Memory component and method of manufacturing the same

By using a control structure of stacked stop layers and oxide layers in the photolithography process to adjust the etching rate, the problem of insufficient etching caused by the loading effect is solved, the effective patterning of the array area and the peripheral area is realized, the floating gate is avoided, and a stacked structure of different densities is formed.

CN115206979BActive Publication Date: 2024-11-12WINBOND ELECTRONICS CORP
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
CN202110400165.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-14
Publication Date
2024-11-12
Estimated Expiration
2041-04-14

AI Technical Summary

Technical Problem

When shrinking critical dimensions, existing photolithography processes face the problem of insufficient etching of memory cells in the array area due to load effects, which can lead to short circuits or gate short circuits.

Method used

A control structure is adopted, including stacked stop layers and oxide layers, and openings of different densities are formed through a self-aligned dual patterning process to adjust the etch rate, thereby reducing the load effect and avoiding short circuits of the floating gate caused by incomplete etching.

Benefits of technology

It effectively reduces the load effect of the etching process, ensures that the target layers of the array area and the peripheral area are patterned at the same time, avoids short circuit problems caused by the floating gate not being completely isolated, and realizes stacked structures with different pattern densities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115206979B_ABST
    Figure CN115206979B_ABST
Patent Text Reader

Abstract

This invention provides a memory component and a method for manufacturing the same. The memory component includes a substrate, a plurality of first stacked structures, and a plurality of second stacked structures. The substrate includes an array region and a peripheral region. The first stacked structures are disposed on the substrate of the array region. Each first stacked structure sequentially includes: a first tunneling dielectric layer, a first floating gate, a first inter-gate dielectric layer, a first control gate, a first metal layer, a first capping layer, and a first stop layer. The second stacked structures are disposed on the substrate of the peripheral region. Each second stacked structure sequentially includes: a second tunneling dielectric layer, a second floating gate, a second inter-gate dielectric layer, a second control gate, a second metal layer, a second capping layer, and a second stop layer. The pattern density of the first stacked structures is greater than the pattern density of the second stacked structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a semiconductor component and a manufacturing method thereof, and in particular to a memory component and a manufacturing method thereof. Background Art

[0002] With the advancement of technology, all kinds of electronic products are developing towards a trend of being thinner, lighter and smaller. Under this trend, the critical dimensions of memory components are also gradually reduced, making the photolithography process more and more difficult. In the existing photolithography process, the method of reducing the critical dimensions is to use optical components with larger numerical aperture (NA), shorter exposure wavelength (such as EUV) or use immersion lithography technology. However, as the resolution of the existing photolithography process approaches the theoretical limit, the traditional photolithography method is no longer sufficient, and the double-patterning (DP) method has begun to be used to overcome the optical problem and thus improve the resolution of the memory components.

[0003] In the current patterning method, due to the different pattern densities between the peripheral region and the array region, the etching process is subject to a loading effect, which in turn causes a circuit short circuit or gate short circuit in the memory cells in the array region due to insufficient etching. Summary of the invention

[0004] The present invention provides a method for manufacturing a memory component, comprising: providing a substrate, wherein the substrate comprises an array area and a peripheral area; sequentially forming a stacking layer, a control structure, a hard mask layer and a mask pattern on the substrate, wherein the control structure comprises at least a first stop layer, a first oxide layer, a second stop layer and a second oxide layer; forming a photoresist layer in the mask pattern of the peripheral area; using the photoresist layer and the mask pattern as masks, removing part of the hard mask layer, part of the second oxide layer and part of the second stop layer in the array area, thereby forming a plurality of first openings in the array area; after removing the photoresist layer, removing part of the hard mask layer in the peripheral area, thereby forming at least one second opening in the peripheral area; performing a first etching process, removing part of the control structure, thereby extending the plurality of first openings and the second openings into the control structure, thereby forming a plurality of third openings and at least one fourth opening, wherein the bottom surface of the fourth opening is higher than the bottom surface of the plurality of third openings; and performing a second etching process, removing part of the stacking layer, thereby extending the plurality of third openings and the fourth openings into the stacking layer, thereby forming a plurality of fifth openings and at least one sixth opening.

