A method for preparing a 1550nm up-conversion polarization photoelectric detection and visualization imaging device
Patent Information
- Application Number
- CN202210702441.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-06-21
AI Technical Summary
由于UCNPs的偏振对几何因子不敏感,且难以在大规模UCNPs中实现优良的对准,因此,基于UCNPs实现可调UC光偏振检测和成像仍然是一个重大挑战
[0020] (1) Directionally arranged ordered-Au@Ag NRs have narrower LSPR absorption and higher scattering cross-section than randomly arranged disordered-Au@Ag NRs, and can polarize enhanced UCL for polarized excitation light, where The DOP of green light emission is 0.46 and the DOP of red light emission is 0.72. By introducing Au@Ag NRs, its LSPR effect can regulate UCL enhancement by 20.7 times.
Smart Images

Figure CN115117255B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polarization-sensitive near-infrared narrow-band photoelectric detection, and in particular relates to a method for preparing a 1550nm up-conversion polarization photoelectric detection and visualization imaging device. Background Art
[0002] Near-infrared (NIR) photodetectors (PDs) are the most basic and important components of various optoelectronic systems such as medical, communication, and military. Polarization-sensitive narrowband PDs can sense the polarization state of light and achieve wavelength-selective detection in a narrowband spectrum, which has attracted great interest in many professional applications such as astronomy, object recognition, polarization imaging, and remote sensing. Typically, polarization-sensitive narrowband PDs require the integration of multiple filters and polarizers to equip commercial NIR broadband photodetectors such as Si, InGaAs, InSb, HgCdTe, etc. [ACS Nano 2020, 14, 16634-16642, Nat. Commun. 2021, 12(1), 6476, ACS Appl. Mater. Interfaces 2020, 12(13), 15414-15421]. This approach faces the disadvantages of complex equipment system, high cost, and low imaging resolution. The key features of the next-generation detection system require miniaturization, integration, and flexibility. To this end, people have been working on finding polarization- or narrowband-sensitive materials to build detectors, such as two-dimensional materials or perovskites.
[0003] Rare earth doped upconversion nanoparticles (UCNPs) have NIR narrowband absorption characteristics due to their 4f electronic configuration, which enables them to have the ability to convert NIR photons, such as converting 808nm, 980nm, and 1550nm photons into visible photons through the anti-Stokes process. At present, NIR narrowband PDs based on UCNPs (half-peak width of about 30-50nm) have been realized, with a specific detection rate D* = ~10 8-10 Jones. For example, Liu et al. reported a MAPbI-based 3 The flexible NIR PDs of UCNPs and UCNPs, under 980nm laser irradiation, the photoresponsivity and detection rate of the device are 0.27AW -1 and 7.6×10 11 Jones [ACS Applied Materials & Interfaces, 9 (22), 19176-19183.]; Ko et al. designed a MLA / Au NPs (150nm)-Au nanostars (15nm) / UCNPs cascade amplification structure for 1550nm NIR detection and obtained 9.8A / W, 8.22×10 12Jones’s narrowband NIR PDs [Advanced materials 34(5), e2106225.]. Therefore, UCNPs are considered to be suitable photoactive materials for the preparation of narrowband NIR PDs. However, polarization-sensitive NIR narrowband PDs based on UCNPs have not been reported so far, especially for the 1550nm band, which is crucial for optical communications, military and industrial imaging. Unlike the size or morphology dependence of the polarization anisotropy of semiconductor materials caused by quantum size effects and dielectric confinement of the light field, the light polarization properties of UCNPs with anisotropic structures are almost unaffected by geometric factors, but are also inseparable from the symmetry of the crystal / coordination structure. Only a few papers have reported on the polarization anisotropy of single NaYF 4 :Ln 3+ UC polarization anisotropy observed in submicron / micron rods, such as the polarization-sensitive properties found in single UC nanorods by Liu et al. [Nano Lett. 2020, 20(6), 4204-4210]. Since the polarization of UCNPs is insensitive to geometric factors and it is difficult to achieve good alignment in large-scale UCNPs, it remains a major challenge to achieve tunable UC light polarization detection and imaging based on UCNPs. At the same time, the relatively low UC emission efficiency and high pumping threshold of UCNPs also limit their detection performance. Summary of the invention
[0004] In order to solve the above problems, the present invention adopts a three-phase interface self-assembly method to prepare a polarization-sensitive large-area single-layer directional and orderly arranged Au@Ag nanorods (ordered-Au@Ag NRs) film, which has a narrow-band localized surface plasmon resonance (LSPR) peak and a high scattering cross section in the 1550nm band.
[0005] Because Er 3+ Narrow-band near-infrared absorption and plasmon polarization effect of ordered-Au@Ag NRs at 1550nm, self-assembled ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+ The composite structure exhibits polarization-sensitive enhanced UCL, where the degrees of polarization (DOP) of green and red emissions are approximately 0.46 and 0.72, respectively. 4 :(10-50)%Er 3+ Composite structure, designed and prepared MAPbI 3 / Ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+Highly polarization-sensitive 1550nm narrowband NIR PDs, DOP up to 0.63, specific detectivity D*~1.69×10 10 Jones, responsivity R ~ 0.32A / W. The photodetector has the polarization angle dependence of the photocurrent response, so it can be applied to the visual photocurrent response system to realize polarized light imaging. The present invention uses polarization structure upconversion nanomaterials to realize polarization-sensitive PDs, and promotes the development of future optical research and NIR PDs.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a 1550nm up-conversion polarization photoelectric detection and visualization imaging device, the specific steps are as follows:
[0008] Step 1: Preparation of Au@Ag NRs using the seed-grown method
[0009] First, the Au nanocones (Au BPs) seed solution for growing the outer Ag shell was prepared: HAuCl was treated with cationic surfactant CTAC and citric acid. 4 Surface modification was performed by adding CTAC, citric acid, NaBH 4 and HAuCl 4 The mixture was mixed in a molar ratio of (100-900): (10-130): (10-200): 1; the mixed solution was slowly stirred at 50-180°C for 2-24h to obtain solution A; CTAB, HAuCl 4 AgNO 3 , HCl and ascorbic acid AA are mixed in a molar ratio of (0.2-30): (0.1-20): (0.05-60): (0.2-100): 1 to obtain solution B; solution B and solution A are mixed in a volume ratio of (1-100): 1, and the mixture is allowed to stand at 20-80° C. for 0.5-24 h; the product is collected by centrifugation at a speed of 5000-15000 rpm and a centrifugation time of 10-40 min; the collected centrifugal product is dispersed in deionized water at a mass fraction of 1-90% to obtain an Au BPs seed solution.
