Natural gas hydrate corrosion evaluation test device and method

By designing a natural gas hydrate corrosion evaluation test device that can adjust temperature and pressure, the problem that the existing technology cannot effectively study the corrosion of natural gas hydrate on pipelines, and real-time monitoring and suppression of the corrosion conditions of natural gas hydrate under different conditions is achieved. Analysis of agent effects provides scientific evaluation methods.

CN114152560BActive Publication Date: 2024-12-06CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010932081.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-08
Publication Date
2024-12-06
Estimated Expiration
2040-09-08

AI Technical Summary

Technical Problem

The prior art cannot effectively study and evaluate the corrosion of natural gas hydrates on pipelines under different pressures, temperatures and flow rates, especially in deep-sea natural gas fields. The impact of natural gas hydrate generation inhibitors on pipeline corrosion is unclear.

Method used

A corrosion evaluation test device for natural gas hydrates is designed, including a circular pipeline with adjustable temperature and pressure and a stirred reactor, equipped with weightless corrosion hangers and rotatable hangers. The circular channels and reactors are compared online by monitoring and comparison of the circular channels and reactors. The corrosion rate within simulates the corrosion rate of natural gas hydrates on the pipeline under different conditions, and can be tested by adding inhibitors or promoters.

Benefits of technology

Real-time observation of the corrosion conditions of natural gas hydrates on pipelines under different temperature and pressure conditions is achieved, the corrosion differences in the ring and reactor environment are compared, the impact of inhibitors on pipeline corrosion is studied, and the generation of hydrates during natural gas transportation is simulated. and to relieve the corrosion conditions of blockage, provide scientific evaluation methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114152560B_ABST
    Figure CN114152560B_ABST
Patent Text Reader

Abstract

The present invention discloses a corrosion evaluation test device and method for natural gas hydrates, the device comprising: a loop pipeline, which is fed with natural gas hydrates under adjustable temperature and pressure, and a weightless corrosion hanging plate is arranged in the loop pipeline; a stirred reactor, which is connected to the loop pipeline and has the same temperature and pressure environment as the loop pipeline, and a rotatable hanging plate is arranged in the stirred reactor; based on the weightlessness and surface morphology changes of the weightless corrosion hanging plate in the loop pipeline and the rotatable hanging plate in the stirred reactor, the comparative situation of the corrosion rates of the two is evaluated. The device and method of the present invention can not only observe the corrosion condition of the pipeline by fluids of different temperatures and pressures, different flow rates, and different natural gas hydrate forms in real time, but also can simultaneously compare the corrosion differences of the samples in the loop environment and the reactor environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of natural gas hydrate gathering and transportation technology and corrosion evaluation, simulating the generation and change of natural gas hydrate under pipeline transportation conditions and the corrosion of hydrate inhibitors or promoters on metal pipelines, and in particular to a natural gas hydrate corrosion evaluation test device and method. Background Art

[0002] Natural gas hydrates are abundant on Earth and are an important potential energy source in the world. In the context of the energy crisis, their investigation and research has become a global hotspot. They are ice-like crystalline compounds composed of water and natural gas under high pressure and low temperature.

[0003] Although natural gas hydrates are an important form of energy, their formation and presence can have serious adverse effects during natural gas pipeline transportation. The actual operation of gas pipelines has shown that natural gas hydrates can cause pipeline corrosion and are prone to ice blockage when the temperature is low, thus affecting the safe and smooth operation of gas pipelines. In order to prevent the formation of natural gas hydrates during pipeline transportation, various inhibitors are widely used to prevent and decompose the formation of hydrate plugs. However, the corrosion effect of the addition of hydrate inhibitors on pipelines is still unclear. In addition, with the development of offshore oil and gas fields towards deep sea and ultra-deep sea, the pipeline temperature is lower, and the cost of conventional means of inhibiting hydrate formation is increased and the effect is limited. The industry has thus introduced the concept of hydrate slurry transportation technology and cold flow, allowing or guiding the natural gas in the fluid to form hydrates. In addition, in application scenarios such as natural gas and carbon dioxide gas separation, in order to promote the formation of natural gas hydrates, various hydrate promoters need to be added. It is not only natural gas hydrates that have practical application value, but also hydrate slurries with flow characteristics. Nowadays, many scholars have begun to study the flow law and characteristics of natural gas hydrate slurry in pipelines and carry out process design of hydrate slurry transportation pipelines. For example, Chinese patent CN208780594U discloses a natural gas hydrate deposition characteristic test device, and Chinese patent CN 208872627 U discloses a high-pressure test device for the flow characteristics of natural gas hydrate slurry. However, research on the corrosion effect of hydrate slurry on pipelines during flow is rarely heard of, and the industry knows little about the corrosion of natural gas hydrate slurry on pipelines.

