addition, as a method for controlling the average value of the occupied area ratio of the magnetic body within the above range, it is possible to mention controlling the hydrophilicity / hydrophobicity of the surface of the magnetic body, and controlling the aggregation degree of the magnetic body at the time of production of the toner particles, etc.
[0053] Defining the storage elastic modulus at 40° C. as E′(40) [Pa] and the storage elastic modulus at 85° C. as E′(85) [Pa], the storage elastic modulus being the storage elastic modulus obtained in the powder dynamic viscoelasticity measurement of the magnetic toner, the following formulas (1) and (2) are satisfied:
[0054] E'(85)≤2.0×10 9 (1)
[0055] [E'(40)-E'(85)]×100 / E'(40)≥70 (2)
[0056] When E'(85) satisfies the above formula (1), the elasticity of the toner becomes appropriate during fixing and the adhesion to paper becomes strong, so that the low-temperature fixing property is improved, the durability of the image against friction is improved, electrostatic offset in a low-temperature environment can be suppressed, and a satisfactory image can be obtained.
[0057] When E'(85) exceeds 2.0×10 9When the elasticity is too high, the adhesion to paper is reduced, so that the low-temperature fixability is reduced and electrostatic offset tends to occur.
[0058] E'(85) can be controlled by the storage modulus of the binder resin and the amount of the crystalline polyester added. The storage elastic modulus of the binder resin can be controlled by appropriately adjusting the type and molecular weight of the constituent monomers.
[0059] In addition, E'(85) is preferably 1.0×10 9 less than 0.7×10 9 the following.
[0060] The lower limit of E'(85) is not particularly limited, but is preferably 0.1×10 9 More preferably, 0.2×10 9 above.
[0061] The fact that E'(40) and E'(85) satisfy formula (2) indicates that the magnetic toner can undergo a rapid elastic change from 40° C. to 85° C. As a result, even in a fixing step with a high process speed, the toner is melted sufficiently quickly, the adhesion of the toner to paper is improved, and low-temperature fixing becomes possible.
[0062] When [E'(40)-E'(85)]×100 / E'(40) is less than 70, elasticity does not change from 40° C. to 85° C., and rapid melting of the toner becomes insufficient. Therefore, since the toner does not melt to a predetermined elasticity in a short time, low-temperature fixability is reduced.
[0063] [E'(40)-E'(85)]×100 / E'(40) is preferably 72 or more. Meanwhile, the upper limit is not particularly limited, but is preferably 90 or less, more preferably 85 or less, and still more preferably 80 or less.
[0064] E'(40) and E'(85) can be controlled by the storage modulus of the binder resin and the amount of the crystalline polyester added. The storage elastic modulus of the binder resin can be controlled by appropriately adjusting the type and molecular weight of the constituent monomers.
[0065] The magnetic toner particles preferably further contain a wax (releasing agent).
[0066] Assuming that the peak temperature of the maximum endothermic peak derived from the crystalline polyester at the first temperature rise in differential scanning calorimetry of the magnetic toner is defined as Tm(1)°C, the endothermic quantity of the maximum endothermic peak is defined as H(1) J / g, and the peak temperature of the maximum endothermic peak derived from the wax is defined as Tm(2)°C, it is preferred that the following formulas (3) to (5) are satisfied.
[0067] 5.0≤Tm(2)-Tm(1)≤35.0 (3)
[0068] 55.0≤Tm(2)≤100.0 (4)
[0069] H(1)≥10.0 (5)
[0070] When Tm(2)-Tm(1) is 5.0°C or more, the crystalline polyester and the wax are less likely to be compatible with each other, the crystallinity of the crystalline polyester is satisfactorily maintained, the sharp melting property of the toner is improved, and the low temperature fixing property is improved.
[0071] When Tm(2)-Tm(1) is 35.0°C or less, the wax easily oozes out when the binder resin melts at a high temperature, so that the fixing release property is improved and the paper curl can be suppressed.
[0072] Tm(2)-Tm(1) is more preferably 10.0°C to 25.0°C.
[0073] The melting point Tm(2) of the wax is preferably 55.0° C. to 100.0° C. When Tm(2) is 55° C. or higher, the wax is less likely to be exposed on the toner particle surface, and the heat-resistant storage stability is improved. When Tm(2) is 100.0° C. or lower, the wax oozes out when the binder resin melts, and the low-temperature fixability is improved.
[0074] Tm(2) is more preferably 60.0°C to 90.0°C.
[0075] When the endothermic amount H(1) is 10.0 J / g or more, the domain of the crystalline polyester in the binder resin becomes appropriately large, so that the binder resin is likely to be plasticized by melting the crystalline polyester during low-temperature fixing, thereby improving low-temperature fixing property.
[0076] H(1) is more preferably 12.0 J / g or more. The upper limit is not particularly limited, but is preferably 30.0 J / g or less, and more preferably 27.0 J / g or less.
[0077] The toner particles include a crystalline polyester. The crystalline polyester is preferably a polycondensate of a monomer including an aliphatic diol and / or an aliphatic dicarboxylic acid. As referred to herein, a crystalline resin refers to a resin showing a clear melting point by measurement using a differential scanning calorimeter (DSC).
[0078] The crystalline polyester preferably includes a monomer unit derived from an aliphatic diol having 2 to 12 carbon atoms and / or a monomer unit derived from an aliphatic dicarboxylic acid having 2 to 12 carbon atoms.
[0079] Examples of the aliphatic diol having 2 to 12 carbon atoms include the following compounds.
[0080] 1,2-ethanediol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol.
[0081] In addition, an aliphatic diol having a double bond can also be used. Examples of the aliphatic diol having a double bond include the following compounds.
[0082] 2-Butene-1,4-diol, 3-hexene-1,6-diol and 4-octene-1,8-diol.
[0083] The aliphatic dicarboxylic acid having 2 to 12 carbon atoms can be exemplified by the following compounds.
[0084] Oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid. Lower alkyl esters and anhydrides of these aliphatic dicarboxylic acids may also be used.
[0085] Among these, sebacic acid, adipic acid and 1,10-decanedicarboxylic acid and lower alkyl esters and anhydrides thereof are preferred.These may be used alone or in combination of two or more thereof.
[0086] In addition, aromatic carboxylic acids can also be used. Aromatic dicarboxylic acids can be exemplified by the following compounds. Terephthalic acid, isophthalic acid, 2,6-naphthalene dicarboxylic acid, and 4,4'-biphenyl dicarboxylic acid. Among these, terephthalic acid is preferred from the viewpoint of easy availability and easy formation of a polymer having a low melting point.
[0087] In addition, a dicarboxylic acid having a double bond may be used. A dicarboxylic acid having a double bond may be suitably used in order to suppress hot offset at the time of fixing because such an acid makes it possible to crosslink the entire resin by using a double bond.
[0088] Such dicarboxylic acids can be exemplified by fumaric acid, maleic acid, 3-hexenedioic acid and 3-octenoic acid. Also included are lower alkyl esters and anhydrides thereof. Among these, fumaric acid and maleic acid are more preferred.
[0089] The method for producing the crystalline polyester is not particularly limited, and can be exemplified by a general polyester polymerization method in which a dicarboxylic acid component and a diol component react with each other. For example, a direct polycondensation method or an ester exchange method can be used depending on the kind of monomer.
[0090] The peak temperature of the maximum endothermic peak of the crystalline polyester measured using a differential scanning calorimeter (DSC) is preferably 50.0° C. to 100.0° C., and more preferably 60.0° C. to 90.0° C. from the viewpoint of low-temperature fixability.
[0091] The weight average molecular weight Mw of the crystalline polyester is preferably 5,000 to 50,000, and more preferably 10,000 to 45,000.
[0092] The number average molecular weight Mn of the crystalline polyester is preferably 1,000 to 20,000, and more preferably 2,000 to 15,000.
[0093] The amount of the crystalline polyester is preferably 30.0% by mass or more based on the total amount of the binder resin and the crystalline polyester. More preferably, the amount of the crystalline polyester is 31.0% by mass to 60.0% by mass.
[0094] The amount of the crystalline polyester is 30.0% by mass or more, and the crystalline polyester is contained in a preferred amount so that the crystalline polyester plasticizes the binder resin and the low-temperature fixability is improved.
[0095] Furthermore, when the amount of the crystalline polyester is within the above range, the occupied area ratio of the magnetic body is less likely to decrease, so that excessive aggregation of the magnetic body can be suppressed, and a decrease in image density can be suppressed.
[0096] The magnetic toner particles may contain wax.
[0097] Well-known waxes can be used. Specific examples of the waxes are as follows.
[0098] For example, petroleum waxes such as paraffin, microcrystalline wax, and vaseline and their derivatives, montan wax and its derivatives, hydrocarbon waxes obtained by the Fischer-Tropsch process and their derivatives, polyolefin waxes represented by polyethylene and polypropylene and their derivatives, natural waxes such as carnauba wax and candelilla wax and their derivatives, and ester waxes, etc.
[0099] Here, the derivatives include oxides, block copolymers with vinyl monomers, and graft-modified products.
[0100] In addition, a monoester compound including one ester bond in one molecule, and a polyfunctional ester compound such as a diester compound including two ester bonds in one molecule, a tetrafunctional ester compound including four ester bonds in one molecule, and a hexafunctional ester compound including six ester bonds in one molecule can be used as the ester wax.
[0101] The ester wax preferably includes at least one compound selected from the group consisting of monoester compounds and diester compounds.
[0102] Specific examples of the monoester compounds include waxes mainly composed of fatty acid esters such as carnauba wax and montanate wax; compounds obtained by partially or completely removing acid components from fatty acid esters such as deacidified carnauba wax, compounds obtained by hydrogenating vegetable oils and fats, and methyl ester compounds having a hydroxyl group; and saturated fatty acid monoesters such as stearyl stearate and behenyl behenate.
[0103] Furthermore, specific examples of the diester compound include dibehenyl sebacate, nonyl dibehenate, dibehenyl terephthalate, distearyl terephthalate, and the like.
[0104] In addition, the wax may include well-known other waxes other than the above-mentioned compounds. In addition, one kind of wax may be used alone, or two or more kinds may be used in combination.
[0105] The amount of the wax is preferably 1.0 parts by mass to 30.0 parts by mass, and more preferably 3.0 parts by mass to 25.0 parts by mass relative to 100 parts by mass of the binder resin.
[0106] Examples of magnetic bodies include iron oxides such as magnetite, hematite, and ferrite; metals such as iron, cobalt, and nickel, alloys of these metals with metals such as aluminum, copper, magnesium, tin, zinc, beryllium, calcium, manganese, selenium, titanium, tungsten, and vanadium, and mixtures thereof.
[0107] The number average particle diameter of the primary particles of the magnetic body is preferably 0.50 μm or less, and more preferably 0.05 μm to 0.30 μm.
[0108] The number average particle size of the primary particles of the magnetic substance present in the toner particles can be measured using a transmission electron microscope.
[0109] Specifically, after the toner particles to be observed are fully dispersed in the epoxy resin, curing is performed for 2 days in an atmosphere at a temperature of 40°C to obtain a cured product. The resulting cured product is cut into a thin sheet sample by a microtome, an image with a magnification of 10,000 to 40,000 is taken in a transmission electron microscope (TEM), and the projected area of 100 primary particles of the magnetic body in the image is measured. Then, the equivalent diameter of a circle equal to the projected area is taken as the particle size of the primary particles of the magnetic body, and the average value of the 100 particle sizes is taken as the number average particle size of the primary particles of the magnetic body.
[0110] The oil absorption of the magnetic body is preferably 15.0 ml / 100 g to 25.0 ml / 100 g, and more preferably 17.0 ml / 100 g to 23.0 ml / 100 g. When the oil absorption is 15.0 ml / 100 g or more, the magnetic body and the binder resin become more compatible with each other, and the magnetic body is less likely to aggregate, so that the coloring property of the toner is improved.