[0010] Ag shell was grown on the basis of Au BPs seed solution to prepare Au@Ag NRs: CTAC, AgNO 3, ascorbic acid AA according to a molar ratio of (0.1-2.5): (0.05-10): 1 to obtain solution C; solution C is mixed with Au BPs seed solution according to a volume ratio of (1-50): 1, and the mixture is allowed to stand for 0.5-48 hours at 20-100° C.; the product is collected by centrifugation at a speed of 2000-15000 rpm and a centrifugation time of 10-40 minutes; the collected centrifugal product is dispersed in deionized water with a mass fraction of 1-90% to obtain Au@Ag NRs solution.
[0011] Step 2: Preparation of oriented ordered Au@Ag NRs thin films using the three-phase interface self-assembly method
[0012] PVP and ethanol are mixed in a mass ratio of (0.01-0.2):1 to obtain an ethanol solution of PVP with a mass fraction of 1-20%; Au@Ag NRs solution and PVP ethanol solution are mixed in a volume ratio of (0.1-100):1, and ultrasonicated for 20-100 minutes to fully dissolve them to obtain an Au@Ag NRs solution wrapped by PVP; dichloromethane, deionized water, and PVP ethanol solution are mixed in a volume ratio of (2-200):(2-300):1 to obtain solution D; solution D is then mixed with n-hexane in a volume ratio of (2-100):1, and allowed to stand for 5-120 minutes, at which time Au@Ag NRs are driven to the interface between water and n-hexane; Au@Ag NRs are transferred to a glass sheet by a pulling method to obtain an ordered-Au@Ag NRs film.
[0013] Step 3: Synthesis of upconversion nanoparticles NaYF by solvothermal method 4 :(10-50)%Er 3+ The ordered-Au@Ag NRs / NaYF was prepared on the ordered-Au@Ag NRs film substrate using a three-phase self-assembly method. 4 :(10-50)%%Er 3+ Composite film.
[0014] PVP and ethanol are mixed in a mass ratio of (0.002-0.2):1 to obtain an ethanol solution of PVP with a mass fraction of 0.2-20%; upconversion nanoparticles NaYF 4 :(10-50)%Er 3+ Dissolve in cyclohexane to obtain NaYF with a molar concentration of (0.01-0.8) mol / L 4 :(10-50)%Er 3+ Cyclohexane solution, NaYF 4 :(10-50)%Er 3+The cyclohexane solution and the ethanol solution of PVP were mixed in a volume ratio of (0.1-100):1, and ultrasonicated for 20-100 min to fully dissolve them to prepare NaYF coated with PVP. 4 :(10-50)%Er 3+ Solution; dichloromethane, deionized water, and PVP ethanol solution were mixed in a volume ratio of (2-200): (2-300): 1 to obtain solution E; solution E was then mixed with n-hexane in a volume ratio of (2-100): 1, ultrasonicated for 5-120 minutes, and allowed to stand for 5-120 minutes. At this time, the upconversion nanoparticles NaYF 4 :(10-50)%Er 3+ The upconversion nanoparticles NaYF 4 :(10-50)%Er 3+ Transfer the ordered-Au@Ag NRs film prepared in step 2 to the glass substrate to obtain ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+ Composite film.
[0015] Step 4: Preparation of MAPbI 3 / Ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+ Polarization-sensitive 1550 nm narrow-band photodetector: Ordered-Au@Ag NRs / NaYF prepared in step 3 4 :(10-50)%Er 3+ Based on the composite film, a two-step method was used to prepare the photodetector in a glove box atmosphere.
[0016] First, prepare the perovskite precursor solution: DMF and DMSO are mixed in a volume ratio of (1-8):1 to obtain solution F; PbI 2 Mix with MAI in a molar ratio of (0.1-10):1 to obtain a mixture G; add the mixture G to the solution F and let it stand for 1-20 hours until PbI 2 The perovskite precursor solution was completely dissolved with MAI to obtain the perovskite precursor solution; the perovskite precursor solution was mixed with the ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+ The composite film was transferred into the glove box; the perovskite precursor solution was dropped on the ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+On the composite film, turn on the spin coater and set it to low speed 200-1000rpm, maintain for 2-10s, high speed 2000-8000rpm, maintain for 20-100s, and obtain perovskite precursor / ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+ Composite film; start timing when the spin coater changes from low speed to high speed, and after 10-40s, the perovskite precursor / ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+ Chlorobenzene was dripped onto the composite film, and the volume ratio of chlorobenzene to perovskite precursor solution was (2-20):1. After the spin coater stopped, the glass sheet was transferred to the heating table and heated in stages, first at a low temperature of 10-100°C, maintained for 1-20 min, and then raised to a high temperature of 100-260°C, maintained for 1-20 min, to obtain MAPbI 3 / Ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+ Composite film; MAPbI 3 / Ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+ The composite film is transferred to a vacuum evaporator, and a Ag electrode is evaporated on the composite film to obtain a NIR narrow-band photodetector.
