Non-aqueous electrolyte for lithium secondary battery and lithium secondary battery containing the same
By using a non-aqueous electrolyte containing lithium salts, organic solvents, Lewis alkali compounds and lithium difluorophosphate in lithium-ion batteries, a stable SEI is formed, and the problem of increased resistance and decreased capacity of lithium-ion batteries at high temperatures is solved. Significantly improves the battery's high temperature durability and life.
Patent Information
- Application Number
- CN202080030603.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-11
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-08-11
AI Technical Summary
Lithium-ion batteries have increased resistance and decreased capacity at high temperatures due to side reactions caused by lithium salt decomposition, which affects their durability.
Using a non-aqueous electrolyte containing lithium salts, organic solvents, Lewis alkali compounds and lithium difluorophosphate, these additives form a stable solid electrolyte interface (SEI), which eliminates the lithium salt decomposition product, inhibits the initial resistance of the battery and increases the High temperature durability.
It significantly improves the resistance increase rate and capacity retention rate of lithium secondary batteries at high temperatures, extends the battery life, and improves the high-temperature storage characteristics.
Smart Images

Figure CN113767501B_ABST
Abstract
Description
Technical Field
[0001] This application claims the benefit of Korean Patent Application No. 10-2019-0102520, filed on August 21, 2019, the disclosure of which is incorporated herein by reference.
[0002] The present invention relates to a non-aqueous electrolyte for a lithium secondary battery, comprising an additive having an excellent effect of removing decomposition products generated from a lithium salt, and also to a lithium secondary battery having improved high-temperature durability by comprising the electrolyte. Background Art
[0003] With the development of the information society, the growth of personal IT devices and computer networks, and the resulting increase in society's overall dependence on electrical energy, there is a need to develop technologies for efficiently storing and utilizing electrical energy.
[0004] Among the technologies developed for this purpose, those based on secondary batteries are the most suitable for various applications. Since secondary batteries can be miniaturized for personal IT equipment and can be applied to electric vehicles and power storage equipment, people have aroused interest in secondary batteries. Among these secondary battery technologies, lithium-ion batteries have attracted much attention as a battery system with the highest theoretical energy density and are currently used in various devices.
[0005] Lithium-ion batteries are composed of a positive electrode formed of a lithium-containing transition metal oxide, a negative electrode formed of a carbon material (such as graphite) capable of storing lithium, an electrolyte that serves as a medium for transmitting lithium ions, and a separator. It is important to appropriately select these components to improve the electrochemical properties of the battery.
[0006] A disadvantage of lithium-ion batteries is that resistance increases and capacity decreases during charging and discharging or storage at high temperatures, resulting in performance degradation. One of the causes of this problem that has been revealed is a side reaction caused by degradation of the electrolyte at high temperatures, particularly degradation due to decomposition of lithium salts.
[0007] LiPF6 has been mainly used as a lithium salt to obtain suitable secondary battery characteristics, among which, due to the PF6 - Anions are very fragile to heat and are therefore known to generate Lewis acids such as PF5 by thermal decomposition when the battery is exposed to high temperatures.
[0008] The PF5 thus formed not only causes a decomposition reaction of organic solvents such as ethylene carbonate, but also destroys the solid electrolyte interphase (SEI) formed on the surface of active materials (e.g., graphite) at an operating voltage outside the electrochemical stability window of the electrolyte, thereby causing additional decomposition of the electrolyte and leading to an increase in resistance and a decrease in battery life.
[0009] Therefore, various methods have been proposed to maintain the passivation ability of the SEI when exposed to heat and suppress the degradation behavior of the battery by scavenging PF5 formed by the thermal decomposition of LiPF6-based salts. Summary of the invention
[0010] [Technical issues]
[0011] One aspect of the present invention provides a non-aqueous electrolyte for a lithium secondary battery, the non-aqueous electrolyte comprising an additive having an excellent effect of removing decomposition products generated from a lithium salt in the electrolyte.
[0012] Another aspect of the present invention provides a lithium secondary battery, wherein the effect of improving high-temperature durability is enhanced by including the non-aqueous electrolyte for a lithium secondary battery.
[0013] [Technical solution]
[0014] According to one aspect of the present invention, there is provided a non-aqueous electrolyte for a lithium secondary battery, comprising:
[0015] Lithium salts;
[0016] Organic solvents;
[0017] a compound represented by Formula 1 as a first additive; and
[0018] Lithium difluorophosphate (LiDFP) as the second additive.
[0019] [Formula 1]
[0020]
[0021] Among them, in formula 1,
[0022] R is a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms.
[0023] According to another aspect of the present invention, a lithium secondary battery is provided, which includes the non-aqueous electrolyte for lithium secondary batteries of the present invention.
[0024] [Beneficial Effects]
[0025] Since the non-aqueous electrolyte of the present invention includes a Lewis base material as a first additive capable of forming a solid electrolyte interface (SEI), it can ensure the passivation ability of SEI during high temperature storage by removing the decomposition products formed by the pyrolysis of lithium salts and enhancing SEI. In addition, since the non-aqueous electrolyte of the present invention combines the second additive with the first additive having an excellent film-forming effect, it can suppress the initial resistance of the battery by forming the desired film on the surface of the positive and negative electrodes. Therefore, if the non-aqueous electrolyte of the present invention is used, a lithium secondary battery with improved high temperature durability can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a graph showing the resistance increase rate of the secondary battery of Example 1 and the secondary battery of Comparative Example 1 after storage at a high temperature (60° C.);
[0027] Figure 2 This is a graph showing the resistance increase rate of the secondary battery of Example 1 and the secondary battery of Comparative Example 1 after 200 cycles at a high temperature (45° C.). DETAILED DESCRIPTION
[0028] Hereinafter, the present invention will be described in more detail.
[0029] It will be understood that the words or terms used in the specification and claims should not be interpreted as the meanings defined in commonly used dictionaries, and it will also be understood that, based on the principle that the inventor can appropriately define the meanings of words or terms to best explain the present invention, the words or terms should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology and the technical idea of the present invention.
[0030] For lithium secondary batteries, high temperature storage characteristics are improved by forming a film with passivation ability on the surface of the positive and negative electrodes while the non-aqueous electrolyte decomposes during the first charge and discharge. However, this film may be degraded by acids (such as HF and PF5) formed by the pyrolysis of lithium salts (LiPF6, etc.) widely used in lithium ion batteries. The dissolution of transition metal elements occurs at the positive electrode due to acid erosion, while the surface resistance of the electrode increases due to changes in the surface structure, and the theoretical capacity is reduced due to the loss of metal elements as redox centers, so the capacity may be reduced. Moreover, since the so-dissolved transition metal ions are electrodeposited on the negative electrode that reacts within the strong reduction potential range, this not only consumes electrons, but also destroys the film during electrodeposition to expose the negative electrode surface, thereby causing additional electrolyte decomposition reactions. As a result, the negative electrode resistance increases, and the battery capacity may decrease continuously, while the irreversible capacity increases.
[0031] Therefore, the present invention attempts to provide a non-aqueous electrolyte and a lithium secondary battery comprising the non-aqueous electrolyte, wherein the non-aqueous electrolyte can enhance the solid electrolyte interphase (SEI) on the surface of the negative electrode by comprising an additive capable of forming SEI as a Lewis base compound as a component of the non-aqueous electrolyte, while preventing the dissolution of transition metals from the positive electrode or the degradation of SEI during high temperature storage by removing the acid caused by the decomposition of the lithium salt.
