Polarizing film with adhesive layer
By using a binder layer containing (meth)acrylic polymer and ionic compounds in a liquid crystal display device, combined with an amide-based monomer, the problem of static electricity and malfunction in a humidified environment is solved, and the problem of static electricity and malfunction of the liquid crystal display device is realized. Stable antistatic function and high sensitivity.
Patent Information
- Application Number
- CN202210298396.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2015-09-29
- Filing Date
- 2016-09-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2036-09-20
AI Technical Summary
The existing liquid crystal display devices with touch sensing function have serious problems in the humidified environment of static electricity generation and malfunction, resulting in uneven static electricity and reduced sensitivity of the touch panel.
Using an adhesive layer containing (meth)acrylic polymer and ionic compounds, the first and second polarization films are arranged on the visible side of the liquid crystal cell, and an amide-containing monomer is introduced into the adhesive layer. , improve the surface resistance value stability and compatibility of the adhesive layer, and prevent segregation of ionic compounds.
It effectively suppresses the generation and malfunction of static electricity, maintains the anti-static function of the LCD panel, improves the sensitivity and durability of the touch panel, and performs well in humidified environments.
Smart Images

Figure CN114609824B_ABST
Abstract
Description
[0001] The present application is a divisional application of an application filed on September 20, 2016, with application number 201680056807.4 and invention name “LIQUID CRYSTAL PANEL AND LIQUID CRYSTAL DISPLAY DEVICE WITH TOUCH SENSING FUNCTION”. Technical Field
[0002] The present invention relates to a liquid crystal panel and a liquid crystal display device with a touch sensing function. The liquid crystal display device with a touch sensing function of the present invention can be used as various input display devices such as mobile devices. Background Art
[0003] Liquid crystal display devices usually adhere polarizing films from both sides of the liquid crystal unit through adhesive layers according to their image formation method. In addition, products that mount touch panels on the display screen of liquid crystal display devices have also been put into practical use. As touch panels, there are various methods such as capacitive, resistive film, optical, ultrasonic or electromagnetic induction, but capacitive is beginning to be widely used. In recent years, liquid crystal display devices with touch sensing functions that have built-in capacitive sensors as touch sensor parts have been used.
[0004] On the other hand, when manufacturing a liquid crystal display device, when the polarizing film with an adhesive layer is attached to a liquid crystal cell, a release film is peeled off from the adhesive layer of the polarizing film with an adhesive layer, but static electricity is generated due to the peeling of the release film. The static electricity generated in this way affects the orientation of the liquid crystal layer inside the liquid crystal display device, resulting in defects. The generation of static electricity can be suppressed by, for example, forming an antistatic layer on the outer surface of the polarizing film.
[0005] On the other hand, the capacitive sensor in a liquid crystal display device with a touch sensing function detects the weak capacitance formed between the transparent electrode pattern and the finger when the user's finger approaches the surface. When there is a conductive layer such as an antistatic layer between the transparent electrode pattern and the user's finger, the electric field between the drive electrode and the sensor electrode is disturbed, the sensor electrode capacitance becomes unstable, and the sensitivity of the touch panel is reduced, which becomes a cause of malfunction. In a liquid crystal display device with a touch sensing function, it is required to suppress the malfunction of the capacitive sensor while suppressing the generation of static electricity. For example, in order to reduce the occurrence of poor display and malfunction in a liquid crystal display device with a touch sensing function, it is proposed to configure a liquid crystal layer with a surface resistance of 1.0×10 9 ~1.0×10 11 A polarizing film having an antistatic layer of Ω / □ (Patent Document 1).
[0006] In addition, an optical film adhesive having an antistatic function has been proposed for the purpose of preventing unevenness of a liquid crystal panel, adhesion of foreign matter, and the like caused by static electricity.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2013-105154 Summary of the invention
[0010] Problems to be solved by the invention
[0011] The polarizing film having an antistatic layer described in Patent Document 1 can suppress static electricity generation to a certain extent. However, in Patent Document 1, since the antistatic layer is arranged at a position different from the original position where static electricity is generated, it is not as effective as imparting an antistatic function to the adhesive layer.
[0012] In addition, compared with the antistatic layer provided on the above-mentioned polarizing film, the adhesive layer containing an ionic compound is effective in suppressing the generation of static electricity and preventing static unevenness. However, it is known that the antistatic function of the adhesive layer containing an ionic compound deteriorates over time. In particular, it is known that in a humidified environment (after a humidification reliability test), the ionic compound in the adhesive layer segregates at the interface with the optical film (polarizing film) or transfers to the optical film (polarizing film), and the surface resistance value of the adhesive layer becomes larger, and the antistatic function is significantly reduced. It is known that the reduction in the antistatic function of such an adhesive layer has become the main cause of the generation of static unevenness and malfunction of a liquid crystal display device with a touch sensing function.
[0013] The object of the present invention is to provide a liquid crystal panel with a touch sensing function, wherein an optical film is bonded to the visible side of a liquid crystal unit with a built-in touch sensing function through an adhesive layer containing an ionic compound, and a stable antistatic function can be achieved even in a humidified environment. In addition, the object of the present invention is to provide a liquid crystal display device using the above liquid crystal panel.
[0014] Solutions to the problem
[0015] The present inventors have conducted intensive studies to solve the above problems, and as a result, have found that the above problems can be solved by the following liquid crystal panel with a touch sensing function, thereby completing the present invention.
[0016] That is, the present invention relates to a liquid crystal panel with a built-in touch sensing function, which has:
[0017] A liquid crystal cell having a liquid crystal layer and a touch sensor portion with a built-in touch sensing function;
[0018] A first polarizing film disposed on the visible side of the liquid crystal cell and a second polarizing film disposed on the opposite side of the visible side; and
[0019] a first adhesive layer disposed between the first polarizing film and the liquid crystal cell,
[0020] The first adhesive layer is formed of an adhesive composition comprising a (meth)acrylic polymer (A) and an ionic compound (B), wherein the (meth)acrylic polymer (A) comprises an alkyl (meth)acrylate (a1) and an amide group-containing monomer (a2) as monomer units, and
[0021] The first adhesive layer satisfies: the variation ratio of the surface resistance value (b / a) ≤ 5,
[0022] Among them, a first polarizing film with an adhesive layer is prepared in which the first adhesive layer is provided on the first polarizing film, and a diaphragm is provided on the first adhesive layer. The above-mentioned a represents the surface resistance value of the first adhesive layer when the diaphragm is peeled off immediately after the first polarizing film with an adhesive layer is prepared, and the above-mentioned b represents the surface resistance value of the first adhesive layer when the diaphragm is peeled off after the first polarizing film with an adhesive layer is placed in a humidified environment of 60°C / 95%RH for 250 hours and further dried at 40°C for 1 hour.
[0023] In the above liquid crystal panel with built-in touch sensor function, it is preferred that the above amide group-containing monomer (a2) is an N-vinyl lactam-containing monomer.
[0024] In the liquid crystal panel with a built-in touch sensor function, the (meth)acrylic polymer (A) preferably contains 0.1 wt % or more of the amide group-containing monomer (a2) as a monomer unit.
[0025] In the liquid crystal panel with built-in touch sensor function, the ionic compound (B) is preferably an alkali metal salt, and preferably contains 0.01 parts by weight or more of the ionic compound (B) based on 100 parts by weight of the (meth)acrylic polymer (A).
[0026] The liquid crystal panel with built-in touch sensor function can be suitably used in a case where the touch sensor portion is in direct contact with the first adhesive layer.
[0027] In addition, the present invention relates to a liquid crystal display device having the above-mentioned liquid crystal panel with a built-in touch sensing function.
[0028] Effects of the Invention
[0029] In the panel with built-in touch sensing function of the present invention, the first adhesive layer provided between the liquid crystal unit containing the touch sensor part and the first polarizing film arranged on the visible side of the liquid crystal unit is formed by a (meth) acrylic polymer (A) and an ionic compound (B), wherein the (meth) acrylic polymer (A) contains an amide group-containing monomer (a2) as a monomer unit. The first adhesive layer contains the ionic compound (B), which can reduce the surface resistance value of the first adhesive layer and suppress the generation of static electricity.