[0017] Step 5: Preparation of MAPbI 3 / Ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+ Polarization-sensitive 1550nm polarization photodetection and visualization imaging device: MAPbI prepared in step 4 3 / Ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+ Based on the polarization-sensitive 1550nm narrow-band photodetector, a polarization photodetection and visualization imaging device was prepared.
[0018] The prepared polarization-sensitive 1550nm narrow-band photodetectors are arranged in an array, and each photodetector in the array is an imaging pixel point, forming a polarization photodetection and visualization imaging device as a whole, which is used to detect 1550nm polarized laser.
[0019] Beneficial effects of the present invention:
[0020] (1) The oriented ordered-Au@Ag NRs have narrower LSPR absorption and higher scattering cross section than the randomly arranged disordered-Au@Ag NRs, and can polarization enhance the UCL for polarized excitation light, with the DOP of green light emission being 0.46 and the DOP of red light emission being 0.72. By introducing Au@Ag NRs, its LSPR effect can regulate the UCL enhancement by 20.7 times.
[0021] (2) The polarization-sensitive 1550nm polarization photodetection and visualization imaging device is based on MAPbI 3 / Ordered-Au@Ag NRs / NaYF 4 :(10-50)%Er 3+ PDs of composite structures. Compared with randomly arranged MAPbI 3 / disordered-Au@AgNRs / NaYF 4 :(10-50)%Er 3+ The composite structure of PDs can produce a photocurrent response with a DOP of 0.63 to the polarized light of 1550nm, and the device has a specific detection rate of D*~1.69×10 10 Jones, responsivity R ~ 0.32A / W. After placing a template in the middle of the polarized excitation light, the device can be used for imaging the polarized excitation light. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 are transmission electron microscopy images, where (a) is the transmission electron microscopy image of Au BPs, and (b) is the transmission electron microscopy image of Au@Ag NRs. The enlarged part is the Au BPs in the Au@Ag NRs.
[0023] Figure 2 Scanning electron microscopy image of oriented ordered-Au@Ag NRs.
[0024] Figure 3 Directed ordered-Au@Ag NRs / NaYF 4 :20%Er 3+ SEM images of the composite structure.
[0025] Figure 4 MAPbI 3 / Ordered-Au@Ag NRs / NaYF 4 :20%Er 3+ With MAPbI 3 / disordered-Au@Ag NRs / NaYF 4 :20%Er 3+ Polar plots of the polarization-sensitive photocurrent responses of the composite structure PDs.
[0026] Figure 5 Schematic diagram of the application process of polarization-sensitive 1550nm narrow-band photodetector.
[0027] Figure 6 These are the imaging effects of the polarization-sensitive NIR narrow-band photoelectric detection and imaging device when the template is a vase under non-polarized excitation light, polarization angles of 0°, and 90°. DETAILED DESCRIPTION
[0028] The present invention is specifically described below by way of examples, but the present invention is not limited to the following examples.
[0029] Embodiment 1:
[0030] (1) Take 200mM CTAC, 20mM citric acid, 25mM NaBH 4 , 0.5 mM HAuCl 4 After mixing and vigorously stirring for 2 min, the mixed solution was slowly stirred at 80 °C for 6 h;
[0031] (2) Take 100mM CTAB and 25mM HAuCl 4 , 10 mM AgNO 3 , 1 M HCl, and 100 mM ascorbic acid AA were mixed and stirred vigorously for 30 s;
[0032] (3) mixing the mixed solution of step (1) with the mixed solution of step (2) at a volume ratio of 18.76:1, stirring vigorously for 2 minutes, and then standing the obtained mixed solution at 30° C. for 2 hours;
[0033] (4) Collect the product by centrifugation at 10,000 rpm for 20 min, take the precipitate and disperse it in 10 mL of deionized water to obtain the Au BPs seed solution;
[0034] (5) Take 80mM CTAC and 10mM AgNO 3 , 100 mM ascorbic acid AA, and stirred vigorously for 2 min;
[0035] (6) The mixed solution obtained in step (5) and the Au BPs seed solution obtained in step (4) were mixed at a volume ratio of 11.5:1, stirred vigorously for 2 minutes, and then allowed to stand at 60° C. for 6 hours;
[0036] (7) Collect the product by centrifugation at 4000 rpm for 20 min, take the precipitate and disperse it in 10 mL of deionized water to obtain Au@Ag NRs solution. Figure 1As shown, the transmission electron microscopy image shows that Au@Ag NRs were successfully prepared, with a length of about 132nm and a width of about 24nm. Transmission electron microscopy measurement: Transmission electron microscopy was tested using a Hitachi H-8100IV transmission electron microscope at an accelerating voltage of 200kV;
[0037] (8) Using ethanol to prepare an ethanol solution of PVP with a mass fraction of 1%, the Au@Ag NRs solution obtained in step (7) was mixed with the ethanol solution of PVP in a volume ratio of 1:1, and ultrasonicated for 20 minutes to fully dissolve it. At this time, the Au@Ag NRs solution wrapped by PVP was prepared;
[0038] (9) Mix dichloromethane, deionized water, and the PVP-coated Au@Ag NRs solution obtained in step (8) in a volume ratio of 16:36:1;
[0039] (10) Take the mixed solution of step (9), mix it again with n-hexane at a volume ratio of 4.4:1, ultrasonicate for 5 minutes, and let it stand for 30 minutes. During the standing process, Au@Ag NRs are driven to the interface between water and n-hexane. The Au@Ag NRs are transferred to a glass sheet (length, width = 0.5 cm square) by using a pulling method and tweezers to pick up the glass sheet. The preparation of the oriented ordered-Au@Ag NRs film is completed. Figure 2 As shown, the scanning electron microscopy image of the oriented ordered-Au@Ag NRs film demonstrates that the three-phase interface self-assembly method can be used to prepare a large-area, flat, single-layer, Au NRs oriented film.
