Fiber reinforced composite materials and sandwich structures
By designing porous structural components in fiber reinforced composite materials, combining microporous and coarse hollows, the problem of lightweight and mechanical properties is solved, and a high-performance fiber reinforced composite material is achieved.
Patent Information
- Application Number
- CN202080082189.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-29
- Filing Date
- 2020-11-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-11-16
AI Technical Summary
While existing fiber-reinforced composite materials pursue lightweight, their mechanical properties often decrease significantly, making it difficult to achieve a balance between lightweight and mechanical properties at the same time.
Porous structural components, including resin and reinforced fibers, microporous with an average pore diameter of less than 500 μm was measured by mercury insulating method, and a large cavity was formed in the section opening, with a maximum length of more than 500 μm to achieve lightweight and mechanical properties. Take into account both.
A fiber-reinforced composite material with high levels of lightweight and mechanical properties is achieved, which improves the overall performance of the material and is suitable for a variety of application fields.
Smart Images

Figure CN114761212B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a fiber-reinforced composite material that achieves both lightness and mechanical properties. Background Art
[0002] Fiber-reinforced composite materials, which use thermosetting resins and thermoplastic resins as a matrix and are combined with reinforcing fibers such as carbon fibers and glass fibers, are used in a large number of fields such as aviation and aerospace, automobiles, railway vehicles, ships, civil engineering, electronic equipment, industrial machinery, and sporting goods because of their light weight and excellent mechanical properties such as strength and rigidity, flame retardancy, and corrosion resistance. On the other hand, from the perspective of improving fuel consumption and portability, as components and shells, further lightweighting is required, and porous fiber-reinforced composite materials with pores formed inside have also been developed. However, such porous fiber-reinforced composite materials have the following problems: the larger the proportion of pores is for the purpose of lightweighting, the more sharply the mechanical properties decrease. Therefore, a technology is required to lightweight fiber-reinforced composite materials and achieve mechanical properties at the same time.
[0003] As a technology for achieving both lightweight and mechanical properties of fiber-reinforced composite materials, Patent Document 1 discloses a composite structure having reinforcing fibers, resin, and pores, and having a protrusion for reinforcement. Patent Document 2 discloses a core structure composed of a cured resin and a non-woven sheet and having a serrated cross section. Patent Document 3 discloses a structure composed of paper containing carbon fibers of different diameter cross sections, and a core structure obtained by folding the above structure in a manner that the cross section becomes serrated.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2018 / 117181
[0007] Patent Document 2: Japanese Patent Application No. 2012-500864
[0008] Patent Document 3: Japanese Patent Application Publication No. 2013-511629. Summary of the invention
[0009] Problems to be solved by the invention
[0010] Patent Document 1 is a technology that achieves lightweighting by increasing the total amount of micropores, but there is a problem that the mechanical properties decrease significantly along with the lightweighting. In this document, reinforcing structures such as ribs and bosses are used, but they are reinforcing structures arranged on the surface of the composite structure, require specific molding molds, and there are problems in thinning the walls. In the methods described in Patent Documents 2 and 3, the resin is impregnated without controlling the diameter and amount of the pores. In addition, with respect to the serrated structure, it is easy for the serrated structure to open due to the load in the bending direction, which is not enough to achieve both lightweighting and mechanical properties. The purpose of the present invention is to provide a fiber-reinforced composite material that achieves both lightweighting and mechanical properties.
[0011] Means for solving problems
[0012] The present invention for solving the above-mentioned problems is a fiber-reinforced composite material, which comprises: a porous structure portion, which contains a resin (A) and reinforcing fibers (B) and has micropores with an average pore diameter of 500 μm or less as measured by mercury intrusion; and a coarse cavity portion, which is divided by the porous structure portion and has a maximum length of more than 500 μm as a cross-sectional opening.
[0013] Effects of the Invention
[0014] According to the present invention, it is possible to obtain a fiber-reinforced composite material that achieves both lightness and high-level mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] [ Figure 1 ] is a schematic diagram showing an embodiment of the fiber-reinforced composite material of the present invention.
[0016] [ Figure 2 ] is a schematic diagram enlarging the porous structure portion in one embodiment of the fiber-reinforced composite material of the present invention.
[0017] [ Figure 3 ] is a schematic cross-sectional view showing an embodiment of the fiber-reinforced composite material of the present invention.
[0018] [ Figure 4 ] is a schematic diagram for illustrating the folding angle of the reinforcing fiber substrate (B') in one embodiment of the prepreg.
[0019] [ Figure 5 ] is a schematic diagram showing the folded state of the reinforcing fiber substrate (B') in one embodiment of the prepreg.
[0020] [ Figure 6 ] is a cross-sectional schematic diagram showing an embodiment of a prepreg blank.
[0021] [ Figure 7 ] Figure 6 The schematic diagram of the cross section of a part of the prepreg of the embodiment shown is enlarged.
[0022] [ Figure 8 ] is a schematic diagram enlarging the periphery of the reinforcing fiber substrate (B') in one embodiment of the prepreg.
[0023] [ Fig. 9 ] is a schematic diagram showing the folded state of the reinforcing fiber substrate (B') in the prepreg produced in Example 1.
[0024] [ Fig.10 ] is a schematic diagram showing the folded state of the reinforcing fiber substrate (B') in the prepreg produced in Example 5.
[0025] [ Fig.11 ] is a schematic diagram showing an embodiment of the fiber-reinforced composite material produced in Comparative Example 3. DETAILED DESCRIPTION
[0026] <Fiber-reinforced composite materials>
[0027] The fiber-reinforced composite material of the present invention comprises: a porous structure portion, which comprises a resin (A) and reinforcing fibers (B) and has micropores having an average pore diameter of 500 μm or less as measured by mercury intrusion porosimetry; and a coarse cavity portion, which is divided by the porous structure portion and has a maximum length of a cross-sectional opening exceeding 500 μm.
[0028] Hereinafter, the fiber-reinforced composite material of the present invention will be described with reference to the accompanying drawings as appropriate, but the present invention is not limited to these drawings. However, as those skilled in the art will readily understand, the descriptions related to the embodiments described in the accompanying drawings can also function as descriptions related to the fiber-reinforced composite material of the present invention (which is a general concept).
[0029] Figure 1 This is a schematic diagram showing an embodiment of the fiber-reinforced composite material of the present invention together with an enlarged image of a porous structure. A coarse cavity 4 is shown divided by a porous structure 6, which is a space with a roughly triangular cross-section (defined as described below). As shown in the enlarged image, the porous structure 6 contains a resin (A) 2 and reinforcing fibers (B) 3. It should be noted that Figure 1 In the embodiment, the porous structure 6 also includes micropores 5.
[0030] Figure 3 for Figure 1 A schematic cross-sectional view of a fiber-reinforced composite material according to an embodiment of the present invention, taken along a cross section perpendicular to the direction in which the coarse cavity extends. Figure 2It is a schematic diagram of an embodiment of a porous structure part. It should be noted that in this specification, unless otherwise specified, the "cross section" of the fiber reinforced composite material refers to a cross section orthogonal to the extension direction of the coarse void part. That is, the coarse void part of the fiber reinforced composite material of the present invention is extended.
[0031] like Figure 1 As shown in FIG. 1 , the porous structure 6 includes reinforcing fibers (B) 3 and a resin (A) 2 as a matrix, and has a large number of micropores 5 in the resin (A). It should be noted that the porous structure does not need to have micropores throughout the entire structure, as long as micropores are formed in the region where the reinforcing fibers (B) exist. Figure 3 As shown in the figure, when there is a region containing only resin (A) 2 outside the region where the reinforcing fiber (B) exists, both are collectively referred to as a porous structural portion in this specification, but micropores may not be formed in the latter. That is, in this specification, in the fiber-reinforced composite material of the present invention, the structure forming the skeleton other than the coarse cavity portion is referred to as a porous structural portion.