[0030] In addition, there is an amide group introduced into the side chain of the (meth) acrylic polymer (A) as the base polymer in the first adhesive layer. Due to the presence of the amide group, even in a humidified environment, the surface resistance value of the first adhesive layer adjusted by the coordination of the ionic compound (B) can be suppressed from changing and becoming larger, and can be maintained within the range of the desired value. It can be considered that due to the presence of the amide group of the side chain introduced into the (meth) acrylic polymer (A) as a comonomer, the compatibility of the (meth) acrylic polymer (A) and the ionic compound (B) is improved. As a result, even in a humidified environment, the segregation and movement of the ionic compound (B) in the first adhesive layer to the interface of the polarizing film can be suppressed, and the first adhesive layer can keep the surface resistance value within the range of the desired value. It can be considered that according to the liquid crystal panel with a touch sensing function having such a first adhesive layer of the present invention, the unevenness caused by static electricity can be suppressed, and the occurrence of malfunctions can be suppressed, and the sensitivity of the touch panel can be suppressed. The liquid crystal panel with a touch sensor function of the present invention is particularly suitable when an in-cell liquid crystal cell or an on-cell liquid crystal cell is used as a liquid crystal cell with a built-in touch sensor function.
[0031] In addition, the adhesive layer has an amide group introduced into the side chain of the (meth) acrylic polymer (A) as the base polymer, so it has good durability against both glass and transparent conductive layer (ITO layer, etc.), and can suppress peeling, warping, etc. when attached to a liquid crystal panel. In addition, even in a humidified environment (after a humidified reliability test), it can also meet the durability requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a cross-sectional view showing an example of a liquid crystal panel with a touch sensor function according to the present invention.
[0033] Figure 2 This is a cross-sectional view showing an example of a liquid crystal panel with a touch sensor function according to the present invention.
[0034] Figure 3 This is a cross-sectional view showing an example of a liquid crystal panel with a touch sensor function according to the present invention.
[0035] Explanation of symbols
[0036] 11, 12 First and second polarizing films
[0037] 21, 22 first and second adhesive layers
[0038] 3 Liquid crystal layer
[0039] 41, 42 first and second transparent substrates
[0040] 5 Touch sensor part
[0041] 6 Driving electrode and sensor part
[0042] 7. Driving Electrode
[0043] C Liquid crystal unit DETAILED DESCRIPTION
[0044] The liquid crystal panel with built-in touch sensing function of the present invention is described with reference to the accompanying drawings. The liquid crystal panel with built-in touch sensing function of the present invention has: a liquid crystal unit C having a liquid crystal layer 3 and a touch sensor portion 5; a first polarizing film 11 arranged on the visible side of the liquid crystal unit C and a second polarizing film 12 arranged on the opposite side of the visible side; and a first adhesive layer 21 arranged between the first polarizing film 11 and the liquid crystal unit C. The above-mentioned components of the liquid crystal panel with built-in touch sensing function of the present invention can be simply represented as first polarizing film 11 / first adhesive layer 21 / liquid crystal unit C / second polarizing film 12 from the visible side. In the above-mentioned liquid crystal panel with built-in touch sensing function, the order of each component is simply shown, but other components can also be appropriately provided between each component.
[0045] A specific example of a liquid crystal panel with a built-in touch sensor function of the present invention is shown in, for example Figures 1 to 3 .
[0046] Figure 1 It is a so-called embedded type liquid crystal panel with built-in touch sensing function, and has a structure of first polarizing film 11 / first adhesive layer 21 / first transparent substrate 41 / touch sensor part 5 / liquid crystal layer 3 / driving electrode and sensor part 6 / second transparent substrate 42 / second adhesive layer 22 / second polarizing film 12 from the visible side. Figure 1 In an embedded type liquid crystal panel with a built-in touch sensing function, for example, a liquid crystal unit C has a touch sensor portion 5 and a drive electrode and sensor portion 6 in a first glass substrate and a second glass substrate 41 and 42 sandwiching a liquid crystal layer 3 (inside the liquid crystal unit).
[0047] in addition, Figure 2It is a modified example of a so-called embedded type (semi-embedded type) liquid crystal panel with a built-in touch sensing function, and has a structure of first polarizing film 11 / first adhesive layer 21 / touch sensor unit 5 / first transparent substrate 41 / liquid crystal layer 3 / driving electrode and sensor unit 6 / second transparent substrate 42 / second adhesive layer 22 / second polarizing film 12 from the visible side. Figure 2 In an embedded liquid crystal panel with a built-in touch sensing function, for example, the touch sensor portion 5 of the liquid crystal unit C is in direct contact with the first adhesive layer 21 on the outside of the first transparent substrate 41, and has a driving electrode and sensor portion 6 on one side of the second transparent substrate 42 within the first glass substrate and the second glass substrates 41 and 42 (inside the liquid crystal unit) that clamp the liquid crystal layer 3.
[0048] in addition, Figure 3 It is a so-called external embedded type liquid crystal panel with built-in touch sensing function, and has a structure of first polarizing film 11 / first adhesive layer 21 / touch sensor unit 5 / driving electrode and sensor unit 6 / first transparent substrate 41 / liquid crystal layer 3 / driving electrode 7 / second transparent substrate 42 / / second adhesive layer 22 / second polarizing film 12 from the visible side. Figure 3 In an externally embedded liquid crystal panel with a built-in touch sensing function, for example, a liquid crystal unit C has a touch sensor portion 5 and a drive electrode and sensor portion 6 on the outside of a first transparent substrate 41, the touch sensor portion 5 is in direct contact with the first adhesive layer 21, and has a drive electrode 7 on one side of a second transparent substrate 42 within the first glass substrate and the second glass substrates 41 and 42 (inside the liquid crystal unit) that clamp the liquid crystal layer 3.
[0049] In the liquid crystal panel with built-in touch sensor function, when the touch sensor part 5 of the above-mentioned liquid crystal unit C is in direct contact with the first adhesive layer 21, the antistatic function of the first adhesive layer 21 (containing an ionic compound) is easily reduced, especially in a humid environment. Therefore, in the above-mentioned example, the liquid crystal panel with built-in touch sensor function of the present invention is suitably applicable to Figure 2 The embedded type (variation) shown or Figure 3 The following is an on-cell type LCD panel with built-in touch sensor function.
[0050] The first polarizing film 11 and the second polarizing film 12 are usually polarizing films having transparent protective films on one or both sides of a polarizer. The first polarizing film 11 and the second polarizing film 12 are arranged on both sides of the liquid crystal layer 3 so that the transmission axes (or absorption axes) are orthogonal.
[0051] There is no particular limitation on the polarizer, and various polarizers can be used. Examples of the polarizer include: polarizers obtained by adsorbing dichroic materials such as iodine and dichroic dyes on hydrophilic polymer films such as polyvinyl alcohol films, partially formalized polyvinyl alcohol films, and partially saponified films of ethylene-vinyl acetate copolymers, and then uniaxially stretching them; polyene oriented films such as dehydrated products of polyvinyl alcohol and dehydrochlorinated products of polyvinyl chloride, etc. Among them, polarizers containing dichroic materials such as polyvinyl alcohol films and iodine are preferred. There is no particular limitation on the thickness of these polarizers, but it is generally about 80 μm or less.
[0052] In addition, as a polarizer, a thin polarizer with a thickness of 10 μm or less can be used. From the viewpoint of thinning, the thickness is preferably 1 to 7 μm. Such a thin polarizer has less uneven thickness, excellent visual recognition, and less dimensional change, so it has excellent durability, and the thickness of the polarizing film can also be thinned, which is preferred in this respect.
[0053] As the material constituting the transparent protective film, for example, a thermoplastic resin having excellent transparency, mechanical strength, thermal stability, moisture barrier property, isotropy, etc. can be used. Specific examples of such thermoplastic resins include: cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (such as norbornene resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. It should be noted that a transparent protective film can be attached to one side of the polarizer through an adhesive layer, and a thermosetting resin or ultraviolet curing resin such as (meth)acrylic, urethane, acrylic urethane, epoxy, silicone, etc. can be used as a transparent protective film on the other side.