[0004] Therefore, it is urgent to establish scientific test equipment and methods to evaluate the corrosion of pipelines by fluids in the presence of natural gas hydrates. At present, patent CN 107991225 A discloses an in-situ monitoring system for pipeline corrosion in solid fluidized gas hydrate production, which is mainly aimed at the study of the mixed lifting process and pipeline scouring corrosion of natural gas hydrate production. However, it is impossible to study the effects of the generation form, flow rate and additives of natural gas hydrates under different pressure and temperature conditions on pipeline corrosion.

[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0006] The purpose of the present invention is to provide a natural gas hydrate corrosion evaluation test device and method, which can not only observe in real time the corrosion conditions of pipelines caused by fluids with different temperatures and pressures, different flow rates, and different natural gas hydrate forms, but also can simultaneously compare the corrosion differences between samples in a ring environment and a reactor environment.

[0007] To achieve the above-mentioned purpose, according to the first aspect of the present invention, there is provided a corrosion evaluation test device for natural gas hydrates, comprising: a loop pipeline, through which natural gas hydrates are introduced under temperature and pressure adjustable conditions, wherein a weightlessness corrosion hanging plate is arranged in the loop pipeline; a stirred reactor, which is connected to the loop pipeline and has the same temperature and pressure environment as the loop pipeline, wherein a rotatable hanging plate is arranged in the stirred reactor; based on the weightlessness and surface morphology changes of the weightlessness corrosion hanging plate in the loop pipeline and the rotatable hanging plate in the stirred reactor, a comparative evaluation of the corrosion rates of the two is performed.

[0008] Furthermore, in the above technical solution, an injection unit is provided on the loop pipeline for injecting a hydrate inhibitor or an accelerator into the loop pipeline.

[0009] Further, in the above technical solution, the loop pipeline includes: a first pipe section, which is a detachable pipeline, in which a first pressure sensor and a first temperature sensor are arranged, and a first high and low temperature bath with independently adjustable temperature is arranged outside; the first pipe section area can connect pipelines of different diameters. A second pipe section, which is a pipeline elbow, in which a second pressure sensor and a second temperature sensor are arranged, and a second high and low temperature bath with independently adjustable temperature is arranged outside; the second pipe section is used to simulate the erosion of the pipeline by the natural gas hydrate slurry in a moving state. A third pipe section, in which a resistance corrosion probe and / or an electrochemical linear polarization resistance corrosion probe is arranged, in which a third pressure sensor and a third temperature sensor are also arranged, and a third high and low temperature bath with independently adjustable temperature is arranged outside; the third pipe section is used to monitor the corrosion condition in the pipeline online, and to measure the cumulative corrosion amount and instantaneous corrosion rate per unit time. A fourth pipe section, in which multiple weightlessness corrosion coupons are placed in the sample placement area located in the center of the pipe section, a fourth pressure sensor and a fourth temperature sensor are also arranged in the fourth pipe section, and a fourth high and low temperature bath with independently adjustable temperature is arranged outside.

[0010] Furthermore, in the above technical solution, the sample placement area is a groove structure evenly arranged along the circumference of the hollow part of the pipeline, and the weightlessness corrosion hanging piece is embedded in the groove and is interference fit and / or adhesively fit with the groove.

[0011] Furthermore, in the above technical solution, the outer wall and the inner tank of the stirred reactor are provided with transparent windows, and a high-definition camera and an LED auxiliary light source are provided outside the transparent window of the outer wall; a rotatable hanging plate is provided at the end of the stirring blade; and a fifth pressure sensor and a fifth temperature sensor are provided in the stirred reactor.

[0012] Furthermore, in the above technical solution, pure water in natural gas hydrate is injected by a water injection pump, natural gas is transported to the loop pipeline through a steel cylinder and gas circulation is achieved through a gas circulation pump; natural gas hydrate slurry is circulated through a magnetic circulation pump.

[0013] Furthermore, in the above technical solution, an online particle size analyzer is provided in the loop pipeline, which measures the particle size, morphology and content of the natural gas hydrate in real time through focused light beam reflection; a direct-insertion densitometer for online density analysis is also provided in the loop pipeline.

[0014] Furthermore, in the above technical solution, a gas-liquid separator with a liquid level meter is provided in the loop pipeline.

[0015] Furthermore, in the above technical solution, a differential pressure sensor may be provided between the four pipe sections.

[0016] According to the second aspect of the present invention, the present invention provides a corrosion evaluation test method for natural gas hydrates, comprising the following steps: injecting pure water into a loop pipeline and allowing the pure water to reach a preset temperature; introducing natural gas into the loop pipeline and pressurizing it to a preset pressure, and generating natural gas hydrates after a preset reaction time; after the natural gas hydrate slurry circulates stably in the loop pipeline, driving a rotatable hanging plate in a stirred reactor to rotate; online observing and recording the hydrate morphology of the natural gas hydrate slurry in the loop pipeline; taking out the weightlessness corrosion hanging plate placed in the loop pipeline and the rotatable hanging plate in the stirred reactor, comparing and observing the corrosion surface morphology of the two and measuring the corrosion rate.