[0111] When the oil absorption is 25.0 ml / 100 g or less, the dispersibility of the magnetic body is improved, the contact between the magnetic body and the ester bond of the crystalline polyester can be suppressed, and the charging property of the toner is improved.
[0112] The isoelectric point of the magnetic body is preferably pH 8.5 to pH 10.5, and more preferably pH 8.5 to pH 10.0.
[0113] When the isoelectric point is pH 8.5 or higher, the affinity between the magnetic body and the binder resin is improved during aggregation in the emulsion aggregation method, and the magnetic body is not easily aggregated, so that the coloring property of the toner is improved. When the isoelectric point is pH 10.5 or lower, the affinity between the magnetic body and the water in the dispersion medium can be appropriately maintained in the emulsion aggregation method while improving the dispersibility of the magnetic body. Therefore, the magnetic body is less likely to be exposed on the surface of the toner particles, and under a high temperature and high humidity environment, water is less likely to be adsorbed on the toner surface, so that the charge retention is improved.
[0114] As the magnetic properties of the magnetic body with 795.8 kA / m applied, the coercive force (Hc) is preferably 1.6 kA / m to 12.0 kA / m. The magnetization intensity (σs) is preferably 50 Am 2 / kg to 200Am 2 / kg, and more preferably 50Am 2 / kg to 100Am 2 / kg. At the same time, the residual magnetization (σr) is preferably 2Am 2 / kg to 20Am 2 / kg.
[0115] The amount of the magnetic body in the magnetic toner is preferably from 10.0% by mass to 50.0% by mass, and more preferably from 15.0% by mass to 45.0% by mass.
[0116] When the amount of the magnetic body is 10.0% by mass or more, the dispersibility of the magnetic body inside the toner particles is improved while maintaining satisfactory magnetization of the toner particles, so that the adsorption force to the developer carrying member that maintains magnetism in the one-component non-contact developing method can be satisfactorily controlled. Therefore, when an AC developing bias is applied, fogging in the non-contact developing method can be suppressed. In addition, colorability is also improved.
[0117] When the amount of the magnetic body is within the above range, the magnetic attraction with the magnet roller in the developing sleeve is appropriate.
[0118] The amount of the magnetic body in the magnetic toner can be measured using a thermal analyzer TGAQ5000IR manufactured by Perkin Elmer Co. The measuring method is as follows: the magnetic toner is heated from normal temperature to 900° C. at a temperature increase rate of 25° C. / min in a nitrogen atmosphere, the mass loss from 100° C. to 750° C. is taken as the mass of the components other than the magnetic body in the magnetic toner, and the remaining mass is taken as the mass of the magnetic body.
[0119] The magnetic body can be produced, for example, by the following method.
[0120] An alkali such as sodium hydroxide is added to an aqueous solution of ferrous salt in an amount equivalent to or greater than the amount of the iron component to prepare an aqueous solution including ferrous hydroxide. Air is blown into the prepared aqueous solution while maintaining the pH of the aqueous solution at 7 or greater, and while the aqueous solution is heated to 70° C. or greater, an oxidation reaction of the ferrous hydroxide is performed, and seed crystals to be used as magnetic iron oxide nuclei are first generated.
[0121] Next, an aqueous solution of ferrous sulfate containing about 1 equivalent of alkali previously added is added to the slurry containing the seed crystals. The pH of the mixed solution is maintained at 5 to 10, the reaction of ferrous hydroxide is promoted while blowing air, and magnetic iron oxide is grown on the seed crystals as a core. At this time, the shape and magnetic properties of the magnetic body can be controlled by selecting any one of pH, reaction temperature and stirring conditions. As the oxidation reaction proceeds, the pH of the mixed solution moves to the acidic side, but the pH of the mixed solution should not be less than 5. The magnetic body can be obtained by filtering, washing and drying the magnetic body thus obtained according to a conventional method.
[0122] Furthermore, the magnetic body may be subjected to a known surface treatment as required.
[0123] The dielectric loss tangent of the magnetic toner at 100kHz is preferably 0.01 or more. The dielectric loss tangent is more preferably 0.04 to 0.15. The dielectric loss tangent represents the ratio of the dielectric constant to the dielectric loss ratio, and the larger the value of the dielectric loss tangent, the higher the ratio of the dielectric loss ratio, indicating that charging relaxation after polarization is likely to occur.
[0124] In the one-component non-contact development, an AC bias is applied to develop a latent image of a photosensitive member between a toner carried on a developer carrying member and a photosensitive member. At this time, it is necessary to control the dielectric loss tangent of the toner as a sensitivity to the frequency of the AC bias.
[0125] When the dielectric loss tangent is within the above range, the charged state of the toner becomes appropriate even in a low-temperature environment, electrostatic offset is suppressed by not causing excessive charging, and a satisfactory image can be obtained.
[0126] When the dielectric loss tangent is 0.01 or more, charging relaxation is likely to occur and it is difficult to hold excess charge. As a result, when the toner is frictionally charged under a low temperature environment, excessive charging is less likely to occur and electrostatic offset can be suppressed.
[0127] The dielectric loss tangent can be controlled by the dispersibility (aggregation) of the magnetic body in the toner particles. By dispersing the magnetic body in the toner particles without agglomeration, dielectric polarization is likely to occur, and the value of the dielectric loss tangent can be reduced. Conversely, the value of the dielectric loss tangent can be increased by causing aggregation and making dielectric polarization less likely to occur. In addition, it can also be controlled by the dispersion state of the magnetic body in the toner particles.
[0128] Here, the frequency is set to 100kHz as a reference for measuring the dielectric loss tangent because such a frequency is suitable for verifying the dispersion state of the magnetic body. If the frequency is lower than 100kHz, the dielectric loss tangent becomes small, so it is difficult to understand the change in the dielectric loss tangent of the toner, and if the frequency is higher than 100kHz, the difference in the dielectric loss tangent becomes undesirably small when the temperature changes.
[0129] The binder resin is not particularly limited, and a known resin for toner can be used. Specific examples of the binder resin include non-crystalline polyester, polyurethane resin, and vinyl resin.
[0130] Examples of monomers that can be used in the production of the vinyl resin are listed below.
[0131] Aliphatic vinyl hydrocarbons: olefins such as ethylene, propylene, butene, isobutylene, pentene, heptene, diisobutylene, octene, dodecene, octadecene, and other α-olefins; and
[0132] Dienes, for example butadiene, isoprene, 1,4-pentadiene, 1,6-hexadiene and 1,7-octadiene.
[0133] Alicyclic vinyl hydrocarbons: monocyclic or bicyclic alkenes and dienes, such as cyclohexene, cyclopentadiene, vinylcyclohexene, and ethylidenebicycloheptene; and
[0134] Terpenes, such as pinene, limonene, and indene.
[0135] Aromatic vinyl hydrocarbons: styrene and hydrocarbon (alkyl, cycloalkyl, aralkyl and / or alkenyl) substitutes thereof, such as α-methylstyrene, vinyltoluene, 2,4-dimethylstyrene, ethylstyrene, isopropylstyrene, butylstyrene, phenylstyrene, cyclohexylstyrene, benzylstyrene, crotylbenzene, divinylbenzene, divinyltoluene, divinylxylene, trivinylbenzene; and vinylnaphthalene.
[0136] Carboxyl-containing vinyl monomers and metal salts thereof: unsaturated monocarboxylic acids having 3 to 30 carbon atoms, unsaturated dicarboxylic acids, their anhydrides and their monoalkyl (having 1 to 27 carbon atoms) esters. For example, carboxyl-containing vinyl monomers such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, monoalkyl esters of maleic acid, fumaric acid, monoalkyl esters of fumaric acid, crotonic acid, itaconic acid, monoalkyl esters of itaconic acid, itaconic acid glycol monoether, citraconic acid, monoalkyl esters of citraconic acid and cinnamic acid.
[0137] Vinyl esters such as vinyl acetate, vinyl butyrate, vinyl propionate, vinyl butyrate, diallyl phthalate, diallyl adipate, isopropenyl acetate, vinyl methacrylate, methyl 4-vinylbenzoate, cyclohexyl methacrylate, benzyl methacrylate, phenyl acrylate, phenyl methacrylate, vinyl methoxyacetate, vinyl benzoate, ethyl α-ethoxyacrylate, alkyl acrylates and alkyl methacrylates having an alkyl group (linear or branched) having 1 to 22 carbon atoms (methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, lauryl acrylate, lauryl methacrylate, myristyl acrylate, myristyl methacrylate, hexadecyl acrylate, hexadecyl methacrylate, stearyl acrylate, stearyl methacrylate, dimethacrylate acrylate, behenyl acrylate, behenyl methacrylate, etc.), dialkyl fumarate (dialkyl fumarate, two alkyl groups are straight chain, branched chain or alicyclic group with carbon number from 2 to 8), dialkyl maleate (dialkyl maleate, two alkyl groups are straight chain, branched chain or alicyclic group with carbon number from 2 to 8), polyaryloxyalkanes (diaryloxyethane, triaryloxyethane, tetraaryloxyethane, tetraaryloxypropane, tetraaryloxybutane), alkyl, and tetramethylallyloxyethane), vinyl monomers having a polyalkylene glycol chain (polyethylene glycol (molecular weight 300) monoacrylate, polyethylene glycol (molecular weight 300) monomethacrylate, polypropylene glycol (molecular weight 500) monoacrylate, polypropylene glycol (molecular weight 500) monomethacrylate, methanol ethylene oxide (ethylene oxide hereinafter referred to as EO) 10 mole adduct acrylate, methanol ethylene oxide 10 mole adduct methacrylate, lauryl alcohol EO 30 mol adduct acrylate, lauryl EO30 mol adduct methacrylate), polyacrylates and polymethacrylates (polyacrylates and polymethacrylates of polyols: ethylene glycol diacrylate, ethylene glycol dimethacrylate, propylene glycol diacrylate, propylene glycol dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, polyethylene glycol diacrylate, and polyethylene glycol dimethacrylate).
[0138] Carboxyl group-containing vinyl esters: for example, carboxylalkyl acrylates having an alkyl chain having 3 to 20 carbon atoms, and carboxylalkyl methacrylates having an alkyl chain having 3 to 20 carbon atoms.
[0139] Among these, styrene, butyl acrylate, β-carboxyethyl acrylate and the like are preferred.
[0140] Examples of monomers that can be used for the production of non-crystalline polyesters include generally known divalent, trivalent or higher polyvalent carboxylic acids and divalent, trivalent or higher polyvalent alcohols. Specific examples of these monomers are listed below.
[0141] Examples of dicarboxylic acids include dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,13-tridecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,16-hexadecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, phthalic acid, isophthalic acid, terephthalic acid, and dodecenylsuccinic acid, anhydrides thereof or lower alkyl esters thereof, and aliphatic unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, and citraconic acid. Lower alkyl esters and anhydrides of these dicarboxylic acids may also be used.
[0142] Furthermore, examples of the trivalent or higher carboxylic acid include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, anhydrides thereof, lower alkyl esters thereof, and the like.
[0143] These may be used alone, or two or more thereof may be used in combination.
[0144] Examples of the diol include alkylene glycols (1,2-ethanediol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,20-eicosandiol); alkylene ether glycols (polyethylene glycol and polypropylene glycol); alicyclic glycols (1,4-cyclohexanedimethanol); bisphenols (bisphenol A); alkylene oxide (ethylene oxide and propylene oxide) adducts of alicyclic glycols, and alkylene oxide (ethylene oxide and propylene oxide) adducts of bisphenols (bisphenol A).
[0145] The alkyl moiety of the alkylene glycol and the alkylene ether glycol may be linear or branched. In the present invention, an alkylene glycol having a branched structure can also be preferably used.
[0146] In addition, an aliphatic diol having a double bond can also be used. As the aliphatic diol having a double bond, the following compounds can be mentioned.