[0032] Non-aqueous electrolyte for lithium secondary batteries
[0033] First, the nonaqueous electrolyte solution for a lithium secondary battery of the present invention will be described.
[0034] The non-aqueous electrolyte for lithium secondary batteries of the present invention includes: (1) a lithium salt, (2) an organic solvent, (3) a compound represented by the following formula 1 as a first additive, and (4) lithium difluorophosphate (LiDFP) as a second additive:
[0035] [Formula 1]
[0036]
[0037] Among them, in formula 1,
[0038] R is a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms.
[0039] (1) Lithium salt
[0040] First, in the non-aqueous electrolyte for lithium secondary batteries according to the embodiment of the present invention, any lithium salt commonly used in the electrolyte for lithium secondary batteries can be used as the lithium salt without limitation. For example, the lithium salt may include Li + as cations, and may include a group consisting of F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - 、AlO4 - 、AlCl4 - PF6 - 、SbF6 - 、AsF6 - , B 10 Cl 10 - 、BF2C2O4 - , BC4O8 - PF4C2O4 - PF2C4O8 -、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - 、C4F9SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、CH3SO3 - CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - At least one of the group consisting of as anion. Specifically, the lithium salt may include a selected from the group consisting of LiCl, LiBr, LiI, LiBF4, LiClO4, LiAlO4, LiAlCl4, LiPF6, LiSbF6, LiAsF6, LiB 10 Cl 10 , LiBOB (LiB (C2O4) 2), LiCF3SO3, LiTFSI (LiN (SO2CF3) 2), LiFSI (LiN (SO2F) 2), LiCH3SO3, LiCF3CO2, LiCH3CO2 and LiBETI (LiN (SO2CF2CF3) 2). More specifically, the lithium salt may include a single material selected from the group consisting of LiBF4, LiClO4, LiPF6, LiBOB (LiB (C2O4) 2), LiCF3SO3, LiTFSI (LiN (SO2CF3) 2), LiFSI (LiN (SO2F) 2) and LiBETI (LiN (SO2CF2CF3) 2), or a mixture of two or more thereof.
[0041] The lithium salt may be appropriately varied within a generally available range, but may be contained in the electrolyte at a concentration of 0.8 M to 3.0 M, for example, 1.0 M to 3.0 M, to obtain an optimal effect of forming a film for preventing corrosion of the electrode surface.
[0042] If the concentration of the lithium salt is less than 0.8M, the capacity characteristics may be reduced due to the reduced mobility of lithium ions. If the concentration of the lithium salt is greater than 3.0M, the electrolyte wettability may be reduced due to the excessive increase in the viscosity of the non-aqueous electrolyte, and the film-forming effect may be reduced.
[0043] (2) Organic solvents
[0044] As the organic solvent, various organic solvents generally used in lithium electrolytes may be used without limitation. For example, the organic solvent may include a cyclic carbonate-based organic solvent, a linear carbonate-based organic solvent, or a mixed organic solvent thereof.
[0045] Cyclic carbonate organic solvents are high-viscosity organic solvents that can well dissociate lithium salts in electrolytes due to their high dielectric constants. Specific examples of cyclic carbonate organic solvents may be at least one organic solvent selected from ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate and vinylene carbonate, wherein the cyclic carbonate organic solvent may include ethylene carbonate.
[0046] In addition, linear carbonate organic solvents are organic solvents with low viscosity and low dielectric constant, wherein a typical example of the linear carbonate organic solvent can be at least one organic solvent selected from dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methylpropyl carbonate and ethylpropyl carbonate, and the linear carbonate organic solvent can specifically include ethyl methyl carbonate (EMC).
[0047] In order to prepare an electrolyte having high ion conductivity, the organic solvent may include a cyclic carbonate-based organic solvent and a linear carbonate-based organic solvent in a volume ratio of 1:9 to 5:5, for example, 2:8 to 4:6.
[0048] Furthermore, if necessary, the organic solvent may further contain a linear ester organic solvent and / or a cyclic ester organic solvent generally used in a lithium secondary battery electrolyte in addition to the cyclic carbonate organic solvent and / or the linear carbonate organic solvent.
[0049] As a specific example, the linear ester organic solvent may include at least one organic solvent selected from methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate.
[0050] As a specific example, the cyclic ester organic solvent may include at least one organic solvent selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, and ε-caprolactone.
[0051] In addition to the carbonate-based organic solvent or the ester-based organic solvent, an ether-based organic solvent or a nitrile-based organic solvent may be further mixed to use the organic solvent, if necessary.
[0052] As the ether solvent, any one selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether and ethyl propyl ether, or a mixture of two or more thereof can be used.
[0053] The nitrile solvent may include at least one selected from acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanecarbonitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile and 4-fluorophenylacetonitrile.
[0054] (3) First additive
[0055] The non-aqueous electrolyte of the present invention includes a compound represented by the following Formula 1 as a first additive.
[0056] [Formula 1]
[0057]
[0058] In formula 1,
[0059] R is a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms.
[0060] In Formula 1, R may be a substituted or unsubstituted alkyl group having 1 to 3 carbon atoms. In particular, the compound represented by Formula 1 may be a compound represented by the following Formula 1a.
[0061] [Formula 1a]
[0062]
[0063] The compound represented by Formula 1 may be included in an amount of 0.1 to 5 wt %, specifically 0.1 to 4 wt %, and more specifically 1 to 3 wt %, based on the total weight of the non-aqueous electrolyte.
[0064] When the amount of the compound represented by Formula 1 satisfies the above range, a secondary battery with further improved overall performance can be prepared due to the excellent effect of removing lithium salt decomposition products while suppressing disadvantages such as side reactions caused by additives, capacity decrease and resistance increase as much as possible.
[0065] If the amount of the first additive is less than 0.1 wt%, HF or PF5 can be removed, but the removal effect may become less obvious over time. Similarly, if the amount of the first additive is greater than 5.0 wt%, the viscosity of the non-aqueous electrolyte may not only increase due to the excess of the additive, but also reduce the ion conductivity due to the increase in viscosity, thereby adversely affecting the ion mobility in the battery, so during high temperature storage, the rate performance or low temperature life characteristics may deteriorate. In addition, the resistance of the battery may increase due to the decomposition of the excess additive.
[0066] As described above, by including a Lewis base compound containing a C=S functional group (e.g., a compound represented by Formula 1), the non-aqueous electrolyte of the present invention can easily remove byproducts that cause battery degradation at high temperatures, such as Lewis acids (e.g., HF) formed by decomposition of lithium salts. - or PF5 - ). Therefore, since the degradation behavior caused by the chemical reaction of the film on the surface of the positive electrode or the negative electrode caused by Lewis acid can be suppressed, the additional decomposition of the battery electrolyte due to the destruction of the film can be prevented, and the high temperature storage characteristics can be improved by reducing the self-discharge of the secondary battery.
[0067] In particular, since the compound represented by Formula 1 included as a non-aqueous electrolyte additive has a double bond and a C=S bond functional group, it can form a stronger SEI. In other words, since the compound represented by Formula 1 of the present invention has a C=S bond as an electron-rich functional group instead of a C=O bond, a sulfur (S)-containing interface can be formed when the compound is reduced to form SEI. Therefore, compared with the case of including a compound represented by Formula 3 below, the initial resistance can be further reduced. In addition, since the molecular weight of the compound represented by Formula 1 is lower than that of the ionic bond (e.g., SO3) having an ester bond represented by Formula 4 below - ) compound, and therefore has high solubility in organic solvents used in lithium ion batteries, so it has the advantage of being more likely to function as an additive.