[0005] The present invention provides a memory component, comprising: a substrate, a plurality of first stacking structures and a plurality of second stacking structures. The substrate comprises an array region and a peripheral region. The first stacking structure is arranged on the substrate in the array region. Each of the first stacking structures sequentially comprises: a first tunneling dielectric layer, a first floating gate, a first intergate dielectric layer, a first control gate, a first metal layer, a first cap layer and a first stop layer. The second stacking structure is arranged on the substrate in the peripheral region. Each of the second stacking structures sequentially comprises: a second tunneling dielectric layer, a second floating gate, a second intergate dielectric layer, a second control gate, a second metal layer, a second cap layer and a second stop layer.

[0006] The present invention provides a patterning method, comprising: sequentially forming a control structure, a hard mask layer and a mask pattern on a target layer, wherein the control structure comprises a plurality of stop layers and a plurality of oxide layers stacked on each other; forming a photoresist layer in the mask pattern on the hard mask layer; using the photoresist layer and the mask pattern as masks, removing a portion of the hard mask layer and a portion of the control structure to form a plurality of first openings; removing the photoresist layer and the hard mask layer thereunder to form at least one second opening, wherein the bottom surface of the second opening is higher than the bottom surfaces of the plurality of first openings; and performing one or more etching processes to extend the plurality of first openings and the second openings into the control structure and the target layer, thereby separating the target layer and the control structure into a plurality of stacked structures.

[0007] In the embodiment of the present invention, a control structure can be formed between the target layer and the hard mask layer. The control structure includes multiple stop layers and multiple oxide layers stacked on each other, thereby controlling the etching rate of the array area and the peripheral area to effectively reduce the load effect of the etching process and avoid the short circuit problem caused by incomplete isolation between the floating gates due to incomplete etching of adjacent floating gates in the array area. In this case, the target layers in the array area and the peripheral area are patterned at the same time, thereby forming multiple stacked structures with different pattern densities in the array area and the peripheral area.

[0008] In order to make the above features and advantages of the present invention more clearly understood, embodiments are given below with reference to the accompanying drawings for detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figures 1A to 1H is a cross-sectional schematic diagram of a method for manufacturing a memory component according to an embodiment of the present invention;

[0010] Figure 2 is a cross-sectional schematic diagram of a control structure of another embodiment of the present invention;

[0011] Figure 3 is a cross-sectional schematic diagram of a control structure of another embodiment of the present invention;

[0012] Figure 4is a flow chart of a patterning method according to an embodiment of the present invention. DETAILED DESCRIPTION

[0013] Figures 1A to 1H FIG. 4 is a cross-sectional schematic diagram of a manufacturing process of a memory component according to an embodiment of the present invention. Figure 2 It is a cross-sectional schematic diagram of a control structure of another embodiment of the present invention. Figure 3 It is a cross-sectional schematic diagram of a control structure of another embodiment of the present invention.

[0014] Please refer to Figure 1A An embodiment of the present invention provides a method for manufacturing a memory component, and the steps are as follows. First, a substrate 100 is provided. The substrate 100 may include an array region R1 and a peripheral region R2. In this embodiment, the array region R1 may be a memory array region having one or more memory cells, and the peripheral region R2 may be a peripheral circuit region having one or more selection gates.

[0015] Next, a stacked layer 110 (also referred to as a target layer) is formed on the substrate 100. Specifically, Figure 1A As shown, the stacked layer 110 includes, from bottom to top, a tunnel dielectric layer 102 , a floating gate 104 , an inter-gate dielectric layer 106 , a control gate 108 , a metal layer 112 , and a cap layer 114 .

[0016] In one embodiment, the material of the tunnel dielectric layer 102 may be, for example, silicon oxide. In one embodiment, the material of the floating gate 104 may include a conductive material, such as doped polysilicon, undoped polysilicon, or a combination thereof. In one embodiment, the intergate dielectric layer 106 may be, for example, a composite layer composed of nitride / oxide / nitride / oxide / nitride (Nitride / Oxide / Nitride / Oxide / Nitride, NONON), but the present invention is not limited thereto, and this composite layer may be three layers, five layers or more layers;. In one embodiment, the material of the control gate 108 may include a conductive material, such as doped polysilicon, undoped polysilicon, or a combination thereof. In one embodiment, the material of the metal layer 112 may be, for example, W, Co, Ni, or a combination thereof. In one embodiment, the material of the cap layer 114 may include a dielectric material, such as silicon nitride, silicon oxynitride, or a combination thereof.