[0054] As the material of the above-mentioned transparent protective film, cellulose resin and (meth) acrylic resin are preferred because they can control the above-mentioned variation ratio (b / a) of the surface resistance value of the first adhesive layer provided on the transparent protective film to a smaller level. In particular, (meth) acrylic resin is preferred in that the above-mentioned variation ratio (b / a) of the surface resistance value of the first adhesive layer can be controlled to a smaller level compared to cellulose resin. It should be noted that as a (meth) acrylic resin, a (meth) acrylic resin having a lactam ring structure is preferably used. As a (meth) acrylic resin having a lactam ring structure, the (meth) acrylic resin having a lactam ring structure described in Japanese Patent Publication No. 2000-230016, Japanese Patent Publication No. 2001-151814, Japanese Patent Publication No. 2002-120326, Japanese Patent Publication No. 2002-254544, Japanese Patent Publication No. 2005-146084, etc. can be cited.
[0055] A functional layer such as a hard coat layer, an antireflection layer, an anti-sticking layer, a diffusion layer, an anti-glare layer, etc. may be provided on the side of the transparent protective film to which the polarizer is not bonded.
[0056] The adhesive used in laminating the polarizer and the transparent protective film is not particularly limited as long as it is optically transparent. Various forms of adhesives such as water-based, solvent-based, hot melt, free radical curing, and cation curing can be used, and water-based adhesives or free radical curing adhesives are preferred.
[0057] It should be noted that the first polarizing film 11 disposed on the visible side of the liquid crystal unit C and the second polarizing film 12 disposed on the opposite side of the above-mentioned visible side can be used after being laminated with other optical films according to the adaptability of their respective configuration positions. As the above-mentioned other optical films, for example, reflective plates, anti-transmission plates, phase difference films (including 1 / 2 wave plates, 1 / 4 wave plates, etc.), visual compensation films, brightness enhancement films, etc., which are optical films that are sometimes used as optical layers in the formation of liquid crystal display devices, etc., can be listed. These other optical films can be used in one layer or two or more layers. When using these other optical films, it is also preferred that the adhesive layer on the side closest to the liquid crystal layer 3 is used as the above-mentioned first adhesive layer 21.
[0058] The first adhesive layer 21 is formed of an adhesive composition containing a (meth)acrylic polymer (A) and an ionic compound (B), wherein the (meth)acrylic polymer (A) contains an alkyl (meth)acrylate (a1) and an amide group-containing monomer (a2) as monomer units. The details of the adhesive composition will be described later.
[0059] The second adhesive layer 22 is formed by an adhesive. As the adhesive, various adhesives can be used, for example: rubber adhesives, acrylic adhesives, silicone adhesives, urethane adhesives, vinyl alkyl ether adhesives, polyvinyl pyrrolidone adhesives, polyacrylamide adhesives, cellulose adhesives, etc. The adhesive base polymer is selected according to the type of the above adhesive. Among the above adhesives, acrylic adhesives are preferably used from the perspective of excellent optical transparency, suitable adhesive properties such as wettability, cohesion and adhesion, weather resistance, heat resistance, etc. There is no special restriction on the thickness of the second adhesive layer 22, for example, it is about 1 to 100 μm. Preferably, it is 2 to 50 μm, more preferably 2 to 40 μm, and further preferably 5 to 35 μm.
[0060] The liquid crystal layer 3 of the liquid crystal unit C uses a liquid crystal layer suitable for a liquid crystal panel with a built-in touch sensing function, which contains liquid crystal molecules uniformly oriented in the absence of an electric field. As the liquid crystal layer 3, it is preferred to use a liquid crystal layer of, for example, an IPS mode. In addition, as the liquid crystal layer 3, any type of liquid crystal layer such as a TN type, STN type, π type, VA type, etc. can be used. The thickness of the above-mentioned liquid crystal layer is, for example, about 1.5μm to 4μm.
[0061] In the liquid crystal cell C, the first transparent substrate 41 and the second transparent substrate 42 can sandwich the liquid crystal layer 3 to form a liquid crystal cell. According to the form of the liquid crystal panel with a built-in touch sensing function, the touch sensor unit 5, the drive electrode and sensor unit 6, the drive electrode 7, etc. are formed inside or outside the liquid crystal cell. In addition, a color filter substrate can be provided on the liquid crystal cell (the first transparent substrate 41).
[0062] The material forming the transparent substrate may be, for example, glass or a polymer film. Examples of the polymer film include polyethylene terephthalate, polycycloolefin, polycarbonate, etc. When the transparent substrate is formed of glass, its thickness is, for example, about 0.3 mm to 1 mm. When the transparent substrate is formed of a polymer film, its thickness is, for example, about 10 μm to 200 μm. The transparent substrate may have an easy-adhesion layer or a hard coating layer on its surface.
[0063] The touch sensor unit 5 (capacitive sensor), the driving electrode and sensor unit 6, and the driving electrode 7 are formed in the form of a transparent conductive layer. As the constituent material of the above-mentioned transparent conductive layer, there is no special limitation, and examples thereof include metals such as gold, silver, copper, platinum, palladium, aluminum, nickel, chromium, titanium, iron, cobalt, tin, magnesium, tungsten, and alloys of these metals. In addition, as the constituent material of the above-mentioned transparent conductive layer, metal oxides of indium, tin, zinc, potassium, antimony, zirconium, and cadmium can be listed, and specifically, metal oxides composed of indium oxide, tin oxide, titanium oxide, cadmium oxide, and mixtures thereof can be listed. In addition, other metal compounds composed of copper iodide and the like are used. As needed, the above-mentioned metal oxides may further contain oxides of the metal atoms shown in the above group. For example, it is preferred to use indium oxide (ITO) containing tin oxide, tin oxide containing antimony, and the like, and ITO is particularly preferred. As ITO, it is preferred to contain 80 to 99% by weight of indium oxide and 1 to 20% by weight of tin oxide.
[0064] There is no limitation on the position of the touch sensor layer 5 in the liquid crystal unit C, and the touch sensor layer 5 can be formed according to the form of the liquid crystal panel with a built-in touch sensing function. Figures 1 to 3In the figure, an example is given in which the touch sensor layer 5 is arranged between the first polarizing film 11 and the liquid crystal layer 3. The touch sensor layer 5 can be formed, for example, in the form of a transparent electrode pattern on the first transparent substrate 41. For the driving electrode and sensor portion 6 and the driving electrode 7, a transparent electrode pattern can also be formed according to the form of a liquid crystal panel with a built-in touch sensing function in a conventional manner. The above-mentioned transparent electrode pattern is usually electrically connected to a lead wire (not shown) formed at the end of the transparent substrate, and the above-mentioned lead wire is connected to a controller IC (not shown). In addition to a comb shape, the shape of the transparent electrode pattern can be any shape such as a stripe shape, a diamond shape, etc. according to the application. The height of the transparent electrode pattern is, for example, 10nm to 100nm, and the width is 0.1mm to 5mm.
[0065] In addition, a liquid crystal panel with a built-in touch sensor function can be suitably used as a member for forming a liquid crystal display device, such as a member using a backlight or a reflector in a lighting system.
[0066] The adhesive composition forming the first adhesive layer 21 is described below. The adhesive composition contains a (meth) acrylic polymer (A) and an ionic compound (B), and the (meth) acrylic polymer (A) contains an alkyl (meth) acrylate (a1) and an amide group-containing monomer (a2). It should be noted that (meth) acrylate refers to acrylate and / or methacrylate, which has the same meaning as (meth) in the present invention.
[0067] The (meth)acrylic polymer (A) contains a (meth)acrylic acid alkyl ester (a1) as a monomer unit as a main component. As the (meth)acrylic acid alkyl ester constituting the main skeleton of the (meth)acrylic polymer, there can be exemplified a (meth)acrylic acid alkyl ester having a linear or branched alkyl carbon number of 1 to 18. For example, as the above-mentioned alkyl group, there can be cited a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a pentyl group, a hexyl group, a cyclohexyl group, a heptyl group, a 2-ethylhexyl group, an isooctyl group, a nonyl group, a decyl group, an isodecyl group, a dodecyl group, an isotetradecyl group, a lauryl group, a tridecyl group, a pentadecyl group, a hexadecyl group, a heptadecanyl group, an octadecyl group, etc. They can be used alone or in combination. The average carbon number of these alkyl groups is preferably 3 to 9.
[0068] In terms of monomer units, the weight ratio of the alkyl (meth)acrylate (a1) is preferably 70% by weight or more in the weight ratio of all the constituent monomers (100% by weight) constituting the (meth)acrylic polymer (A). The weight ratio of the alkyl (meth)acrylate (a1) can be considered to be the remainder of the amide group-containing monomer (a2) and other copolymerizable monomers. It is preferable to set the weight ratio of the alkyl (meth)acrylate (a1) to the above range in terms of ensuring adhesion.