[0017] Furthermore, in the above technical solution, the preset temperature of pure water is 276.15 to 281.15 K; the preset pressure of natural gas is 5 to 10 Mpa; and the preset reaction time is 100 to 1000 minutes.

[0018] Furthermore, in the above technical solution, the natural gas hydrate slurry is controlled to circulate stably in the loop pipeline by a magnetic circulation pump, and the flow rate is controlled in the range of 0.5 to 2 m / s.

[0019] Furthermore, in the above technical solution, four pipe sections are arranged in the loop pipeline, and the corrosion conditions of different pipe sections at different temperatures, pressures, and different flow rates and forms of the natural gas hydrate slurry are tested respectively.

[0020] Furthermore, in the above technical solution, a hydrate inhibitor or accelerator is injected into the loop pipeline through the injection unit; and the corrosion test results with the addition of the hydrate inhibitor or accelerator are compared and analyzed with the corrosion test results in a pure water environment.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1) The device and method of the present invention can observe in real time the corrosion condition of pipelines caused by fluids of different temperatures and pressures, different flow rates, and different natural gas hydrate forms;

[0023] 2) The corrosion differences between samples in the loop environment and the reactor environment can be compared simultaneously;

[0024] 3) It is also possible to study the effects of additives such as hydrate inhibitors on pipeline corrosion conditions;

[0025] 4) The circulation pipeline can be used to simulate the formation of hydrates caused by cooling during natural gas pipeline transportation, and to simulate the release of natural gas hydrate blockage in valves and narrow and long pipelines during heating;

[0026] 5) The test pipeline includes four test sections, which can simultaneously simulate the hydrate formation and pipeline corrosion conditions at different temperatures. Some pipelines are designed to be detachable to achieve offline testing and testing with variable pipe diameters;

[0027] 6) The test pipeline contains pressure and temperature measuring points, and a computer acquisition system can be used to measure the gradient changes of pressure and temperature in the pipeline.

[0028] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, and to make the above and other purposes, technical features and advantages of the present invention easier to understand, one or more preferred embodiments are listed below and described in detail with the accompanying drawings as follows. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the connection of the natural gas hydrate corrosion evaluation test device of the present invention.

[0030] Figure 2 It is a structural schematic diagram of a visual stirring reactor in the corrosion evaluation test device of the present invention.

[0031] Figure 3 It is a schematic diagram of the installation structure of the weightlessness corrosion hanging piece in the fourth pipe section of the d zone of the corrosion evaluation test device of the present invention.

[0032] Description of main reference numerals:

[0033] 1-gas cylinder, 1'-buffer cylinder, 2-gas booster pump, 3-gas circulation pump, 4-water injection pump, 5-drug injection pump, 6-separator with liquid level meter, 7-magnetic circulation pump, 8-online particle size analyzer, 9-stirring reactor, 91-reaction reactor outer wall, 92-reaction reactor liner, 93-stirring blade, 94-rotatable hanging piece, 95-LED light source, 96-high-definition camera, 10-internal component of the fourth pipe section, 101-connecting hole, 102-sealing ring, 103-weightlessness corrosion hanging piece placement area, 1030-groove;

[0034] a-first pipe segment, b-second pipe segment, c-third pipe segment, d-fourth pipe segment. DETAILED DESCRIPTION

[0035] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.

[0036] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.

[0037] In this document, for the convenience of description, spatial relative terms such as "below", "below", "down", "above", "above", "upper", etc. may be used to describe the relationship between one element or feature and another element or feature in the accompanying drawings. It should be understood that the spatial relative terms are intended to include different directions of objects in use or operation in addition to the directions drawn in the drawings. For example, if the object in the figure is turned over, the elements described as being "below" or "below" other elements or features will be oriented "above" the elements or features. Therefore, the exemplary term "below" can include both below and above directions. Objects may also have other orientations (rotated 90 degrees or other orientations) and the spatial relative terms used in this document should be interpreted accordingly.

[0038] In this document, the terms "first", "second", etc. are used to distinguish two different elements or parts, and are not used to limit a specific position or relative relationship. In other words, in some embodiments, the terms "first", "second", etc. can also be interchangeable.