[0040] (11) Synthesis of upconversion nanoparticles NaYF by a classical solvothermal method 4 :20%Er 3+ . Take 0.24g of yttrium chloride hexahydrate powder and 0.076g of erbium chloride hexahydrate powder in a three-necked bottle, add 6ml of oleic acid and 15ml of octadecene solution, fix it in an oil bath, under nitrogen protection at 160℃, stir at 700rpm until the drugs in the three-necked bottle are completely dissolved, and then cool to 30℃.
[0041] (12) Take 0.1g of sodium hydroxide and 0.148g of ammonium fluoride powder and dissolve them in 6ml of methanol solution. Slowly add the methanol mixed solution into the mixed solution obtained in step (11), and after sufficient stirring (about 1h), the temperature is raised from room temperature to 125°C. During the heating process, bubbles continue to emerge from the three-necked flask. After there is no foam in the three-necked flask, a condenser is connected. The temperature of the solution in the three-necked flask is slowly raised to 300°C, and after sufficient stirring for 2h, the heating is stopped and the temperature is lowered to 30°C.
[0042] (13) The mixed solution obtained in step (12) was divided into centrifuge tubes, 18 ml of ethanol solution was added to the centrifuge tubes, and the mixture was centrifuged at 10,000 rpm for 20 min. The supernatant was poured out, 18 ml of cyclohexane solution was added, and the precipitate was dissolved by ultrasonication. Then, 18 ml of ethanol solution was added and centrifuged again. This step was repeated twice to obtain NaYF 4 :20%Er 3+ After the precipitate was collected in the centrifuge tube, 5 ml of cyclohexane was added and the NaYF solution with a molar concentration of 0.2 mol / L was obtained after ultrasonication. 4 :20%Er 3+ Cyclohexane solution.
[0043] (14) Prepare a 1% PVP ethanol solution using ethanol, and take the NaYF 4 :20%Er 3+ The cyclohexane solution and the ethanol solution of PVP were mixed in a volume ratio of 1:1 and ultrasonicated for 20 min to fully dissolve the NaYF encapsulated by PVP. 4 :20%Er 3+ The solution preparation is completed;
[0044] (15) Take dichloromethane, deionized water, and the PVP-coated NaYF obtained in step (14) 4 :20%Er 3+ The solutions were mixed in a volume ratio of 16:36:1;
[0045] (16) Take the mixed solution of step (15), mix it again with n-hexane at a volume ratio of 4.4:1, sonicate for 5 minutes, and let it stand for 30 minutes. During the standing period, the upconversion nanoparticles NaYF 4 :20%Er 3+ The ordered Au@Ag NRs thin film glass sheet obtained in step (10) was picked up by tweezers using the pulling method, and the upconversion nanoparticles NaYF 4 :20%Er 3+ Transferred to a glass slide (length, width = 0.5 cm square), that is, the oriented ordered-Au@AgNRs / NaYF 4 :20%Er 3+ The composite film is prepared. Figure 3 As shown, the oriented ordered-Au@Ag NRs / NaYF 4 :20%Er 3+ The scanning electron microscope image of the composite film shows that a large-area, flat, layered composite film was successfully prepared using the three-phase interface self-assembly method again.
[0046] (17) 1 mL of a DMF / DMSO mixed solution was prepared in a volume ratio of 2.33:1, and then 0.1 mmol of PbI was added to the mixed solution. 2 and 0.1mmol MAI, and let stand for 3h. 2 After complete dissolution with MAI, it indicates that the preparation of perovskite precursor solution is complete;
[0047] (18) Transfer the perovskite precursor solution obtained in step (17) to the ordered-Au@AgNRs / NaYF prepared in step (16) 4 :20%Er 3+ The composite film was transferred to a glove box. 80 μL of the perovskite precursor solution was dropped onto the ordered Au@Ag NRs / NaYF prepared in step (16). 4 :20%Er 3+ The spin coater was set to a low speed of 600 rpm for 6 s and a high speed of 4000 rpm for 40 s. The timing started when the spin coater changed from low speed to high speed. After 15 s, the perovskite precursor / ordered-Au@Ag NRs / NaYF 4 :20%Er 3+ 400 μL of chlorobenzene was added dropwise onto the composite film;
[0048] (19) After the spin coating was stopped, the glass slide was transferred to a heating table and heated in stages, first at 60 °C for 5 min, then at 100 °C for 10 min, and then MAPbI 3 / Ordered-Au@Ag NRs / NaYF 4 :20%Er 3+ The composite film is prepared;
[0049] (20) MAPbI prepared in step (19) 3 / Ordered-Au@Ag NRs / NaYF 4 :20%Er 3+ The composite film is transferred to a vacuum evaporator, and an Ag electrode is evaporated on the composite film. Thus, a polarization-sensitive 1550nm narrow-band photodetector is prepared. Figure 4 As shown, a polarization-sensitive 1550nm narrow-band photodetector MAPbI 3 / Ordered-Au@Ag NRs / NaYF 4 :20%Er 3+ PDs and non-polarization-sensitive 1550nm narrow-band photodetector MAPbI 3 / disordered-Au@Ag NRs / NaYF 4 :20%Er3+ Polar coordinate diagram of the photocurrent response of PDs to 1550nm polarized light at different polarization angles. Thanks to the polarization-sensitive properties of the oriented ordered-Au@Ag NRs array, MAPbI 3 / Ordered-Au@Ag NRs / NaYF 4 :20%Er 3+ The PDs exhibited good polarization sensitivity, DOP=0.63.