[0147] 2-Butene-1,4-diol, 3-hexene-1,6-diol and 4-octene-1,8-diol.
[0148] Furthermore, examples of the trivalent or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol.
[0149] These may be used alone, or two or more thereof may be used in combination.
[0150] For the purpose of adjusting the acid value and the hydroxyl value, monobasic acids such as acetic acid and benzoic acid, and monohydric alcohols such as cyclohexanol and benzyl alcohol may be used as necessary.
[0151] The binder resin preferably includes a non-crystalline polyester.
[0152] Among these, the weight average molecular weight Mw of the non-crystalline polyester is preferably 90,000 or less from the viewpoint of paper adhesion.
[0153] Furthermore, from the viewpoint of the difference in image density before and after repeated use, the weight average molecular weight is preferably 1500 or more.
[0154] The synthesis method of the non-crystalline polyester is not particularly limited, and for example, an ester exchange method or a direct polycondensation method may be used alone or in combination.
[0155] The number average molecular weight Mn of the non-crystalline polyester is preferably 1,000 to 50,000, and more preferably 5,000 to 40,000.
[0156] For the non-crystalline polyester, it is preferred to use succinic acid or its anhydride substituted with an alkenyl group having 6 to 18 carbon atoms. That is, the non-crystalline polyester preferably includes a structure in which succinic acid substituted with an alkenyl group having 6 to 18 carbon atoms and a polyol are condensed. The non-crystalline polyester more preferably has a structure in which dodecenyl succinic acid or its anhydride is condensed.
[0157] Since the non-crystalline polyester has a structure derived from alkenyl succinic acid, the crystalline polyester can easily acquire a crystalline structure and rapidly increase in solubility.
[0158] In the non-crystalline polyester, the amount of the structure in which succinic acid (preferably dodecenylsuccinic acid) or its anhydride substituted with an alkenyl group having 6 to 18 carbon atoms is polycondensed is preferably 1 to 30% by mass, and more preferably 5 to 25% by mass.
[0159] As the binder resin, resins such as non-crystalline polyester, polyurethane, and vinyl resin may be used alone or in combination of two or more thereof. From the viewpoint of using crystalline polyester, the binder resin preferably includes non-crystalline polyester, and more preferably non-crystalline polyester. When two or more binder resins are used together, the resins may be used in the form of a composite resin in which the resins are chemically bonded together.
[0160] The glass transition temperature (Tg) of the binder resin is preferably 40.0°C to 120.0°C from the viewpoint of low-temperature fixability.
[0161] The magnetic toner particles preferably have a core-shell structure. That is, it is preferred that the magnetic toner particles have a shell layer. Furthermore, it is more preferred that the magnetic toner particles have a core particle including a binder resin, a magnetic body and a crystalline polyester, and a shell layer on the surface of the core particle. The shell layer does not necessarily cover the entire core particle, and the core particle may be partially exposed.
[0162] The amount of the shell layer is preferably 1 part by mass to 20 parts by mass, and more preferably 5 parts by mass to 15 parts by mass, relative to 100 parts by mass of the binder resin.
[0163] The shell layer preferably includes a non-crystalline polyester having an ethylenically unsaturated bond (double bond) (hereinafter, also referred to as "non-crystalline unsaturated polyester"), and is more preferably made of a non-crystalline unsaturated polyester. The non-crystalline unsaturated polyester is not particularly limited as long as it has an ethylenically unsaturated bond in the molecule.
[0164] The unsaturated bond equivalent of the non-crystalline unsaturated polyester is preferably 4000 g / eq or less, more preferably 1500 g / eq or less, and even more preferably 1000 g / eq or less.
[0165] The unsaturated bond equivalent refers to a value measured by the following method. The molecular weight per unsaturated bond is calculated by performing NMR analysis (H analysis) of the resin, identifying the monomer type and composition ratio, and determining the ratio of the monomer having an unsaturated double bond. The non-crystalline unsaturated polyester is a non-crystalline polyester having an ethylenically unsaturated bond (e.g., vinyl or vinylidene) in the molecule.
[0166] Specifically, for example, the non-crystalline unsaturated polyester may be a polycondensate of a polycarboxylic acid and a polyol in which a monomer having an ethylenically unsaturated bond (eg, vinyl or vinylidene group) as an unsaturated polyester component is used as at least one of the polycarboxylic acid and the polyol.
[0167] From the viewpoint of stability, the non-crystalline unsaturated polyester is preferably a polycondensate of a polycarboxylic acid having an ethylenically unsaturated bond (e.g., vinyl or vinylidene) and a polyol. The non-crystalline unsaturated polyester is more preferably a polycondensate of a dicarboxylic acid having an ethylenically unsaturated bond (e.g., vinyl or vinylidene) and a diol (i.e., a linear polyester).
[0168] When the non-crystalline unsaturated polyester is a polycondensate of a polycarboxylic acid having an ethylenically unsaturated bond and a polyol, a polycarboxylic acid having no ethylenically unsaturated bond may be used as part of the polycarboxylic acid as required. Specific examples of the polycarboxylic acid having no ethylenically unsaturated bond include the polycarboxylic acids described in the section on the non-crystalline polyester.
[0169] Examples of dicarboxylic acids having an ethylenically unsaturated bond (e.g., vinyl or vinylidene) include fumaric acid, maleic acid, maleic anhydride, citraconic acid, mesaconic acid, itaconic acid, glutaconic acid, allylmalonic acid, isopropylidene succinic acid, acetylene dicarboxylic acid, and lower (carbon number 1 to 4) alkyl esters thereof.
[0170] Examples of trivalent or higher carboxylic acids having an ethylenically unsaturated bond (e.g., vinyl or vinylidene) include propylene tricarboxylic acid, 3-butene-1,2,3-tricarboxylic acid, 4-pentene-1,2,4-tricarboxylic acid, 1-pentene-1,1,4,4-tetracarboxylic acid, and lower (carbon number 1 to 4) alkyl esters thereof.
[0171] These polycarboxylic acids may be used alone or in combination of two or more.
[0172] Examples of the diol include bisphenol A, hydrogenated bisphenol A, ethylene oxide or propylene oxide adducts of bisphenol A, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, and neopentyl glycol.
[0173] Examples of the trivalent or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol.
[0174] In addition to the polyols, monobasic acids such as acetic acid and benzoic acid and monohydric alcohols such as cyclohexanol and benzyl alcohol may be used in combination as necessary for the purpose of adjusting the acid value and the hydroxyl value. These polyols may be used alone or in combination of two or more.
[0175] Among the non-crystalline unsaturated polyesters which are polycondensates of these polycarboxylic acids and polyols, polycondensates of at least one dicarboxylic acid selected from fumaric acid, maleic acid, and maleic anhydride and diols are preferred.
[0176] That is, the unsaturated polyester component of the non-crystalline unsaturated polyester is preferably a component derived from at least one dicarboxylic acid selected from fumaric acid, maleic acid, and maleic anhydride.
[0177] In all the polycarboxylic acids and polyols constituting the non-crystalline unsaturated polyester, the proportion of the monomer having an ethylenically unsaturated bond is preferably 5 mol% to 25 mol%, and more preferably 10 mol% to 22.5 mol%. In all the polycarboxylic acids and polyols constituting the non-crystalline unsaturated polyester, the proportion of the monomer having an ethylenically unsaturated bond is preferably 1 mass % to 25 mass %, and more preferably 5 mass % to 20 mass %.
[0178] In all polycarboxylic acids, the ratio of monomers (polycarboxylic acids) having ethylenically unsaturated bonds is preferably 12.5 mol% to 22.5 mol%, and more preferably 12.5 mol% to 20 mol%. In addition, the ratio of monomers (polycarboxylic acids) having ethylenically unsaturated bonds relative to all polycarboxylic acids is preferably 10% to 60% by mass, and more preferably 20% to 50% by mass.
[0179] There is no particular limitation on the production method of the non-crystalline unsaturated polyester, and for example, an ester exchange method or a direct polycondensation method may be used alone or in combination.
[0180] The weight average molecular weight (Mw) of the non-crystalline unsaturated polyester is, for example, preferably from 30,000 to 300,000, more preferably from 30,000 to 200,000, and even more preferably from 35,000 to 150,000.
[0181] The glass transition temperature (Tg) of the non-crystalline unsaturated polyester is preferably 50 to 80° C., and more preferably 50 to 65° C. The glass transition temperature of the non-crystalline unsaturated polyester is determined as a peak temperature of an endothermic peak obtained by differential scanning calorimetry (DSC).
[0182] The magnetic toner particles may include a charge control agent. The magnetic toner is preferably a negatively chargeable toner.
[0183] As the charge control agent for negative charging, an organic metal complex and a chelate compound are effective, and examples thereof include a monoazo metal complex; an acetylacetone metal complex; and a metal complex of an aromatic hydroxycarboxylic acid or an aromatic dicarboxylic acid, and the like.
[0184] Specific examples of commercially available products include SPILON BLACK TRH, T-77, T-95 (Hodogaya Chemical Industry Co., Ltd.), and BONTRON (registered trademark) S-34, S-44, S-54, E-84, E-88, and E-89 (Orient Chemical Industry Co., Ltd.).
[0185] The charge control agent may be used alone or in combination of two or more thereof.
[0186] From the viewpoint of charge amount, the amount of the charge control agent is preferably 0.1 parts by mass to 10.0 parts by mass, and more preferably 0.1 parts by mass to 5.0 parts by mass relative to 100 parts by mass of the binder resin.
[0187] The glass transition temperature (Tg) of the magnetic toner is preferably 45.0°C to 70.0°C, and more preferably 50.0°C to 65.0°C.
[0188] When the glass transition temperature is within the above range, both storage stability and low-temperature fixability can be achieved at a high level. The glass transition temperature can be controlled by the composition of the binder resin, the kind of the crystalline polyester, the molecular weight of the binder resin, and the like.
[0189] The production method of the magnetic toner is not particularly limited, and any of a dry production method (eg, kneading pulverization method, etc.) and a wet production method (eg, emulsification aggregation method, suspension polymerization method, and dissolution suspension method, etc.) may be used.
[0190] Among these, it is preferred to use the emulsification aggregation method.
[0191] When the emulsion aggregation method is used, it is easy to adjust the coefficient of variation of the occupied area ratio of the magnetic body to the above range.
[0192] The method of producing toner particles using the emulsion aggregation method will be described using specific examples.
[0193] The emulsification aggregation method is roughly divided into the following four steps:
[0194] (a) a step of preparing a fine particle dispersion, (b) an aggregation step of forming aggregated particles, (c) an aggregation step of forming toner particles by melting and aggregation, and (d) a washing and drying step.
[0195] (a) Step of preparing fine particle dispersion
[0196] The particle dispersion is obtained by dispersing fine particles of each material such as a binder resin, a magnetic body, and a crystalline polyester in an aqueous medium.
[0197] Examples of the aqueous medium include water such as distilled water and ion-exchanged water, and alcohols. These may be used alone or in combination of two or more thereof.
[0198] An auxiliary agent for dispersing fine particles in an aqueous medium may be used, and a surfactant is an example of the auxiliary agent.
[0199] The surfactant includes anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants.
[0200] Specific examples include anionic surfactants such as alkylbenzene sulfonates, α-olefin sulfonates, and phosphates; cationic surfactants of the amine salt type such as alkylamine salts, amino alcohol fatty acid derivatives, polyamine fatty acid derivatives, and imidazolines, or cationic surfactants of the quaternary ammonium salt type such as alkyltrimethylammonium salts, dialkyldimethylammonium salts, alkyldimethylbenzylammonium salts, pyridinium salts, alkylisoquinolinium salts, and benzethonium chloride; nonionic surfactants such as fatty acid amide derivatives and polyol derivatives; and amphoteric surfactants such as alanine, dodecyldi(aminoethyl)glycine, di(octylaminoethyl)glycine, and N-alkyl-N,N-dimethylammonium betaine.