[0032] like Figure 2 As shown, it is preferred that the porous structure is formed by impregnating the resin (A) between the reinforcing fibers (B), and the resin (A) between the reinforcing fibers (B) has micropores. By forming this structure, it is possible to achieve a lightweight as a porous body and to exert the reinforcing effect brought by the reinforcing fibers (B).
[0033] In the cross section of the fiber reinforced composite material, the opening of the macroscopic cavity and the porous structure surrounding the opening are observed. That is, the macroscopic cavity exists as a tunnel-like space surrounded by the porous structure.
[0034] The coarse cavity portion is a structure in which the average value of the maximum length of the cross-sectional opening portion exceeds 500 μm. Here, the maximum length of the cross-sectional opening portion refers to the maximum length that can be drawn in a straight line in the opening portion in the cross section of the fiber-reinforced composite material. When the average value of the maximum length of the opening portion exceeds 500 μm, a significant lightweight effect can be obtained. The average value of the maximum length of the cross-sectional opening portion of the coarse cavity portion is preferably greater than 1000 μm and less than 10000 μm, more preferably greater than 1500 μm and less than 6500 μm, and further preferably greater than 2500 μm and less than 4500 μm.
[0035] In this way, by having a structure in which a coarse cavity portion is surrounded and reinforced by a porous structure portion, and the micropores of the porous structure portion are reinforced by reinforcing fibers (B), it is possible to simultaneously achieve lightweighting due to an increase in the amount of pores and suppression of pore deformation, thereby achieving lightweighting and suppression of a decrease in mechanical properties at a high level.
[0036] Figure 3 In the illustrated embodiment, the opening of the large cavity portion is shown as a substantially triangle having three sides surrounded by the porous structure portion in cross section.
[0037] As described above, the coarse cavity portion of the present invention is surrounded by a porous structure portion, but even if the above-mentioned opening portion is a substantially trapezoidal cavity portion with three sides formed by a porous structure portion (i.e., a cavity portion with one side not surrounded), it can also be regarded as a coarse cavity portion of the present invention if it has a porous structure portion. The coarse cavity portion of the present invention is preferably surrounded by a porous structure portion.
[0038] The shape of the cross-sectional opening of the coarse cavity is not particularly limited, but is preferably a substantially polygonal shape or a substantially elliptical shape (including a substantially circular shape), and more preferably a substantially triangular shape or a substantially circular shape.
[0039] In the present invention, the resin (A) constituting the matrix of the porous structure portion may be a thermoplastic resin or a thermosetting resin, but is preferably a thermoplastic resin. When the resin (A) is a thermosetting resin, the heat resistance is excellent, but in the manufacturing method of the prepreg described later, if the resin (A) is cured, it is sometimes not ideal. The prepreg is formed by a resin (A) and a reinforcing fiber substrate (B') as a sheet-like reinforcing fiber (B). If the resin (A) is cured, the restoring force of the folded structure of the reinforcing fiber substrate (B') of the prepreg is sometimes not presented. By making the resin (A) a thermoplastic resin, the melting and softening of the resin (A) during the heat molding are stably carried out, and a fiber-reinforced composite material with excellent lightness can be obtained, so it is preferred.
[0040] Examples of the thermoplastic resin include polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyolefins such as polyethylene, polypropylene, polybutene, and modified polypropylene, polyoxymethylene, polyamide 6, and polyamide 66, polycarbonate, polymethyl methacrylate, polyvinyl chloride, polyarylene sulfide such as polyphenylene sulfide, polyphenylene ether, modified polyphenylene ether, polyimide, polyamide-imide, polyetherimide, polysulfone, modified polysulfone, polyethersulfone, polyketone, polyetherketone, polyetheretherketone, polyetherketoneketone, and polyarylene etherketone, polyarylate, polyethernitrile, and phenoxy resins. In addition, these thermoplastic resins may be copolymers, modified products, and / or resins obtained by blending two or more thereof.
[0041] Among these, the thermoplastic resin is more preferably at least one thermoplastic resin selected from the group consisting of polyolefin, polycarbonate, polyester, polyarylene sulfide, polyamide, polyoxymethylene, polyetherimide, polyethersulfone, and polyarylene ether ketone, from the viewpoint of the balance between molding processability and heat resistance and mechanical properties, and is more preferably polypropylene from the viewpoint of productivity and cost.
[0042] The resin (A) may contain other fillers and additives as appropriate within the scope of not impairing the purpose of the present invention, depending on the application, etc. For example, inorganic fillers, flame retardants, conductivity imparting agents, crystal nucleating agents, ultraviolet absorbers, antioxidants, damping agents, antibacterial agents, insect repellents, deodorants, anti-coloring agents, heat stabilizers, mold release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, foaming agents, coupling agents, etc. may be mentioned.
[0043] The melting point of the thermoplastic resin used as resin (A) is preferably 100°C to 400°C, more preferably 120°C to 300°C, and further preferably 140°C to 250°C. By making it in the above temperature range, it is possible to achieve both the molding processability to the fiber-reinforced composite material and the heat resistance of the obtained fiber-reinforced composite material, so it is preferred. In addition, the glass transition temperature of the thermoplastic resin used as resin (A) is preferably 0°C to 250°C, more preferably 50°C to 200°C, and further preferably 100°C to 160°C. In particular, when the resin (A) is an amorphous thermoplastic resin, by making the glass transition temperature of the thermoplastic resin in the above range, it is possible to achieve both the molding processability to the fiber-reinforced composite material and the heat resistance of the obtained fiber-reinforced composite material, so it is preferred.
[0044] Reinforcing fiber (B) can include carbon fiber, glass fiber, metal fiber, aromatic polyamide fiber, aramid fiber, aluminum oxide fiber, silicon carbide fiber, boron fiber, basalt fiber, etc. These can be used alone or in combination with two or more thereof. Among these, from the viewpoint of lightness and excellent mechanical properties, reinforcing fiber (B) is preferably carbon fiber. The elastic modulus of reinforcing fiber (B) is preferably more than 200GPa. In addition, as reinforcing fiber, carbon fiber is preferred, and particularly preferably carbon fiber with an elastic modulus of more than 200GPa.
[0045] In the present invention, the reinforcing fiber (B) is preferably a discontinuous fiber, more specifically, the number average fiber length is preferably 1 mm or more and 50 mm or less, and the number average fiber length is more preferably 3 mm or more and 20 mm or less, and further preferably 4 mm or more and 10 mm or less. By making it within the above range, it is easy to expand the interval between the reinforcing fibers (B) and the formation of micropores is easy to control, so it is preferred. In addition, in the porous structure, it is preferred that the discontinuous fibers are randomly dispersed. By making the discontinuous fibers randomly dispersed, the concentration unevenness of the resin (A) and the reinforcing fibers (B) becomes smaller, and a fiber-reinforced composite material with excellent isotropy can be obtained.
[0046] The porous structure has micropores having an average pore diameter of 500 μm or less as measured by mercury intrusion. The average pore diameter is preferably 200 μm or less, more preferably 10 μm or more and 150 μm or less, and further preferably 30 μm or more and 100 μm or less. If the average pore diameter is too small, the weight reduction effect is insufficient, and if it is too large, the mechanical properties are reduced.
[0047] Mercury intrusion porosimeter is a method for measuring pore diameter using a mercury intrusion porosimeter. Mercury is injected into a sample at high pressure, and the pore diameter can be determined from the applied pressure and the amount of mercury injected. The average pore diameter is a value that can be determined by the following formula (1).
[0048] (Average pore diameter)=4×(pore volume) / (specific surface area)···Formula (1).