[0050] (21) The prepared polarization-sensitive 1550nm narrow-band photodetectors are arranged in an array, and each photodetector in the array is an imaging pixel point. The whole constitutes a polarization photodetection and visualization imaging device, which can be used to detect 1550nm polarized laser. Before the test, a scanning electron microscope is used to observe the arrangement direction of the ordered-Au@Ag NRs. The polarization angle is set to 0° in the direction parallel to the ordered-Au@Ag NRs. The polarization angle gradually increases as the polarized light rotates clockwise. When applied, the template to be imaged is placed between the polarized excitation light and the device. The polarization angle of the incident light is changed by adjusting the polarizer. Under the condition of external bias, the photocurrent of each photodetector in the imaging array is recorded, which leads to differences in the final imaging results. When the polarization angle is 0°, the photoresponse current value at this time is recorded as I max ; When the polarization angle is 90°, the photoresponse current value is I min , the polarization sensitivity (Degree of polarization, DOP) of the device is obtained according to the following formula:
[0051] DOP=(I max -I min ) / (I max +I min )
[0052] The imaging process of the optoelectronic imaging device obtained in this embodiment is as follows: Figure 5 As shown in the figure, the 1550nm excitation light is converted into polarized light after passing through the polarizer, and then irradiated to MAPbI through the imaging template. 3 / Ordered-Au@Ag NRs / NaYF 4 :20%Er 3+ On the PDs array, by changing the angle of the polarizer, the data of each detector in the detector array is recorded. Figure 6 As shown, the photocurrent data of each detector is recorded, and after being processed by Origin software, the imaging results are displayed.
[0053] Embodiment 2:
[0054] (1) Take 400mM CTAC, 65mM citric acid, 72mM NaBH 4 , 2 mM HAuCl 4 After mixing and vigorously stirring for 2 min, the mixed solution was slowly stirred at 105 °C for 13 h;
[0055] (2) Take 300mM CTAB and 75mM HAuCl 4 , 80 mM AgNO 3 , 1.2 M HCl, and 120 mM ascorbic acid AA were mixed and stirred vigorously for 30 s;
[0056] (3) mixing the mixed solution of step (1) with the mixed solution of step (2) at a volume ratio of 22.6:1, stirring vigorously for 2 minutes, and then standing the obtained mixed solution at 45° C. for 5 hours;
[0057] (4) Collect the product by centrifugation at 12000 rpm for 30 min, take the precipitate and disperse it in 50 mL of deionized water to obtain the Au BPs seed solution;
[0058] (5) Take 92mM CTAC and 18mM AgNO 3 , 120 mM ascorbic acid AA, and stirred vigorously for 2 min;
[0059] (6) The mixed solution obtained in step (5) and the Au BPs seed solution obtained in step (4) were mixed at a volume ratio of 32.5:1, stirred vigorously for 2 minutes, and then allowed to stand at 82° C. for 15 hours;
[0060] (7) The product was collected by centrifugation at 8000 rpm for 30 min, and the precipitate was dispersed in 45 mL of deionized water to obtain an Au@Ag NRs solution.
[0061] (8) Using ethanol to prepare an ethanol solution of PVP with a mass fraction of 10%, the Au@Ag NRs solution obtained in step (7) was mixed with the ethanol solution of PVP at a volume ratio of 65:1, and ultrasonicated for 35 minutes to fully dissolve it. At this time, the Au@Ag NRs solution wrapped by PVP was prepared;
[0062] (9) Mix dichloromethane, deionized water, and the PVP-coated Au@Ag NRs solution obtained in step (8) in a volume ratio of 61.3:86.8:1;
[0063] (10) Take the mixed solution of step (9), mix it again with n-hexane at a volume ratio of 50:1, ultrasonicate for 5 minutes, and let it stand for 80 minutes. During the standing process, Au@Ag NRs are driven to the interface between water and n-hexane. The Au@Ag NRs are transferred to a glass slide (length, width = 0.5 cm square) by using a Czochralski method and tweezers to pick up the glass slide. The ordered-Au@Ag NRs film is prepared.
[0064] (11) Synthesis of upconversion nanoparticles NaYF by a classical solvothermal method 4 :35%Er 3+ . Take 0.197g of yttrium chloride hexahydrate powder and 0.134g of erbium chloride hexahydrate powder in a three-necked bottle, add 10ml of oleic acid and 25ml of octadecene solution, fix it in an oil bath, under nitrogen protection at 180℃, stir at 850rpm until the drugs in the three-necked bottle are completely dissolved, and then cool to 38℃.
[0065] (12) Take 0.2g of sodium hydroxide and 0.498g of ammonium fluoride powder and dissolve them in 10ml of methanol solution. Slowly add the methanol mixed solution into the mixed solution obtained in step (11), and after sufficient stirring (about 1h), the temperature is raised from room temperature to 135°C. During the heating process, bubbles continue to emerge from the three-necked flask. After there is no bubble in the three-necked flask, a condenser is connected. The temperature of the solution in the three-necked flask is slowly raised to 310°C, and after sufficient stirring for 2h, the heating is stopped and the temperature is lowered to 38°C.
[0066] (13) The mixed solution obtained in step (12) was divided into centrifuge tubes, 28 ml of ethanol solution was added to the centrifuge tubes, and the mixture was centrifuged at 11000 rpm for 30 min. The supernatant was poured out, 28 ml of cyclohexane solution was added, and the precipitate was dissolved by ultrasonication. Then 28 ml of ethanol solution was added and centrifuged again. This step was repeated twice to obtain NaYF 4 :35%Er 3+ After the precipitate was collected in the centrifuge tube, 2 ml of cyclohexane was added and the NaYF solution with a molar concentration of 0.5 mol / L was obtained after ultrasonication. 4 :35%Er 3+ Cyclohexane solution.