[0201] These surfactants may be used alone or in combination of two or more thereof.
[0202] The preparation method of the fine particle dispersion can be appropriately selected according to the kind of dispersoid.
[0203] For example, the method of dispersing the dispersoid by using common dispersing machines such as a rotary shearing type homogenizer, a ball mill with a medium, a sand mill or a dyno mill can be mentioned. In addition, in the case where the dispersoid is dissolved in an organic solvent, the dispersoid can be dispersed in an aqueous medium by using a phase inversion emulsification method. In the phase inversion emulsification method, the material to be dispersed is dissolved in an organic solvent in which the material is soluble, the organic continuous phase (O phase) is neutralized, and then an aqueous medium (W phase) is put into to carry out the conversion (so-called phase inversion) of the resin from W / O to O / W, resulting in the formation of a discontinuous phase and being dispersed in an aqueous medium in the form of particles.
[0204] The solvent used in the phase inversion emulsification method is not particularly limited as long as the solvent dissolves the resin, but for the purpose of forming droplets, it is preferred to use a hydrophobic or amphoteric organic solvent.
[0205] It is also possible to prepare fine particle dispersions by polymerization after forming droplets in an aqueous medium, as in emulsion polymerization. Emulsion polymerization is a method for obtaining a fine particle dispersion in which the material is dispersed in an aqueous medium by first mixing a precursor of the material to be dispersed, an aqueous medium, and a polymerization initiator, and then stirring or shearing. At this time, an organic solvent or a surfactant can be used as an emulsifying auxiliary agent. In addition, common equipment can be used for stirring or shearing, and examples thereof are common dispersers such as rotary shear type homogenizers.
[0206] When the magnetic body is dispersed, the particles with the target primary particle diameter can be dispersed in an aqueous medium. For dispersion, for example, conventional dispersion machines such as a rotary shearing homogenizer, a ball mill with a medium, a sand mill, or a Dino mill can be used. Since the specific gravity of the magnetic body is higher than that of water and has a high sedimentation velocity, it is preferred to perform the aggregation step immediately after dispersion.
[0207] The number average particle diameter of the dispersoid of the fine particle dispersion is preferably, for example, 0.01 μm to 1 μm, more preferably 0.08 μm to 0.8 μm, and even more preferably 0.1 μm to 0.6 μm, from the viewpoint of controlling the aggregation speed and simplicity of coalescence.
[0208] From the viewpoint of controlling the aggregation speed, the dispersoid in the fine particle dispersion is preferably 5% by mass to 50% by mass, and more preferably 10% by mass to 40% by mass, based on the total amount of the dispersion.
[0209] (b) Aggregation step
[0210] After the fine particle dispersion is prepared, one fine particle dispersion or two or more particle dispersions are mixed to prepare an agglomerated particle dispersion in which agglomerated particles in which fine particles are agglomerated are dispersed.
[0211] There is no particular limitation on the mixing method, and mixing can be performed using a common stirrer.
[0212] Aggregation is controlled by the temperature, pH, and flocculant of the aggregate particle dispersion, and the like, and any method may be used.
[0213] The temperature for forming aggregated particles is preferably the glass transition temperature of the binder resin minus 30.0° C. to the glass transition temperature of the binder resin. From an industrial viewpoint, the time is preferably about 1 minute to 120 minutes.
[0214] Flocculants can be exemplified by inorganic metal salts, and metal complexes of divalence or higher, etc. When a surfactant is used as an auxiliary agent in a fine particle dispersion, it is also effective to use a surfactant of opposite polarity. In particular, when a metal complex is used as a flocculant, the amount of surfactant used is reduced, and the charging characteristics are improved. Examples of inorganic metal salts include metal salts such as sodium chloride, calcium chloride, calcium nitrate, barium chloride, magnesium chloride, magnesium sulfate, zinc chloride, aluminum chloride, and aluminum sulfate, and inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide.
[0215] From the viewpoint of low temperature fixability and charge retention, the flocculant is preferably a metal salt including at least one metal selected from the group consisting of Mg, Ca, Sr, Al, Fe, and Zn. That is, it is preferred that the magnetic toner particles include a polyvalent metal and the polyvalent metal is at least one metal selected from the group consisting of Mg, Ca, Sr, Al, Fe, and Zn (more preferably Mg).
[0216] In the case of the above-mentioned metal salt, it is easy to contribute to the stabilization of charging performance before and after long-term use.
[0217] In the magnetic toner particles, the total amount of at least one polyvalent metal selected from the group consisting of Mg, Ca, Sr, Al, Fe, and Zn (more preferably, the amount of Mg) is preferably 25 ppm to 1000 ppm on a mass basis. Within the above range, sufficient charging performance is maintained even under high temperature and high humidity. More preferably, the total amount is 30 ppm to 500 ppm.
[0218] There is no particular limitation on the mixing timing of the fine particle dispersion, and the fine particle dispersion may be further added after the aggregated particle dispersion has been formed or during the formation to aggregate.
[0219] By controlling the timing of adding the fine particle dispersion, the internal structure of the toner particles can be controlled.
[0220] In order to control the aggregation degree of the magnetic body, for example, a pre-aggregation step of adding a flocculant to the magnetic body dispersion and stirring can be performed before aggregating each fine particle dispersion. In the pre-aggregation step, for example, about 0.3 to 2.0 parts by mass of a flocculant is preferably added to 100 parts by mass of the magnetic body at about 20° C. to 60° C. and stirred for about 5 seconds to 5 minutes.
[0221] Alternatively, a method in which a magnetic body dispersion liquid is added thereto and agglomeration is further performed after agglomerating a fine particle dispersion liquid other than the magnetic body dispersion liquid is agglomerated is also preferred.
[0222] Furthermore, in the aggregation step, a stirring device capable of controlling the stirring speed may be used. The stirring device is not particularly limited, and any general-purpose emulsifier and disperser may be used.
[0223] For example, a batch emulsifier such as ULTRA TURRAX (manufactured by IKA Corporation), POLYTRON (manufactured by Kinematica Co.), TKHOMOMIXER (manufactured by Tokushu Kika Kogyo Co., Ltd.), EBARAMILDER (manufactured by Ebara Corp.), TKHOMOMIC LINE FLOW (manufactured by Tokushu Kika Kogyo Co., Ltd.), CREAMIX (manufactured by M Technique Co., Ltd.), PHILMIX (manufactured by Tokushu Kika Kogyo Co., Ltd.), or both a batch and a continuous emulsifier can be used.
[0224] The stirring speed can be appropriately adjusted according to the production scale.
[0225] In particular, a magnetic body with a heavy specific gravity is easily affected by the stirring speed. By adjusting the stirring speed and stirring time, the desired particle size can be controlled. When the stirring speed is high, aggregation is likely to be promoted, the aggregation of the magnetic body proceeds, and a toner with low brightness is likely to be formed in the end.
[0226] Furthermore, when the stirring speed is low, the magnetic body tends to settle, the aggregated particle dispersion becomes non-uniform, and a difference in the amount of magnetic body introduced between particles is easily caused.
[0227] At the same time, the aggregation state can also be controlled by adding surfactants.
[0228] Preferably, aggregation is stopped when the aggregated particles reach a target particle size.
[0229] The stopping of aggregation can be carried out by dilution, temperature control, pH control, addition of chelating agent, and addition of surfactant, etc., and from the viewpoint of production, the addition of chelating agent is preferred. In addition, a more preferred method is to stop aggregation by the addition of chelating agent and the adjustment of pH. When the addition of chelating agent and the adjustment of pH are used in combination, it is preferred to form toner particles in which the magnetic body is slightly aggregated after the subsequent coalescence step.
[0230] Furthermore, from the viewpoints of low temperature fixing property, hot offset resistance, transferability, and charge retention, it is preferred that the toner production method includes a metal removal step of adding a chelate compound having chelate ability with respect to metal ions to a dispersion liquid including toner particles to remove metal.
[0231] The pH can be adjusted by a known method using an aqueous solution of sodium hydroxide, etc. The pH is preferably adjusted to 7.0 to 11.0, and more preferably 7.5 to 10.0.
[0232] As the chelating agent, a water-soluble chelating agent is preferred. Specific examples of the chelating agent include, for example, hydroxycarboxylic acids such as tartaric acid, citric acid, and gluconic acid, iminodiacid (IDA), nitrilotriacetic acid (NTA), and ethylenediaminetetraacetic acid (EDTA) and the like.
[0233] The amount of the chelating agent added is, for example, preferably 10.0 parts by mass to 100.0 parts by mass, and more preferably 20.0 parts by mass to 70.0 parts by mass relative to 100 parts by mass of the magnetic body.
[0234] (c) Agglomeration step
[0235] After the aggregated particles are formed, the particles are heated to form toner particles by melting and coalescence. The heating temperature is preferably equal to or higher than the glass transition temperature of the binder resin. For example, 45°C to 130°C.
[0236] Industrially, the time is preferably 1 minute to 900 minutes, and more preferably 5 minutes to 500 minutes.
[0237] Furthermore, toner particles having a core / shell structure can also be formed by heating and coalescing aggregated particles, then mixing a solution in which particles such as a resin are dispersed, and further performing step (b) of forming aggregated particles and step (c) of melting and coalescing.
[0238] After coalescence, the toner particles may be cooled by a known method. The cooling rate is preferably about 0.1° C. / min to 500° C. / min.
[0239] (d) Washing and drying steps
[0240] Well-known washing methods, solid-liquid separation methods, and drying methods can be used without particular limitation.
[0241] However, in the washing step, from the viewpoint of charging performance, it is preferred to fully perform displacement washing with ion exchange water. In the solid-liquid separation step, from the viewpoint of productivity, it is preferred to perform suction filtration and pressure filtration. In the drying step, from the viewpoint of productivity, it is preferred to perform freeze drying, flash jet drying, fluidized drying, and vibration-type fluidized drying.
[0242] The magnetic toner particles may be mixed with an external additive to prepare a magnetic toner, as necessary, in order to improve the fluidity and / or charging performance of the toner. For example, a known device such as a Henschel mixer may be used for mixing the external additive.
[0243] As the external additive, inorganic fine particles having a primary particle number average particle diameter of 4 nm to 80 nm are preferable, and inorganic fine particles having a primary particle number average particle diameter of 6 nm to 40 nm are more preferable.
[0244] When hydrophobizing treatment is carried out, inorganic fine particles can further improve the charging performance and environmental stability of toner. Examples of treating agents for hydrophobizing treatment include organosilicon varnishes, various modified organosilicon varnishes, silicone oils, various modified silicone oils, silane compounds, silane coupling agents, other organoboron compounds, and organotitanium compounds, etc. These treating agents can be used alone or in combination of two or more thereof.
[0245] The number average particle diameter of the primary particles of the inorganic fine particles can be calculated using an image of the toner taken by a scanning electron microscope (SEM).
[0246] Examples of inorganic fine particles include silica fine particles, titanium oxide fine particles, and aluminum oxide fine particles, etc. As the silica fine particles, for example, dry silica such as silica or fumed silica produced by a so-called dry process and generated by gas phase oxidation of silicon halide, and so-called wet silica produced from water glass, etc. can be used.
[0247] However, there are fewer silanol groups on the surface and inside of the silica fine particles and less Na2O and SO3 2- Dry silica such as production residues is preferred.
[0248] In the production step of dry silica, composite fine particles of silica and other metal oxides can also be obtained, for example, by using other metal halides such as aluminum chloride and titanium chloride together with silicon halide in the production process, and the concept of dry silica includes such particles.
[0249] The amount of the inorganic fine particles is preferably 0.1 parts by mass to 3.0 parts by mass relative to 100 parts by mass of the toner particles.The amount of the inorganic fine particles can be quantitatively determined from a calibration curve prepared from a standard sample using a fluorescent X-ray analyzer.