[0049] In the present invention, the specific gravity of the porous structure is preferably 0.3 g / cm 3 Above, 0.8g / cm 3 Below, more preferably 0.4 g / cm 3 Above, 0.7g / cm 3 If the value is less than the above range, the mechanical properties may be reduced, and if it is greater than the above range, the weight reduction effect may be insufficient. The specific gravity here is the mass [g] of the sample obtained by cutting out only the porous structure part divided by the volume [cm 3 ] is the arithmetic mean of the specific gravity measured by 5 randomly selected samples.
[0050] The specific gravity of the fiber-reinforced composite material as a whole is preferably 0.001 g / cm 3 Above, 0.2g / cm 3 Below, more preferably 0.01 g / cm 3 Above, 0.15g / cm 3 Below, more preferably 0.01 g / cm 3 Above, 0.1g / cm 3 Below. When it is less than this range, the mechanical properties may become insufficient. When it is greater than this range, the weight reduction effect may become insufficient. Specific gravity is 0.1 g / cm 3 In the following cases, it is usually particularly difficult to exhibit mechanical properties, and the effect of the present invention can be effectively exerted, so it is preferred. The specific gravity here is the sample mass [g] divided by the volume [cm 3 ] and the value obtained.
[0051] In addition, in the fiber-reinforced composite material of the present invention, when the resin (A) is 100 parts by mass, the reinforcing fiber (B) is preferably 10 parts by mass or more and 100 parts by mass or less, and the reinforcing fiber (B) is more preferably 20 parts by mass or more and 50 parts by mass or less. When the amount is less than this range, the reinforcing effect brought by the reinforcing fiber (B) may be insufficient. When the amount is greater than this range, the weight reduction effect brought by the reinforcing fiber (B) may be insufficient.
[0052] The thickness of the fiber-reinforced composite material is preferably 0.1 mm or more and 5 mm or less, more preferably 0.6 mm or more and 3 mm or less. By making it within the above range, the effect of the present invention (i.e., light weight and excellent mechanical properties) can be effectively exerted even with a thin wall, so it is preferred. In particular, for fiber-reinforced composite materials with pores, there is a tendency to be difficult to maintain pressure in a process such as a pressing process in which other materials are crimped. The fiber-reinforced composite material of the present invention that achieves both light weight and mechanical properties by controlling the pores can also be appropriately used in such a crimping process, so it is preferred.
[0053] In addition, the fiber-reinforced composite material of the present invention preferably has a structure in which the openings of the coarse cavity in the cross section are arranged in the in-plane direction, and further, it can also have a laminated structure in which layers having such a structure are stacked in multiple layers. By having this laminated structure, it is easy to obtain a molded product with a thick wall or a thickness deviation, so it is preferred. In addition, it is more preferred to have a laminated structure in which the layers with the openings arranged in the in-plane direction are stacked while changing the extension direction of the coarse cavity in each layer, and it is further preferred to have a laminated structure in which the extension direction of the coarse cavity in each layer is orthogonal. In this case, in the description related to the fiber-reinforced composite material of the present invention described above, the content described using the extension direction of the coarse cavity should be understood as a description for each layer. As the number of layers, it is preferably more than 2 layers and less than 50 layers, and more preferably more than 2 layers and less than 10 layers.
[0054] There are no particular restrictions on the lamination method, and examples include a method of heating the prepreg after lamination and a method of laminating the fiber-reinforced composite material that has been preheated and molded. During lamination, there are no particular restrictions on the bonding between the layers, and examples include bonding using an adhesive, thermal fusion, etc. In particular, the fiber-reinforced composite material of the present invention, which has excellent expansion force as described later, is also excellent in the ability to maintain pores in the heating and pressurizing process during thermal fusion, and is therefore preferred.
[0055] <Sandwich structure>
[0056] The fiber-reinforced composite material of the present invention is also preferably made into a sandwich structure in which a skin layer formed of another fiber-reinforced resin is arranged on both sides. Preferably, the skin layer is a layer having a higher elastic modulus than the fiber-reinforced composite material. There is no particular limitation on the method of joining the skin layers, and examples thereof include joining with an adhesive, thermal fusion, etc. In particular, the fiber-reinforced composite material of the present invention, which has excellent expansion force described later, and its laminate are also excellent in the ability to maintain pores in the heating and pressurizing process during thermal fusion, so they are preferred.
[0057] The reinforcing fibers contained in the fiber-reinforced resin of the epidermis layer can preferably be the same fibers as the reinforcing fibers (B) mentioned above, and carbon fibers are preferred from the viewpoints of lightness, mechanical properties, and economy. As for the reinforcing fibers of the fiber-reinforced resin constituting the epidermis layer, the number average fiber length is preferably 100 mm or more, and more preferably 150 mm or more. There is no particular limit on the upper limit of the length of the reinforcing fibers, and the reinforcing fibers can be continuous within the entire epidermis layer in the fiber orientation direction, or they can be disconnected midway. It should be noted that, from the viewpoint of the mechanical properties of the sandwich structure, it is preferred that the continuous reinforcing fibers are arranged in a unidirectional manner. In addition, from the viewpoint of the isotropy of the mechanical properties, the epidermis layer is particularly preferably provided with the following structure: the fiber-reinforced resin layer in which the reinforcing fibers are arranged in a unidirectional manner is stacked with multiple layers while changing the stacking angle (i.e., while changing the arrangement direction of the reinforcing fibers of each layer).
[0058] In addition, the resin contained in the fiber-reinforced resin of the epidermis is preferably a thermosetting resin. As the thermosetting resin, for example, unsaturated polyester resin, vinyl ester resin, epoxy resin, phenolic resin, urea resin, melamine resin, thermosetting polyimide resin, cyanate resin, bismaleimide resin, benzoxazine resin, or their copolymers, modified products, and resins obtained by blending at least two of them. Among them, as the thermosetting resin, epoxy resin is preferred because of its excellent mechanical properties, heat resistance, and adhesion to reinforcing fibers.
[0059] <Method for producing fiber-reinforced composite material>
[0060] As an example, the fiber-reinforced composite material of the present invention can be manufactured by heating the following prepreg to a temperature above which the resin (A) melts or softens and molding it, wherein the prepreg is a prepreg formed by impregnating the resin (A) into a reinforcing fiber substrate (B') as a sheet-like reinforcing fiber (B), and the reinforcing fiber substrate (B') exists in a folded state with a plurality of folds having a folding angle of 0° or more and less than 90° in the prepreg. By folding the reinforcing fiber substrate (B') at a folding angle of 0° or more and less than 90°, the restoring force (i.e., the restoring force as a force in the direction of the folding angle expansion) that the folds want to stretch and return to the structure before folding is released, and in the molding of the prepreg into the fiber-reinforced composite material, the expansion force in the thickness direction of the prepreg can be obtained. It should be noted that the reinforcing fiber substrate (B') in the prepreg becomes the reinforcing fiber (B) in the fiber-reinforced composite material through the heating and molding.
[0061] The following is an explanation of such a prepreg. It should be noted that the folding angle in this specification refers to the cross section perpendicular to the fold direction (hereinafter, unless otherwise specified in this specification, the "cross section" of the prepreg refers to the cross section perpendicular to the fold direction.) Figure 4 As shown, it refers to the angle θ formed by the bending portion centered on the fold 31 of the reinforcing fiber substrate (B') 3. The folding angle of the reinforcing fiber substrate (B') is preferably 0° to 75°, more preferably 0° to 45°, further preferably 0° to 15°, and particularly preferably 1° to 5°. By making it within the above range, the expansion force in the molding of the fiber-reinforced composite material can be increased, so it is preferred.