[0017] Then, a control structure 120 is formed on the stacked layer 110. Specifically, Figure 1AAs shown, the control structure 120 includes a first stop layer 122, a first oxide layer 124, a second stop layer 126, and a second oxide layer 128 from bottom to top. In one embodiment, the first stop layer 122 and the second stop layer 126 may have the same dielectric material, such as silicon nitride, silicon oxynitride, or a combination thereof. In one embodiment, the first oxide layer 124 and the second oxide layer 128 may have the same material, such as silicon oxide. In this embodiment, the material of the first stop layer 122 and the second stop layer 126 is different from the material of the first oxide layer 124 and the second oxide layer 128. For example, the first stop layer 122 and the second stop layer 126 may be a silicon nitride layer, and the first oxide layer 124 and the second oxide layer 128 may be a silicon oxide layer. In an alternative embodiment, the first stop layer 122 and the second stop layer 126 and the first oxide layer 124 and the second oxide layer 128 may have dielectric materials with different etching selectivities. In addition, the thickness of the first oxide layer 124 may be greater than the thickness of the second oxide layer 128, and the thickness of the first stop layer 122 may be greater than the thickness of the second stop layer 126. However, the present invention is not limited thereto.

[0018] Although Figure 1A The control structure 120 shown includes two stop layers and two oxide layers, but the present invention is not limited thereto. In one embodiment, the control structure 120 may include a plurality of stop layers and a plurality of oxide layers stacked on each other. Specifically, Figure 2 As shown, the control structure 220 may include three stop layers 222 and three oxide layers 224 stacked on top of each other. Figure 3 As shown, the control structure 320 may include four stop layers 322 and four oxide layers 324 stacked on each other. In other words, the number of stop layers and oxide layers can be adjusted according to demand, and the present invention is not limited thereto. In one embodiment, the thickness T1 of the control structure 120 may be substantially greater than, less than, or equal to the thickness T2 of the control structure 220; and the thickness T2 of the control structure 220 may be substantially greater than, less than, or equal to the thickness T3 of the control structure 320. However, the present invention is not limited thereto. In addition, as Figure 2 and Figure 3 As shown, the stop layers 222 and 322 may have the same thickness, and the oxide layers 224 and 324 may also have the same thickness. However, the present invention is not limited thereto, and in other embodiments, the stop layers 222 and 322 may have different thicknesses, and the oxide layers 224 and 324 may also have different thicknesses.

[0019] Please refer back Figure 1A After forming the control structure 120, a hard mask stack 130 is formed on the control structure 120. Specifically, Figure 1AAs shown, the hard mask stack 130 includes a hard mask layer 132, a carbide layer 134, and an anti-reflection layer 136 from bottom to top. In one embodiment, the material of the hard mask layer 132 may be, for example, polysilicon. In one embodiment, the material of the carbide layer 134 may be, for example, spin-on-carbon (SoC). In one embodiment, the material of the anti-reflection layer 136 may be, for example, silicon oxynitride.

[0020] Afterwards, a photoresist pattern 138 is formed on the hard mask stack 130. In one embodiment.

[0021] Please refer to Figure 1B , a self-aligned double patterning (SADP) process is performed to form a mask pattern 140 on the hard mask layer 140. In detail, the anti-reflection layer 136 and the carbide layer 134 are patterned using the photoresist pattern 138. Next, a mask layer is first deposited on the sidewalls of the patterned reflective layer 136 and the sidewalls of the patterned carbide layer 134, and the etchback stops on the anti-reflection layer 136 or the carbide layer 134 to form a mask pattern 140, wherein the mask pattern 140 is formed on the above-mentioned sidewalls in the form of a spacer. Then, the patterned reflective layer 136 and the patterned carbide layer 134 are removed. In an alternative embodiment, a self-aligned quadruple patterning (SAQP) process may also be performed to form a mask pattern 140 with a higher pattern density on the hard mask layer 140.