[0068] [Formula 3]
[0069]
[0070] [Formula 4]
[0071]
[0072] (4) Second additive
[0073] The non-aqueous electrolyte of the present invention contains lithium difluorophosphate (LiDFP) represented by the following Formula 2 as a second additive.
[0074] [Formula 2]
[0075]
[0076] Lithium difluorophosphate (LiDFP) is a component for obtaining the effect of improving the long-term life characteristics of secondary batteries, wherein the lithium ion components decomposed during the first charge process are electrochemically decomposed on the surface of the negative electrode to form a stable SEI. The formation of SEI can not only improve the mobility of lithium (Li) toward the negative electrode, but also reduce the interface resistance. In addition, the difluorophosphate anions decomposed during the first charge can improve the stabilization and discharge characteristics of the positive electrode when present on the positive electrode surface. Therefore, the effect of improving the long-term life characteristics of the secondary battery can be achieved.
[0077] The content of lithium difluorophosphate (LiDFP) as the second additive may be 0.1 wt % to 5 wt %, specifically 0.5 wt % to 3 wt %, and more specifically 1 wt % to 3 wt %, based on the total weight of the non-aqueous electrolyte.
[0078] When the amount of lithium difluorophosphate (LiDFP) satisfies the above range, a strong SEI formation effect and a film formation effect can be obtained.
[0079] If the amount of lithium difluorophosphate (LiDFP) is greater than 5.0 wt %, the viscosity of the electrolyte may not only increase due to the excess compound, but also an excessively thick film may be formed on the electrode surface, resulting in increased resistance and decreased capacity characteristics. If the amount of lithium difluorophosphate (LiDFP) is less than 0.1 wt %, the film-forming effect on the electrode surface may not be significant.
[0080] The weight ratio of the first additive to the second additive in the non-aqueous electrolyte of the present invention may be 1:1 to 1:10, specifically 1:1 to 1:5, and more specifically 1:1 to 1:3.
[0081] When the first additive and the second additive are mixed in the above ratio, the wetting of the electrolyte can be improved by reducing the surface tension. In addition, since a stable SEI is formed without increasing the resistance, the side reaction between the electrode and the electrolyte during charging at high temperature can be suppressed.
[0082] If the weight ratio of the second additive to the first additive is greater than 10, the output may be reduced because the initial interface resistance increases when an excessively thick film is formed on the electrode surface. In addition, if the weight ratio of the second additive to the first additive is less than 1, the effect of forming SEI is not significant, so the effect of suppressing the side reaction between the electrode and the electrolyte may be reduced.
[0083] (5) Additional additives
[0084] In addition, in order to prevent the non-aqueous electrolyte from decomposing and causing collapse of the negative electrode under a high output environment, or to further improve the low-temperature high-rate discharge characteristics, high-temperature stability, overcharge protection and battery expansion inhibition effect at high temperatures, if necessary, the non-aqueous electrolyte for the lithium secondary battery of the present invention may further include an additional third additive in the non-aqueous electrolyte.
[0085] As a typical example, these third additives may include at least one additive selected from the group consisting of cyclic carbonate compounds, halogenated carbonate compounds, sultone compounds, sulfate ester / salt compounds, phosphate ester / salt compounds, borate ester / salt compounds, nitrile compounds, benzene compounds, amine compounds, silane compounds and lithium salt compounds.
[0086] The cyclic carbonate-based compound may include vinylene carbonate (VC) or vinylethylene carbonate.
[0087] The halogenated carbonate-based compound may include fluoroethylene carbonate (FEC).
[0088] The sultone compound may include at least one compound selected from 1,3-propane sultone (PS), 1,4-butane sultone, ethane sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone.
[0089] The sulfate compound may include ethylene sulfate (Esa), trimethylene sulfate (TMS) or methyltrimethylene sulfate (MTMS).
[0090] In addition to the lithium difluorophosphate included as the second additive, the phosphate ester / salt compound may include at least one compound selected from the group consisting of lithium difluorobis(oxalyl)phosphate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tris(2,2,2-trifluoroethyl)phosphate and tris(trifluoroethyl)phosphite compounds.
[0091] The borate ester compounds may include tetraphenyl borate and lithium oxalyldifluoroborate.
[0092] The nitrile compound may include at least one compound selected from succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanecarbonitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile and 4-fluorophenylacetonitrile.
[0093] The benzene compound may include fluorobenzene, the amine compound may include triethanolamine or ethylenediamine, and the silane compound may include tetravinylsilane.
[0094] The lithium salt compound is a compound different from the lithium salt contained in the non-aqueous electrolyte, wherein the lithium salt compound may include at least one compound selected from the group consisting of LiPO2F2, LiODFB, LiBOB (lithium bis(oxalyl)borate (LiB(C2O4)2) and LiBF4.
[0095] In the case of including vinylene carbonate, vinyl ethylene carbonate, or succinonitrile among these additional additives, a more robust SEI may be formed on the negative electrode surface during the initial activation process of the secondary battery.
[0096] In the case where LiBF 4 is included, the high temperature stability of the secondary battery can be improved by suppressing gas generation that may be generated due to decomposition of the electrolyte at high temperature.
[0097] The third additive can be used as a mixture of two or more, and its content can be 0.01% to 50% by weight, especially 0.01% to 10% by weight, preferably 0.05% to 5% by weight, based on the total weight of the non-aqueous electrolyte. If the amount of the additive is less than 0.01% by weight, the effect of improving low-temperature output, high-temperature storage characteristics and high-temperature life characteristics is not obvious. If the amount of the additional additive is greater than 50% by weight, the side reaction in the electrolyte may occur excessively during the charging and discharging process of the battery. In particular, since the third additive may not be fully decomposed at high temperatures when an excess of the third additive is added, the third additive may be present in the electrolyte in the form of unreacted material or precipitate at room temperature. Therefore, side reactions that deteriorate the life or resistance characteristics of the secondary battery may occur.
[0098] Lithium secondary battery
[0099] In addition, in another embodiment of the present invention, a lithium secondary battery is provided, which includes the non-aqueous electrolyte for lithium secondary batteries of the present invention.
[0100] The lithium secondary battery of the present invention can be prepared by forming an electrode assembly in which a positive electrode, a negative electrode and a separator disposed between the positive electrode and the negative electrode are stacked in sequence, housing the electrode assembly in a battery box, and then injecting the non-aqueous electrolyte of the present invention.
[0101] Conventional methods known in the art can be used as the method for preparing the lithium secondary battery of the present invention. Specifically, the method for preparing the lithium secondary battery of the present invention is as follows.
[0102] (1) Positive electrode
[0103] The positive electrode may be prepared by coating a positive electrode collector with a positive electrode slurry including a positive electrode active material, a binder, a conductive agent, and a solvent, and then drying and roll-pressing the coated positive electrode collector.
[0104] There is no particular limitation on the positive electrode current collector as long as it has conductivity and does not cause adverse chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, fired carbon, or aluminum or stainless steel surface-treated with one of carbon, nickel, titanium or silver can be used.