[0062] In the cross section, when an arbitrarily selected fold is set as the first fold, when the two folds adjacent to the two sides of the first fold are counted as the second fold, the two folds further adjacent to the outside of the second fold are counted as the third fold, and the two folds further adjacent to the outside of the third fold are counted as the fourth fold, the reinforcing fiber substrate (B') is preferably folded in a form in which the first fold and at least one of the two folds of the nth (n is an integer greater than 4) fold are close. By folding in this way, when the fold is stretched, the area folded into the close folds is easy to form a space, and a coarse cavity is easy to form. It should be noted that in this specification, the term "close" is used as a term to express the concept that also includes the case of contact. In addition, in the following specification, the first fold close to each other in this form and the nth fold close to the first fold are sometimes referred to as "a pair of close folds".
[0063] In this case, when the linear distance between a pair of close folds in the cross section is Lr and the distance between a pair of close folds along the reinforcing fiber substrate (B') is Lf, it is preferred that Lr / Lf is 0.3 or less and Lf is 1 mm or more and 200 mm or less. Lr / Lf is more preferably 0.2 or less, and further preferably 0.05 or less. Lf is more preferably 1 mm or more and 100 mm or less, further preferably 2 mm or more and 50 mm or less, and particularly preferably 3 mm or more and 10 mm or less. By making it within the above range, it is easy to control the pore size when molding into a fiber-reinforced composite material, so it is preferred.
[0064] For easier understanding, the folded state of the reinforcing fiber substrate (B') will be described below with reference to the drawings specifically illustrating the folded state of the reinforcing fiber substrate (B'). The folded state of the reinforcing fiber substrate (B') is not limited to these drawings.
[0065] Figure 5 This is a perspective schematic diagram showing only the reinforcing fiber base material (B') taken out and illustrated in order to explain the folded state of the reinforcing fiber base material (B') in the prepreg in one embodiment. Figure 6 is a schematic cross-sectional view of a prepreg according to the same embodiment, Figure 7 It is a cross-sectional schematic diagram in which a part thereof is further enlarged.
[0066] In this embodiment, when an arbitrarily selected fold is set as the first fold in the cross section, the reinforcing fiber substrate (B') is in a folded state including a Z-shaped structure having one of the second folds adjacent to the first fold and the first fold as bending points. Figure 7 When the fold shown in 31A is set as the first fold, in the cross section, the reinforcing fiber substrate (B') is folded in a manner to form a Z-shaped structure with the first fold and one of the second folds adjacent to the first fold shown in 31B as bending points. By forming such a folded structure, a force that the Z-shaped structure wants to stretch up and down can be generated, and a large cavity portion is easily formed in the fiber-reinforced composite material. When the reinforcing fiber substrate (B') exists in such a Z-shaped structure in a continuous folded state, a large restoring force can be obtained as a whole.
[0067] More specifically, in the present embodiment, in a cross section, when a certain fold is set as the first fold, when two folds adjacent to both sides of the first fold are set as the second fold, two folds further adjacent to the outer side of the second fold are set as the third fold, and two folds further adjacent to the outer side of the third fold are set as the fourth fold, the reinforcing fiber substrate (B') has a bending structure including a roughly triangular structure, wherein the roughly triangular structure is formed by one of the fourth folds being close to the first fold. For example, Figure 7 When the fold shown in 31A is set as the first fold, one of the second folds becomes the fold shown in 31B, one of the third folds becomes the fold shown in 31C, and one of the fourth folds becomes the fold shown in 31D, the reinforcing fiber substrate (B') has a bending structure including a roughly triangular structure, and the roughly triangular structure is formed by the first fold 31A and the fourth fold 31D being close. Here, the first fold 31A and the fourth fold 31D can be in contact or separated by a certain degree. That is, according to the above description, in this embodiment, the fold 31A and the fold 31D are a pair of folds that are close. In the former case, it can be considered that the roughly triangular structure is formed by the contact point between the first fold 31A and the fourth fold 31D, the second fold 31B, and the third fold 31C; in the latter case, it can be considered that the roughly triangular structure with one end open is formed by the first fold 31A and the fourth fold 31D being separated by a gap. In this specification, "substantially triangular" is used as a term including such a structure. By forming such a folded structure, a force that the substantially triangular structure tends to stretch up and down can be generated, and a restoring force can be obtained.
[0068] In addition, in this embodiment, if Figure 6 As shown, the reinforcing fiber substrate (B') has a folding structure that is continuous while the bending structure including the roughly triangular structure is turned over. By having such a regular folding structure, it is easy to control the expansion force in the desired direction. It should be noted that, not limited to this embodiment, in order to obtain a uniform expansion force, the reinforcing fiber substrate (B') preferably has a regular folding structure within the entire range of the prepreg.
[0069] In this embodiment, when the straight-line distance between the first fold and the fourth fold close to the first fold is Lr, and the distance from the first fold to the fourth fold along the reinforcing fiber substrate (B') is Lf, it is preferred that Lr / Lf is 0.3 or less and Lf is 1 mm or more and 200 mm or less. Figure 7 As shown in FIG. 1 , Lr is the shortest distance between the surfaces of the reinforcing fiber substrate (B') in a pair of adjacent folds. Lf corresponds to the distance between a pair of adjacent folds, i.e. Figure 7The length of the reinforcing fiber substrate (B') from the first fold 31A to the fourth fold 31D in the fold. Lr / Lf is preferably less than 0.2, more preferably less than 0.05. Lf is more preferably from 1 mm to 100 mm, further preferably from 2 mm to 50 mm, and particularly preferably from 3 mm to 10 mm. By making the ratio of Lr to Lf within the above range, it is easy to eliminate the restoring force in the in-plane direction and suppress the expansion in the in-plane direction, and it is easy to form a coarse cavity portion with a circumference corresponding to Lf, and it is easy to control the pore size of the coarse cavity portion.
[0070] The reinforcing fiber substrate (B') is preferably a nonwoven fabric composed of discontinuous reinforcing fibers (B). Figure 8 : is a schematic diagram of an embodiment of the reinforcing fiber substrate (B') contained in the above-mentioned prepreg blank, together with the resin (A) impregnated therein. In this embodiment, the reinforcing fiber substrate (B') is a non-woven fabric composed of discontinuous reinforcing fibers. In the reinforcing fiber substrate (B') impregnated with the resin (A) and in a compressed state, the resin (A) melts or softens, so that the compressed state is released, thereby causing rebound. Through this rebound, as shown in FIG. Figure 2 As shown, fine pores are formed between the reinforcing fibers and in the resin (A). That is, micropores are formed in the reinforcing fiber substrate (B'). As the reinforcing fiber substrate (B'), a non-woven fabric in which discontinuous reinforcing fibers (B) are randomly dispersed is particularly preferred, and the non-woven fabric can be manufactured by air-laid method, carding method, papermaking method, etc.
[0071] The coarse cavity portion of the fiber-reinforced composite material of the present invention can be formed by the restoring force of the folded structure of the reinforcing fiber base material (B') in the prepreg described above in order to stretch. Figure 3 To illustrate the use Figure 6 Schematic cross-sectional view of an example of a fiber-reinforced composite material obtained by molding the prepreg shown. By heating the prepreg, the resin (A) becomes molten or softened, and the restoring force of the folded structure of the reinforcing fiber substrate (B') is released. This restoring force becomes an expansion force in the thickness direction of the prepreg, and through this expansion force, a coarse cavity portion roughly surrounded by the reinforcing fiber substrate (B') is formed.
[0072] Therefore, the folding structure of the reinforcing fiber substrate is substantially the same as that of the prepreg, and the description of the folding structure follows that of the prepreg. However, when the prepreg is used for molding, the folding angle of the reinforcing fiber substrate (B') becomes larger due to molding.
[0073] In this embodiment, the resin (A) is a resin impregnated in the reinforcing fiber substrate (B'), more specifically, a resin impregnated in both the interior of the reinforcing fiber substrate (B') and the space between the reinforcing fiber substrates (B') formed by folding the reinforcing fiber substrate (B'). Figure 3 As shown, the coarse cavity portion preferably has a structure in which a pair of adjacent folds 31 of the reinforcing fiber (B) are bonded by the resin (A). By forming this structure, deformation caused by the openings at the adjacent pair of folds when a load is applied to the fiber-reinforced composite material is suppressed.