[0067] (14) Prepare an ethanol solution of PVP with a mass fraction of 11% using ethanol, and take the NaYF 4 :35%Er 3+ The cyclohexane solution and the ethanol solution of PVP were mixed in a volume ratio of 65.5:1 and ultrasonicated for 36 min to fully dissolve the NaYF encapsulated by PVP. 4 :35%Er 3+ The solution preparation is completed;
[0068] (15) Take dichloromethane, deionized water, and the PVP-coated NaYF obtained in step (14) 4 :35%Er 3+ The solutions were mixed in a volume ratio of 64.5:87.2:1;
[0069] (16) The mixed solution of step (15) was mixed again with n-hexane at a volume ratio of 51:1, ultrasonicated for 5 minutes, and then allowed to stand for 80 minutes. During the standing period, the upconversion nanoparticles NaYF 4 :35%Er 3+ The ordered Au@Ag NRs thin film glass sheet obtained in step (10) was picked up by tweezers using the pulling method, and the upconversion nanoparticles NaYF 4 :35%Er 3+ Transferred to a glass slide (length, width = 0.5 cm square), that is, the oriented ordered-Au@AgNRs / NaYF 4 :35%Er 3+ The composite film preparation is completed.
[0070] (17) Prepare 2 mL of a DMF / DMSO mixed solution at a volume ratio of 4.68:1, and then add 2 mmol of PbI 2 and 2 mmol of MAI, and allowed to stand for 10 h. 2 After complete dissolution with MAI, it indicates that the preparation of perovskite precursor solution is complete;
[0071] (18) Transfer the perovskite precursor solution obtained in step (17) to the ordered-Au@AgNRs / NaYF prepared in step (16) 4 :35%Er 3+ The composite film was transferred to a glove box. 202 μL of the perovskite precursor solution was dropped onto the ordered-Au@Ag NRs / NaYF prepared in step (16). 4 :35%Er 3+ The spin coater was set to a low speed of 800 rpm for 8 s and a high speed of 6000 rpm for 80 s. The timing started when the spin coater changed from low speed to high speed. After 32 s, the perovskite precursor / ordered-Au@Ag NRs / NaYF 4 :35%Er 3+ 1400 μL of chlorobenzene was added dropwise onto the composite film;
[0072] (19) After the spin coating was stopped, the glass slide was transferred to the heating stage and heated in stages, first at 80 °C for 12 min, then at 180 °C for 16 min, and then MAPbI 3 / Ordered-Au@Ag NRs / NaYF 4 :35%Er 3+ The composite film is prepared;
[0073] (20) MAPbI prepared in step (19) 3 / Ordered-Au@Ag NRs / NaYF 4 :35%Er 3+ The composite film is transferred to a vacuum evaporator, and a Ag electrode is evaporated on the composite film. Thus, a polarization-sensitive 1550nm narrow-band photodetector is prepared.
[0074] (21) The prepared polarization-sensitive 1550 nm narrow-band photodetectors are arranged in an array, and each photodetector in the array is an imaging pixel point, and the whole constitutes a polarization photodetection and visualization imaging device.
[0075] Embodiment 3:
[0076] (1) Take 650mM CTAC, 100mM citric acid, 142mM NaBH 4 , 3 mM HAuCl 4 After mixing and vigorously stirring for 2 min, the mixed solution was slowly stirred at 175 °C for 18 h;
[0077] (2) Take 320mM CTAB and 105mM HAuCl 4 , 120 mM AgNO 3 , 1.5 M HCl, and 145 mM ascorbic acid AA were mixed and stirred vigorously for 30 s;
[0078] (3) mixing the mixed solution of step (1) with the mixed solution of step (2) at a volume ratio of 88.2:1, stirring vigorously for 2 minutes, and then standing the obtained mixed solution at 75° C. for 18 hours;
[0079] (4) Collect the product by centrifugation at 14000 rpm for 40 min, take the precipitate and disperse it in 80 mL of deionized water to obtain the Au BPs seed solution;
[0080] (5) Take 102mM CTAC and 46mM AgNO 3 , 147 mM ascorbic acid AA, and stirred vigorously for 2 min;
[0081] (6) The mixed solution obtained in step (5) and the Au BPs seed solution obtained in step (4) were mixed at a volume ratio of 50:1, stirred vigorously for 2 minutes, and then allowed to stand at 130° C. for 38 hours;
[0082] (7) The product was collected by centrifugation at 15000 rpm for 40 min, and the precipitate was dispersed in 100 mL of deionized water to obtain an Au@Ag NRs solution.
[0083] (8) Using ethanol to prepare an ethanol solution of PVP with a mass fraction of 20%, the Au@Ag NRs solution obtained in step (7) was mixed with the ethanol solution of PVP at a volume ratio of 100:1, and ultrasonicated for 100 minutes to fully dissolve it. At this time, the Au@Ag NRs solution wrapped by PVP was prepared;
[0084] (9) Mix dichloromethane, deionized water, and the PVP-coated Au@Ag NRs solution obtained in step (8) in a volume ratio of 198.2:260:1;
[0085] (10) Take the mixed solution of step (9), mix it again with n-hexane at a volume ratio of 100:1, ultrasonicate for 5 minutes, and let it stand for 120 minutes. During the standing process, Au@Ag NRs are driven to the interface between water and n-hexane, and the Au@Ag NRs are transferred to a glass slide (length, width = 0.5 cm square) by using tweezers to pick up the glass slide by the pulling method, and the ordered-Au@AgNRs film is prepared.
[0086] (11) Synthesis of upconversion nanoparticles NaYF by a classical solvothermal method 4 :50%Er 3+ . Take 0.152g of yttrium chloride hexahydrate powder and 0.191g of erbium chloride hexahydrate powder in a three-necked bottle, add 20ml of oleic acid and 45ml of octadecene solution, fix it in an oil bath, under nitrogen protection at 190℃, stir at 950rpm until the drugs in the three-necked bottle are completely dissolved, and then cool to 42℃.