[0250] The magnetic toner may include other additives as long as the effects of the present invention are not adversely affected.
[0251] Examples of other additives include lubricant powders such as fluorocarbon resin powder, zinc stearate powder, and polyvinylidene fluoride powder; abrasives such as cerium oxide powder, boron carbide powder, and strontium titanate powder; and anti-caking agents, etc. Other additives may also be used after the surface is hydrophobized.
[0252] The volume average particle diameter (Dv) of the magnetic toner is preferably 3.0 μm to 8.0 μm, and more preferably 5.0 μm to 7.0 μm.
[0253] By setting the volume average particle diameter (Dv) of the toner within the above range, dot reproducibility can be sufficiently satisfied while improving toner operability.
[0254] Furthermore, the ratio (Dv / Dn) of the volume average particle diameter (Dv) to the number average particle diameter (Dn) of the magnetic toner is preferably less than 1.25.
[0255] The average circularity of the magnetic toner is preferably from 0.970 to 0.985, and more preferably from 0.975 to 0.985.
[0256] When the average circularity is within the above range, the toner is less likely to be compacted and the fluidity of the toner is easily maintained even in a system with a strong shear force such as a one-component contact development system. As a result, when a large amount of image output is performed, the reduction in fixation separation can be further suppressed.
[0257] The average circularity can be controlled by a method generally used in toner production. For example, in the emulsification aggregation method, it is preferred to control the duration of the coalescence step and the amount of surfactant added.
[0258] The following describes the measurement methods of the values of various physical properties according to the present invention.
[0259] Calculation method of the occupied area ratio of the magnetic body in the magnetic toner particles, its average value and its coefficient of variation (CV3) Law
[0260] The occupied area ratio of the magnetic body in the magnetic toner particles, its average value and its coefficient of variation (CV3) are calculated as follows.
[0261] First, a transmission electron microscope (TEM) is used to obtain an image of a cross section of a magnetic toner particle. The obtained cross-sectional image is used to obtain a frequency histogram of the occupied area ratio of the magnetic body in each divided grid based on the division method.
[0262] Then, the coefficient of variation of the occupied area ratio of each obtained divided mesh is determined and taken as the coefficient of variation of the occupied area ratio (CV3).
[0263] Specifically, first, the magnetic toner was compression-molded into a tablet. The tablet was obtained by filling a tablet former having a diameter of 8 mm with 100 mg of the magnetic toner, applying a force of 35 kN, and standing for 1 minute.
[0264] The obtained ingot was sliced with an ultrasonic ultramicrotome (Leica Co., Ltd., UC7) to obtain a thin section sample with a thickness of 250 nm.
[0265] The STEM image of the obtained thin-section sample was taken using a transmission electron microscope (JEOL Co., JEM 2800).
[0266] The probe size for taking STEM images is 1.0 nm, and the image size is 1024×1024 pixels. At this time, by adjusting the contrast of the detector control panel of the bright field image to 1425, the brightness to 3750, the contrast with the image control panel to 0.0, the brightness to 0.5, and the gamma to 1.00, it is possible to take an image with only the dark magnetic body part. With this setting, a STEM image suitable for image processing can be obtained.
[0267] The acquired STEM images were digitized using an image processing device (Nireco, Inc., LUZEX AP).
[0268] Specifically, a frequency histogram of the occupied area ratio of the magnetic body in a square grid with a side length of 0.8 μm was obtained by a division method. At this time, the classification interval of the histogram was 5%.
[0269] Furthermore, the coefficient of variation is obtained from the occupied area ratio of each cross-sectional mesh, and is taken as the coefficient of variation CV3 of the occupied area ratio. In addition, the average value of the occupied area ratio is the average value of the occupied area ratios of each divided mesh.
[0270] Measurement of Dielectric Loss Tangent of Magnetic Toner
[0271] The dielectric characteristics of the magnetic toner are measured by the following method.
[0272] A total of 1 g of the magnetic toner is weighed, and a load of 20 kPa is applied for 1 minute to form a disk-shaped measurement sample having a diameter of 25 mm and a thickness of 1.5±0.5 mm.
[0273] The measurement sample was mounted on ARES (manufactured by TA Instruments) equipped with a dielectric measurement jig (electrode) having a diameter of 25 mm. A dielectric constant of 250 g / cm was applied thereto at a measurement temperature of 30°C. 2 The dielectric loss tangent was calculated from the measured value of the complex dielectric constant at 100 kHz and a temperature of 30° C. under a load of .
[0274] Method for measuring dynamic viscoelasticity of magnetic toner powder
[0275] The measurement is performed using a dynamic viscoelasticity measuring apparatus DMA 8000 (manufactured by Perkin Elmer Inc.).
[0276] Measuring fixture: Material bag (P / N: N533-0322)
[0277] A total of 80 mg of magnetic toner was contained in a material bag, and the material bag was attached to the single cantilever and fixed by tightening a screw with a torque wrench.
[0278] The measurement was performed using dedicated software "DMA Control Software" (manufactured by Perkin Elmer Inc.) The measurement conditions were as follows.
[0279] Oven: Standard air oven
[0280] Measurement Type: Temperature Scan
[0281] DMA conditions: Single frequency / strain (G)
[0282] Frequency: 1Hz
[0283] Strain: 0.05mm
[0284] Starting temperature: 25℃
[0285] End temperature: 180℃
[0286] Scanning speed: 20℃ / min
[0287] Deformation mode: single cantilever (B)
[0288] Cross-section: Rectangular (R)
[0289] Test piece size (length): 17.5 mm
[0290] Test piece size (width): 7.5 mm
[0291] Test piece size (thickness): 1.5 mm
[0292] From the curve of the storage elastic modulus E' obtained by the measurement, E'(40) and E'(85) were read, and the value of [E'(40)-E'(85)]×100 / E'(40) was calculated.
[0293] The following describes the measurement methods of the values of various physical properties according to the present invention.
[0294] Method for measuring volume average particle diameter (Dv) and number average particle diameter (Dn) of magnetic toner
[0295] The volume average particle diameter (Dv) and the number average particle diameter (Dn) of the magnetic toner are calculated in the following manner.
[0296] A precision particle size distribution measuring device "CoulterCounter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.) equipped with a 100 μm orifice tube and based on the pore resistance method was used as a measuring device. The dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.) attached to the device was used to set the measurement conditions and perform measurement data analysis. The measurement was performed with 25,000 effective measurement channels.
[0297] A solution prepared by dissolving special grade sodium chloride in ion exchange water to a concentration of about 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter, Inc.) can be used as the electrolytic aqueous solution.
[0298] Prior to measurement and analysis, the dedicated software was set in the following manner.
[0299] On the "Change Standard Measurement Method (SOM)" screen in the dedicated software, set the total count in the control mode to 50,000 particles, the number of measurements to 1, and the value obtained using "Standard Particles 10.0 μm" (manufactured by Beckman Coulter, Inc.) as the Kd value. The threshold and noise level are automatically set by pressing the "Threshold / Noise Level Measurement Button". In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flushing of the Orifice Tube after Measurement".
[0300] In the "Pulse to Size Conversion Settings" screen of the dedicated software, set the cell spacing to logarithmic size, the size cells to 256 size cells, and the size range to 2 μm to 60 μm.
[0301] The specific measurement method is described below.
[0302] (1) Place approximately 200 mL of the electrolytic aqueous solution in a 250 mL glass round-bottom beaker dedicated to the Multisizer 3, place the beaker on the sample stage, and stir counterclockwise at 24 rpm with a stirring rod. Remove dirt and bubbles in the nozzle using the "Rinse nozzle" function of the dedicated software.
[0303] (2) About 30 mL of the electrolytic aqueous solution was placed in a 100 mL glass flat-bottom beaker. Then, about 0.3 mL of a dilution solution obtained by diluting "CONTAMINON N" (a 10% by mass aqueous solution of a neutral detergent for washing precision measuring instruments composed of a nonionic surfactant, an anionic surfactant, and an organic builder, pH 7, manufactured by Wako Pure Chemical Industries, Ltd.) by 3 times by mass with ion exchange water was added.
[0304] (3) An ultrasonic disperser "Ultrasonic Dispersion System Tetora 150" (manufactured by Nikkaki Bios Co., Ltd.) having a power output of 120 W and in which two oscillators having an oscillation frequency of 50 kHz were built with a phase shift of 180 degrees was prepared. About 3.3 L of ion-exchanged water was put into the water tank of the ultrasonic disperser, and about 2 mL of CONTAMINON N was added to the water tank.
[0305] (4) The beaker of (2) is placed in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is started. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolytic aqueous solution in the beaker is maximized.
[0306] (5) In a state where the electrolytic aqueous solution in the beaker of the above (4) is irradiated with ultrasonic waves, about 10 mg of the magnetic toner is added little by little to the electrolytic aqueous solution and dispersed therein. Then, the ultrasonic dispersion treatment is further continued for 60 seconds. In the ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to a temperature of 10° C. to 40° C.
[0307] (6) The electrolytic aqueous solution of (5) above in which the toner is dispersed is dropped into the round-bottom beaker of (1) above set in the sample stage by using a pipette, and the measurement concentration is adjusted to about 5%. Then, measurement is performed until the number of particles measured reaches 50,000.
[0308] (7) The measurement data is analyzed with the dedicated software attached to the device, and the volume average particle diameter (Dv) and the number average particle diameter (Dn) are calculated. The "50% D diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen obtained when the graph / (volume %) is set in the dedicated software is taken as the volume average particle diameter (Dv), and the "arithmetic diameter" on the "Analysis / Number Statistics (Arithmetic Mean)" screen obtained when the graph / (number %) is set in the dedicated software is taken as the number average particle diameter (Dn).
[0309] Method for measuring average circularity of magnetic toner
[0310] The average circularity of the magnetic toner is measured with a flow-type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corp.) under the measurement and analysis conditions used in the calibration operation.
[0311] The specific measurement method is described below.
[0312] First, about 20mL of ion exchange water from which solid impurities etc. have been removed in advance is put into a glass container. Add about 0.2mL of the dilution prepared by diluting three times of mass of "CONTAMINON N" (a 10% by mass aqueous solution of a neutral detergent for washing precision measuring instruments consisting of a nonionic surfactant, anionic surfactant and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) with ion exchange water as a dispersant. In addition, about 0.02g of the measurement sample is added, and an ultrasonic disperser is used to carry out dispersion treatment for 2 minutes to obtain a measurement dispersion liquid. At this time, the dispersion liquid is suitably cooled to a temperature of 10 ℃ to 40 ℃. As an ultrasonic disperser, using an oscillation frequency of 50kHz and an electrical output as a desktop ultrasonic cleaner disperser ("VS-150" (manufactured by VELVO-CLEAR Co.) of 150W, a predetermined amount of ion exchange water is put into a water tank, and 2mL CONTAMINON N is added into the water tank.
[0313] For the measurement, a flow type particle image analyzer equipped with "LUCPLFLN" (magnification 20×, numerical aperture 0.40) as an objective lens was used, and a particle sheath "PSE-900A" (manufactured by Sysmex Corporation) was used as a sheath liquid. The dispersion prepared according to the above steps was introduced into the flow type particle image analyzer, and 2000 magnetic toner particles were measured in the HPF measurement mode and the total count mode. From the results, the average circularity of the magnetic toner was calculated.
[0314] In the measurement, automatic focusing is performed using standard latex particles (for example, "RESEARCH AND TEST PARTICLES Latex MicrosphereSuspensions 5100A" manufactured by Duke Scientific Inc. diluted with ion-exchanged water) before the start of the measurement. Thereafter, focusing is preferably performed every 2 hours from the start of the measurement.
[0315] The flow-type particle image analyzer used in this case was calibrated by Sysmex Corporation and was accompanied by a calibration certificate issued by Sysmex Corporation.