[0022] Please refer to Figure 1C , a photoresist layer 142 is formed in the mask pattern 140 in the peripheral region R2.

[0023] Please refer to Figure 1C and Figure 1D , using the photoresist layer 142 and the mask pattern 140 as masks, remove a portion of the hard mask layer 132, a portion of the second oxide layer 128, and a portion of the second stop layer 126 in the array region R1, thereby forming a plurality of first openings 10 in the array region R1. Next, remove the photoresist layer 142 to expose the hard mask layer 132 in the peripheral region R2.

[0024] Please refer to Figure 1E , a dielectric layer 144, an anti-reflection layer 146 and a photoresist pattern 148 are sequentially formed on the substrate 100. The photoresist pattern 148 has at least one opening 11 corresponding to the hard mask layer 132 of the peripheral region R2.

[0025] Please refer to Figure 1E and Figure 1F, using the photoresist pattern 148 as a mask, remove part of the anti-reflection layer 146, part of the dielectric layer 144, and part of the hard mask layer 132 in the peripheral region R2 to form at least one second opening 12 in the peripheral region R2. Next, remove the remaining dielectric layer 144, anti-reflection layer 146, and photoresist pattern 148. After removal, a portion of the dielectric layer 144a is disposed next to the mask pattern 140 in the peripheral region R2 to surround the second opening 12, as shown in FIG. Figure 1F shown.

[0026] It is worth noting that the second opening 12 stops on the control structure 120 of the peripheral region R2 and exposes the top surface of the second oxide layer 128 of the peripheral region R2. The first opening 10 exposes the top surface of the first oxide layer 124 of the array region R1. In other words, the bottom surface of the first opening 10 can be lower than the bottom surface of the second opening 12, such as Figure 1F In one embodiment, the width 10w of the first opening 10 may be smaller than the width 12w of the second opening 12 .

[0027] Please refer to Figure 1F and Figure 1G , a first etching process is performed to remove a portion of the control structure 120, so as to extend the first opening 10 and the second opening 12 into the control structure 120, thereby forming a plurality of third openings 20 and at least one fourth opening 22. After the first etching process is performed, Figure 1G As shown, the fourth opening 22 stops on the first stop layer 122 of the peripheral region R2 (or exposes the top surface of the first stop layer 122 of the peripheral region R2), and the third opening 20 stops on the stacked layer 110 of the array region R1 (or exposes the top surface of the stacked layer 110 of the array region R1). In other words, the bottom surface of the third opening 20 can be lower than the bottom surface of the fourth opening 22.

[0028] It is worth noting that, since the opening density of the peripheral region R2 is greater than that of the array region R1, the removal rate of the control structure 120 in the peripheral region R2 is greater than that of the control structure 120 in the array region R1. In this case, the present embodiment can adjust the removal rates of the control structures 120 in the array region R1 and the peripheral region R2 through at least two stop layers 122 and 126 to prevent the depth of the fourth opening 22 from being deeper than the depth of the third opening 20.

[0029] Please refer to Figure 1G and Figure 1H , a second etching process is performed to remove a portion of the stack layer 110 so as to extend the third opening 20 and the fourth opening 22 into the stack layer 110, thereby forming a plurality of fifth openings 30 and at least one sixth opening 32. After the second etching process is performed, Figure 1HAs shown, the fifth opening 30 and the sixth opening 32 both stop on the tunnel dielectric layer 102 (or expose the top surface of the tunnel dielectric layer 102 ) to separate the stack layer 110 into a plurality of first stack structures 210 and a plurality of second stack structures 310 .

[0030] It is worth noting that the present embodiment can adjust the removal rate of the stacked layer 110 in the array region R1 and the peripheral region R2 by controlling at least two stop layers 122 and 126 in the structure 120, so that the fifth opening 30 and the sixth opening 32 can stop on the tunnel dielectric layer 102 at the same time. In other words, by having at least two stop layers in the control structure 120, the present embodiment can effectively reduce the load effect of the etching process and avoid the floating gate short circuit problem caused by the floating gates 104a on both sides of the fifth opening 30 not being completely isolated when the floating gates 104 in the array region R1 are not completely etched. In this case, if Figure 1H As shown, the bottom surface of the fifth opening 30 and the bottom surface of the sixth opening 32 can be considered flush.