[0105] The positive electrode active material is a compound that can reversibly insert and remove lithium, wherein the positive electrode active material may include a lithium transition metal oxide containing lithium and at least one metal selected from cobalt, manganese, nickel or aluminum, and may specifically include lithium manganese oxides, lithium iron phosphate and lithium nickel manganese cobalt oxides (for example, Li(Ni p Co q Mn r1 )O2(where 0 <p<1,0<q<1,0<r1<1,p+q+r1=1)。
[0106] Specifically, the lithium manganese-based oxide may include LiMn2O4, and the lithium iron phosphate may, for example, include LiFePO4.
[0107] In addition, the lithium nickel manganese cobalt oxide may include a 1 / 3 Mn 1 / 3 Co 1 / 3 )O2、Li(Ni 0.6 Mn 0.2 Co 0.2 )O2、Li(Ni 0.5 Mn 0.3 Co 0.2 )O2、Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 and Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, wherein the lithium nickel manganese cobalt oxide preferably includes a lithium transition metal oxide in which the amount of nickel in the transition metal is 60 atomic % or more. That is, since the higher the amount of nickel in the transition metal, the higher the capacity that can be achieved, it is more advantageous to use a lithium transition metal oxide in which the nickel content is 60 atomic % or more to achieve high capacity. That is, the lithium transition metal oxide may include a lithium transition metal oxide selected from Li(Ni 0.6 Mn 0.2 Co 0.2 )O2、Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 and Li(Ni 0.8 Mn 0.1 Co 0.1 ) at least one of O2.
[0108] In addition to the above lithium transition metal oxides, the positive electrode active material of the present invention may further include: lithium manganese oxides, such as LiMnO2, LiMn2O4, etc.; lithium cobalt oxides, such as LiCoO2, etc.; lithium nickel oxides, such as LiNiO2, etc.; lithium nickel manganese oxides, such as LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-Z Ni z O4 (where 0 < Z < 2); lithium nickel cobalt oxides, such as LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1); lithium manganese cobalt oxides, such as LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn 2-Z1 Co z1 O4 (where 0 < Z1 < 2); lithium nickel manganese cobalt oxides, such as Li(Ni p Co q Mn r1 )O2 (where 0 < p < 1, 0 < q < 1, 0 < r1 < 1, p + q + r1 = 1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2, p1 + q1 + r2 = 2); or lithium nickel cobalt transition metal (M) oxides, such as Li(Ni p2 Co q2 Mn r3 M S2 )O2 (where M is selected from the group consisting of aluminum (Al), iron (Fe), vanadium (V), chromium (Cr), titanium (Ti), tantalum (Ta), magnesium (Mg), and molybdenum (Mo), and p2, q2, r3, and s2 are atomic fractions of various independent elements, where 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < S2 < 1, and p2 + q2 + r3 + S2 = 1), and may further include any one or more of the above compounds.
[0109] Based on the total weight of the solids in the positive electrode slurry, the content of the positive electrode active material may be 80% by weight to 99% by weight, such as 90% by weight to 99% by weight. When the content of the positive electrode active material is less than 80% by weight, the capacity may decrease due to the reduction of the energy density.
[0110] The binder is a component that helps the active material to adhere to the conductive agent and to the current collector, wherein the binder is usually added in an amount of 1 wt % to 30 wt % based on the total weight of the solids in the positive electrode slurry. Examples of the binder may be polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer, styrene-butadiene rubber, fluororubber and various copolymers thereof.
[0111] Also, the conductive agent is a material that provides conductivity without causing adverse chemical changes in the battery, wherein the added amount thereof may be 1 wt % to 20 wt % based on the total weight of the solids in the positive electrode slurry.
[0112] As typical examples of conductive agents, the following conductive materials can be used: carbon powder, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black or thermal black; graphite powder, such as natural graphite, artificial graphite or graphite with a fully developed crystal structure; conductive fibers, such as carbon fibers or metal fibers; conductive powders, such as fluorocarbon powder, aluminum powder and nickel powder; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or polyphenylene derivatives.
[0113] In addition, the solvent may include an organic solvent, such as N-methyl-2-pyrrolidone (NMP), and its amount may be such that a desired viscosity is obtained when the positive electrode active material and optional binder and conductive agent are included. For example, the content of the solvent may be such that the concentration of solids in the slurry including the positive electrode active material and optional binder and conductive agent is in the range of 10 wt % to 60 wt %, for example 20 wt % to 50 wt %.
[0114] (2) Negative electrode
[0115] The negative electrode may be prepared by coating a negative electrode collector with a negative electrode slurry including a negative electrode active material, a binder, a conductive agent, and a solvent, and then drying and roll-pressing the coated negative electrode collector.
[0116] The thickness of the negative electrode collector is generally 3 μm to 500 μm. The negative electrode collector is not particularly limited as long as it has high conductivity and does not cause adverse chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, fired carbon, or copper or stainless steel surface-treated with one of carbon, nickel, titanium or silver, and aluminum-cadmium alloys can be used. In addition, similar to the positive electrode collector, the negative electrode collector can have a fine surface roughness to improve the bonding strength with the negative electrode active material, and the negative electrode collector can be used in various shapes, such as films, sheets, foils, nets, porous bodies, foams, and non-woven fabrics.
[0117] In addition, the negative electrode active material may include at least one selected from the group consisting of: lithium metal, a carbon material capable of reversibly intercalating / deintercalating lithium ions, a metal or an alloy of lithium and the metal, a metal composite oxide, a material capable of doping and dedoping lithium, and a transition metal oxide.
[0118] As the carbon material capable of reversibly intercalating / deintercalating lithium ions, carbon-based negative electrode active materials commonly used in lithium ion secondary batteries can be used without particular limitation. As typical examples, crystalline carbon and / or amorphous carbon can be used. Examples of crystalline carbon can be graphite, such as natural graphite or artificial graphite that is irregular, planar, flaky, spherical, or fibrous. Examples of amorphous carbon can be soft carbon (low-temperature sintered carbon) or hard carbon, mesophase pitch carbide, and calcined coke.
[0119] As the metal or the alloy of lithium and the metal, a metal selected from the group consisting of copper (Cu), nickel (Ni), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), silicon (Si), antimony (Sb), lead (Pb), indium (In), zinc (Zn), barium (Ba), radium (Ra), germanium (Ge), aluminum (Al), and tin (Sn), or an alloy of lithium and the metal can be used.
[0120] As the metal composite oxide, one selected from the group consisting of PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3 (0 ≤ x ≤ 1), Li x WO2 (0 ≤ x ≤ 1), and Sn x Me 1-x Me' y O z (Me: manganese (Mn), Fe, Pb, or Ge; Me': Al, boron (B), phosphorus (P), Si, elements of Groups I, II, and III of the periodic table, or a halogen, 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8) can be used.
[0121] The metal capable of doping and dedoping lithium may include: Si, SiO x(0 < x ≤ 2), Si-Y alloy (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO2, and Sn-Y (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), and a mixture of SiO2 with at least one of them can also be used. Element Y can be selected from Mg, Ca, Sr, Ba, Ra, scandium (Sc), yttrium (Y), Ti, zirconium (Zr), hafnium (Hf), (Rf), V, niobium (Nb), Ta, (Db), Cr, Mo, tungsten (W), (Sg), technetium (Tc), rhenium (Re), (Bh), Fe, Pb, ruthenium (Ru), osmium (Os), (Hs), rhodium (Rh), iridium (Ir), palladium (Pd), platinum (Pt), Cu, silver (Ag), gold (Au), Zn, cadmium (Cd), B, Al, gallium (Ga), Sn, In, Ge, P, arsenic (As), Sb, bismuth (Bi), sulfur (S), selenium (Se), tellurium (Te), polonium (Po), and combinations thereof.