[0316] Except that the analyzed particle size is limited to an equivalent circle diameter of 1.977 μm or more and less than 39.54 μm, the measurement is performed under the measuring and analyzing conditions when the calibration certificate is received.
[0317] Method for measuring the peak temperature (or melting point) of the maximum endothermic peak
[0318] Using a differential scanning calorimeter (DSC) Q2000 (manufactured by TA Instruments), the peak temperatures (Tm(1) and Tm(2)) of the maximum endothermic peaks and the endothermic amount H(1) were measured under the following conditions.
[0319] Heating rate: 10℃ / min
[0320] Measurement start temperature: 20°C
[0321] Measurement end temperature: 180℃
[0322] The melting points of indium and zinc are used for temperature correction of the device detection unit, and the heat of fusion of indium is used for caloric correction.
[0323] Specifically, about 5 mg of the sample (magnetic toner) is accurately weighed, placed in an aluminum pan, and measured once. An empty aluminum pan is used as a reference. The peak temperature and the endothermic amount of the maximum endothermic peak at this time are measured. The endothermic amount of the endothermic peak is the integral value of the endothermic peak.
[0324] The maximum endothermic peak derived from the crystalline polyester and the maximum endothermic peak derived from the wax can be distinguished by measuring each material separated by the following method.
[0325] Method for separating materials from toner
[0326] Each material can be separated from the toner by using a difference in solubility of each material contained in the toner in a solvent.
[0327] First separation: The toner is dissolved in methyl ethyl ketone (MEK) at 23° C. to separate a soluble component (non-crystalline resin in the binder resin) and an insoluble component (crystalline polyester, wax, magnetic body, inorganic fine particles, etc.).
[0328] Second separation: The insoluble components (crystalline polyester, wax, magnetic body, inorganic fine particles, etc.) obtained by the first separation are dissolved in MEK at 100°C, and the soluble components (crystalline polyester, wax) and the insoluble components (magnetic body, inorganic fine particles, etc.) are separated.
[0329] Third separation: The soluble component (crystalline polyester, wax) obtained by the second separation was dissolved in chloroform at 23°C, and the soluble component (crystalline polyester) and the insoluble component (wax) were separated.
[0330] The peak temperatures of the maximum endothermic peaks of the separated crystalline polyester and wax were measured and coincided with the measurement results of the toner alone.
[0331] Measurement method of glass transition temperature (Tg)
[0332] The glass transition temperature of the magnetic toner or resin can be determined from a reverse heat flow curve at the time of temperature increase obtained by differential scanning calorimetry when the peak temperature of the maximum endothermic peak is measured. The glass transition temperature is the temperature (° C.) at a point where a straight line equidistant in the longitudinal direction from a straight line obtained by extending a base line before and after a specific heat change intersects a curve of a step-like change portion of glass transition in the reverse heat flow curve.
[0333] Method for measuring number average molecular weight (Mn), weight average molecular weight (Mw) and peak molecular weight (Mp) of resins, etc.
[0334] The number average molecular weight (Mn), weight average molecular weight (Mw), and peak molecular weight (Mp) of resins and other materials are measured using gel permeation chromatography (GPC) in the following manner.
[0335] (1) Preparation of measurement samples
[0336] Sample and tetrahydrofuran (THF) are mixed with the concentration of 5.0mg / mL. The mixture is placed at room temperature for 5 hours to 6 hours, and then fully shaken, and the sample and THF are fully mixed until the sample aggregation is loose. Thereafter, each component is left to stand at room temperature for more than 12 hours. At this point, the time from the mixing of sample and THF to the end of standing is set to more than 72 hours, to obtain tetrahydrofuran (THF) soluble matter of sample.
[0337] Subsequently, it was filtered through a solvent-resistant membrane filter (pore diameter: 0.45 μm to 0.50 μm, Myshory Disc H-25-2 (manufactured by Tosoh Corporation)) to produce a sample solution.
[0338] (2) Sample measurement
[0339] The obtained sample solution was used to perform measurement under the following conditions.
[0340] Apparatus: High-speed GPC apparatus LC-GPC 150C (manufactured by Waters Co.)
[0341] Column: 7-column combination of Shodex GPC KF-801, 802, 803, 804, 805, 806, 807 (manufactured by Showa Denko KK)
[0342] Mobile phase: THF
[0343] Flow rate: 1.0mL / min
[0344] Column temperature: 40°C
[0345] Sample injection volume: 100 μL
[0346] Detector: RI (refractive index) detector
[0347] When the molecular weight of a sample is measured, the molecular weight distribution of the sample is calculated from the relationship between the logarithmic value of a calibration curve prepared using several monodisperse polystyrene standard samples and the counts.
[0348] The molecular weight of 6.0×10 produced by Pressure Chemical Co. or Tosoh Corporation was 2 , 2.1×10 3 4.0×10 3 , 1.75×10 4 , 5.1×10 4 , 1×10 5 , 3.9×10 5 , 8.6×10 5 , 2.0×10 6 , and 4.48×10 6 The samples were used as standard polystyrene samples for making the calibration curve.
[0349] Method for measuring particle size of dispersion in fine particle dispersion
[0350] The particle diameter of each fine particle dispersion such as a resin particle dispersion and a magnetic body dispersion is measured using a laser diffraction / scattering particle size distribution measuring apparatus. Specifically, the measurement is performed in accordance with JIS Z 8825-1 (2001).
[0351] As a measuring apparatus, a laser diffraction / scattering type particle size distribution measuring apparatus “LA-920” (manufactured by Horiba, Ltd.) was used.
[0352] For the setting of the measurement conditions and the analysis of the measurement data, the dedicated software "HORIBA LA-920 (registered trademark) WET (LA-920) Ver.2.02 for Windows" attached to the LA-920 was used. In addition, ion exchange water from which solid impurities and the like had been removed in advance was used as the measurement solvent. The measurement procedure was as follows.
[0353] (1) Attach the batch unit holder to the LA-920.
[0354] (2) A predetermined amount of ion exchange water is poured into the batch unit, and the batch unit is set in a batch unit holder.
[0355] (3) Stir the interior of the batch unit using a dedicated stirrer tip.
[0356] (4) Press the "REFRACTIVE INDEX" button on the "Display Condition Setting" screen, and set the relative refractive index to the value of the corresponding particle.
[0357] (5) On the "Display Condition Setting" screen, set the particle size standard to volume standard.
[0358] (6) After performing the warm-up operation for 1 hour or more, perform adjustment of the optical axis, fine adjustment of the optical axis, and blank measurement.
[0359] (7) A total of 3 mL of fine particle dispersion was placed in a 100 mL flat-bottomed beaker made of glass. Then, 57 ml of ion exchange water was added to dilute the fine particle dispersion. Then, about 0.3 mL of a dilution prepared by diluting "CONTAMINON N" (a 10% by mass aqueous solution of a neutral detergent for washing precision measuring instruments, composed of a nonionic surfactant, anionic surfactant, and an organic builder, pH 7, manufactured by Wako Pure Chemical Industries, Ltd.) with ion exchange water by about three times the mass was added as a dispersant.
[0360] (8) An ultrasonic disperser "Ultrasonic Dispersion System Tetora 150" (manufactured by Nikkaki Bios Co., Ltd.) having a power output of 120 W and in which two oscillators having an oscillation frequency of 50 kHz were built with a phase shift of 180 degrees was prepared. About 3.3 L of ion-exchanged water was put into the water tank of the ultrasonic disperser, and about 2 mL of CONTAMINON N was added to the water tank.
[0361] (9) The beaker of (7) above is placed in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is started. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolytic aqueous solution in the beaker is maximized.
[0362] (10) The ultrasonic dispersion treatment is further continued for 60 seconds. During the ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to a temperature of 10°C to 40°C.
[0363] (11) The fine particle dispersion prepared in (10) above is added little by little to the batch unit while being careful not to generate bubbles, thereby adjusting the transmittance of the tungsten lamp to 90% to 95%. Then, the particle size distribution is measured. Based on the volume-based particle size distribution data thus obtained, the particle size of the dispersion in the fine particle dispersion is calculated.
[0364] Measurement of the total amount of polyvalent metals in toner particles
[0365] The amount of metal in the toner particles is measured using a multi-element simultaneous type ICP emission spectrometer Vista-PRO (manufactured by Hitachi High-TechScience Co., Ltd.).
[0366] Sample: 50mg
[0367] Solvent: nitric acid 6mL
[0368] The above-mentioned respective components were weighed and subjected to decomposition treatment using a microwave sample pretreatment device ETHOS UP (manufactured by Milestone General K.K.).
[0369] Temperature: from 20°C to 230°C and maintain at 230°C for 30 minutes
[0370] After passing through the filter paper (5C), the decomposed liquid is transferred to a 50 mL volumetric flask, and the volume is set to 50 mL with ultrapure water. The amount of polyvalent metal elements (Mg, Ca, Al, Zn, etc.) and the amount of monovalent metal elements (Na, Li, and K) in the toner particles can be quantified by measuring the aqueous solution in the volumetric flask with a multi-element simultaneous ICP emission spectrophotometer Vista-PRO under the following conditions. The amount is quantified by using a calibration curve made with a standard sample of the element to be quantified, and is calculated based on the calibration curve.
[0371] Condition: RF power 1.20kW
[0372] Argon: plasma flow rate 15.0L / min
[0373] Auxiliary flow: 1.50L / min
[0374] MFC: 1.50L / min
[0375] Atomizer flow rate: 0.90L / min
[0376] Liquid delivery pump speed: 15rpm
[0377] Repeat measurement: 3 times
[0378] Measuring time: 1.0 seconds
[0379] Measurement of toner to which inorganic fine particles including at least one metal selected from the group consisting of Mg, Ca, Al, and Zn are externally added
[0380] When measuring the amount of metal in the colorant particles of a colorant to which inorganic fine particles including at least one metal selected from the group consisting of Mg, Ca, Al, and Zn are externally added, the measurement is performed after the inorganic fine particles are separated from the colorant so as to avoid calculating the amount of metal derived from the inorganic fine particles other than the metal forming a crosslink with the polar portion.
[0381] The following describes a step for separating the inorganic fine particles from the toner.
[0382] A total of 6 mL of CONTAMINON N (a 10% aqueous solution of a neutral detergent for washing precision measuring instruments, pH 7, composed of a nonionic surfactant, anionic surfactant, and an organic builder, manufactured by WakoPure Chemical Industries, Ltd.) was poured into 100 mL of ion exchange water to prepare a dispersion medium. A total of 5 g of magnetic toner was added to the dispersion medium and dispersed for 5 minutes with an ultrasonic disperser (AS ONE Corporation, VS-150). Thereafter, a dispersion was set in a "KM Shaker" (model: V.SX) manufactured by Iwaki Sangyo Co., Ltd., and vibrated for 20 minutes at 350 cycles per minute.
[0383] Thereafter, the toner particles are constrained using a neodymium magnet to remove the supernatant. The precipitated toner particles are collected and dried.
[0384] Method for measuring oil absorption of magnetic body
[0385] The oil absorption of the magnetic body is measured according to the method described in JIS K 5101-1978 (Pigment Testing Method: Purified Amani Oil Method).
[0386] Specifically, it complies with the JIS standard.
[0387] Method for measuring the isoelectric point of magnetic particles
[0388] The magnetic particles were dissolved or dispersed in ion exchange water at 25°C, and the sample concentration was adjusted to 2.0% by volume. The zeta potential was measured by titration with 1 mol / L HCl using an ultrasonic zeta potential measuring device DT-1200 (manufactured by Dispersion Technology). The pH when the zeta potential was 0 mV was taken as the isoelectric point.