[0039] The natural gas hydrate corrosion evaluation test device of the present invention can observe in real time the corrosion condition of pipelines caused by fluids of different temperatures and pressures, different flow rates, and different natural gas hydrate forms, and can also compare the corrosion differences of samples in the ring environment and the reactor environment at the same time. Figure 1 As shown, the corrosion evaluation test device of the present invention includes a loop pipeline and a stirred reactor 9. Among them, the loop pipeline simulates the transportation pipeline of natural gas hydrate, and natural gas hydrate can be introduced under the condition that the temperature and pressure are adjustable. A weightlessness corrosion hanging plate is arranged in the loop pipeline. Specifically, a jacket cold circulation and heat circulation device is arranged on the outside of the loop pipeline to adjust the temperature of the loop environment. The jacket cold circulation and heat circulation device further includes a temperature control instrument, a heating system, a temperature control system, a constant temperature bath and a refrigeration temperature control system, which together constitute a high and low temperature bath. The heating temperature control system mainly includes a heating electric heating pipe, a hot air blower, etc., and the refrigeration temperature control system mainly includes a refrigeration system, a cooling unit, a cold box, a cold circulation pump, a cold liquid delivery pipeline and corresponding insulation, etc. The stirred reactor 9 is connected to the loop pipeline and has the same temperature and pressure environment as the loop pipeline. A rotatable hanging plate 94 is provided in the stirred reactor (see Figure 2 ). According to the weight loss and surface morphology changes of the weight loss corrosion hanging piece in the loop pipeline and the rotatable hanging piece 94 in the stirred reactor 9, the comparative situation of the corrosion rates of the two can be evaluated.

[0040] Further Figure 2As shown, the stirred reactor 9 is provided with transparent observation windows on the outer wall 91 and the inner tank 92, which can effectively and clearly observe the changes in the liquid and the formation of hydrates in the reactor 9 in combination with the cold light source. The temperature of the reactor is measured by a precision platinum resistor (not shown in the figure), and the measurement can be divided into two points, upper and lower. The upper part of the reactor 9 is provided with a gas discharge port, a liquid filling port, a pressure measuring port, and an evacuation port, and the lower part is provided with a liquid discharge port. The rotatable hanging piece 94 is arranged at the lower part of the stirring blade 93, and can rotate with the blade to simulate the corrosion of the material in the detection reactor. The stirring blade 93 can be connected to a magnetic stirring unit, and the magnetic stirring unit (not shown in the figure) is mainly composed of internal and external magnetic stirring mechanisms, a servo motor, a servo controller and other parts.

[0041] Further Figure 1 As shown, the present invention takes into account that inhibitors or promoters are generally added to the pipeline under actual working conditions, thereby hindering or accelerating the formation of natural gas hydrates. In order to simulate this environment, preferably but not restrictively, an injection unit is provided on the loop pipeline of the present invention, which is used to inject hydrate inhibitors or promoters into the loop pipeline. Specifically, an injection pump 5 is provided in the loop pipeline to inject additives. The injection pump 5 can adopt a large-flow horizontal flow pump plus a corresponding supporting pipeline, wherein the horizontal flow pump is mainly used to inject inhibitors or promoters into the circulation pipeline.

[0042] Further Figure 1 As shown, the pure water in the natural gas hydrate of the present invention is injected by the water injection pump 4, and the water injection pump 4 can be a frequency-modulated plunger pump. Natural gas is transported to the loop pipeline through the gas cylinder 1 and a stable circulation of the gas is achieved through the gas circulation pump 3. The gas injection needs to control the injection amount of natural gas. A manual throttle valve and a gas flow meter can be set. The manual throttle valve has a pressure resistance of 16 MPa. The gas flow meter is mainly used to measure the injection amount of gas, and the maximum flow range is 250 L / min. The gas booster pump 2 is part of the booster unit, which includes a natural gas air compressor, a high-pressure buffer storage tank (i.e. Figure 1 The buffer cylinder 1'), pressure regulating valve and other components in the gas compressor. The natural gas compressor is mainly used to compress and pressurize natural gas. In view of the special requirements of natural gas, the natural gas compressor must meet the corresponding explosion-proof requirements and technical indicators. The GS15 natural gas compressor can be used. The high-pressure gas buffer storage tank can use the ZR-I type container with a maximum pressure resistance of 25 MPa, which is mainly used to store pressurized gas. The natural gas hydrate slurry is circulated stably through the magnetic circulation pump 7.

[0043] Further Figure 1 As shown, preferably but not restrictively, in order to simulate various working conditions of the natural gas pipeline and adopt different measurement methods to evaluate the pipeline corrosion, the present invention divides the loop pipeline into four sections, namely the first section in area a, the second section in area b, the third section in area c and the fourth section in area d.