[0074] As an example, the above-mentioned prepreg can be produced by a production method including the following steps [1] and [2] in sequence.
[0075] Step [1]: a step of folding the reinforcing fiber substrate (B') into a folded state having a plurality of folds;
[0076] Step [2]: a step of compounding the resin (A) and the reinforcing fiber substrate (B') in a folded state.
[0077] In step [1], the reinforcing fiber substrate (B') is folded into the above-mentioned folded state. Generally, the higher the elastic modulus of the reinforcing fiber, the lower the elongation, and there is a tendency to break easily due to bending. In step [1], by folding the reinforcing fiber substrate (B') in advance, the curvature of the reinforcing fiber single yarn can be suppressed by the gaps between the reinforcing fibers, and the folding can be performed while suppressing fiber breakage.
[0078] In step [2], as a method for compounding the resin (A) and the reinforcing fiber substrate (B'), there can be cited: a method of directly injecting a molten resin (A) into the reinforcing fiber substrate (B'); a method of compounding a film-like, powdery or fibrous resin (A) with the reinforcing fiber substrate (B') and impregnating the composite by heating and melting. From the viewpoint of ease of manufacture, the following method is preferred: applying pressure in a state heated to a temperature above the temperature at which the resin (A) melts or softens, so that the resin (A) is impregnated into the reinforcing fiber substrate (B'). As equipment for implementing the impregnation method, a press molding machine or a double-belt press machine can be preferably used. The intermittent case is the former, and an intermittent pressing system obtained by placing two or more units for heating and cooling in parallel can achieve an improvement in productivity. The continuous case is the latter, and since continuous processing can be easily performed, continuous productivity is excellent.
[0079] The fiber-reinforced composite material of the present invention can be manufactured by the following method: the above-mentioned prepreg is heated to a temperature above the melting or softening temperature of the resin (A) and molded. By heating to a temperature above the melting or softening temperature of the resin (A) and softening it, the restoring force of the folded structure of the reinforcing fiber substrate (B') to restore it to the structure before folding, that is, the force in the direction of the folding angle expansion is released. This restoring force becomes an expansion force in the thickness direction of the prepreg, and the prepreg expands in the form of being pushed up by the reinforcing fiber substrate (B') through the reinforcing fiber substrate (B') having this expansion force. Figure 3 To illustrate the use Figure 6 Schematic cross-sectional view of an example of a fiber-reinforced composite material obtained by molding the prepreg shown in FIG. In this way, the resin (A) is softened by heating the prepreg, so that the reinforcing fiber substrate (B') is deformed in a direction in which the folding angle of the reinforcing fiber substrate (B') is increased, and the prepreg expands. Typically, as Figure 3 As shown, by this expansion, coarse cavity portions 4 partitioned by the porous structure portion are formed.
[0080] Regarding the temperature at which the resin (A) melts or softens, specifically, when the resin (A) is a crystalline thermoplastic resin, the temperature may be higher than the melting point, and is preferably a temperature 20° C. or higher than the melting point. In addition, when the resin (A) is an amorphous thermoplastic resin, the temperature may be higher than the glass transition temperature, and is preferably a temperature 20° C. or higher than the glass transition temperature. As the upper limit temperature, a temperature below the thermal decomposition temperature of the resin (A) is preferred.
[0081] In addition, during molding, it is preferred to adjust the thickness of the prepreg that expands due to heating. As a method for thickness control, as long as the obtained fiber-reinforced composite material can be controlled to the target thickness, the method is not limited. From the perspective of the simplicity of manufacturing, a method of limiting the thickness using a metal plate, a method of directly controlling the thickness by adjusting the applied force, etc. are preferred. As equipment for implementing this method, a press molding machine or a double-belt press machine can be preferably used. The intermittent case is the former, and an intermittent pressing system obtained by arranging more than two units for heating and cooling in parallel can be formed to achieve an increase in productivity. The continuous case is the latter, and since continuous processing can be easily performed, continuous productivity is excellent.
[0082] Example
[0083] The materials used in Examples and Comparative Examples are as follows.
[0084] [PP resin]
[0085] The following crystalline polypropylene resin composition was used, which contained 80% by mass of polypropylene ("Prime Polypro" (registered trademark) J105G manufactured by Prime Polymer Co., Ltd.) and 20% by mass of acid-modified polypropylene ("ADMER" QB510 manufactured by Mitsui Chemicals Co., Ltd.), and had a melting point of 160°C as measured in accordance with JIS K7121 (2012). For the polypropylene resin composition, polypropylene and acid-modified polypropylene as thermoplastic resins were mixed in the above-mentioned mass ratio as raw materials, and melt-kneaded using a twin-screw extruder with a barrel temperature of 200°C to produce resin pellets. Furthermore, the resin pellets were press-molded using a press molding machine adjusted in such a way that the mold surface temperature was 180°C and the film thickness was 0.22 mm, to produce a film having a unit area weight of 200 g / cm 2 PP resin film.
[0086] [PC resin]
[0087] The following amorphous polycarbonate resin was used, which was formed of polycarbonate ("Iupilon" (registered trademark) H-4000 manufactured by Mitsubishi Engineering-Plastics (KK)) and had a glass transition temperature of 150°C as measured in accordance with JIS K7121 (2012). A polycarbonate resin pellet as a thermoplastic resin was press-molded using a press molding machine adjusted so that the mold surface temperature was 240°C and the film thickness was 0.17 mm, and a film having a unit area weight of 200 g / cm 2 PC resin film.
[0088] [Epoxy resin film]
[0089] An uncured epoxy resin composition was prepared by heating and kneading 5 parts by mass of polyvinyl formal ("Vinylec (registered trademark)" K manufactured by Chisso Co., Ltd.) in epoxy resin ("EPIKOTE (registered trademark)" 828:30 parts by mass, "EPIKOTE (registered trademark)" 1001:35 parts by mass, "EPIKOTE (registered trademark)" 154:35 parts by mass) using a kneader to uniformly dissolve the polyvinyl formal. Then, 3.5 parts by mass of a curing agent dicyandiamide (DICY7 manufactured by Japan Epoxy Resins Co., Ltd.) and 7 parts by mass of a curing agent 4,4-methylenebis(phenyldimethylurea) ("Omicure (registered trademark) 52 manufactured by PTI Japan Co., Ltd.) were kneaded using a kneader to prepare a coating having a weight per unit area of 200 g / m 2 Epoxy resin film.
[0090] [Carbon fiber nonwoven fabric]
[0091] A carbon fiber bundle with a total number of 12,000 single fibers was obtained by spinning, calcining, and surface oxidation treatment from a copolymer mainly composed of polyacrylonitrile. As for the characteristics of the carbon fiber bundle, the tensile elastic modulus measured in accordance with JIS R7608 (2007) was 220 GPa, and the single fiber diameter was 7 μm. The above-mentioned carbon fiber bundle was cut into 6 mm lengths using a cartridge cutter to obtain short-cut carbon fibers. A dispersion containing water and a surfactant (polyoxyethylene lauryl ether (trade name) manufactured by NACALAITESQUE (KK)) with a concentration of 0.1% by mass was prepared, and a carbon fiber substrate was prepared using the dispersion and short-cut carbon fibers. The manufacturing device is equipped with a cylindrical container with a diameter of 1000 mm having an opening and closing cock at the bottom of the container as a dispersion tank, and is equipped with a linear conveying portion (inclination angle 30°) connecting the dispersion tank to the papermaking tank. The opening on the upper surface of the dispersion tank is provided with a stirrer, and chopped carbon fibers and a dispersion liquid (dispersion medium) can be put in from the opening. The papermaking tank is provided with a mesh conveyor having a papermaking surface with a width of 500 mm at the bottom, and a conveyor capable of transporting a carbon fiber substrate (papermaking substrate) is connected to the mesh conveyor. Papermaking is performed under the condition that the carbon fiber concentration in the dispersion liquid is 0.05% by mass. The papermaking carbon fiber substrate is dried in a drying furnace at 200°C for 30 minutes to form a carbon fiber nonwoven fabric in which the orientation direction of the single fibers of the carbon fiber is randomly dispersed.