[0122] The transition metal oxides can include lithium-containing titanium composite oxide (LTO), vanadium oxide, and lithium vanadium oxide.
[0123] Based on the total weight of the solids in the negative electrode paste, the content of the negative electrode active material can be 80% to 99% by weight.
[0124] The binder is a component that helps the adhesion between the conductive agent, the active material, and the current collector. Among them, based on the total weight of the solids in the negative electrode paste, the addition amount of the binder is usually 1% to 30% by weight. Examples of the binder can be polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, styrene-butadiene rubber, and fluororubber.
[0125] The conductive agent is a component for further improving the conductivity of the negative electrode active material, wherein the conductive agent can be added in an amount of 1 wt % to 20 wt % based on the total weight of the solids in the negative electrode slurry. Any conductive agent can be used without particular limitation, as long as it has conductivity and does not cause adverse chemical changes in the battery, for example, the following conductive materials can be used: carbon powder, such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black or thermal black; graphite powder, such as natural graphite, artificial graphite or graphite with a fully developed crystal structure; conductive fibers, such as carbon fibers or metal fibers; metal powders, such as fluorocarbon powders, aluminum powders and nickel powders; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or polyphenylene derivatives.
[0126] The solvent may include water or an organic solvent, such as NMP and alcohol, and its amount may be such that a desired viscosity is obtained when the negative electrode active material and optional binder and conductive agent are included. For example, the content of the solvent may be such that the concentration of solids in the slurry including the negative electrode active material and optional binder and conductive agent is in the range of 50 wt % to 75 wt %, such as 50 wt % to 65 wt %.
[0127] (3) Diaphragm
[0128] As the separator included in the lithium secondary battery of the present invention, a commonly used typical porous polymer film, for example, a porous polymer film prepared from a polyolefin polymer (for example, an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer) can be used alone or in a stacked manner, and a typical porous non-woven fabric can be used, for example, a non-woven fabric formed from high-melting point glass fiber or polyethylene terephthalate fiber, but the present invention is not limited thereto.
[0129] The shape of the lithium secondary battery of the present invention is not particularly limited, but a cylindrical type using a can, a prismatic type, a pouch type, or a coin type may be used.
[0130] Hereinafter, the present invention will be described in more detail according to the embodiments. However, the present invention can be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein. On the contrary, these exemplary embodiments are provided to make this description fully complete and to fully convey the scope of the present invention to those skilled in the art.
[0131] Example
[0132] Example 1
[0133] (Preparation of non-aqueous electrolyte for lithium secondary battery)
[0134] 0.5 g of the compound represented by Formula 1a as a first additive, 1.0 g of lithium difluorophosphate as a second additive, and 0.1 g of tetravinylsilane, 1.0 g of ethylene sulfonate, 0.5 g of 1,3-propane sultone, 0.2 g of LiBF4 and 6.0 g of fluorobenzene as a third additive were added to 90.7 g of an organic solvent (ethylene carbonate: ethyl methyl carbonate = 3:7 volume ratio) in which 0.7 M LiPF6 and 0.3 M LiFSI were dissolved, thereby preparing a non-aqueous electrolyte for a lithium secondary battery.
[0135] (Secondary Battery Preparation)
[0136] The positive electrode active material (Li(Ni 0.8 Co 0.1 Mn 0.1 )O2:Li(Ni 0.6 Co 0.2 Mn 0.2 )O2=7:3 weight ratio), carbon black as a conductive agent and polyvinylidene fluoride as a binder were added to N-methyl-2-pyrrolidone (NMP) as a solvent in a weight ratio of 97.5:1:1.5 to prepare a positive electrode slurry (solid content: 50 weight %). A 15 μm thick positive electrode current collector (Al film) was coated with the positive electrode slurry, dried and then rolled to prepare a positive electrode.
[0137] The negative electrode active material (graphite: SiO = 95:5 weight ratio), binder (SBR-CMC) and conductive agent (carbon black) were added to water as a solvent at a weight ratio of 95:3.5:1.5 to prepare a negative electrode slurry (solid content: 60 weight %). A 6 μm thick copper (Cu) film as a negative electrode current collector was coated with the negative electrode slurry, dried and then rolled to prepare a negative electrode.
[0138] The positive electrode, the polyolefin porous separator coated with inorganic particles (Al2O3) and the negative electrode are stacked in sequence to prepare an electrode assembly.
[0139] The prepared electrode assembly was housed in a battery case, and a non-aqueous electrolyte for a lithium secondary battery was injected therein to prepare a lithium secondary battery.
[0140] Example 2
[0141] (Preparation of non-aqueous electrolyte for lithium secondary battery)
[0142] 0.2 g of the compound represented by Formula 1a as a first additive, 1.0 g of lithium difluorophosphate as a second additive, and 1.0 g of ethylene sulfonate, 0.5 g of 1,3-propane sultone, 0.2 g of LiBF4, and 6.0 g of fluorobenzene as a third additive were added to 91.1 g of an organic solvent (ethylene carbonate: ethyl methyl carbonate = 3:7 volume ratio) in which 0.7 M LiPF6 and 0.3 M LiFSI were dissolved, thereby preparing a non-aqueous electrolyte for a lithium secondary battery.
[0143] (Secondary Battery Preparation)
[0144] The positive electrode active material (Li(Ni 0.8 Co 0.1 Mn 0.1 )O2), carbon black as a conductive agent and polyvinylidene fluoride as a binder were added to N-methyl-2-pyrrolidone (NMP) as a solvent in a weight ratio of 97.5:1:1.5 to prepare a positive electrode slurry (solid content: 50 wt%). A 15 μm thick positive electrode current collector (Al film) was coated with the positive electrode slurry, dried and then rolled to prepare a positive electrode.
[0145] The negative electrode active material (graphite: SiO = 95:5 weight ratio), binder (SBR-CMC) and conductive agent (carbon black) were added to water as a solvent at a weight ratio of 95:3.5:1.5 to prepare a negative electrode slurry (solid content: 60 weight %). A 6 μm thick copper (Cu) film as a negative electrode current collector was coated with the negative electrode slurry, dried and then rolled to prepare a negative electrode.
[0146] The positive electrode, the polyolefin porous separator coated with inorganic particles (Al2O3) and the negative electrode are stacked in sequence to prepare an electrode assembly.
[0147] The prepared electrode assembly was housed in a battery case, and a non-aqueous electrolyte for a lithium secondary battery was injected therein to prepare a lithium secondary battery.
[0148] Example 3
[0149] (Preparation of non-aqueous electrolyte for lithium secondary battery)
[0150] 0.3 g of the compound represented by formula 1a as a first additive, 1.0 g of lithium difluorophosphate as a second additive, and 1.0 g of ethylene sulfonate, 0.5 g of 1,3-propane sultone, 0.2 g of LiBF4 and 6.0 g of fluorobenzene as a third additive were added to 91.0 g of an organic solvent (ethylene carbonate: ethyl methyl carbonate = 3:7 volume ratio) dissolved with 1.2 M LiPF6 to prepare a non-aqueous electrolyte for a lithium secondary battery.