[0087] (12) Take 0.5g of sodium hydroxide and 0.762g of ammonium fluoride powder and dissolve them in 30ml of methanol solution. Slowly add the methanol mixed solution into the mixed solution obtained in step (11), and after sufficient stirring (about 1h), the temperature is raised from room temperature to 145°C. During the heating process, bubbles continue to emerge from the three-necked flask. After there is no bubble in the three-necked flask, a condenser is connected. The temperature of the solution in the three-necked flask is slowly raised to 330°C, and after sufficient stirring for 3h, the heating is stopped and the temperature is lowered to 42°C.
[0088] (13) The mixed solution obtained in step (12) was divided into centrifuge tubes, 48 ml of ethanol solution was added to the centrifuge tubes, and the mixture was centrifuged at 12000 rpm for 40 min. The supernatant was poured out, 48 ml of cyclohexane solution was added, and the precipitate was dissolved by ultrasonication. Then 48 ml of ethanol solution was added and centrifuged again. This step was repeated twice to obtain NaYF 4 :50%Er 3+ The precipitate in the centrifuge tube was collected and added with 60 ml of cyclohexane. After ultrasonication, NaYF with a molar concentration of 0.02 mol / L was obtained. 4 :50%Er 3+ Cyclohexane solution.
[0089] (14) Prepare an ethanol solution of PVP with a mass fraction of 21.6% using ethanol, and take the NaYF 4 :50%Er 3+ The cyclohexane solution and the ethanol solution of PVP were mixed in a volume ratio of 99:1 and ultrasonicated for 100 min to fully dissolve the NaYF encapsulated by PVP. 4 :50%Er 3+ The solution preparation is completed;
[0090] (15) Take dichloromethane, deionized water, and the PVP-coated NaYF obtained in step (14) 4 :50%Er 3+ The solutions were mixed in a volume ratio of 199:249:1;
[0091] (16) Take the mixed solution of step (15), mix it again with n-hexane at a volume ratio of 100:1, sonicate for 5 minutes, and let it stand for 120 minutes. During the standing period, the upconversion nanoparticles NaYF 4 :50%Er 3+ The ordered Au@Ag NRs thin film glass sheet obtained in step (10) was picked up by tweezers using the pulling method, and the upconversion nanoparticles NaYF 4 :50%Er 3+ Transferred to a glass slide (length, width = 0.5 cm square), that is, the oriented ordered-Au@Ag NRs / NaYF 4 :50%Er 3+ The composite film preparation is completed.
[0092] (17) 8.2 mL of a DMF / DMSO mixed solution was prepared in a volume ratio of 7.93:1, and then 8.2 mmol of PbI was added to the mixed solution. 2 and 8.2 mmol of MAI, and allowed to stand for 20 h.2 After complete dissolution with MAI, it indicates that the preparation of perovskite precursor solution is complete;
[0093] (18) Transfer the perovskite precursor solution obtained in step (17) to the ordered-Au@AgNRs / NaYF prepared in step (16) 4 :50%Er 3+ The composite film was transferred to the glove box. 300 μL of the perovskite precursor solution was dropped onto the ordered-Au@Ag NRs / NaYF prepared in step (16). 4 :50%Er 3+ The spin coater was set to a low speed of 1000 rpm for 10 s and a high speed of 8000 rpm for 100 s. The timing was started when the spin coater changed from low speed to high speed. After 40 s, the perovskite precursor / ordered-Au@Ag NRs / NaYF 4 :50%Er 3+ 2000 μL of chlorobenzene was added dropwise onto the composite film;
[0094] (19) After the spin coating was stopped, the glass sheet was transferred to the heating table and heated in stages, first at 90 °C for 20 min, then at 260 °C for 20 min, and then MAPbI 3 / Ordered-Au@Ag NRs / NaYF 4 :50%Er 3+ The composite film is prepared;
[0095] (20) MAPbI prepared in step (19) 3 / Ordered-Au@Ag NRs / NaYF 4 :50%Er 3+ The composite film is transferred to a vacuum evaporator, and a Ag electrode is evaporated on the composite film. Thus, a polarization-sensitive 1550nm narrow-band photodetector is prepared.
[0096] (21) The prepared polarization-sensitive 1550 nm narrow-band photodetectors are arranged in an array, and each photodetector in the array is an imaging pixel point, and the whole constitutes a polarization photodetection and visualization imaging device.