[0389] Measurement of the amount of magnetic material in magnetic toner
[0390] The amount of the magnetic body in the magnetic toner particles can be measured using a thermal analyzer [TGA7] manufactured by PerkinElmer Corp. The measuring method is as follows. The magnetic toner is heated from room temperature to 900° C. at a heating rate of 25° C. / min in a nitrogen atmosphere. The weight loss mass % between 100° C. and 750° C. is the amount of the binder resin, and the remaining mass is the amount of the magnetic body.
[0391] Measurement of the amount of crystalline polyester in the binder resin
[0392] First, each material is separated from the toner by using the difference in solubility of each material contained in the toner in a solvent.The amount of the crystalline polyester is measured based on the following separation.
[0393] First separation: The toner is dissolved in methyl ethyl ketone (MEK) at 23° C. to separate a soluble component (binder resin) and an insoluble component (crystalline polyester, wax, magnetic body, inorganic fine particles, etc.).
[0394] Second separation: The insoluble components (crystalline polyester, wax, magnetic body, inorganic fine particles, etc.) obtained by the first separation are dissolved in MEK at 100°C, and the soluble components (crystalline polyester, wax) and the insoluble components (magnetic body, inorganic fine particles, etc.) are separated.
[0395] Third separation: The soluble component (crystalline polyester, wax) obtained by the second separation was dissolved in chloroform at 23°C, and the soluble component (crystalline polyester) and the insoluble component (wax) were separated.
[0396] The amount of the crystalline polyester when the sum of the first separated binder resin and the third separated crystalline polyester is 100% by mass is calculated.
[0397] Example
[0398] The present invention will be described in more detail below by way of the following Examples and Comparative Examples, but the present invention is not limited thereto. In the Examples and Comparative Examples, parts and % are based on mass unless otherwise specified.
[0399] Production Example of Non-Crystallinous Polyester A1
[0400]
[0401] The above materials were placed in a heated and dried two-necked flask, nitrogen was introduced into the container to maintain an inert atmosphere, and the temperature was raised under stirring. Thereafter, a polycondensation reaction was performed at 150° C. to 230° C. for about 12 hours, and the pressure was gradually reduced at 210° C. to 250° C. to obtain non-crystalline polyester A1.
[0402] The number average molecular weight (Mn) of the non-crystalline polyester A1 was 20,500, the weight average molecular weight (Mw) was 74,100, and the glass transition temperature (Tg) was 58.6°C.
[0403] Production Examples of Non-Crystalline Polyesters A2 to A5
[0404] Non-crystalline polyesters A2 to A5 were obtained in the same manner as in the production example of the non-crystalline polyester A1 except that the formulation was changed as shown in Table 1.
[0405] [Table 1]
[0406]
[0407] In the table, "Mn" represents the number average molecular weight, and "Mw" represents the weight average molecular weight. In the table, the abbreviations are as follows.
[0408] BPA-EO: Bisphenol A ethylene oxide (2 mol) adduct
[0409] BPA-PO: Bisphenol A propylene oxide (2 mol) adduct
[0410] Production Example of Crystalline Polyester B1
[0411] -1,10-decanedicarboxylic acid 79.0 parts
[0412] -1,6-Hexanediol 56.0 parts
[0413] -Dibutyltin oxide 0.1 parts
[0414] The above materials were placed in a heated and dried two-necked flask, nitrogen was introduced into the container to maintain an inert atmosphere, and the temperature was raised under stirring. Then, stirring was performed at 180°C for 6 hours. Thereafter, the temperature was gradually raised to 230°C under reduced pressure while continuing stirring, and the temperature was further maintained for 2 hours. Crystalline polyester B1 was synthesized by cooling with air and stopping the reaction once a viscous state was reached. The weight average molecular weight (Mw) of crystalline polyester B1 was 22500, and the melting point was 73.0°C.
[0415] Production Example of Crystalline Polyesters B2 and B3
[0416] Crystalline polyesters B2 and B3 were obtained in the same manner as in the production example of the crystalline polyester B1, except that the formulations were changed as shown in Table 2. These crystalline polyesters have clear melting points.
[0417] [Table 2]
[0418]
[0419] In the tables, "Mn" represents the number average molecular weight, and "Mw" represents the weight average molecular weight.
[0420] Production Example of Resin Particle Dispersion D-1
[0421] A total of 112.5 parts of ethyl acetate, 37.5 parts of non-crystalline polyester A1, 0.3 parts of 0.1 mol / L sodium hydroxide, and 0.2 parts of anionic surfactant (Neogen RK, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were put into a beaker equipped with a stirrer, heated to 60.0° C., and stirred until dissolution was completed to prepare a resin solution D-1.
[0422] While further stirring the resin solution D-1, a total of 112.5 parts of ion exchange water was gradually added, phase inversion emulsification was performed, and solvent removal was performed to obtain a resin particle dispersion D-1 (solid content concentration: 25.0% by mass).
[0423] The volume average particle size of the resin particles in the resin particle dispersion D-1 was 0.19 μm.
[0424] Production Examples of Resin Particle Dispersions D-2 to D-8
[0425] Resin particle dispersions D-2 to D-8 were obtained in the same manner as in the production example of the resin particle dispersion D-1, except that the formulation was changed as shown in Table 3. The formulations and physical properties are shown in Table 3.
[0426] [Table 3]
[0427]
[0428] Production Example of Wax Dispersion W-1
[0429] - Paraffin (melting point 73°C) 50.0 parts
[0430] - 0.3 parts of anionic surfactant
[0431] (Neogen RK, manufactured by Daiichi Kogyo Seiyaku Co.,Ltd.)
[0432] - 150.0 parts of ion exchange water
[0433] The above components were mixed, heated to 95° C., and dispersed using a homogenizer (ULTRA TURRAX T50, manufactured by IKA Corporation). Thereafter, dispersion was performed using a Manton-Gaulin high pressure homogenizer (manufactured by Gaulin Co., Ltd.) to prepare a wax dispersion W-1 (solid content concentration: 25% by mass) in which wax particles were dispersed. The volume average particle diameter of the obtained wax particles was 0.21 μm.
[0434] Production Example of Wax Dispersion W-2
[0435] -Fischer-Tropsch wax (melting point 105°C) 50.0 parts
[0436] - 0.3 parts of anionic surfactant
[0437] (Neogen RK, manufactured by Daiichi Kogyo Seiyaku Co.,Ltd.)
[0438] - 150.0 parts of ion exchange water
[0439] The above components were mixed, heated to 95° C., and dispersed using a homogenizer (ULTRA TURRAX T50, manufactured by IKA Corporation). Thereafter, dispersion was performed using a Manton-Gaulin high pressure homogenizer (manufactured by Gaulin Co., Ltd.) to prepare a wax dispersion W-2 (solid content concentration: 25% by mass) in which wax particles were dispersed. The volume average particle diameter of the obtained wax particles was 0.22 μm.
[0440] Production Example of Wax Dispersion W-3
[0441] -Fischer-Tropsch wax (melting point 90°C) 50.0 parts
[0442] - 0.3 parts of anionic surfactant
[0443] (Neogen RK, manufactured by Daiichi Kogyo Seiyaku Co.,Ltd.)
[0444] - 150.0 parts of ion exchange water
[0445] The above components were mixed, heated to 95° C., and dispersed using a homogenizer (ULTRA TURRAX T50, manufactured by IKA Corporation). Thereafter, dispersion was performed using a Manton-Gaulin high pressure homogenizer (manufactured by Gaulin Co., Ltd.) to prepare a wax dispersion W-3 (solid content concentration: 25% by mass) in which wax particles were dispersed. The volume average particle diameter of the obtained wax particles was 0.23 μm.
[0446] Production Example of Magnetic Material 1
[0447] A total of 55 L of 4.0 mol / L sodium hydroxide aqueous solution and 50 L of 2.0 mol / L Fe 2+ The aqueous solution was kept at 85° C. and oxidized for 2 hours while blowing air at 20 L / min to obtain a slurry including core particles.
[0448] The obtained slurry was filtered and washed with a filter press, and then the core particles were redispersed in water. Sodium silicate was added in an amount of 0.20 mass % in terms of silicon relative to 100 parts of the core particles to obtain a reslurry solution, the pH of the slurry solution was adjusted to 6.0, and stirred to obtain magnetic iron oxide particles having a silicon-rich surface.
[0449] The obtained slurry solution was filtered with a filter press, washed, and re-slurried with ion exchange water. 500 parts (10% by mass relative to magnetic iron oxide) of ion exchange resin SK110 (manufactured by Mitsubishi Chemical Co., Ltd.) were added to the re-slurry solution (solid content: 50 parts / L), and stirred for 2 hours for ion exchange. Thereafter, the ion exchange resin was removed by filtering through a mesh, followed by filtering and washing with a filter press, and dried and pulverized to obtain a magnetic body 1 having a primary particle number average particle diameter of 0.21 μm.
[0450] Production Examples of Magnetic Substances 2 to 5
[0451] Magnetic bodies 2 to 5 were obtained in the same manner as in the production example of the magnetic body 1, except that the oxidation reaction time was adjusted as described in Table 4. Table 4 shows the physical properties of each magnetic body.
[0452] Production Example of Magnetic Dispersion Liquid M-1
[0453] -Magnetic substance 1 25.0 parts
[0454] - 75.0 parts of ion exchange water
[0455] The above materials were mixed and dispersed at 8000 rpm for 10 minutes using a homogenizer (ULTRA TURRAX T50, manufactured by IKA Corporation) to obtain magnetic body dispersion M-1. The volume average particle diameter of the magnetic body in magnetic body dispersion M-1 was 0.21 μm.
[0456] Production Examples of Magnetic Dispersions M-2 to M-5
[0457] Magnetic body dispersions M-2 to M-5 were produced in the same manner as in the production example of magnetic body dispersion M-1, except that magnetic body 1 was respectively changed to magnetic bodies 2 to 5. The physical properties of each magnetic body are shown in Table 4.
[0458] [Table 4]
[0459]
[0460] Production Example of Magnetic Toner Particles 1
[0461] Aggregation Step
[0462]
[0463] The above materials were put into a beaker, adjusted to a total number of parts of water of 250 parts, and then adjusted to 30.0° C. Then, the materials were mixed by stirring at 5000 rpm for 10 minutes using a homogenizer (ULTRA TURRAX T50, manufactured by IKA Corporation).
[0464] Furthermore, 10.0 parts of a 2.0 mass % aqueous solution of magnesium sulfate was gradually added as a flocculant.
[0465] The raw material dispersion was transferred to a polymerization kettle equipped with a stirrer and a thermometer, and heated to 50.0° C. with a mantle heater and stirred to promote the growth of aggregated particles.
[0466] After 60 minutes had passed, 200.0 parts of a 5.0 mass % aqueous solution of ethylenediaminetetraacetic acid (EDTA) was added to prepare Aggregate Particle Dispersion Liquid 1 .
[0467] Shell formation steps
[0468] Subsequently, the aggregated particle dispersion 1 was adjusted to pH 10.0 by using a 0.1 mol / L sodium hydroxide aqueous solution, and then heated to 85.0° C. and left for 180 minutes (aging time) to allow the aggregated particles to bond. Then, 10 parts of the resin particle dispersion D-3 was further added.
[0469] After 180 minutes, a toner particle dispersion liquid 1 in which toner particles are dispersed is obtained. After cooling at a temperature drop rate of 2.0° C. / min, the toner particle dispersion liquid 1 is filtered and washed with ion exchange water, and when the conductivity of the filtrate becomes 50 mS or less, cake-like toner particles are taken out.
[0470] Next, the cake-like toner particles were put into ion exchange water measured in an amount 20 times the mass of the toner particles, and stirred with a three-in-one motor. When the toner particles were sufficiently loose, re-filtration, washing with running water, and solid-liquid separation were performed. The resulting cake-like toner particles were pulverized in a sample mill and dried in an oven at 40° C. for 24 hours. In addition, the obtained powder was pulverized with a sample mill, and vacuum dried in an oven at 40° C. for 5 hours to obtain magnetic toner particles 1.