[0151] (Secondary Battery Preparation)
[0152] The positive electrode active material (Li(Ni 0.8 Co 0.1 Mn 0.1 )O2), carbon black as a conductive agent and polyvinylidene fluoride as a binder were added to N-methyl-2-pyrrolidone (NMP) as a solvent in a weight ratio of 97.5:1:1.5 to prepare a positive electrode slurry (solid content: 50 wt%). A 15 μm thick positive electrode current collector (Al film) was coated with the positive electrode slurry, dried and then rolled to prepare a positive electrode.
[0153] The negative electrode active material (graphite), binder (SBR-CMC) and conductive agent (carbon black) were added to water as a solvent at a weight ratio of 95:3.5:1.5 to prepare a negative electrode slurry (solid content: 60 wt%). A 6 μm thick copper (Cu) film as a negative electrode current collector was coated with the negative electrode slurry, dried and then rolled to prepare a negative electrode.
[0154] The positive electrode, the polyolefin porous separator coated with inorganic particles (Al2O3) and the negative electrode are stacked in sequence to prepare an electrode assembly.
[0155] The prepared electrode assembly was housed in a battery case, and a non-aqueous electrolyte for a lithium secondary battery was injected therein to prepare a lithium secondary battery.
[0156] Example 4
[0157] (Preparation of non-aqueous electrolyte for lithium secondary batteries)
[0158] 0.3 g of the compound represented by formula 1a as a first additive, 1.5 g of lithium difluorophosphate as a second additive, and 1.0 g of ethylene sulfonate and 0.5 g of 1,3-propane sultone as a third additive were added to 96.7 g of an organic solvent (ethylene carbonate: ethylmethyl carbonate = 3:7 volume ratio) dissolved with 1.2 M LiPF6 to prepare a non-aqueous electrolyte for a lithium secondary battery.
[0159] (Secondary Battery Preparation)
[0160] A lithium secondary battery was prepared in the same manner as in Example 3, except that the non-aqueous electrolyte for lithium secondary batteries prepared above was injected instead of the non-aqueous electrolyte for lithium secondary batteries of Example 3.
[0161] Comparative Example 1
[0162] (Preparation of non-aqueous electrolyte for lithium secondary batteries)
[0163] 1.0 g of lithium difluorophosphate as a second additive and 0.1 g of tetravinylsilane, 1.0 g of ethylene sulfonate, 0.5 g of 1,3-propane sultone, 0.2 g of LiBF4 and 6.0 g of fluorobenzene as a third additive were added to 91.2 g of an organic solvent (ethylene carbonate: ethylmethyl carbonate = 3:7 volume ratio) in which 0.7 M LiPF6 and 0.3 M LiFSI were dissolved to prepare a non-aqueous electrolyte for a lithium secondary battery.
[0164] (Secondary Battery Preparation)
[0165] The positive electrode active material (Li(Ni 0.8 Co 0.1 Mn 0.1 )O2:Li(Ni 0.6 Co 0.2 Mn 0.2 )O2=7:3 weight ratio), carbon black as a conductive agent and polyvinylidene fluoride as a binder were added to N-methyl-2-pyrrolidone (NMP) as a solvent in a weight ratio of 97.5:1:1.5 to prepare a positive electrode slurry (solid content: 50 weight %). A 15 μm thick positive electrode current collector (Al film) was coated with the positive electrode slurry, dried and then rolled to prepare a positive electrode.
[0166] The negative electrode active material (graphite: SiO = 95:5 weight ratio), binder (SBR-CMC) and conductive agent (carbon black) were added to water as a solvent at a weight ratio of 95:3.5:1.5 to prepare a negative electrode slurry (solid content: 60 weight %). A 6 μm thick copper (Cu) film as a negative electrode current collector was coated with the negative electrode slurry, dried and then rolled to prepare a negative electrode.
[0167] The positive electrode, the polyolefin porous separator coated with inorganic particles (Al2O3) and the negative electrode are stacked in sequence to prepare an electrode assembly.
[0168] The prepared electrode assembly was housed in a battery case, and a non-aqueous electrolyte for a lithium secondary battery was injected therein to prepare a lithium secondary battery.
[0169] Comparative Example 2
[0170] (Secondary Battery Preparation)
[0171] The positive electrode active material (Li(Ni 0.8 Co 0.1 Mn 0.1)O2), carbon black as a conductive agent and polyvinylidene fluoride as a binder were added to N-methyl-2-pyrrolidone (NMP) as a solvent in a weight ratio of 97.5:1:1.5 to prepare a positive electrode slurry (solid content: 50 wt%). A 15 μm thick positive electrode current collector (Al film) was coated with the positive electrode slurry, dried and then rolled to prepare a positive electrode.
[0172] The negative electrode active material (graphite: SiO = 95:5 weight ratio), binder (SBR-CMC) and conductive agent (carbon black) were added to water as a solvent at a weight ratio of 95:3.5:1.5 to prepare a negative electrode slurry (solid content: 60 weight %). A 6 μm thick copper (Cu) film as a negative electrode current collector was coated with the negative electrode slurry, dried and then rolled to prepare a negative electrode.
[0173] The positive electrode, the polyolefin porous separator coated with inorganic particles (Al2O3) and the negative electrode are stacked in sequence to prepare an electrode assembly.
[0174] The prepared electrode assembly was housed in a battery case, and the non-aqueous electrolyte for a lithium secondary battery prepared in Comparative Example 1 was injected therein to prepare a lithium secondary battery.
[0175] Comparative Example 3
[0176] (Preparation of non-aqueous electrolyte for lithium secondary battery)
[0177] 1.0 g of lithium difluorophosphate as a second additive and 0.1 g of tetravinylsilane (TVS), 1.0 g of ethylene sulfonate, 0.5 g of 1,3-propane sultone, 0.2 g of LiBF4 and 6.0 g of fluorobenzene as a third additive were added to 91.2 g of an organic solvent (ethylene carbonate: ethyl methyl carbonate = 3:7 volume ratio) dissolved with 1.2 M LiPF6 to prepare a non-aqueous electrolyte for a lithium secondary battery.
[0178] (Preparation of Secondary Battery)
[0179] The positive electrode active material (Li(Ni 0.8 Co 0.1 Mn 0.1 )O2), carbon black as a conductive agent and polyvinylidene fluoride as a binder were added to N-methyl-2-pyrrolidone (NMP) as a solvent at a weight ratio of 97.5:1:1.5 to prepare a positive electrode slurry (solid content: 50 wt%). A 15 μm thick positive electrode current collector (Al film) was coated with the positive electrode slurry, dried, and then rolled to prepare a positive electrode.
[0180] The negative electrode active material (graphite), binder (SBR-CMC) and conductive agent (carbon black) were added to water as a solvent at a weight ratio of 95:3.5:1.5 to prepare a negative electrode slurry (solid content: 60 wt %). A 6 μm thick copper (Cu) film as a negative electrode current collector was coated with the negative electrode slurry, dried, and then rolled to prepare a negative electrode.
[0181] The positive electrode, the polyolefin porous separator coated with inorganic particles (Al2O3) and the negative electrode are stacked in sequence to prepare an electrode assembly.
[0182] The prepared electrode assembly was housed in a battery case, and a non-aqueous electrolyte for a lithium secondary battery was injected therein to prepare a lithium secondary battery.