[0069] The amide group-containing monomer (a2) is a compound containing an amide group in its structure and containing a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Specific examples of the amide group-containing monomer (a2) include acrylamide monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropylacrylamide, N-methyl(meth)acrylamide, N-butyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-hydroxymethyl(meth)acrylamide, N-hydroxymethyl-N-propyl(meth)acrylamide, aminomethyl(meth)acrylamide, aminoethyl(meth)acrylamide, mercaptomethyl(meth)acrylamide, and mercaptoethyl(meth)acrylamide; N-acryloyl heterocyclic monomers such as N-(meth)acryloylmorpholine, N-(meth)acryloylpiperidine, and N-(meth)acryloylpyrrolidine; and N-vinyl lactam-containing monomers such as N-vinylpyrrolidone and N-vinyl-ε-caprolactam. The amide-containing monomer (a2) is preferred in terms of suppressing the increase of the surface resistance value over time (especially in a humidified environment) and satisfying the durability. In particular, among the amide-containing monomers (a2), the N-vinyl lactam-containing monomers are preferred in terms of suppressing the increase of the surface resistance value over time (especially in a humidified environment) and satisfying the durability of the transparent conductive layer (touch sensor layer). It should be noted that, although not exemplified above, the amide-containing monomers having a hydroxyl group tend to have improved conductivity when combined with an ionic compound (B). In addition, when the proportion of the amide-containing monomers having a hydroxyl group is increased, there are problems with the anchoring force with the polarizing film (optical film) and the reoperation (repeeling, rework) of the transparent conductive layer (touch sensor layer), so it is preferably not used.
[0070] From the viewpoint of suppressing the increase of the surface resistance value over time (especially in a humidified environment), the weight ratio of the amide group-containing monomer (a2) is preferably 0.1% by weight or more. The weight ratio is preferably 0.3% by weight or more, and more preferably 0.5% by weight or more. On the other hand, when the weight ratio becomes too large, there is a tendency for the anchoring property to the substrate film such as the polarizing film to decrease, and therefore, the weight ratio is preferably 35% by weight or less, more preferably 30% by weight or less, and more preferably 25% by weight or less.
[0071] In addition to the above monomer units, one or more comonomers having a polymerizable functional group having an unsaturated double bond such as a (meth)acryloyl group or a vinyl group may be introduced into the (meth)acrylic polymer (A) by copolymerization for the purpose of improving adhesion and heat resistance.
[0072] As the above-mentioned comonomer, for example, (meth)acrylate containing an aromatic ring can be used. (Meth)acrylate containing an aromatic ring is a compound containing an aromatic ring structure and a (meth)acryloyl group in its structure. Examples of the aromatic ring include a benzene ring, a naphthalene ring, or a biphenyl ring.
[0073] Specific examples of the (meth)acrylate containing an aromatic ring include benzyl (meth)acrylate, phenyl (meth)acrylate, o-phenylphenol (meth)acrylate, phenoxy (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypropyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, ethylene oxide-modified nonylphenol (meth)acrylate, ethylene oxide-modified cresol (meth)acrylate, phenol ethylene oxide-modified (meth)acrylate, 2-(meth)acrylate. (Meth)acrylates having a benzene ring, such as -hydroxy-3-phenoxypropyl, methoxybenzyl (meth)acrylate, chlorobenzyl (meth)acrylate, toluene (meth)acrylate, and polystyrene (meth)acrylate; (meth)acrylates having a naphthalene ring, such as hydroxyethylated β-naphthol acrylate, 2-naphthylethyl (meth)acrylate, 2-naphthyloxyethyl acrylate, and 2-(4-methoxy-1-naphthyloxy)ethyl (meth)acrylate; (meth)acrylates having a biphenyl ring, such as biphenyl (meth)acrylate.
[0074] As the (meth)acrylate containing an aromatic ring, benzyl (meth)acrylate and phenoxyethyl (meth)acrylate are preferred from the viewpoint of adhesive properties and durability, and phenoxyethyl (meth)acrylate is particularly preferred.
[0075] The weight ratio of the (meth)acrylate containing an aromatic ring is preferably 25% by weight or less, more preferably 3 to 25% by weight, further preferably 8 to 22% by weight, and further preferably 12 to 18% by weight. When the weight ratio of the (meth)acrylate containing an aromatic ring is 3% by weight or more, it is preferred in terms of suppressing uneven display. On the other hand, when it is greater than 25% by weight, the suppression of uneven display is insufficient, and there is a tendency for durability to decrease.
[0076] Moreover, as said copolymerization monomer, a carboxyl group-containing monomer and a hydroxyl group-containing monomer are mentioned.
[0077] The carboxyl group-containing monomer is a compound containing a carbonyl group in its structure and containing polymerizable unsaturated double bonds such as (meth)acryloyl and vinyl groups. Specific examples of carboxyl group-containing monomers include (meth)acrylic acid, (meth)carboxyethyl acrylate, (meth)carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, etc. Among the above-mentioned carboxyl group-containing monomers, acrylic acid is preferred from the viewpoints of copolymerizability, price and adhesive properties.
[0078] The hydroxyl-containing monomer is a compound containing a hydroxyl group in its structure and containing polymerizable unsaturated double bonds such as (meth)acryloyl and vinyl groups. Specific examples of hydroxyl-containing monomers include: 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate and other hydroxyalkyl (meth)acrylates, (4-hydroxymethylcyclohexyl)methyl acrylate, etc. Among the above-mentioned hydroxyl-containing monomers, 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are preferred from the aspect of durability, and 4-hydroxybutyl (meth)acrylate is particularly preferred.
[0079] When the adhesive composition contains a crosslinking agent, the carboxyl-containing monomer and the hydroxyl-containing monomer become the reaction points with the crosslinking agent. Since the reactivity of the carboxyl-containing monomer and the hydroxyl-containing monomer with the intermolecular crosslinking agent is high, they are preferably used in order to improve the cohesiveness and heat resistance of the obtained adhesive layer. In addition, the carboxyl-containing monomer is preferred in terms of durability and reoperability, and the hydroxyl-containing monomer is preferred in terms of reoperability.
[0080] The above-mentioned weight ratio of carboxyl-containing monomer is preferably below 2 weight %, more preferably 0.01~2 weight %, further preferably 0.05~1.5 weight %, further preferably 0.1~1 weight %, most preferably 0.1~0.5 weight %. The weight ratio of carboxyl-containing monomer is set to 0.01 weight % or more in terms of durability. On the other hand, when greater than 2 weight %, it is not preferred from the aspect of reoperability.
[0081] The weight ratio of the hydroxyl-containing monomer is preferably 3% by weight or less, more preferably 0.01 to 3% by weight, further preferably 0.1 to 2% by weight, and further more preferably 0.2 to 2% by weight. From the perspective of crosslinking the adhesive layer, durability, and adhesive properties, the weight ratio of the hydroxyl-containing monomer is preferably set to 0.01% by weight or more. On the other hand, when it is greater than 3% by weight, it is not preferred from the perspective of durability.
[0082] Specific examples of other copolymer monomers other than the above include: anhydride group-containing monomers such as maleic anhydride and itaconic anhydride; caprolactone adducts of acrylic acid; sulfonic acid group-containing monomers such as allyl sulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, and (meth)acrylate sulfopropyl ester; phosphate group-containing monomers such as 2-hydroxyethylacryloyl phosphate, etc.
[0083] Examples of monomers for modification include: alkylaminoalkyl (meth)acrylates such as aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and tert-butylaminoethyl (meth)acrylate; alkoxyalkyl (meth)acrylates such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexam ... Succinimide monomers such as (methyl) acryloyl-8-oxyoctamethylene succinimide; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-laurylitaconimide.
[0084] In addition, as the modifying monomer, vinyl monomers such as vinyl acetate and vinyl propionate; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate; glycol (meth)acrylates such as polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate; acrylate monomers such as tetrahydrofurfuryl (meth)acrylate, fluorine-containing (meth)acrylate, silicone (meth)acrylate, 2-methoxyethyl acrylate, etc. can also be used. In addition, isoprene, butadiene, isobutylene, vinyl ether, etc. can be cited.