[0471] Production Example of Magnetic Toner 1
[0472] A total of 0.3 parts of sol-gel silica fine particles having a primary particle number average particle size of 115 nm were added to 100 parts of magnetic toner particles 1 and mixed using an FM mixer (manufactured by Nippon Coke Kogyo Co., Ltd.). Thereafter, 0.9 parts of silica fine particles having a primary particle number average particle size of 12 nm obtained by treating with hexamethyldisilazane and then with silicone oil were added. 2 / g of hydrophobic silica fine particles were added, and similar mixing was carried out using an FM mixer (manufactured by Japan Coke Industry Co., Ltd.) to obtain a magnetic toner 1.
[0473] The following results are shown in Table 6 regarding the obtained Magnetic Toner 1.
[0474] Production Examples of Magnetic Toner Particles 2 to 29
[0475] Magnetic toner particles 2 to 29 were obtained in the same manner as in the production example of the magnetic toner particle 1, except that the conditions of the aggregation step and the shell layer forming step were changed to the conditions shown in Table 5 and Table 6.
[0476] For Magnetic Toners 19 to 22, a 5.0 mass % aqueous solution of citric acid was used as a chelating agent.
[0477] [Table 5]
[0478]
[0479] In Tables 5 and 6, "DS" indicates dispersion, "Floc." indicates flocculant, Temp. indicates temperature, "AC" indicates "aqueous solution of chelating agent", "AT" indicates "aggregation time", and "MT" indicates "ripening time".
[0480] [Table 6]
[0481]
[0482] Example 1
[0483] Image forming equipment
[0484] The evaluation apparatus was a commercially available magnetic one-component printer HP LaserJet Enterprise M609dn (manufactured by Hewlett-Packard Co., Ltd., process speed 420 mm / s). Using this evaluation apparatus, the following evaluation was performed using Toner 1.
[0485] Evaluation of image density under low temperature and low humidity environment
[0486] A total of 100 g of the magnetic toner 1 was filled in the above-modified apparatus, and a repeated use test was conducted under a low-temperature and low-humidity environment (15.0° C. / 10.0% RH).
[0487] As a test output image, a horizontal line image with a printing rate of 1% was printed on 4,000 sheets by intermittent paper passing.
[0488] In addition, the basis weight is 75g / m 2 Commercial 4200 (manufactured by Xerox Co., Ltd.) was used for the evaluation paper for the test.
[0489] A solid black image portion was formed, and the density of the solid black image was measured with a Macbeth reflection densitometer (manufactured by Macbeth Co.).
[0490] The judgment criteria of the reflection density of the solid black image before repeated use are as follows.
[0491] Evaluation Criteria
[0492] A: 1.45 or more
[0493] B: 1.40 or more and less than 1.45
[0494] C: 1.35 or more and less than 1.40
[0495] D: less than 1.35
[0496] The judgment criteria of the change (uniformity) in image density after repeated use are as follows.
[0497] In the repeated use test, the smaller the difference between the reflection density of the solid black image before repeated use and the reflection density of the solid black image output after printing 4000 sheets, the better.
[0498] Evaluation Criteria
[0499] A: Concentration difference is less than 0.10
[0500] B: The concentration difference is 0.10 or more and less than 0.15
[0501] C: The concentration difference is 0.15 or more and less than 0.20
[0502] D: Concentration difference is 0.20 or more
[0503] Evaluation of electrostatic fouling in low temperature and low humidity environment
[0504] In the evaluation, the temperature of the fixing unit of the image forming apparatus was set to 180°C, and a 3 cm square isolated dot image (image density was set to 0.75 to 0.80) was output onto Fox RIVER BOND paper (90 g / m 2 ), and then visually judge the level of electrostatic offset generated in the solid white area below the dot image.
[0505] Evaluation Criteria
[0506] A: Cannot be confirmed visually
[0507] B: Very slight level can be confirmed
[0508] C: The stained part can be visually confirmed, but there are also unstained parts
[0509] D: Can clearly identify a 3cm square
[0510] Evaluation of fixation separation
[0511] The evaluation environment was a normal temperature and humidity environment (25.0°C / 50%RH), by using the above-mentioned image forming apparatus, and a base weight of 75 g / m 2 Commercial 4200 (manufactured by Xerox Co.) was used as the evaluation paper.
[0512] Then, a solid black image having a length of 5.0 cm and a width of 20.0 cm was formed on a recording medium using the filled toner so that the toner laid-on amount was 0.90 mg / cm2 At this time, the image is formed while changing the range of the blank portion at the upper end in the paper passing direction.
[0513] The unfixed image was fixed at a set temperature of 160° C. The minimum margin where the paper was not wrapped around the fixing roller was evaluated according to the following criteria.
[0514] Evaluation Criteria
[0515] A: No entanglement
[0516] B: The blank space from the top is more than 1mm and less than 4mm
[0517] C: The margin from the top is 4 mm or more and less than 7 mm
[0518] D: The blank space from the top is more than 7mm
[0519] Evaluation of heat storage resistance
[0520] A total of 10 g of the toner to be evaluated was put into a 100 ml resin cup and left to stand under an environment of 53° C. for 3 days, and then the state of the powder was visually evaluated.
[0521] Evaluation Criteria
[0522] A: Confirm that there is no aggregation at all and the state is basically the same as the initial state.
[0523] B: Powder appears to aggregate, but can be easily loosened with fingers.
[0524] C: Powder clumped but could be loosened with fingers.
[0525] D: Powder solidification.
[0526] Evaluation of low temperature fixability
[0527] In a normal temperature and humidity environment (25.0°C / 50%RH), by using the above-mentioned image forming apparatus and a base weight of 75 g / m 2 Commercial 4200 (manufactured by Xerox Co.) was used as the evaluation paper for evaluation.
[0528] spot
[0529] The evaluation image was a solid black image, and the set temperature of the fixing unit of the image forming apparatus was adjusted to 140° C. During the evaluation, the fixing device was removed, and the following evaluation was performed while the fixing device was sufficiently cooled using a fan or the like. By sufficiently cooling the fixing device after the evaluation, the temperature of the fixing nip portion that had been raised after the output of the image was cooled, so that the fixability of the toner could be strictly evaluated with satisfactory reproducibility.
[0530] In a state where the fixing device is sufficiently cooled, a solid black image is output on the above paper using Toner 1. At this time, the toner load on the paper is adjusted to 0.90 mg / cm 2 In the evaluation results of Toner 1, a satisfactory solid black image without spots was obtained. The judgment criteria of spots are described below.
[0531] For the solid black image output according to the above steps, the level of spots was visually evaluated. The judgment criteria were as follows.
[0532] Evaluation Criteria
[0533] A: No spots at all
[0534] B: Some spots are seen upon close inspection
[0535] C: Spots are visible, but not obvious
[0536] D: obvious spots
[0537] Evaluation of paper adhesion
[0538] The evaluation image was a halftone image, and the image was output by lowering the set temperature of the fixing unit of the image forming apparatus from 200° C. by 5° C. Then, Silbon paper was used at 55 g / cm 2 The fixed image was rubbed ten times under a load of , and the temperature at which the density reduction rate of the fixed image after rubbing exceeded 10% was taken as the lower limit fixing temperature.
[0539] Evaluation was performed according to the following criteria: The lower the lower limit fixing temperature, the better the low-temperature fixing property.
[0540] Evaluation Criteria
[0541] A: less than 150℃
[0542] B: 150℃ or higher and less than 160℃
[0543] C: 160℃ or higher and less than 175℃
[0544] D: 175℃ or above
[0545] [Table 7]
[0546]
[0547] In the table, "CPES" means "crystalline polyester", "MB" means "magnetic body", "DL" means "dielectric loss tangent of toner", and "TC" means "average circularity of toner". The amount of crystalline polyester is based on the total content of binder resin and crystalline polyester. The amount of magnetic body is the amount in magnetic toner. "A" means the total amount (ppm) of polyvalent metals (Mg, Ca, Sr, Al, Fe, and Zn).
[0548] Examples 2 to 18 and Comparative Examples 1 to 11
[0549] The same evaluation as in Example 1 was performed using Magnetic Toners 2 to 29. The results are shown in Table 8.
[0550] [Table 8]
[0551]
[0552] In the table, "CE" means "Comparative Example".
[0553] While the present invention has been described with reference to exemplary embodiments, it is to be understood that the invention is not limited to the disclosed exemplary embodiments.The scope of the following claims is to be accorded the broadest interpretation so as to encompass all such modifications and equivalent structures and functions.
Claims
1. A magnetic toner comprising magnetic toner particles comprising a binder resin, a magnetic body and a crystalline polyester, It is characterized in that In cross-sectional observation of the magnetic toner particles using a transmission electron microscope, When the cross section of the magnetic toner particle is divided by a square grid having a side length of 0.8 μm, the coefficient of variation CV3 of the occupied area ratio of the magnetic body is 40.0 to 80.0%, and Assuming that the storage elastic modulus at 40° C. is defined as E′(40) Pa and the storage elastic modulus at 85° C. is defined as E′(85) Pa, the storage elastic modulus being the storage elastic modulus obtained in the powder dynamic viscoelasticity measurement of the magnetic toner, the following equations (1) and (2) are satisfied, E'(85)≤2.0×10 9 (1) [E'(40)-E'(85)]×100 / E'(40)≥70 (2), wherein the amount of the crystalline polyester is 30.0% by mass or more based on the total amount of the binder resin and the crystalline polyester.
2. The magnetic toner according to claim 1, wherein The magnetic toner particles further contain wax, and Assuming that the peak temperature of the maximum endothermic peak derived from the crystalline polyester at the first temperature rise in differential scanning calorimetry of the magnetic toner is defined as Tm(1)°C, the endothermic quantity of the maximum endothermic peak is defined as H(1) J / g, and the peak temperature of the maximum endothermic peak derived from the wax is defined as Tm(2)°C, the following formulas (3) to (5) are satisfied, 5.0≤Tm(2)-Tm(1)≤35.0 (3) 55.0≤Tm(2)≤100.0 (4) H(1)≥10.0 (5)。 3 . The magnetic toner according to claim 1 , wherein the magnetic toner has a dielectric loss tangent of 0.01 or more at 100 kHz.
4. The magnetic toner according to claim 1 or 2, wherein the oil absorption of the magnetic body is from 15.0 to 25.0 ml / 100 g.
5. The magnetic toner according to claim 1 or 2, wherein the isoelectric point of the magnetic body is pH 8.5 to 10.
5. 6 . The magnetic toner according to claim 1 , wherein the magnetic toner particles have a shell layer, and the shell layer comprises a non-crystalline polyester having an ethylenically unsaturated bond.
7. The magnetic toner according to claim 1 or 2, wherein the amount of the magnetic body in the magnetic toner is 10.0 to 50.0 mass%.
8. The magnetic toner according to claim 1 or 2, wherein the average circularity of the magnetic toner is from 0.970 to 0.
985.
9. The magnetic toner according to claim 1 or 2, wherein the binder resin comprises a non-crystalline polyester.
10. The magnetic toner according to claim 9, wherein the non-crystalline polyester comprises a structure in which succinic acid substituted with an alkenyl group having 6 to 18 carbon atoms is polycondensed with a polyol.
11. The magnetic toner according to claim 1 or 2, wherein The magnetic toner particles further comprise a multivalent metal, The polyvalent metal is at least one metal selected from the group consisting of Mg, Ca, Sr, Al, Fe, and Zn, and The total amount of the multivalent metal in the magnetic toner particles is from 25 to 1000 ppm by mass.
Citation Information
Patent Citations
Magnetic toner
JP2005338538A
toner
JP2013137420A
Black toner
JP2019003129A
Magnetic toner and image formation method
JP2019015957A
Magnetic toner
CN110989303A