[0044] Among them, the first pipe section in area a is designed as a detachable pipe. The detachable pipe can be replaced with pipes of different diameters for testing. The change of pipe diameter can also simulate natural gas hydrates of different flow rates. In order to effectively monitor the temperature and pressure of the pipe section, a first pressure sensor and a first temperature sensor are provided in the pipe section, and a first high and low temperature bath with independently adjustable temperature is provided outside the pipe section (the temperature of this pipe section can be adjusted separately). The first pipe section in area a is used to carry out corrosion tests and hydrate inhibitor evaluation tests on pipe mother bodies of different diameters and different materials under different hydrate slurry operating conditions. Different hydrate slurries can be carbon dioxide hydrate slurries, methane hydrate slurries, hydrogen sulfide hydrate slurries, etc. The present invention mainly evaluates the corrosion of natural gas hydrate slurries. Hydrate slurry operating conditions refer to different operating conditions of temperature, pressure, and flow rate. When natural gas hydrates can be generated, there will be a certain amount of carbon dioxide hydrate in the loop.

[0045] Among them, the second pipe section in zone b is set as a pipeline elbow (depending on whether online detection is selected, the pipe section can be a disassembled pipe section or a non-disassembled pipe section), a second pressure sensor and a second temperature sensor are arranged in the pipeline elbow, and a second high and low temperature bath with independently adjustable temperature is arranged outside the pipeline elbow. The second pipe section is used to simulate the erosion condition of the pipeline elbow by the natural gas hydrate slurry in a moving state. Preferably, but not restrictively, the corrosion degree can be detected in the second pipe section by an ultrasonic polycrystalline sensor.

[0046] Among them, the third pipe section in the c zone is provided with a resistance corrosion probe and / or an electrochemical linear polarization resistance corrosion probe, which can monitor the corrosion situation in the pipeline online, measure the cumulative corrosion amount and instantaneous corrosion rate per unit time. Similar to the above two pipe sections, this pipe section is also provided with a third pressure sensor and a third temperature sensor, and a third high and low temperature bath with independently adjustable temperature is provided on the outside. After the fluid circulation of the pipe section is stable, the three-electrode system on the in-situ monitoring tee can be connected to the corresponding interface of the electrochemical workstation through a signal transmission line to form an electrochemical test system. The pipeline is tested for corrosion in situ through this test system. Through test items such as open circuit potential, linear polarization, dynamic potential polarization, electrochemical impedance and cyclic polarization, parameters such as corrosion potential, corrosion current density, impedance and pitting potential in the process of corrosion in the pipe are obtained, and then these parameters are used to conduct a more in-depth study on the corrosion mechanism in the pipe, and provide life prediction for pipelines for natural gas hydrate transportation. For example, the potential and polarization curve are measured by a probe, and the corrosion current density and pitting potential are calculated based on the obtained curve. The corrosion rate can be calculated by the corrosion current density, and the pitting potential can be used to determine whether pitting corrosion exists in the hydrate environment or whether it is just uniform corrosion. This method can be used to study whether pitting corrosion occurs at the site where hydrates are precipitated, that is, whether pitting corrosion is easily formed when natural gas hydrates are precipitated and attached to the pipe wall, accelerating local corrosion of the pipeline.

[0047] The fourth pipe section in zone d is provided with a weightlessness hanging plate test device (i.e., the fourth pipe section internal component 10). Figure 3 As shown, multiple (four in the figure) weightless corrosion coupons are placed in the sample placement area located in the center of the pipe section. The weightless corrosion coupon placement area 103 is a groove structure uniformly arranged along the circumference of the hollow part of the pipeline. The weightless corrosion coupon is embedded in the groove 1030 and is interference fit and / or adhesively fitted with the groove 1030 so as to be firmly installed. The placement direction of the coupon is the same as the flow direction of the fluid. The fourth pipe section internal component 10 is provided with a connecting hole 101 for fixing on the pipe section. In order to achieve the sealing of the pipe section gap, a sealing ring 102 is also provided. The fourth pipe section is also provided with a fourth pressure sensor and a fourth temperature sensor, and a fourth high and low temperature bath with independently adjustable temperature is provided outside. The weightless corrosion coupon is taken out for inspection regularly, and the surface morphology of the coupon is observed, the surface corrosion products are analyzed, the weightlessness and corrosion rate of the coupon are calculated, and the type of corrosion is determined. At the same time, it can be compared with the corrosion condition of the rotatable coupon 94 in the stirred reactor 9, so as to compare the difference in corrosion conditions under different fluid flow modes in the ring channel and the reactor under the same working conditions. The high and low temperature constant temperature system of the stirred reactor 9 operates at a temperature of -10 to 60 °C, and uses air bath heating and cooling. Within the visible window, the rotation state of the natural gas hydrate slurry and the corrosion coupon in the reactor can be observed online in real time through the LED auxiliary light source and high-definition camera recording.

[0048] Further Figure 1 As shown, in order to make the pressure value reading more intuitive, easier to read and record, a differential pressure sensor is provided between the four pipe sections.