[0085] In addition, as copolymerizable monomers other than the above, silane monomers containing silicon atoms can be cited. As silane monomers, for example, 3-acryloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 4-vinylbutyltrimethoxysilane, 4-vinylbutyltriethoxysilane, 8-vinyloctyltrimethoxysilane, 8-vinyloctyltriethoxysilane, 10-methacryloxydecyltrimethoxysilane, 10-acryloxydecyltrimethoxysilane, 10-methacryloxydecyltriethoxysilane, 10-acryloxydecyltriethoxysilane, etc. can be cited.
[0086] In addition, as the comonomer, a polyfunctional monomer having two or more unsaturated double bonds such as (meth)acrylic acid or vinyl groups, such as esters of (meth)acrylic acid and polyols such as tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, caprolactone-modified dipentaerythritol hexa(meth)acrylate, and polyester (meth)acrylates, epoxy (meth)acrylates, urethane (meth)acrylates, and the like in which two or more unsaturated double bonds such as (meth)acryloyl groups or vinyl groups are added to the skeleton of polyester, epoxy, urethane, and the like as the same functional groups as the monomer components can be used.
[0087] The ratio of the other copolymerizable monomers in the (meth)acrylic polymer (A) is preferably about 0 to 10% by weight, more preferably about 0 to 7%, and even more preferably about 0 to 5% based on the weight ratio of all monomers constituting the (meth)acrylic polymer (A) (100% by weight).
[0088] The weight average molecular weight of the (meth) acrylic polymer (A) of the present invention is generally preferably 1 million to 2.5 million. If durability, especially heat resistance, is taken into consideration, the weight average molecular weight is preferably 1.2 million to 2 million. When the weight average molecular weight is 1 million or more, it is preferred in terms of heat resistance. In addition, when the weight average molecular weight is greater than 2.5 million, there is a tendency for the adhesive to harden easily and peeling occurs easily. In addition, the weight average molecular weight (Mw) / number average molecular weight (Mn) representing the molecular weight distribution is preferably 1.8 or more and 10 or less, more preferably 1.8 to 7, and further preferably 1.8 to 5. When the molecular weight distribution (Mw / Mn) is greater than 10, it is not preferred in terms of durability. It should be noted that the weight average molecular weight and the molecular weight distribution (Mw / Mn) are determined by GPC (gel permeation chromatography) and calculated by polystyrene conversion.
[0089] Such (meth)acrylic polymer (A) can be produced by appropriately selecting known production methods such as solution polymerization, bulk polymerization, emulsion polymerization, various radical polymerizations, etc. The obtained (meth)acrylic polymer (A) may be any copolymer such as a random copolymer, a block copolymer, or a graft copolymer.
[0090] It should be noted that in solution polymerization, as a polymerization solvent, for example, ethyl acetate, toluene, etc. can be used. As a specific solution polymerization example, the reaction is carried out under a stream of an inert gas such as nitrogen, with a polymerization initiator added, usually at about 50 to 70° C. for about 5 to 30 hours.
[0091] The polymerization initiator, chain transfer agent, emulsifier, etc. used in the free radical polymerization are not particularly limited and can be appropriately selected for use. It should be noted that the weight average molecular weight of the (meth)acrylic polymer (A) can be controlled by the amount of the polymerization initiator, the amount of the chain transfer agent, the reaction conditions, etc., and their amounts can be appropriately adjusted according to their types.
[0092] The adhesive composition of the present invention contains an ionic compound (B). As the ionic compound (B), an alkali metal salt and / or an organic cation-anion salt can be preferably used. Alkali metal salts can use organic salts and inorganic salts of alkali metals. It should be noted that the "organic cation-anion salt" mentioned in the present invention refers to an organic salt whose cation part is composed of an organic substance, and the anion part can be an organic substance or an inorganic substance. "Organic cation-anion salt" is also called an ionic liquid or an ionic solid.
[0093] <Alkali Metal Salt>
[0094] Examples of the alkali metal ions constituting the cation portion of the alkali metal salt include ions of lithium, sodium, potassium, etc. Among these alkali metal ions, lithium ions are preferred.
[0095] The anion part of the alkali metal salt may be composed of an organic substance or an inorganic substance. Examples of the anion part constituting the organic salt include: CH 3 COO - CF 3 COO - , CH 3 SO 3 - CF 3 SO 3 - ,(CF 3 SO 2 ) 3 C - , C 4 F 9 SO 3 - , C 3 F 7 COO - ,(CF 3 SO 2 )(CF 3 CO)N - ,- O 3 S(CF 2 ) 3 SO 3 - PF 6 - , CO 3 2- , anions represented by the following general formulas (1) to (4), etc.
[0096] (1): (C n F 2n+1 SO 2 ) 2 N - (where n is an integer from 1 to 10),
[0097] (2) CF 2 (C m F 2m SO 2 ) 2 N - (wherein m is an integer from 1 to 10),
[0098] (3): - O 3 S(CF 2 ) l SO 3 - (wherein l is an integer from 1 to 10),
[0099] (4): (C p F 2p+1 SO 2 )N - (C q F 2q+1 SO 2 )(wherein p and q are integers from 1 to 10).
[0100] In particular, the anion part containing fluorine atoms is preferably used because it can obtain an ionic compound with good ionization. As the anion part constituting the inorganic salt, Cl - Br - ,I - 、AlCl 4 - 、Al 2 Cl 7 - , BF 4 - PF 6 - , ClO 4 - 、NO 3- , AsF 6 - , SbF 6 - ,NbF 6 - 、TaF 6 - 、(CN) 2 N - As the anion part, preferably (CF 3 SO 2 ) 2 N - , (C 2 F 5 SO 2 ) 2 N - The (perfluoroalkylsulfonyl)imide represented by the above general formula (1) is particularly preferably (CF 3 SO 2 ) 2 N - The trifluoromethanesulfonyl imide shown.
[0101] Specific examples of organic salts of alkali metals include sodium acetate, sodium alginate, sodium lignin sulfonate, sodium toluene sulfonate, LiCF 3 SO 3 、Li(CF 3 SO 2 ) 2 N、Li(CF 3 SO 2 ) 2 N、Li(C 2 F 5 SO 2 ) 2 N、Li(C 4 F 9 SO 2 ) 2 N、Li(CF 3 SO 2 ) 3 C. KO 3 S(CF 2 ) 3 SO 3 K、LiO 3 S(CF 2 ) 3 SO 3 K, etc. Among these, LiCF 3 SO 3 、Li(CF 3 SO 2 ) 2 N、Li(C2 F 5 SO 2 ) 2 N、Li(C 4 F 9 SO 2 ) 2 N、Li(CF 3 SO 2 ) 3 C, etc., more preferably Li(CF 3 SO 2 ) 2 N、Li(C 2 F 5 SO 2 ) 2 N、Li(C 4 F 9 SO 2 ) 2 Fluorine-containing imide lithium salts in the form of bis(fluorosulfonyl)imide lithium salts such as N, etc., are particularly preferably (perfluoroalkylsulfonyl)imide lithium salts. In addition, 4,4,5,5-tetrafluoro-1,3,2-dithiazolidine-1,1,3,3-tetraoxide lithium salts and the like are exemplified.
[0102] In addition, examples of inorganic salts of alkali metals include lithium perchlorate and lithium iodide.
[0103] <Organic cation-anion salt>
[0104] The organic cation-anion salt used in the present invention is composed of a cation component and an anion component, wherein the cation component is composed of an organic substance. Specific examples of the cation component include: pyridine Cation, piperidine Cation, pyrrolidine Cation, cation having a pyrroline skeleton, cation having a pyrrole skeleton, imidazole Cation, Tetrahydropyrimidine Cation, dihydropyrimidine Cation, pyrazole Cationic, pyrazoline Cations, tetraalkylammonium cations, trialkylsulfonium cations, tetraalkyl Cations, etc.
[0105] Examples of the anion component include Cl - Br - ,I - 、AlCl 4 - 、Al 2 Cl 7 - , BF 4- PF 6 - , ClO 4 - 、NO 3 - , CH 3 COO - CF 3 COO - , CH 3 SO 3 - CF 3 SO 3 - ,(CF 3 SO 2 ) 3 C - , AsF 6 - , SbF 6 - ,NbF 6 - 、TaF 6 - 、(CN) 2 N - , C 4 F 9 SO 3 - , C 3 F 7 COO - ,(CF 3 SO 2 )(CF 3 CO)N - , - O 3 S(CF 2 ) 3 SO 3 - , anions represented by the following general formulas (1) to (4), etc.