[0183] Comparative Example 4
[0184] (Preparation of non-aqueous electrolyte for lithium secondary battery)
[0185] 1.5 g of lithium difluorophosphate as a second additive and 1.0 g of ethylene sulfonate and 0.5 g of 1,3-propane sultone as a third additive were added to 97 g of an organic solvent (ethylene carbonate:ethylmethyl carbonate=3:7 volume ratio) in which 1.2 M LiPF6 was dissolved to prepare a non-aqueous electrolyte for a lithium secondary battery.
[0186] (Preparation of Secondary Battery)
[0187] A secondary battery was prepared in the same manner as in Example 3, except that the nonaqueous electrolyte for a lithium secondary battery prepared above was injected instead of the nonaqueous electrolyte for a lithium secondary battery of Example 3.
[0188] Experimental example
[0189] Experimental Example 1-1 High temperature (60°C) storage durability evaluation (1)
[0190] After each of the lithium secondary batteries prepared in Example 1 and Comparative Example 1 was activated at a CC of 0.1 C, degassing was performed.
[0191] Subsequently, each secondary battery was charged to 4.20V at a rate of 0.33C under constant current and constant voltage (CC-CV) conditions at 25°C, then cut off at a current of 0.05C, and discharged to 2.5V at a rate of 0.33C under constant current conditions. After setting the above charge and discharge to 1 cycle and performing 3 cycles, each lithium secondary battery was charged to a state of charge (SOC) of 50%, and then the initial resistance was calculated by the voltage drop obtained when a discharge pulse was applied to each lithium secondary battery for 10 seconds at 2.5C. The voltage drop was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A).
[0192] Subsequently, each lithium secondary battery was recharged at a CC of 0.33 C to a state of charge (SOC) of 100%, and then stored at a high temperature (60° C.) for 13 weeks.
[0193] After every 2 weeks, 4 weeks, 8 weeks, 10 weeks, and 13 weeks, each lithium secondary battery was charged to a state of charge (SOC) of 50%, and then the resistance after storage (DC-iR) was calculated by the voltage drop obtained when a discharge pulse was applied to each lithium secondary battery for 10 seconds at 2.5 C. The voltage drop was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A).
[0194] The calculated initial resistance and the resistance after high-temperature storage measured each week were substituted into the following [Equation 1] to calculate the resistance increase rate (%), and the results are then presented in Figure 1 middle.
[0195] [Equation 1]
[0196] Resistance increase rate (%) = {(resistance after high temperature storage - initial resistance) / initial resistance} × 100
[0197] See also Figure 1 It can be understood that, compared with Comparative Example 1, the resistance increase rate of the secondary battery of Example 1 after high-temperature storage is significantly improved.
[0198] Experimental Example 1-2: High temperature (60°C) storage durability evaluation (2)
[0199] After the lithium secondary battery prepared in Example 2 and the lithium secondary battery prepared in Comparative Example 2 were each activated at a CC of 0.1 C, degassing was performed.
[0200] Subsequently, each secondary battery was charged to 4.20V at a rate of 0.33C under constant current and constant voltage (CC-CV) conditions at 25°C, then cut off at a current of 0.05C, and discharged to 2.5V at a rate of 0.33C under constant current conditions. After setting the above charge and discharge to 1 cycle and performing 3 cycles, the initial discharge capacity was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A). Then, after each lithium secondary battery was charged to a state of charge (SOC) of 50%, the initial resistance was calculated by the voltage drop obtained when a discharge pulse was applied to each lithium secondary battery for 10 seconds at 2.5C. The voltage drop was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A).
[0201] Subsequently, each lithium secondary battery was recharged at a CC of 0.33 C to a state of charge (SOC) of 100%, and then stored at a high temperature (60° C.) for 2 weeks.
[0202] After two weeks, CC-CV charging and discharging was performed at a CC of 0.33C, and then the discharge capacity after high temperature storage was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A). In addition, after each lithium secondary battery was charged to a state of charge (SOC) of 50%, the resistance after high temperature storage (DC-iR) was calculated by the voltage drop obtained when a discharge pulse was applied to each lithium secondary battery at 2.5C for 10 seconds. Among them, the voltage drop was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A).
[0203] The calculated initial resistance and the resistance after high-temperature storage for 2 weeks were substituted into [Equation 1] to calculate the resistance increase rate (%), and the results are then presented in Table 1 below.
[0204] Furthermore, the initial discharge capacity and the discharge capacity after 2 weeks of high-temperature storage were substituted into the following [Equation 2], the capacity retention rate (%) was calculated, and the results thereof are then presented in Table 1 below.
[0205] [Equation 2]
[0206] Discharge capacity retention rate (%) = (discharge capacity after high temperature storage / initial discharge capacity) × 100
[0207] [Table 1]
[0208]
[0209] Referring to Table 1, it can be understood that the resistance increase rate and capacity retention rate of the secondary battery of Example 2 after high-temperature storage are improved compared with those of Comparative Example 2.
[0210] Experimental Example 1-3: High temperature (60°C) storage durability evaluation (3)
[0211] After the lithium secondary battery prepared in Example 3 and the lithium secondary battery prepared in Comparative Example 3 were each activated at a CC of 0.1 C, degassing was performed.
[0212] Subsequently, each secondary battery was charged to 4.20V at a rate of 0.33C under constant current and constant voltage (CC-CV) conditions at 25°C, then cut off at a current of 0.05C, and discharged to 2.5V at a rate of 0.33C under constant current conditions. After setting the above charge and discharge to 1 cycle and performing 3 cycles, the initial discharge capacity was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A). Then, after each lithium secondary battery was charged to a state of charge (SOC) of 50%, the initial resistance was calculated by the voltage drop obtained when a discharge pulse was applied to each lithium secondary battery for 10 seconds at 2.5C. The voltage drop was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A).
[0213] Next, each lithium secondary battery was recharged at a CC of 0.33C to a state of charge (SOC) of 100%, and then stored at a high temperature (60°C) for 4 weeks.
[0214] After 4 weeks, CC-CV charging and discharging was performed at a CC of 0.33C, and then the discharge capacity after high temperature storage was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A). In addition, after each lithium secondary battery was charged to a state of charge (SOC) of 50%, the resistance (DC-iR) after high temperature storage was calculated by the voltage drop obtained when a discharge pulse was applied to each lithium secondary battery at 2.5C for 10 seconds. Among them, the voltage drop was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A).
[0215] The calculated initial resistance and the resistance after 4 weeks of high-temperature storage were substituted into [Equation 1] to calculate the resistance increase rate (%), and the results are then presented in Table 2 below.
[0216] Furthermore, the measured initial discharge capacity and the discharge capacity after 4 weeks of high-temperature storage were substituted into [Equation 2], the capacity retention rate (%) was calculated, and the results are then presented in Table 2 below.
[0217] [Table 2]
[0218]
[0219] Referring to Table 2, it can be understood that the resistance increase rate and the capacity retention rate of the secondary battery of Example 3 after high-temperature storage are significantly improved compared with those of Comparative Example 3, respectively.
[0220] Experimental Example 1-4: High temperature (60°C) storage durability evaluation (4)
[0221] After the secondary battery prepared in Example 4 and the lithium secondary battery prepared in Comparative Example 4 were each activated at a CC of 0.1 C, degassing was performed.