[0049] Further Figure 1 As shown, an online particle size analyzer 8 is provided in the loop pipeline, which measures the particle size, morphology and content of the natural gas hydrate in real time through the reflection of the focused light beam. A plug-in density meter for online density analysis is also provided in the loop pipeline. The online particle size analyzer 8 can be used to collect and analyze the particle size data of the natural gas hydrate slurry particles. The particle size range is not less than 0.5-1000μm, the operating temperature range is not less than -10-90℃, the plug-in density meter has a pressure resistance of not less than 15MPa, and a range of 0-2 g / cm 3 , accuracy 0.001 g / cm 3 The fluid test sample parameters can be obtained in real time through the online particle size analyzer 8. The parameters such as the particle size, content, shape, etc. of the generated hydrate can be changed by changing the parameters such as pressure and temperature, so as to study the influence of hydrate slurry under different conditions on the pipeline corrosion condition. In order to control the water injection volume for the test, measure the gas composition after the reaction, etc., a separator 6 with a liquid level meter is also set in the loop pipeline.

[0050] Example 1

[0051] Embodiment 1 of the present invention is a corrosion difference test method for hanging pieces in a ring environment and a reactor environment, and the specific steps are as follows:

[0052] Step 101, connect the test device, remove debris in the loop, check the sealing between each pipe section, ensure that the pipeline and valve are leak-free, and adjust all temperature sensors and pressure sensors to zero;

[0053] Step 102, turn on the water injection pump 4, inject 10 L of pure water into the system, control the amount of pure water added by the flow meter in the water injection pump 4 and the liquid level gauge in the separator 6, so that the pure water level reaches the pipeline height, and use the temperature controller to make the temperature of the separator 6 and the four test pipe sections in the four zones a, b, c and d to be 276.15 K, turn on the stirring device in the separator 6 and make its rotation speed 600 r / min.

[0054] Step 103, open the gas cylinder 1, introduce methane gas into the device, make the feed pressure 5 Mpa through the gas booster pump 2, then close the gas cylinder 1, observe and record the change of the pressure gauge. The pressure drops rapidly within 30 minutes, and then the pressure curve slowly decreases until the reaction time reaches about 960 minutes, when the pressure drops again significantly, and a large amount of natural gas hydrate is generated.

[0055] Step 104, turn on the magnetic circulation pump 7, control the flow rate of natural gas hydrate in the annular channel to 1.2 m / s, so that the hydrate slurry circulates stably in the annular channel. Turn on the visual stirring reactor 9, so that the rotatable hanging piece 94 in the reactor 9 also rotates in the reactor at a linear speed of 1.2 m / s.

[0056] Step 105, during the test, the hydrate morphology during the operation is observed and recorded by the online particle size analyzer 8.

[0057] Step 106, the test is carried out for 7 days, the magnetic circulation pump 7 is turned off, the gas and pure water are released from the loop pipeline, the fourth pipe section of the d zone and the hanging piece in the visual stirring reactor 9 are taken out respectively, the corrosion surface morphology is compared and observed, and the corrosion rate is measured.

[0058] Example 2

[0059] Example 2 of the present invention uses a test method for the corrosion condition of pipelines by fluids with different temperatures, pressures, flow rates and natural gas hydrate forms in four pipe sections, and the specific steps are as follows:

[0060] Step 201, connect the test device, remove debris in the test loop, check the sealing between each pipe section, ensure that the pipeline and valve are leak-free, and adjust all temperature sensors and pressure sensors to zero;

[0061] Step 202, turn on the water injection pump 4, inject 10 L of pure water into the system, control the amount of pure water added by the flow meter in the water injection pump 4 and the liquid level gauge in the separator 6, so that the pure water level reaches the pipeline height, and use the temperature controller to make the temperature of the separator 6 and the four test pipe sections in the four zones a, b, c and d to be 276.15 K, and turn on the stirring device in the separator 6 to make its rotation speed 600 r / min.

[0062] Step 203, open the gas cylinder 1, introduce methane gas into the device, make the feed pressure reach 6 Mpa through the gas booster pump 2, then close the gas cylinder 1, observe and record the change of the pressure gauge. The pressure drops rapidly within 30 minutes, and then the pressure curve slowly decreases until the reaction time reaches about 800 minutes, when the pressure drops significantly again, and a large amount of natural gas hydrate is generated.

[0063] Step 204, turn on the magnetic circulation pump 7, control the flow rate of the natural gas hydrate in the annular channel to 1 m / s, and make the hydrate slurry circulate stably in the annular channel.

[0064] Step 205, during the test, the reading of the resistance probe in the third pipe section of zone c is recorded, and the hydrate morphology during the operation is observed and recorded by the online particle size analyzer 8.