[0092] [Thermosetting prepreg used in skin layer]
[0093] A carbon fiber bundle with a total of 12,000 filaments was obtained by spinning, calcining, and surface oxidation of a copolymer mainly composed of polyacrylonitrile. The properties of the carbon fiber bundle were as follows: the tensile modulus measured in accordance with JIS R7608 (2007) was 220 GPa, and the single fiber diameter was 7 μm and the cross section was circular.
[0094] 5 parts by mass of polyvinyl formal ("Vinylec (registered trademark)" K manufactured by Chisso Co., Ltd.) was heat-kneaded in epoxy resin (Japan Epoxy Resins Co., Ltd. "EPIKOTE (registered trademark)" 828:30 parts by mass, "EPIKOTE (registered trademark)" 1001:35 parts by mass, "EPIKOTE (registered trademark)" 154:35 parts by mass) using a kneader to uniformly dissolve the polyvinyl formal. Then, 3.5 parts by mass of a curing agent dicyandiamide (Japan Epoxy Resins Co., Ltd. DICY7) and 7 parts by mass of a curing agent 4,4-methylenebis(phenyldimethylurea) (PTI Japan Co., Ltd. "Omicure (registered trademark) 52) were kneaded using a kneader to prepare an uncured epoxy resin composition. A coating having a weight per unit area of 132 g / m was prepared from the uncured epoxy resin composition using a knife coater. 2 Epoxy resin film.
[0095] Then, a sheet material in which the carbon fiber bundles are oriented in one direction is prepared, and epoxy resin films are overlapped on both sides of the sheet material, and the epoxy resin is impregnated by heating and pressurizing to obtain a carbon fiber sheet with a mass of 125 g / m2 per unit area. 2 , a thermosetting prepreg with a fiber volume content of 60% and a thickness of 0.125 mm.
[0096] The evaluation methods of the structures, physical properties, etc. in each of the Examples and Comparative Examples are as follows.
[0097] [Evaluation of folding angle]
[0098] The sample was cut out from the prepreg blank so that the cross section perpendicular to the fold of the carbon fiber nonwoven fabric became the observation surface, and the cross section was ground so that the fold of the carbon fiber nonwoven fabric could be observed. The obtained sample was observed with a laser microscope (Keyence Co., Ltd., VK-9510), and the angle was measured in the observed image using the software attached to the device. For each fold, Figure 4 As shown, the angle θ formed by the bent portion centered at the fold 31 of the carbon fiber nonwoven fabric 3 was obtained. The folding angles were obtained for a total of 20 folds, and the arithmetic mean was obtained.
[0099] [Evaluation of Lr and Lf]
[0100] The sample was cut out from the prepreg blank in such a way that the cross section orthogonal to the fold of the carbon fiber nonwoven fabric became the observation surface, and the sample was ground in such a way that a pair of close folds of the carbon fiber nonwoven fabric and a cross section connecting the close pair of folds of the continuous carbon fiber nonwoven fabric could be observed. The obtained sample was observed using a laser microscope (Keyence (co., Ltd., VK-9510), and the length was measured using the software attached to the device in the observed image to obtain the linear distance (Lr) between the close pair of folds and the distance (Lf) connecting the close pair of folds along the carbon fiber nonwoven fabric. For a total of 20 close folds, Lr, Lf and Lr / Lf were obtained, and the arithmetic mean was obtained.
[0101] [Evaluation of large cavities]
[0102] The sample is cut out from the fiber reinforced composite material in such a way that the cross section parallel to the thickness direction becomes the observation surface, and the sample is ground in such a way that a pair of folds close to the carbon fiber nonwoven fabric and a cross section connecting the pair of folds close to the continuous carbon fiber nonwoven fabric can be observed. The obtained sample is observed using a laser microscope (Keyence (co., VK-9510), thereby observing the cross section of the coarse cavity as a planar cross-sectional opening. The length is measured using the software attached to the device to find the maximum straight line length that can be drawn in the cross-sectional opening. A total of 20 cross-sectional openings are measured, and the arithmetic mean thereof is used as the maximum length of the cross-sectional opening. It should be noted that samples with close cross-sectional openings and intervals of more than 5 cm in the depth direction are prepared, and their measurement results are used as the value used for the arithmetic mean.
[0103] [Evaluation of average pore diameter]
[0104] As a mercury porosimeter, Autopore IV9510 manufactured by Micromeritics was used to measure the pore diameter within a mercury intrusion pressure range of 4 kPa to 400 MPa. The average pore diameter was determined from the pore volume and specific surface area obtained as the measurement results by formula (1).
[0105] (Average pore diameter)=4×(pore volume) / (specific surface area)···Formula (1).
[0106] [Evaluation of Specific Gravity of Porous Structure]
[0107] The specific gravity of the porous structure portion is determined by cutting out a sample of the porous structure portion from the fiber-reinforced composite material, dividing the sample mass [g] by the volume [cm 3 ] is obtained by the arithmetic mean of the specific gravity measured by 5 randomly selected samples.
[0108] [Evaluation of specific gravity of fiber-reinforced composite materials]
[0109] The specific gravity of the fiber-reinforced composite material can be obtained as the value obtained by dividing the mass [g] of the fiber-reinforced composite material by the volume [cm 3 ] and the value obtained.
[0110] [Evaluation of number average fiber length of reinforcing fibers (B)]
[0111] A sample was cut out of the fiber-reinforced composite material to a mass of 2 g, and the sample was heated in an electric furnace at 500° C. for 1 hour to burn off the resin (A) and separate the reinforcing fibers (B). The sample was observed using a laser microscope (Keyence Co., Ltd., VK-9510), and the fiber lengths of a total of 400 reinforcing fibers (B) were measured using the software attached to the device, and the arithmetic mean value thereof was calculated as the number average fiber length of the reinforcing fibers (B).
[0112] [Evaluation of deflection under load]
[0113] As a testing machine, an "Instron" (registered trademark) 5565 universal material testing machine (manufactured by Instron Japan Co., Ltd.) was used. The sample was placed on a pressing head having an inner diameter of a square with a side length of 100 mm so as to cover the inner diameter. A pressure gauge with a plane area of 10 mm was used from just above the intersection of the diagonal lines of the inner diameter of the square. 2 A load is gradually applied by a cylindrical upper pressure head, and the deflection amount [mm] is obtained by subtracting the displacement at a load of 0.1 N (at the start of contact) from the displacement at a load of 50 N. Evaluation is performed according to the following three levels, with good and fair being considered acceptable.
[0114] Good: The deflection is less than 2 mm.
[0115] Fair: The deflection is greater than 2 mm and less than 3 mm.
[0116] Bad: The deflection is greater than 3mm.
[0117] Hereinafter, the prepregs, fiber-reinforced composite materials, and sandwich structures produced in Examples and Comparative Examples will be described.