[0106] (1): (C n F 2n+1 SO 2 ) 2 N - (where n is an integer from 1 to 10),
[0107] (2) CF 2 (C m F 2m SO 2 ) 2 N - (wherein m is an integer from 1 to 10),
[0108] (3): - O 3 S(CF 2 ) l SO 3 - (wherein l is an integer from 1 to 10),
[0109] (4): (C p F 2p+1 SO 2 )N - (C q F 2q+1 SO 2 ), (wherein p and q are integers from 1 to 10).
[0110] Among them, an anion component containing a fluorine atom is particularly preferably used because it can obtain an ionic compound with good ionization property.
[0111] The organic cation-anion salt is preferably selected from a compound composed of the above-mentioned combination of the cation component and the anion component. Preferred specific examples of the organic cation-anion salt include methyl trioctylammonium bis(trifluoromethanesulfonyl)imide, 1-methyl-1-propylpyrrolidine Bis(trifluoromethanesulfonyl)imide, ethylmethylimidazole Among them, 1-methyl-1-propylpyrrolidine is more preferred. Bis(trifluoromethanesulfonyl)imide, ethylmethylimidazole Bis(fluorosulfonyl imide).
[0112] Examples of the ionic compound (B) include inorganic salts such as ammonium chloride, aluminum chloride, cupric chloride, ferrous chloride, ferric chloride, and ammonium sulfate, in addition to the above-mentioned alkali metal salts and organic cation-anion salts.
[0113] In order to obtain a desired resistance value, the above-mentioned ionic compound (B) can be used alone or in combination of two or more. In particular, the surface resistance value of the adhesive layer is controlled to be 1×10 10 ~1×10 12 When the range of Ω / □ is the goal, the ionic compound (B) is preferably an alkali metal salt from the perspective of improving antistatic performance. By using an alkali metal salt, an adhesive with high antistatic performance can be obtained even if the amount of the alkali metal salt is small. On the other hand, when the surface resistance value of the adhesive layer is controlled to 1×10 8 ~1×10 10When the range of Ω / □ is the purpose, as the above-mentioned ionic compound (B), organic cation-anion salts are preferred from the perspective of improving antistatic performance. By using organic cation-anion salts, a binder with high antistatic performance can be obtained even if the amount of the organic cation-anion salts is small.
[0114] The proportion of the ionic compound (B) in the adhesive composition of the present invention can be appropriately adjusted so as to satisfy the antistatic properties of the adhesive layer and the sensitivity of the touch panel. For example, it is preferred to consider the weight ratio of the amide group-containing monomer (a2) introduced into the (meth)acrylic polymer (A), the type of the transparent protective film of the polarizing film, etc., and adjust the proportion of the ionic compound (B) according to the type of the liquid crystal panel with built-in touch sensing function so that the surface resistance value of the adhesive layer is 1.0×10 8 ~1.0×10 12 Ω / □ range. For example, Figure 1 In the in-cell type liquid crystal panel with built-in touch sensor function, the surface resistance value of the first adhesive layer is preferably controlled to 1×10 8 ~1×10 10 In the range of Ω / □. Figure 2 Semi-embedded type, or Figure 3 In the external cell type liquid crystal panel with built-in touch sensor function shown in FIG. 1 , the surface resistance value of the first adhesive layer is preferably controlled to 1×10 10 ~1×10 12 Ω / □ range.
[0115] In addition, the first adhesive layer is controlled to satisfy a variation ratio (b / a) of surface resistance value ≤ 5. A first polarizing film with an adhesive layer is prepared in which the first adhesive layer is provided on the first polarizing film and a diaphragm is provided on the first adhesive layer. The a represents the surface resistance value of the first adhesive layer when the diaphragm is peeled off immediately after the first polarizing film with an adhesive layer is prepared, and the b represents the surface resistance value of the first adhesive layer when the diaphragm is peeled off after the first polarizing film with an adhesive layer is placed in a humidified environment of 60°C / 95%RH for 250 hours and further dried at 40°C for 1 hour. When the variation ratio (b / a) is greater than 5, the antistatic function of the adhesive layer in a humidified environment is reduced. The variation ratio (b / a) is preferably 5 or less, more preferably 3.5 or less, more preferably 2.5 or less, more preferably 2 or less, and most preferably 1.5 or less.
[0116] Relative to 100 parts by weight of (meth) acrylic polymer (A), the proportion of the above-mentioned ionic compound (B) is preferably used, for example, 0.01 parts by weight or more. By using 0.01 parts by weight or more of the above-mentioned ionic compound (B), it is preferred in terms of improving antistatic performance. From this viewpoint, the above-mentioned ionic compound (B) is preferably 0.1 parts by weight or more, and more preferably 0.5 parts by weight or more. On the other hand, when the above-mentioned ionic compound (B) increases, the surface resistance value becomes too low, and there is a hidden danger of reduced sensitivity of the touch panel due to baseline fluctuations (misoperation during touch caused by too low surface resistance value). In addition, when the above-mentioned ionic compound (B) increases, there is the possibility of precipitation of the ionic compound (B), and it becomes easy to humidify and peel. From this viewpoint, the above-mentioned ionic compound (B) is usually preferably 40 parts by weight or less, more preferably 30 parts by weight or less, further preferably 20 parts by weight or less, and most preferably 10 parts by weight or less.
[0117] The adhesive composition of the present invention may contain a crosslinking agent (C). As the crosslinking agent (C), an organic crosslinking agent or a polyfunctional metal chelate may be used. As the organic crosslinking agent, isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, imine crosslinking agents, etc. may be cited. A polyfunctional metal chelate is a chelate formed by covalent bonding or coordination bonding of a polyvalent metal to an organic compound. As polyvalent metal atoms, Al, Cr, Zr, Co, Cu, Fe, Ni, V, Zn, In, Ca, Mg, Mn, Y, Ce, Sr, Ba, Mo, La, Sn, Ti, etc. may be cited. As atoms in organic compounds that are covalently bonded or coordinately bonded, oxygen atoms, etc. may be cited, and as organic compounds, alkyl esters, alcohol compounds, carboxylic acid compounds, ether compounds, ketone compounds, etc. may be cited.
[0118] As the crosslinking agent (C), an isocyanate crosslinking agent and / or a peroxide crosslinking agent is preferred.
[0119] As the isocyanate crosslinking agent (C), a compound having at least two isocyanate groups can be used, for example, a known aliphatic polyisocyanate, alicyclic polyisocyanate, aromatic polyisocyanate, etc., which are generally used in urethanization reactions.
[0120] As a peroxide, any peroxide that generates free radical active species by heating or light irradiation and crosslinks the base polymer of the adhesive composition can be used appropriately, but considering the operability and stability, it is preferred to use a peroxide with a 1-minute half-life temperature of 80°C to 160°C, and it is more preferred to use a peroxide with a 1-minute half-life temperature of 90°C to 140°C.
[0121] Examples of peroxides that can be used include di(2-ethylhexyl) peroxydicarbonate (1-minute half-life temperature: 90.6° C.), di(4-tert-butylcyclohexyl) peroxydicarbonate (1-minute half-life temperature: 92.1° C.), di-sec-butyl peroxydicarbonate (1-minute half-life temperature: 92.4° C.), tert-butyl peroxyneodecanoate (1-minute half-life temperature: 103.5° C.), tert-hexyl peroxypivalate (1-minute half-life temperature: 109.1° C.), tert-butyl peroxypivalate (1-minute half-life temperature: 110.3° C.), dilauroyl peroxide (1 minute half-life temperature: 116.4℃), dioctanoyl peroxide (1 minute half-life temperature: 117.4℃), 1,1,3,3-tetramethylbutyl peroxide-2-ethylhexanoate (1 minute half-life temperature: 124.3℃), di(4-methylbenzoyl) peroxide (1 minute half-life temperature: 128.2℃), dibenzoyl peroxide (1 minute half-life temperature: 130.0℃), tert-butyl peroxyisobutyrate (1 minute half-life temperature: 136.1℃), 1,1-di(tert-hexylperoxide)cyclohexane (1 minute half-life temperature: 149.2℃), etc. Among them, di(4-tert-butylcyclohexyl) peroxydicarbonate (1 minute half-life temperature: 92.1°C), dilauroyl peroxide (1 minute half-life temperature: 116.4°C), dibenzoyl peroxide (1 minute half-life temperature: 130.0°C), etc. are preferably used because of their particularly excellent cross-linking reaction efficiency.