[0065] Step 206, the test is carried out for 7 days, the magnetic circulation pump 7 is turned off, the gas and pure water are released from the loop pipeline, the first pipe section in area a is disassembled, and the weightlessness corrosion hanging piece of the fourth pipe section in area d is taken out, and the corrosion surface morphology of the pipe section and the hanging piece is observed, and the corrosion rate is measured. It can be compared with the data recorded in the third pipe section in area c to analyze the differences in corrosion rate and morphology of the samples in different pipe section areas.

[0066] This test can change the parameters such as pipe section temperature, pressure and flow rate according to the test needs to compare and measure the corrosion behavior of natural gas hydrate fluid on the pipeline under different conditions.

[0067] Example 3

[0068] Example 3 of the present invention is a test method for evaluating the effect of natural gas hydrate on pipeline corrosion after adding additives such as hydrate inhibitors, and the specific steps are:

[0069] Step 301, connect the test device, remove debris in the test loop, check the sealing between each pipe section, ensure that the pipeline and valve are leak-free, and adjust all temperature sensors and pressure sensors to zero;

[0070] Step 302, turn on the injection pump 5, inject 10 L of sodium dodecyl sulfate (SDS) solution (a hydrate formation promoter solution) into the system, control the amount of sodium dodecyl sulfate (SDS) solution added by the flow meter in the injection pump 5 and the liquid level gauge in the separator 6, make the liquid level of the sodium dodecyl sulfate (SDS) solution reach the pipeline height, make the temperature of the separator 6 and the four pipe sections of the four zones a, b, c and d be 276.15 K by the temperature controller, turn on the stirring device in the separator 6 and make its rotation speed 600 r / min.

[0071] Step 303, open the gas cylinder 1, introduce methane gas into the device, make the feed pressure reach 6 Mpa through the gas booster pump 2, then close the gas cylinder 1, observe and record the change of the pressure gauge. The pressure drops rapidly within 20 minutes, and then the pressure curve slowly decreases until the reaction time reaches about 600 minutes, when the pressure drops again significantly, and a large amount of natural gas hydrate is generated.

[0072] Step 304, turn on the magnetic circulation pump 7, control the flow rate of the natural gas hydrate in the annular channel to 1 m / s, and make the hydrate slurry circulate stably in the annular channel.

[0073] Step 305, during the test, the reading of the resistance probe in the third pipe section of zone c is recorded, and the hydrate morphology during the operation is observed and recorded by the online particle size analyzer 8.

[0074] Step 306, the test is carried out for 7 days, the magnetic circulation pump 7 is turned off, the gas and sodium dodecyl sulfate (SDS) solution are released from the loop pipeline, the first pipe section in area a is disassembled, and the weightlessness corrosion hanging piece of the fourth pipe section in area d is taken out, and the corrosion surface morphology of the pipe section and the hanging piece is observed, and the corrosion rate is measured. It can be compared with the data recorded in the third pipe section in area c to analyze the differences in corrosion rate and morphology of the samples in different pipe section areas.

[0075] The additives in this test can be replaced according to the test requirements (such as tert-butyl alcohol) and other hydrate promoters or inhibitors, and then the corrosion test results are compared and analyzed with the test results in pure water to study the corrosion of the pipeline by the hydrate additives.

[0076] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. Any simple modifications, equivalent changes and modifications made to the above exemplary embodiments should fall within the scope of protection of the present invention.

Claims

1. A natural gas hydrate corrosion evaluation test device, characterized in that: include: A loop pipeline, into which natural gas hydrate is introduced under adjustable temperature and pressure conditions, wherein a weightlessness corrosion hanging sheet is arranged in the loop pipeline; The loop pipeline includes: a first pipe section, which is a detachable pipe, and the first pipe section area can be connected to pipes of different diameters; a second pipe section, which is a pipe elbow, and the second pipe section is used to simulate the erosion of the pipe by the natural gas hydrate slurry in a moving state; a third pipe section, which is used to monitor the corrosion condition in the pipeline online, and measure the cumulative corrosion amount and instantaneous corrosion rate per unit time; a fourth pipe section, and a plurality of weightlessness corrosion coupons are placed in a sample placement area located in the center of the fourth pipe section; A stirred reactor, which is connected to the loop pipeline and has the same temperature and pressure environment as the loop pipeline, and a rotatable hanging plate is provided in the stirred reactor; According to the weight loss and surface morphology changes of the weightlessness corrosion hanging piece in the loop pipeline and the rotatable hanging piece in the stirred reactor, the comparative corrosion rates of the two are evaluated: by observing the surface morphology of the weightlessness corrosion hanging piece, analyzing the surface corrosion products, calculating the weight loss and corrosion rate of the weightlessness corrosion hanging piece, and determining the type of corrosion; at the same time, compared with the corrosion condition of the rotatable hanging piece in the stirred reactor, compare the difference in corrosion conditions under different fluid flow patterns in the loop and the reactor under the same operating conditions.