[0118] [Example 1]
[0119] As a reinforcing fiber substrate (B'), the carbon fiber nonwoven fabric prepared in the above manner is folded into Fig. 9 The cross-sectional structure shown has a unit area weight of 100 g / cm 2Folded substrate. At this time, when making the prepreg blank, in the adjacent pair of folds 8 of the reinforcing fiber substrate (B'), the straight-line distance (Lr) between the adjacent pair of folds is 0 mm, that is, it is folded in a contact manner, and the distance (Lf) between the adjacent pair of folds along the carbon fiber non-woven fabric is 10 mm. In addition, it is folded in a manner that the composition ratio 9 of the adjacent pair of folds becomes a symmetrical structure when the surface and the back of the folded substrate are put together. That is, the folding is repeated in a manner that a pair of adjacent folds on one surface are arranged between a pair of adjacent folds and a pair of adjacent folds arranged next to it. Next, on the carbon fiber non-woven fabric, a resin (A) having a unit area weight of 200 g / cm is laminated. 2 The PP resin film was heated and pressed. In the heating and pressing step, the PP resin was impregnated into the carbon fiber nonwoven fabric under the conditions of a mold temperature of 180°C and a pressure of 3 MPa for 10 minutes to obtain a prepreg blank with a side of 200 mm.
[0120] In addition, a prepreg obtained was heated and expanded for 10 minutes using a press molding machine adjusted so that the mold surface temperature was 180°C and the molded product thickness was 2.8 mm, thereby molding into a fiber-reinforced composite material. The obtained fiber-reinforced composite material has Figure 1 The cross section of the porous structure surrounded by three sides is a substantially triangular opening. The openings of the large voids are arranged in the in-plane direction. The number average fiber length of the reinforcing fibers (B) is 6 mm. The evaluation results are shown in Table 1.
[0121] [Example 2]
[0122] As the reinforcing fiber substrate (B'), the folded substrate structure was changed so that Lr became 1 mm and Lf became 9 mm. The same processing as in Example 1 was performed to obtain a prepreg and a fiber-reinforced composite material. The obtained fiber-reinforced composite material had Figure 1 The porous structure has three sides surrounded by a substantially triangular opening in cross section. The openings of the coarse cavity are arranged in the in-plane direction. The evaluation results are shown in Table 1.
[0123] [Example 3]
[0124] As the reinforcing fiber substrate (B'), the folded substrate structure was changed so that Lr became 2 mm and Lf became 8 mm. The same processing as in Example 1 was performed to obtain a prepreg and a fiber-reinforced composite material. The obtained fiber-reinforced composite material had Figure 1The porous structure has three sides surrounded by a substantially triangular opening in cross section. The openings of the coarse cavity are arranged in the in-plane direction. The evaluation results are shown in Table 1.
[0125] [Example 4]
[0126] As the reinforcing fiber substrate (B'), the same folded substrate as in Example 1 was used, and as the resin (A), a 200 g / cm 2 The PC resin film is stacked and heated and pressed. In the heating and pressing process, the PC resin is impregnated into the carbon fiber nonwoven fabric under the conditions of a mold temperature of 240°C and a pressure of 3MPa for 10 minutes to obtain a prepreg blank with a side of 200mm. A pressing molding machine adjusted in such a way that the mold temperature is 240°C and the thickness of the molded product is 2.2mm is used to heat and expand the obtained prepreg blank for 10 minutes to form a fiber-reinforced composite material. The obtained fiber-reinforced composite material has Figure 1 The porous structure has three sides surrounded by a substantially triangular opening in cross section. The openings of the coarse cavity are arranged in the in-plane direction. The evaluation results are shown in Table 1.
[0127] [Example 5]
[0128] As a reinforcing fiber substrate (B'), a carbon fiber nonwoven fabric is prepared to be Fig.10 The cross-sectional structure shown is folded in such a way that the unit area weight is 100 g / cm 2 Folded substrate. At this time, when the prepreg is made, it is folded in such a manner that the straight-line distance (Lr) between a pair of close folds becomes 0 mm, that is, in contact, and the length (Lf) between the pair of close folds connected along the continuous carbon fiber nonwoven fabric becomes 10 mm. In addition, it is folded in such a manner that the composition ratio of a pair of close folds becomes an asymmetric structure when the surface and the back of the folded substrate are viewed together, that is, in one surface, a pair of close folds on another surface are arranged at a position where the distance between a pair of close folds and a pair of close folds arranged next to them is divided into 1 to 4 and repeated. Next, on the carbon fiber nonwoven fabric, a resin (A) having a unit area weight of 200 g / cm 2 The PP resin film was heated and pressed. In the heating and pressing step, the PP resin was impregnated into the carbon fiber nonwoven fabric under the conditions of a mold temperature of 180°C and a pressure of 3 MPa for 10 minutes to obtain a prepreg blank with a side of 200 mm.
[0129] In addition, a prepreg obtained was heated and expanded for 10 minutes using a press molding machine adjusted so that the mold temperature was 180°C and the thickness of the molded product was 2.8 mm, thereby molding into a fiber-reinforced composite material. The obtained fiber-reinforced composite material has Figure 1 The porous structure has three sides surrounded by a substantially triangular opening in cross section. The openings of the coarse cavity are arranged in the in-plane direction. The evaluation results are shown in Table 1.
[0130] [Example 6]
[0131] Two prepregs obtained in Example 1 were stacked to form a preform, and heated for 10 minutes using a press molding machine adjusted so that the mold temperature was 180°C and the thickness of the molded product was 4.8 mm, thereby forming a fiber-reinforced composite material as a laminate. The obtained fiber-reinforced composite material has Figure 1 The openings of the porous structure having three sides and a substantially triangular cross section are stacked in two layers. The openings of the coarse cavity are arranged in the in-plane direction. The evaluation results are shown in Table 1.
[0132] [Example 7]
[0133] The fiber-reinforced composite material obtained in Example 1 is used for the core layer, and the thermosetting prepreg prepared in the above manner is arranged on the outside as the skin layer. The orientation direction of the reinforcing fiber on the surface of one skin layer is set to 0°, and based on this, the stacking structure is stacked in a manner of [0° / 90° / fiber-reinforced composite material / 90° / 0°]. Then, the thermosetting prepreg is cured by heating and pressing for 10 minutes under the conditions of a mold temperature of 150°C and a pressure of 1MPa to obtain a sandwich structure. The thickness of the fiber-reinforced composite material in the obtained sandwich structure is 2.4mm, and it is not crushed when it is made into a sandwich structure, and can be used as a core layer well.
[0134] [Example 8]
[0135] The fiber-reinforced composite material of the laminate obtained in Example 6 is used for the core layer, and a thermosetting prepreg is arranged on the outside as a skin layer. The orientation direction of the reinforcing fiber on the surface of one skin layer is set to 0°, and based on this, the laminate is stacked in a manner of [0° / 90° / fiber-reinforced composite material / 90° / 0°]. Next, the laminate is heated and pressed for 10 minutes under the conditions of a mold temperature of 150°C and a pressure of 1MPa, thereby curing the thermosetting prepreg to obtain a sandwich structure. The thickness of the laminate in the obtained sandwich structure is 4.3mm, and it is not crushed when it is made into a sandwich structure, and can be used as a core layer well.
[0136] [Comparative Example 1]
[0137] 100g / cm2 on a flat surface without creases 2 The carbon fiber nonwoven fabric has a unit area weight of 200g / cm 2 The PP resin film was heated and pressed. In the heating and pressing process, the PP resin was impregnated into the above-mentioned substrate under the conditions of a mold temperature of 180°C and a pressure of 3MPa for 10 minutes, thereby obtaining a prepreg blank with a side of 200mm. Using a press molding machine with a mold temperature adjusted to 180°C, the obtained prepreg blank was heated and expanded for 10 minutes, thereby forming a fiber-reinforced composite material. The distance between the upper mold and the lower mold of the mold was set to 2.8mm, and molding was performed with the purpose of making the thickness of the molded product 2.8mm, but the prepreg blank did not expand to the thickness between the upper mold and the lower mold of the mold, and no coarse voids were formed in the obtained fiber-reinforced composite material, and the thickness was only 0.9mm. The evaluation results are shown in Table 1.