[0122] The amount of the crosslinking agent (C) used is preferably 3 parts by weight or less, more preferably 0.01 to 3 parts by weight, further preferably 0.02 to 2 parts by weight, and further preferably 0.03 to 1 part by weight relative to 100 parts by weight of the (meth)acrylic polymer (A). It should be noted that when the amount of the crosslinking agent (C) is less than 0.01 parts by weight, there is a risk that the crosslinking of the adhesive layer is insufficient and the durability and adhesive properties cannot be satisfied. On the other hand, when the amount is more than 3 parts by weight, there is a tendency that the adhesive layer becomes too hard and the durability decreases.
[0123] The adhesive composition of the present invention may contain a silane coupling agent (D). By using a silane coupling agent (D), durability can be improved. Specific examples of the silane coupling agent include epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylene)propylamine, and N-phenyl-γ-aminopropyltrimethoxysilane; (meth)acrylic group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane; and isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane. As the silane coupling agent exemplified above, an epoxy group-containing silane coupling agent is preferable.
[0124] In addition, as a silane coupling agent (D), a silane coupling agent having multiple alkoxysilyl groups in the molecule can also be used. Specifically, for example, X-41-1053, X-41-1059A, X-41-1056, X-41-1805, X-41-1818, X-41-1810, X-40-2651, etc. manufactured by Shin-Etsu Chemical Co., Ltd. can be cited. These silane coupling agents having multiple alkoxysilyl groups in the molecule are not easy to volatilize, and are effective in improving durability due to having multiple alkoxysilyl groups, so they are preferred. In particular, when the adherend of the optical film with an adhesive layer is a transparent conductive layer (such as ITO, etc.) in which the alkoxysilyl group is less reactive than glass, the durability is also suitable. In addition, the silane coupling agent having multiple alkoxysilyl groups in the molecule is preferably one having an epoxy group in the molecule, and more preferably one having multiple epoxy groups in the molecule. Silane coupling agents having multiple alkoxysilyl groups and epoxy groups in the molecule tend to have good durability even when the adherend is a transparent conductive layer (such as ITO, etc.). Specific examples of silane coupling agents having multiple alkoxysilyl groups and epoxy groups in the molecule include X-41-1053, X-41-1059A, and X-41-1056 manufactured by Shin-Etsu Chemical Co., Ltd., and X-41-1056 manufactured by Shin-Etsu Chemical Co., Ltd. having a high epoxy group content is particularly preferred.
[0125] The silane coupling agent (D) may be used alone or in combination of two or more thereof. The total content of the silane coupling agent (D) is preferably 5 parts by weight or less, more preferably 0.001 to 5 parts by weight, further preferably 0.01 to 1 part by weight, further preferably 0.02 to 1 part by weight, and further preferably 0.05 to 0.6 part by weight, based on 100 parts by weight of the (meth)acrylic polymer (A). This is an amount that improves durability.
[0126] The adhesive composition of the present invention may contain a polyether compound (E) having a reactive silyl group. The polyether compound (E) is preferred because it can improve reworkability. The polyether compound (E) may be a polyether compound disclosed in Japanese Patent Application Laid-Open No. 2010-275522.
[0127] The proportion of the polyether compound (E) in the adhesive composition of the present invention is preferably 10 parts by weight or less, preferably 0.001 to 10 parts by weight, relative to 100 parts by weight of the (meth)acrylic polymer (A). When the above-mentioned polyether compound (E) is less than 0.001 parts by weight, there is a case where the effect of improving reoperability is insufficient. The above-mentioned polyether compound (E) is preferably 0.01 parts by weight or more, and more preferably 0.1 parts by weight or more. On the other hand, when the above-mentioned polyether compound (E) is more than 10 parts by weight, it is not preferred in terms of durability. The above-mentioned polyether compound (E) is preferably 5 parts by weight or less, and more preferably 2 parts by weight or less. The proportion of the above-mentioned polyether compound (E) can be set to a preferred range using the above-mentioned upper limit or lower limit.
[0128] In addition, other known additives may be contained in the adhesive composition of the present invention, for example, polyether compounds such as polyalkylene glycols such as polypropylene glycol, colorants, powders such as pigments, dyes, surfactants, plasticizers, tackifiers, surface lubricants, leveling agents, softeners, antioxidants, anti-aging agents, light stabilizers, ultraviolet absorbers, polymerization inhibitors, inorganic or organic fillers, metal powders, granular, foil-like objects, etc. may be appropriately added according to the intended use. In addition, redox agents that add reducing agents may also be used within a controllable range. These additives are preferably used in an amount of 5 parts by weight or less, more preferably 3 parts by weight or less, and further preferably 1 part by weight or less relative to 100 parts by weight of the (meth) acrylic polymer (A).
[0129] The first pressure-sensitive adhesive layer 21 of the present invention can be used as a pressure-sensitive adhesive layer-attached optical film to be bonded to an optical film (polarizing film). The pressure-sensitive adhesive layer-attached optical film can be obtained by forming a pressure-sensitive adhesive layer on at least one surface of an optical film using the pressure-sensitive adhesive composition.
[0130] As a method for forming an adhesive layer, the adhesive layer can be prepared by the following methods, for example, the adhesive composition is applied to a separator treated with peeling, etc., and after drying to remove the polymerization solvent, etc. to form an adhesive layer, the adhesive layer is transferred to an optical film (polarizing film); or the adhesive composition is applied to an optical film (polarizing film), and the polymerization solvent is dried to remove the adhesive layer on the optical film, etc. It should be noted that when applying the adhesive, one or more solvents other than the polymerization solvent may be newly added.
[0131] The thickness of the first adhesive layer 21 is not particularly limited, and is, for example, about 1 to 100 μm, preferably 2 to 50 μm, more preferably 2 to 40 μm, and further preferably 5 to 35 μm.
[0132] Example
[0133] The present invention is specifically described below by way of examples, but the present invention is not limited to these examples. It should be noted that the parts and % in each example are all weight basis. In the following, the room temperature storage conditions not specifically specified are all 23° C. and 65% RH.
[0134] <Measurement of Weight Average Molecular Weight of (Meth)Acrylic Polymer (A)>
[0135] The weight average molecular weight (Mw) of the (meth)acrylic polymer (A) was measured by GPC (gel permeation chromatography). Mw / Mn was measured in the same manner.
[0136] Analytical device: HLC-8120GPC manufactured by Tosoh Corporation
[0137] ·Pillar: Made by Tosoh Corporation, G7000HXL+GMHXL+GMHXL
[0138] · Pillar size: 7.8mmφ×30cm each, total 90cm
[0139] Column temperature: 40℃
[0140] Flow rate: 0.8mL / min
[0141] Injection volume: 100μL
[0142] ·Eluent: Tetrahydrofuran
[0143] Detector: Differential Refractometer (RI)
[0144] Standard sample: polystyrene
[0145] <Production of Polarizing Film P1>
[0146] A polyvinyl alcohol film with a thickness of 80 μm was dyed for 1 minute and stretched to 3 times in an iodine solution with a concentration of 0.3% at 30°C between rollers with different speed ratios. Then, it was stretched to a total stretch ratio of 6 times while being immersed in a 60°C aqueous solution containing 4% boric acid and 10% potassium iodide for 0.5 minutes. Next, it was washed by immersing in a 30°C aqueous solution containing 1.5% potassium iodide for 10 seconds, and then dried at 50°C for 4 minutes to obtain a polarizer with a thickness of 30 μm. A (meth) acrylic resin film with a lactam ring structure with a thickness of 20 μm and corona treatment was bonded to both sides of the polarizer with a polyvinyl alcohol adhesive as a transparent protective film to produce a polarizing film P1.
[0147] <Production of Polarizing Film P2>
[0148] Polarizing film P2 was obtained by the same method as that of producing polarizing film P1, except that a saponified triacetyl cellulose film having a thickness of 80 μm was used as the transparent protective film.