[0031] like Figure 1H As shown, the first stacked structure 210 is configured on the substrate 100 of the array region R1. Specifically, each of the first stacked structures 210 may include: a tunneling dielectric layer 102a, a floating gate 104a, an inter-gate dielectric layer 106a, a control gate 108a, a metal layer 112a, a cap layer 114a, a stop layer 122a, and an oxide layer 124a in sequence. In addition, the second stacked structure 310 is configured on the substrate 100 of the peripheral region R2. Each of the second stacked structures 310 includes: a tunneling dielectric layer 102b, a floating gate 104b, an inter-gate dielectric layer 106b, a control gate 108b, a metal layer 112b, a cap layer 114b, a stop layer 122b, and an oxide layer 124b in sequence. The tunneling dielectric layer 102a is connected to the tunneling dielectric layer 102b to form a continuous tunneling dielectric structure 102.

[0032] In the present embodiment, the pattern density of the first stacked structure 210 is greater than the pattern density of the second stacked structure 310. In this case, the width W1 of each first stacked structure 210 may be smaller than the width W2 of the second stacked structure 310. In other words, the aspect ratio of each first stacked structure 210 may be greater than the aspect ratio of each second stacked structure 310. Since the first stacked structure 210 has a higher aspect ratio, each first stacked structure 210 has a shape that is wide at the bottom and narrow at the top, and each fifth opening 30 has a shape that is narrow at the bottom and wide at the top. Similarly, each second stacked structure 310 may also have a shape that is wide at the bottom and narrow at the top, while the sixth opening 32 has a shape that is narrow at the bottom and wide at the top. In addition, the width 30w of the fifth opening 30 may be smaller than the width 32w of the sixth opening 32.

[0033] In this embodiment, the first stacked structure 210 may be a storage unit having a flash memory; and the second stacked structure 310 may be a control unit having a select gate.

[0034] Although the above embodiments use flash memory and select gate as examples to illustrate a series of patterning steps, the present invention is not limited thereto. In other embodiments, the patterning steps may also be used to form contact windows, active areas (AA) of dynamic random access memory (DRAM) or similar target layers / films.

[0035] Figure 4 A flow chart 400 of a patterning method according to an embodiment of the present invention is shown. At step 402, a control structure, a hard mask layer, and a mask pattern are sequentially formed on a target layer. In one embodiment, the target layer comprises a single-layer structure, a double-layer structure, or a multi-layer structure. The control structure comprises a plurality of stop layers and a plurality of oxide layers stacked on each other. Figure 1A to Figure 1B A cross-sectional schematic diagram corresponding to step 402 is shown.

[0036] At step 404, a photoresist layer is formed in the mask pattern on the hard mask layer. Figure 1C A cross-sectional schematic diagram corresponding to step 404 is shown.

[0037] In step 406 , a portion of the hard mask layer and a portion of the control structure are removed using the photoresist layer and the mask pattern as masks, thereby forming a plurality of first openings. Figure 1D A cross-sectional schematic diagram corresponding to step 406 is shown.

[0038] At step 408, the photoresist layer and the hard mask layer thereunder are removed to form at least one second opening. In one embodiment, the bottom surface of the second opening is higher than the bottom surface of the first opening, and the width of the first opening is smaller than the width of the second opening. Figure 1E to Figure 1F A cross-sectional schematic diagram corresponding to step 408 is shown.

[0039] At step 410 , one or more etching processes are performed to extend the first opening and the second opening into the control structure and the target layer, thereby separating the target layer and the control structure into a plurality of stacked structures. Figure 1G to Figure 1H A cross-sectional schematic diagram corresponding to step 410 is shown.

[0040] In summary, the control structure can be formed between the target layer and the hard mask layer in the embodiment of the present invention. The control structure can include multiple stop layers and multiple oxide layers stacked on each other, thereby controlling the etching rate of the array area and the peripheral area to effectively reduce the load effect of the etching process and avoid the gate short circuit problem caused by the floating gate in the array area not being cut off. In this case, the target layers in the array area and the peripheral area can be patterned at the same time, thereby forming multiple stacked structures with different pattern densities in the array area and the peripheral area.