[0138] [Comparative Example 2]
[0139] As a reinforcing fiber substrate (B'), the carbon fiber nonwoven fabric prepared in the above manner is prepared to be Fig. 9 The cross-sectional structure shown is folded in such a way that the unit area weight is 100 g / cm 2 Folded substrate. At this time, when making the prepreg blank, in the adjacent pair of folds 8 of the reinforcing fiber substrate (B'), the straight-line distance (Lr) between the adjacent pair of folds is 0 mm, that is, it is folded in a contact manner, and the distance (Lf) between the adjacent pair of folds along the carbon fiber non-woven fabric is 10 mm. In addition, it is folded in a manner that the composition ratio 9 of the adjacent pair of folds becomes a symmetrical structure when the surface and the back of the folded substrate are put together. That is, it is folded in a manner that a pair of adjacent folds on one surface are arranged in the middle of the adjacent pair of folds and the adjacent pair of folds arranged next to it, and the adjacent pair of folds on another surface are arranged and repeated. Next, on the carbon fiber non-woven fabric, a resin (A) having a unit area weight of 200 g / cm is laminated. 2 The epoxy resin film was heated and pressed. In the heating and pressing step, the carbon fiber nonwoven fabric was impregnated with epoxy resin at a mold temperature of 180° C. and a pressure of 3 MPa for 10 minutes to obtain a cured prepreg blank with a side of 200 mm.
[0140] In addition, a prepreg obtained was heated for 10 minutes using a press molding machine with a mold temperature adjusted to 180°C, thereby molding into a fiber-reinforced composite material. The distance between the upper mold and the lower mold of the mold was set to 2.8 mm, and the molding was performed with the purpose of making the molded product 2.8 mm thick. However, the prepreg did not expand to the thickness between the upper mold and the lower mold of the mold, and no coarse voids and micropores were formed in the obtained fiber-reinforced composite material, and the thickness was only 0.3 mm. The evaluation results are shown in Table 1.
[0141] [Comparative Example 3]
[0142] 100g / cm2 on a flat surface without creases 2 The carbon fiber nonwoven fabric has a unit area weight of 200g / cm 2 The epoxy resin film was heated and pressed. In the heating and pressing step, the epoxy resin was impregnated into the substrate under the conditions of a mold temperature of 60°C and a pressure of 0.5 MPa for 5 minutes to obtain a prepreg with a side of 200 mm. Fig.11 A mold having a cavity formed in the manner of a cross-sectional structure having a vertex 9 of a sawtooth structure as shown in the figure was pressed for 10 minutes under the conditions of a mold temperature of 180°C and a pressure of 0.5 MPa to form a fiber-reinforced composite material. The distance between the upper mold and the lower mold of the mold was adjusted so that the molded product had a thickness of 2.8 mm. No micropores were formed in the obtained fiber-reinforced composite material. The evaluation results are shown in Table 1.
[0143]
[0144] Industrial Applicability
[0145] The fiber-reinforced composite material of the present invention can be suitably used in applications such as aircraft structural members, wind turbine blades, automobile structural members, IC trays, and notebook computer housings.
[0146] Description of Reference Numerals
[0147] 1 Prepreg
[0148] 2 Resin (A)
[0149] 3 Reinforcement fiber (B) or reinforcement fiber matrix (B')
[0150] 31 Creases of reinforcing fiber (B) or reinforcing fiber matrix (B')
[0151] 31A Folding line of reinforcing fiber base material (B') (first folding line)
[0152] 31B Folding line of reinforcing fiber base material (B') (second folding line)
[0153] 31C Folding line of reinforcing fiber base material (B') (3rd folding line)
[0154] 31D Folding line of reinforcing fiber base material (B') (4th folding line)
[0155] Lr The distance between the first fold and the closest fold (the fourth fold)
[0156] Lf The distance along the reinforcing fiber base material (B') from the first fold to the fold closest to the first fold (the fourth fold)
[0157] θ Folding angle
[0158] 4 Space with a roughly triangular cross section (large cavity)
[0159] 5 microporous
[0160] 6. Porous structure
[0161] 7 A pair of adjacent folds of the reinforcing fiber base material (B')
[0162] 8 The composition ratio of a pair of folds that are close to each other when the front and back sides of the folded substrate are put together
[0163] 9 Vertices of the sawtooth structure
Claims
1. A fiber-reinforced composite material having: A porous structure comprising a resin (A) and reinforcing fibers (B), and having micropores having an average pore diameter of 10 μm or more and 150 μm or less as measured by mercury intrusion porosimetry, wherein the micropores are present in the resin (A) between the reinforcing fibers (B); and a coarse cavity portion which is defined by the porous structure portion and has a maximum length of a cross-sectional opening exceeding 500 μm, the coarse cavity portion existing as a tunnel-like space surrounded by the porous structure portion, The reinforcing fiber (B) is a sheet-like reinforcing fiber substrate (B'), the reinforcing fiber substrate (B') is in a folded state having a plurality of folds, and the coarse cavity portion has a structure in which a pair of adjacent folds of the reinforcing fiber (B) are bonded by the resin (A).
2. The fiber-reinforced composite material according to claim 1, wherein: The porous structure is formed by impregnating the resin (A) between the reinforcing fibers (B).
3. The fiber-reinforced composite material according to claim 1 or 2, wherein: The cross-sectional opening of the large cavity portion has a substantially polygonal or elliptical shape.
4. The fiber-reinforced composite material according to claim 1 or 2, wherein: The resin (A) is a thermoplastic resin.
5. The fiber-reinforced composite material according to claim 4, wherein: The thermoplastic resin is at least one thermoplastic resin selected from the group consisting of polyolefin, polycarbonate, polyester, polyarylene sulfide, polyamide, polyoxymethylene, polyetherimide, polyethersulfone, and polyarylene ether ketone.
6. The fiber-reinforced composite material according to claim 1 or 2, wherein: The reinforcing fibers (B) are discontinuous fibers having a number average fiber length of 1 mm to 50 mm.
7. The fiber-reinforced composite material according to claim 6, wherein: In the porous structure, the reinforcing fibers (B) are randomly dispersed.
8. The fiber-reinforced composite material according to claim 1 or 2, wherein: The reinforcing fibers (B) are carbon fibers.
9. The fiber-reinforced composite material according to claim 1 or 2, wherein: The porous structure has an average pore diameter of 30 μm or more and 100 μm or less.
10. The fiber-reinforced composite material according to claim 1 or 2, wherein: The specific gravity of the porous structure is 0.3 g / cm 3 Above 0.8g / cm 3 the following.
11. The fiber-reinforced composite material according to claim 1 or 2, wherein: The average value of the maximum length of the cross-sectional opening of the coarse cavity is 1000 μm or more and 10000 μm or less.
12. The fiber-reinforced composite material according to claim 1 or 2, wherein the specific gravity is 0.001 g / cm 3 Above 0.2g / cm 3 the following. 13 . The fiber-reinforced composite material according to claim 1 , which has a thickness of 0.1 mm to 5 mm.
14. The fiber-reinforced composite material according to claim 1 or 2, having a laminated structure in which a plurality of layers are laminated, wherein the openings of the coarse void portions are arranged in an in-plane direction in a cross section perpendicular to the extending direction of the coarse void portions.
15. A sandwich structure comprising skin layers arranged on both sides of the fiber-reinforced composite material according to any one of claims 1 to 14.
Citation Information
Patent Citations
Foldable cores based on carbon fiber paper and articles made therefrom
JP2013511629A
Composite structure and method for manufacturing same
WO2018117181A1
Intermediate material for forming FRP, and method for production thereof
CN101181828A
Molded article and molding material
CN105683262A
Fluid separation membrane, fluid separation membrane module, and porous carbon fiber
CN108495703A