[0149] Example 1
[0150] (Preparation of acrylic polymer (A))
[0151] A monomer mixture containing 75.8 parts of butyl acrylate, 23 parts of phenoxyethyl acrylate, 0.5 parts of N-vinyl-2-pyrrolidone (NVP), 0.3 parts of acrylic acid, and 0.4 parts of 4-hydroxybutyl acrylate was added to a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube, and a condenser. Furthermore, 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator was added together with 100 parts of ethyl acetate to 100 parts of the above monomer mixture (solid content), and nitrogen was introduced while slowly stirring to replace the nitrogen atmosphere. The liquid temperature in the flask was maintained at about 55°C, and a polymerization reaction was performed for 8 hours to prepare a solution of an acrylic polymer (A) having a weight average molecular weight (Mw) of 1.6 million and Mw / Mn=3.7.
[0152] (Preparation of Adhesive Composition)
[0153] With respect to 100 parts of the solid content of the solution of the acrylic polymer (A1) obtained in Production Example 1, 0.1 parts of lithium bis(trifluoromethanesulfonyl)imide (Li-TFSI) manufactured by Mitsubishi Materials Corporation as an ionic compound, 0.1 parts of an isocyanate crosslinking agent (Takenate D160N manufactured by Mitsui Chemicals, Inc., trimethylolpropane hexamethylene diisocyanate), 0.3 parts of benzoyl peroxide (Nyper BMT manufactured by NOF Corporation) and 0.3 parts of an epoxy group-containing silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd.: X-41-1056) were added to prepare a solution of an acrylic adhesive composition.
[0154] (Production of Polarizing Film with Adhesive Layer)
[0155] Next, the solution of the acrylic adhesive composition was applied to one side of a polyethylene terephthalate film (separator: manufactured by Mitsubishi Chemical Polyester Film Co., Ltd., MRF38) treated with a silicone release agent so that the thickness of the adhesive layer after drying was 20 μm, and dried at 155° C. for 1 minute to form an adhesive layer on the surface of the separator. Next, the adhesive layer formed on the separator was transferred to the polarizing film P1 prepared above to prepare a polarizing film with an adhesive layer.
[0156] Examples 2 to 14, Comparative Examples 1 to 6
[0157] In Example 1, the amount of N-vinyl-2-pyrrolidone (NVP) used in the monomer mixture for preparing the acrylic polymer (A), the type (Li-TFSI or MPP-TFSI) or the mixing ratio of the ionic compound used in preparing the adhesive composition, and the type of polarizing film were changed as shown in Table 1. The same operation as in Example 1 was performed to prepare an acrylic polymer solution and an acrylic adhesive composition solution. In addition, the same operation as in Example 1 was performed using the acrylic adhesive composition solution to prepare a polarizing film with an adhesive layer.
[0158] The polarizing films with adhesive layers obtained in the above-mentioned embodiments and comparative examples were evaluated as follows. The evaluation results are shown in Table 1. It should be noted that in each evaluation, "initial" refers to the value measured immediately after the polarizing film with adhesive layer is produced, and "after humidification" refers to the value measured after the obtained polarizing film with adhesive layer is placed in a humidified environment of 60°C / 95%RH for 250 hours and further dried at 40°C for 1 hour.
[0159] <Surface resistance (Ω / □): Conductivity>
[0160] After peeling the separator from the polarizing film with the adhesive layer, the surface resistance value of the adhesive layer surface was measured. The measurement was carried out using MCP-HT450 manufactured by Mitsubishi Chemical Analytech Co., Ltd.
[0161] It should be noted that the change ratio (b / a) in Table 1 is a value calculated from the surface resistance value (a) of "initial" and the surface resistance value (b) of "after humidification" (rounded off to the second decimal place).
[0162] In addition, as an index with less risk of "malfunction", values with a smaller change ratio were preferably evaluated according to the following criteria.
[0163] ◎: The change ratio is 2 or less.
[0164] ○: The change ratio is greater than 2 and less than 5.
[0165] ×: The change ratio is 5 or more.
[0166] <ESD Test>
[0167] After peeling the separator from the polarizing film with the adhesive layer, it was attached to the visible side of the external type liquid crystal cell or the internal type liquid crystal cell as shown in Table 1, and a liquid crystal panel with a built-in touch sensing function was fabricated. That is, the polarizing films with the adhesive layer obtained in Examples 1 to 3, 6 to 10, 14, and Comparative Examples 1 to 6 were attached to Figure 3 the sensor layer (touch sensor part) of the external type liquid crystal cell shown, and the first adhesive layer and the first polarizing film were formed. The polarizing films with the adhesive layer obtained in Examples 4, 5, 11 to 13 were attached to Figure 1 the first transparent substrate of the internal type liquid crystal cell shown, and the first adhesive layer and the first polarizing film were formed. An ESD (electrostatic discharge) gun (10 kV) was applied to the polarizing film surface of the above liquid crystal panel, and the time until the electrically induced white spot portion disappeared was measured, and judgment was made according to the following criteria.
[0168] (Evaluation Criteria)
[0169] ◎: Within 3 seconds.
[0170] ○: Greater than 3 seconds and within 10 seconds.
[0171] ×: Greater than 10 seconds.
[0172]
[0173] In Table 1, Li-TFSI represents lithium bis(trifluoromethanesulfonyl)imide, and MPP-TFSI represents 1-methyl-1-propylpyrrolidine manufactured by Toyo Gosei Co., Ltd. Bis(trifluoromethanesulfonyl)imide.
[0174] As shown in Table 1, it can be seen from the description of the Examples and Comparative Examples that by adding an ionic compound to an acrylic polymer, even when the initial surface resistance value of the adhesive layer is set to a low level, in the Examples, since the acrylic polymer has an amide group-containing monomer as a monomer unit, the change ratio of the surface resistance value of the adhesive layer after humidification is 5 or less, and the increase in the surface resistance value is suppressed. That is, in the Examples, since the change ratio of the surface resistance value of the adhesive layer is small, the surface resistance value can be maintained within the desired range even after humidification, and the sensitivity of the touch panel can be well maintained. In addition, the ESD test is good and static unevenness can be suppressed.
Claims
1. A polarizing film with an adhesive layer, comprising an adhesive layer, The adhesive layer is formed of an adhesive composition containing a (meth)acrylic polymer (A) and an ionic compound (B), wherein the (meth)acrylic polymer (A) contains an alkyl (meth)acrylate (a1) and an amide group-containing monomer (a2) as monomer units, and The (meth)acrylic polymer (A) contains 0.5 to 25% by weight of the amide group-containing monomer (a2) as a monomer unit, The ionic compound (B) is an organic cation-anion salt, The amide group-containing monomer (a2) is selected from acrylamide monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropylacrylamide, N-methyl(meth)acrylamide, N-butyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-hydroxymethyl(meth)acrylamide, N-hydroxymethyl-N-propyl(meth)acrylamide, aminomethyl(meth)acrylamide, aminoethyl(meth)acrylamide, mercaptomethyl(meth)acrylamide, mercaptoethyl(meth)acrylamide; and at least one selected from N-(meth)acryloylmorpholine, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-vinylpyrrolidone, and N-vinyl-ε-caprolactam. The ionic compound (B) is contained in an amount of 0.01 to 13 parts by weight relative to 100 parts by weight of the (meth)acrylic polymer (A). The surface resistance of the adhesive layer is 1.0×10 8 Ω / □ or more and 1.0×10 10 Ω / □ or less, The adhesive layer satisfies: the variation ratio of the surface resistance value (b / a) ≤ 5, In the formula, a polarizing film with an adhesive layer is prepared in a state in which the adhesive layer is provided on the polarizing film and a diaphragm is provided on the adhesive layer. a represents the surface resistance value of the adhesive layer when the diaphragm is peeled off immediately after the polarizing film with an adhesive layer is prepared. b represents the surface resistance value of the adhesive layer when the diaphragm is peeled off after the polarizing film with an adhesive layer is placed in a humidified environment of 60°C / 95%RH for 250 hours and further dried at 40°C for 1 hour.
2. The polarizing film with an adhesive layer according to claim 1, in, The variation ratio (b / a) of the surface resistance value is 2 or less.
Citation Information
Patent Citations
Production and use of clear heat-resistant resin
JP2000230016A
Method of manufacturing for transparent heat resistant resin and use of the same
JP2001151814A
Transparent thermoplastic resin laminate
JP2002120326A
Thermoplastic resin laminate
JP2002254544A
Lactone ring-containing polymer, and its manufacturing method and application
JP2005146084A