[0222] Subsequently, the discharge capacity retention rate (%) after 2 weeks of high-temperature storage and the resistance increase rate (%) after 2 weeks of high-temperature storage were calculated by the same method as the high-temperature (60°C) storage durability evaluation method of Experimental Example 1-2, and the results are presented in Table 3 below.
[0223] [Table 3]
[0224]
[0225] Referring to Table 3, it can be understood that the capacity retention rate and the resistance increase rate of the secondary battery of Example 4 after high-temperature storage are improved compared with those of Comparative Example 4, respectively.
[0226] Experimental Example 2-1: High temperature (45°C) life characteristics evaluation (1)
[0227] After the lithium secondary battery prepared in Example 1 and the secondary battery prepared in Comparative Example 1 were each activated at a CC of 0.1 C, degassing was performed.
[0228] Subsequently, each secondary battery was charged to 4.20V at a rate of 0.33C under constant current and constant voltage (CC-CV) conditions at 25°C, then cut off at a current of 0.05C, and discharged to 2.5V at a rate of 0.33C under constant current conditions. After setting the above charge and discharge to 1 cycle and performing 3 cycles, the initial discharge capacity was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A). Then, after each lithium secondary battery was charged to a state of charge (SOC) of 50%, the initial resistance was calculated by the voltage drop obtained when a discharge pulse was applied to each lithium secondary battery for 10 seconds at 2.5C. Among them, the voltage drop was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A).
[0229] After that, each lithium secondary battery was charged to 4.20 V at a rate of 0.33 C under constant current-constant voltage (CC-CV) conditions at 45° C., then cut off at 0.05 C current, and discharged to 2.5 V at a rate of 0.33 C under constant current conditions. The above charge and discharge was defined as one cycle, and the resistance increase rate (%) was measured when 200 charge and discharge cycles were performed at high temperature (45° C.).
[0230] In this case, the resistance increase rate (%) was measured at intervals of 50 cycles, wherein each lithium secondary battery was charged to a state of charge (SOC) of 50% after performing charge and discharge cycles, and then the DC internal resistance (hereinafter referred to as "DC-iR") was calculated by the voltage drop obtained when each lithium secondary battery was subjected to a discharge pulse at 2.5C for 10 seconds, and was substituted into the following [Equation 3] to calculate the resistance increase rate (%). The measurement results are presented in Figure 2 In this case, the voltage drop was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5 V, 6 A).
[0231] [Equation 3]
[0232] Resistance increase rate (%) = {(resistance after cycle - initial resistance) / initial resistance} × 100
[0233] Reference Figure 2 For the secondary battery of Example 1, since a stable film is formed on the surface of the positive electrode / negative electrode, it can be confirmed that when long-term charging and discharging is performed at high temperature, the resistance increase rate is improved compared with Comparative Example 1 due to suppression of additional electrolyte decomposition.
[0234] Experimental Example 2-2: High temperature (45°C) life characteristics evaluation (2)
[0235] After the lithium secondary battery prepared in Example 2 and the secondary battery prepared in Comparative Example 2 were each activated at a CC of 0.1 C, degassing was performed.
[0236] Subsequently, each secondary battery was charged to 4.20V at a rate of 0.33C under constant current and constant voltage (CC-CV) conditions at 25°C, then cut off at a current of 0.05C, and discharged to 2.5V at a rate of 0.33C under constant current conditions. After setting the above charge and discharge to 1 cycle and performing 3 cycles, the initial discharge capacity was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A). Then, after each lithium secondary battery was charged to a state of charge (SOC) of 50%, the initial resistance was calculated by the voltage drop obtained when a discharge pulse was applied to each lithium secondary battery for 10 seconds at 2.5C. Among them, the voltage drop was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5V, 6A).
[0237] Afterwards, each lithium secondary battery was charged to 4.20 V at a rate of 0.33 C under constant current constant voltage (CC-CV) conditions at 45°C, then cut off at a current of 0.05 C, and discharged to 2.5 V at a rate of 0.33 C under constant current conditions. The above charge and discharge was defined as one cycle, and 50 charge and discharge cycles were performed at high temperature (45°C).
[0238] After 50 cycles, each lithium secondary battery was charged to 4.2 V at a rate of 0.33 C under constant current constant voltage (CC-CV) conditions at 25°C, and then discharged to 2.5 V at a rate of 0.33 C under constant current conditions, and the discharge capacity was measured using a PNE-0506 charge / discharge device (manufacturer: PNE SOLUTION Co., Ltd., 5 V, 6 A), which was substituted into [Equation 4] to measure the capacity retention rate, and the results are presented in Table 4 below.
[0239] Subsequently, the DC internal resistance (hereinafter referred to as "DC-iR") was calculated by the voltage drop obtained in the state where a discharge pulse of 10 seconds was applied to each lithium secondary battery at 2.5C at 50% SOC, which was substituted into [Equation 3] to calculate the resistance increase rate (%), and then the results are presented in the following Table 4. Among them, the voltage drop was measured using a PNE-0506 charge / discharge device (manufacturer: PNESOLUTION Co., Ltd., 5V, 6A).
[0240] [Equation 4]
[0241] Capacity retention rate (%) = (discharge capacity after cycle / initial discharge capacity) × 100
[0242] [Table 4]
[0243]
[0244] Referring to Table 4, for the secondary battery of Example 2, since a stable film was formed on the surface of the positive electrode / negative electrode, it was confirmed that when long-term charging and discharging was performed at high temperature, the resistance increase rate was improved compared with Comparative Example 2 due to suppression of additional electrolyte decomposition.
Claims
1. A non-aqueous electrolyte for a lithium secondary battery, comprising the following i) to v) composition: i) lithium salts; ii) organic solvents; iii) a compound represented by Formula 1 as a first additive; iv) lithium difluorophosphate (LiDFP) as a second additive; and v) a third additive, wherein the third additive is ethylene sulfonate, 1,3-propane sultone, LiBF 4 and fluorobenzene, or ethylene sulfonate and 1,3-propane sultone; [Formula 1] Among them, in formula 1, R is a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms.
2. The non-aqueous electrolyte for lithium secondary battery according to claim 1, in, In Formula 1, R is a substituted or unsubstituted alkyl group having 1 to 3 carbon atoms.
3. The non-aqueous electrolyte for lithium secondary battery according to claim 1, in, The compounds represented by Formula 1 include compounds represented by Formula 1a: [Formula 1a] 4. The non-aqueous electrolyte for lithium secondary battery according to claim 1, in, The compound represented by Formula 1 may be included in an amount of 0.1 wt % to 5 wt % based on the total weight of the non-aqueous electrolyte.
5. The non-aqueous electrolyte for lithium secondary battery according to claim 1, in, The content of the second additive is 0.1 wt % to 5 wt % based on the total weight of the non-aqueous electrolyte.
6. The non-aqueous electrolyte for lithium secondary battery according to claim 1, in, The weight ratio of the first additive to the second additive is 1:1 to 1:
10.
7. The non-aqueous electrolyte for lithium secondary battery according to claim 6, in, The weight ratio of the first additive to the second additive is 1:1 to 1:
5. 8 . A lithium secondary battery comprising the non-aqueous electrolyte for a lithium secondary battery according to claim 1 .
Citation Information
Patent Citations
Temperature-adjustable modular apparatus of cold storage system
KR1020190102520A
Non-aqueous electrolyte additive, and non-aqueous electrolyte for lithium secondary battery and lithium secondary battery including same
CN113728483A
KR20200089624A