Claims
1. A method for preparing a 1550nm up-conversion polarization photoelectric detection and visualization imaging device, characterized in that: The specific steps are as follows: Step 1: Preparation of Au@Ag NRs using the seed-grown method First, prepare the Au nanocone seed solution Au BPs for growing the outer Ag shell: use the cationic surfactant CTAC and citric acid to modify the surface of HAuCl4, and mix CTAC, citric acid, NaBH4 and HAuCl4 in a molar ratio of (100-900): (10-130): (10-200): 1; slowly stir the mixed solution at 50-180 ° C for 2-24 h to obtain solution A; CTAB, HAuCl4, AgNO3, HCl and ascorbic acid AA in a molar ratio of (0.2 -30): (0.1-20): (0.05-60): (0.2-100): 1 to obtain solution B; solution B and solution A are mixed in a volume ratio of (1-100): 1, and allowed to stand at 20-80° C. for 0.5-24 h; the product is collected by centrifugation at a speed of 5000-15000 rpm for 10-40 min; the collected centrifugal product is dispersed in deionized water at a mass fraction of 1-90% to obtain an Au BPs seed solution; Growing Ag shell on the basis of Au BPs seed solution to prepare Au@Ag NRs: CTAC, AgNO3, and ascorbic acid AA are mixed in a molar ratio of (0.1-2.5): (0.05-10): 1 to obtain solution C; solution C is mixed with Au BPs seed solution in a volume ratio of (1-50): 1, and the mixture is allowed to stand at 20-100°C for 0.5-48h; the product is collected by centrifugation at a speed of 2000-15000rpm and a centrifugation time of 10-40min; the collected centrifugal product is dispersed in deionized water at a mass fraction of 1-90% to obtain Au@Ag NRs solution; Step 2: Preparation of oriented ordered Au@Ag NRs thin films using the three-phase interface self-assembly method PVP and ethanol are mixed in a mass ratio of (0.01-0.2):1 to obtain an ethanol solution of PVP with a mass fraction of 1-20%; Au@Ag NRs solution and PVP ethanol solution are mixed in a volume ratio of (0.1-100):1, and ultrasonicated for 20-100 minutes to fully dissolve them to obtain an Au@Ag NRs solution wrapped by PVP; dichloromethane, deionized water, and PVP ethanol solution are mixed in a volume ratio of (2-200):(2-300):1 to obtain solution D; solution D is then mixed with n-hexane in a volume ratio of (2-100):1, and allowed to stand for 5-120 minutes, at which time Au@Ag NRs are driven to the interface between water and n-hexane; Au@Ag NRs are transferred to a glass sheet by a pulling method to obtain an ordered-Au@Ag NRs film; Step 3: Synthesis of upconversion nanoparticles NaYF4:(10-50)%Er by solvothermal method 3+ , the ordered-Au@Ag NRs / NaYF4:(10-50)%%Er was prepared on the ordered-Au@Ag NRs film substrate using a three-phase self-assembly method. 3+ Composite film; PVP and ethanol are mixed in a mass ratio of (0.002-0.2):1 to obtain an ethanol solution of PVP with a mass fraction of 0.2-20%; upconversion nanoparticles NaYF4: (10-50)% Er 3+ Dissolve in cyclohexane to obtain NaYF4: (10-50)% Er with a molar concentration of (0.01-0.8) mol / L 3+ Cyclohexane solution, NaYF4: (10-50)% Er 3+ The cyclohexane solution and the ethanol solution of PVP were mixed in a volume ratio of (0.1-100):1, and ultrasonicated for 20-100 min to fully dissolve them, thereby preparing NaYF4:(10-50)%Er coated with PVP. 3+ Solution; dichloromethane, deionized water, and PVP ethanol solution were mixed in a volume ratio of (2-200): (2-300): 1 to obtain solution E; solution E was then mixed with n-hexane in a volume ratio of (2-100): 1, ultrasonicated for 5-120 minutes, and allowed to stand for 5-120 minutes. At this time, the upconversion nanoparticles NaYF4: (10-50)% Er 3+ Driven to the interface of water and n-hexane; using the pulling method, the upconversion nanoparticles NaYF4: (10-50)% Er 3+ Transfer to the ordered-Au@Ag NRs film glass substrate prepared in step 2 to obtain ordered-Au@Ag NRs / NaYF4:(10-50)%Er 3+ Composite film; Step 4: Preparation of MAPbI3 / ordered-Au@Ag NRs / NaYF4: (10-50)% Er 3+ Polarization-sensitive 1550 nm narrow-band photodetector: Ordered-Au@Ag NRs / NaYF4:(10-50)%Er prepared in step 3 3+ Based on the composite film, a two-step method was used to prepare the photodetector in the glove box atmosphere; First, a perovskite precursor solution was prepared: DMF and DMSO were mixed in a volume ratio of (1-8):1 to obtain a solution F; PbI2 and MAI were mixed in a molar ratio of (0.1-10):1 to obtain a mixture G; the mixture G was added to the solution F and allowed to stand for 1-20 hours to wait for PbI2 and MAI to be completely dissolved to obtain a perovskite precursor solution; the perovskite precursor solution was mixed with the ordered -Au@AgNRs / NaYF4:(10-50)%Er 3+ The composite film was transferred into the glove box; the perovskite precursor solution was dropped on the ordered-Au@AgNRs / NaYF4:(10-50)%Er 3+ On the composite film, turn on the spin coater and set it to low speed 200-1000rpm, maintain for 2-10s, high speed 2000-8000rpm, maintain for 20-100s, and obtain perovskite precursor / ordered-Au@Ag NRs / NaYF4:(10-50)%Er 3+ Composite film; start timing when the spin coater changes from low speed to high speed, and after 10-40s, spin coater spins the perovskite precursor / ordered-Au@Ag NRs / NaYF4:(10-50)%Er 3+ Chlorobenzene was dripped onto the composite film, and the volume ratio of chlorobenzene to perovskite precursor solution was (2-20):1; after the spin coater stopped, the glass sheet was transferred to a heating table and heated in stages, first at a low temperature of 10-100°C, maintained for 1-20 min, and then raised to a high temperature of 100-260°C, maintained for 1-20 min, to obtain MAPbI3 / ordered-Au@Ag NRs / NaYF4:(10-50)%Er 3+ Composite film; MAPbI3 / ordered-Au@Ag NRs / NaYF4:(10-50)%Er 3+ The composite film is transferred to a vacuum evaporator, and a Ag electrode is evaporated on the composite film to obtain a NIR narrow-band photodetector; Step 5: Preparation of MAPbI3 / ordered-Au@Ag NRs / NaYF4: (10-50)% Er 3+ Polarization-sensitive 1550nm polarization photodetection and visualization imaging device: MAPbI3 / ordered-Au@Ag NRs / NaYF4:(10-50)%Er prepared in step 4 3+ Based on the polarization-sensitive 1550nm narrow-band photodetector, a polarization photodetection and visualization imaging device is prepared; The prepared polarization-sensitive 1550nm narrow-band photodetectors are arranged in an array, and each photodetector in the array is an imaging pixel point, forming a polarization photodetection and visualization imaging device as a whole, which is used to detect 1550nm polarized laser.