2. The natural gas hydrate corrosion evaluation test device according to claim 1, characterized in that: The loop pipeline is provided with an injection unit for injecting a hydrate inhibitor or a promoter into the loop pipeline.

3. The natural gas hydrate corrosion evaluation test device according to claim 2, characterized in that: The first pipe section is provided with a first pressure sensor and a first temperature sensor in the first pipe section, and a first high and low temperature bath with independently adjustable temperature is provided outside the first pipe section.

4. The natural gas hydrate corrosion evaluation test device according to claim 3, characterized in that: The second pipe section is provided with a second pressure sensor and a second temperature sensor inside, and a second high and low temperature bath with independently adjustable temperature is provided outside.

5. The natural gas hydrate corrosion evaluation test device according to claim 4, characterized in that: The third pipe section is provided with a resistance corrosion probe and / or an electrochemical linear polarization resistance corrosion probe, a third pressure sensor and a third temperature sensor, and a third high and low temperature bath with independently adjustable temperature.

6. The natural gas hydrate corrosion evaluation test device according to claim 5, characterized in that: A fourth pressure sensor and a fourth temperature sensor are also arranged in the fourth pipe section, and a fourth high and low temperature bath with independently adjustable temperature is arranged outside the fourth pipe section.

7. The natural gas hydrate corrosion evaluation test device according to claim 6, characterized in that: The sample placement area is a groove structure evenly arranged along the circumference of the hollow part of the pipeline, and the weightlessness corrosion hanging piece is embedded in the groove and is interference fit and / or adhesive fit with the groove.

8. The natural gas hydrate corrosion evaluation test device according to claim 1, characterized in that: The outer wall and the inner tank of the stirred reactor are both provided with transparent windows, and a high-definition camera and an LED auxiliary light source are provided outside the transparent window of the outer wall; the rotatable hanging piece is arranged at the end of the stirring blade; and a fifth pressure sensor and a fifth temperature sensor are provided in the stirred reactor.

9. The natural gas hydrate corrosion evaluation test device according to claim 1, characterized in that: The pure water in the natural gas hydrate is injected by a water injection pump, the natural gas is transported to the loop pipeline through a steel cylinder and the gas circulation is realized by a gas circulation pump; the natural gas hydrate slurry is circulated by a magnetic circulation pump.

10. The natural gas hydrate corrosion evaluation test device according to claim 1, characterized in that: An online particle size analyzer is arranged in the loop pipeline, which measures the particle size, morphology and content of the natural gas hydrate in real time through the reflection of the focused light beam; and a direct insertion density meter for online density analysis is also arranged in the loop pipeline.

11. The natural gas hydrate corrosion evaluation test device according to claim 1, characterized in that: A gas-liquid separator with a liquid level gauge is arranged in the loop pipeline.

12. The natural gas hydrate corrosion evaluation test device according to claim 6, characterized in that: A differential pressure sensor is arranged between the four pipe sections.

13. A corrosion evaluation test method for natural gas hydrate, characterized in that: The device according to any one of claims 1 to 12 comprises the following steps: Injecting pure water into the loop pipeline and allowing the pure water to reach a preset temperature; Introducing natural gas into the loop pipeline and pressurizing it to a preset pressure, and generating natural gas hydrate after a preset reaction time; After the natural gas hydrate slurry circulates stably in the loop pipeline, the rotatable hanging plate in the stirred reactor is driven to rotate; Online observing and recording the hydrate morphology of the natural gas hydrate slurry in the loop pipeline; The weightlessness corrosion hanging plate placed in the loop pipeline and the rotatable hanging plate in the stirred reactor are taken out, and the corrosion surface morphologies of the two are compared and observed and the corrosion rate is measured.

14. The corrosion evaluation test method for natural gas hydrate according to claim 13, characterized in that: The preset temperature of the pure water is 276.15 K to 281.15 K; the preset pressure of the natural gas is 5 to 10 Mpa; and the preset reaction time is 100 to 1000 minutes.

15. The corrosion evaluation test method of natural gas hydrate according to claim 13, characterized in that: The natural gas hydrate slurry is controlled to circulate stably in the loop pipeline by a magnetic circulation pump, and the flow rate is controlled in the range of 0.5 to 2 m / s.

16. The corrosion evaluation test method for natural gas hydrate according to any one of claims 13 to 15, characterized in that: By arranging four pipe sections in the loop pipeline, the corrosion conditions of different pipe sections at different temperatures, pressures, and different flow rates and forms of the natural gas hydrate slurry are tested respectively.

17. The corrosion evaluation test method of natural gas hydrate according to claim 16, characterized in that: A hydrate inhibitor or accelerator is injected into the loop pipeline through an injection unit; and the corrosion test results after adding the hydrate inhibitor or accelerator are compared and analyzed with the corrosion test results in a pure water environment.