[0041] Although the present invention has been disclosed as above by way of embodiments, it is not intended to limit the present invention. Any person skilled in the art may make some changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the claims.

Claims

1. A method for manufacturing a memory component, comprising: Providing a substrate, wherein the substrate comprises an array region and a peripheral region; Sequentially forming a stacked layer, a control structure, a hard mask layer, and a mask pattern on the substrate, wherein the control structure at least includes a first stop layer, a first oxide layer, a second stop layer, and a second oxide layer; forming a photoresist layer in the mask pattern in the peripheral region; Using the photoresist layer and the mask pattern as masks, removing a portion of the hard mask layer, a portion of the second oxide layer, and a portion of the second stop layer in the array region, thereby forming a plurality of first openings in the array region; After removing the photoresist layer, removing a portion of the hard mask layer in the peripheral region to form at least one second opening in the peripheral region; Performing a first etching process to remove a portion of the control structure so as to extend the plurality of first openings and the second opening into the control structure, thereby forming a plurality of third openings and at least one fourth opening, wherein a bottom surface of the fourth opening is higher than a bottom surface of the plurality of third openings; as well as A second etching process is performed to remove a portion of the stack layer to extend the third openings and the fourth opening into the stack layer, thereby forming a plurality of fifth openings and at least one sixth opening. 2 . The method for manufacturing a memory device according to claim 1 , wherein the plurality of first openings expose a top surface of the first oxide layer in the array region, and the second openings expose a top surface of the second oxide layer in the peripheral region. 3 . The method for manufacturing a memory device according to claim 1 , wherein the plurality of third openings expose top surfaces of the stacked layers in the array region, and the fourth opening exposes a top surface of the first stop layer in the peripheral region. 4 . The method for manufacturing a memory device according to claim 1 , wherein a material of the first stop layer and the second stop layer is different from a material of the first oxide layer and the second oxide layer. 5 . The method for manufacturing a memory component according to claim 1 , wherein a width of the plurality of fifth openings is smaller than a width of the sixth opening.

6. A memory component comprising: A substrate, including an array region and a peripheral region; A plurality of first stacked structures are arranged on the substrate in the array region, wherein each of the first stacked structures sequentially comprises: a first tunneling dielectric layer, a first floating gate, a first intergate dielectric layer, a first control gate, a first metal layer, a first cap layer, a first stop layer and a first oxide layer, wherein the first stop layer and the first oxide layer are dielectric materials having different etching selectivities; and A plurality of second stack structures are arranged on the substrate in the peripheral region, wherein each second stack structure sequentially comprises: a second tunnel dielectric layer, a second floating gate, a second intergate dielectric layer, a second control gate, a second metal layer, a second cap layer and a second stop layer. 7 . The memory component of claim 6 , wherein a pattern density of the plurality of first stack structures is greater than a pattern density of the plurality of second stack structures.

8. The memory component of claim 6, wherein the plurality of second stacked structures include select gates.

9. The memory component of claim 6, wherein the first tunneling dielectric layer is connected to the second tunneling dielectric layer to form a continuous tunneling dielectric structure.

10. A patterning method comprising: forming a control structure, a hard mask layer, and a mask pattern in sequence on the target layer, wherein the control structure comprises a plurality of stop layers and a plurality of oxide layers stacked on each other; forming a photoresist layer in the mask pattern on the hard mask layer; Using the photoresist layer and the mask pattern as masks, removing a portion of the hard mask layer and a portion of the control structure, thereby forming a plurality of first openings; removing the photoresist layer and the hard mask layer thereunder to form at least one second opening, wherein a bottom surface of the second opening is higher than bottom surfaces of the plurality of first openings; as well as One or more etching processes are performed to extend the first openings and the second openings into the control structure and the target layer, thereby separating the target layer and the control structure into a plurality of stacked structures.

Citation Information

Patent Citations

  • Method of forming a gate of a semiconductor device

    CN101211770B

  • Equal gate height control method for semiconductor devices with different pattern densities

    CN105575899B

  • Semiconductor device and method for manufacturing the same

    CN109524400A

  • Integrated circuit device and method of forming semiconductor device

    CN112582420A

  • semiconductor device WITH REDUCED TRENCH LOADING EFFECT

    DE102017127203A1