A CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability and its preparation method and application
By using specific components and processes in CsPbBr3 perovskite quantum dot glass, the problem of material weakening luminous intensity at high temperature and high temperature melting during preparation is solved, and high light stability and high thermal stability are achieved, suitable for wide color gamut LED backlight display and reduces energy consumption.
Patent Information
- Application Number
- CN202211337584.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-10-28
AI Technical Summary
The luminous intensity of CsPbBr3 perovskite quantum dot glass is significantly weakened under high temperature and blue light irradiation, and requires high temperature melting and heat treatment during the preparation process, resulting in thermal stability and environmental protection problems.
The high-gloss stability and high thermal stability of components such as NH4H2PO4, SiO2, CaCO3, SrCO3, Al2O3, Pb compounds and bromide are prepared by melt molding and annealing treatment to avoid crystallization operations, which improves the crystallization operation. Thermal stability and environmental protection of the material.
CsPbBr3 perovskite quantum dot glass maintains a room temperature luminous intensity of 64% at 100℃. The luminous intensity remains basically unchanged under long-term operation, with good thermal stability and light stability. It is suitable for wide color gamut LED backlight display, and the preparation process Energy-saving and environmentally friendly.
Smart Images

Figure CN115806385B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of all-inorganic perovskite quantum dot display, and in particular relates to a CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability, and a preparation method and application thereof. Background Art
[0002] Green light materials with narrow-band emission characteristics are the most scarce fluorescent materials in wide color gamut LED backlight displays. CsPbBr3 quantum dots have become one of the most eye-catching green emission materials in the next generation of wide color gamut LED backlight displays due to their high photoluminescence quantum efficiency and extremely narrow half-peak width.
[0003] However, when CsPbBr3 is exposed to oxygen, moisture, heat and light, it is prone to structural decomposition or agglomeration, resulting in irreversible fluorescence quenching, which seriously hinders its application in the field of wide color gamut LED backlight display. In situ precipitation of CsPbBr3 perovskite quantum dots in the glass matrix is considered to be one of the main ways to solve its poor stability. The luminescence quantum efficiency of the CsPbBr3 perovskite quantum dot glass reported so far has been significantly improved, approaching the luminescence performance of colloidal quantum dots. However, its luminescence thermal stability and blue light resistance are still poor. Most CsPbBr3 perovskite quantum dot glasses can only maintain 10-30% of their initial luminescence intensity at 100°C. On blue LED chips, even if the operating current is only 20 mA, there is still obvious degradation. Therefore, CsPbBr3 perovskite quantum dot glass with high thermal stability and high light stability is still in urgent need of development to meet the requirements of wide color gamut LED backlight display for green light materials. In addition, the current main preparation method for quantum dot glass is high-temperature melting, followed by heat treatment and crystallization, which is neither economical nor environmentally friendly. Summary of the invention
[0004] One of the purposes of the present invention is to avoid the shortcomings of the prior art and provide a CsPbBr3 perovskite quantum dot glass with high thermal stability and high light stability. The CsPbBr3 perovskite quantum dot glass can still maintain a high luminous intensity at high temperatures and has high thermal stability. When operated on a blue light LED chip (20V, 20 mA) for a long time, its luminous intensity remains basically unchanged and has high light stability.
[0005] The second object of the present invention is to provide a method for preparing CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability. The preparation method does not require crystallization operation and has the effect of environmental protection and energy saving.
[0006] The third object of the present invention is to provide a CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability for application in the field of wide color gamut LED backlight display.
[0007] To achieve one of the above purposes, the present invention provides the following technical solutions:
[0008] Provided is a CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability, comprising the following components in molar percentage:
[0009] NH4H2PO4 55~75 mol%
[0010] SiO2 5~20 mol%
[0011] CaCO3 3~15 mol%
[0012] SrCO3 1~7 mol%
[0013] Al2O3 1~7 mol%
[0014] Pb compound 5~20 mol%
[0015] Bromide 5~20 mol%
[0016] Cs2CO35~20mol%;
[0017] The Pb compound is PbBr2 or PbO;
[0018] The bromide is NaBr or KBr.
[0019] The beneficial effects of the CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability of the present invention are as follows:
[0020] (1) The high light stability and high thermal stability CsPbBr3 perovskite quantum dot glass of the present invention has an emission main peak at 522 nm and a half-peak width of 25 nm. At 100°C, the CsPbBr3 quantum dot glass powder can still maintain 64% of its room temperature luminescence intensity, and after running on a blue light LED chip (20V, 20 mA) for 60 days, its luminescence intensity remains basically unchanged, that is, the luminescence intensity is basically not attenuated; these advantages can meet the actual use requirements and have excellent application prospects in the field of wide color gamut LED backlight display.
[0021] (2) The CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability of the present invention can be fully recovered after multiple cycles between room temperature and 140 °C. It has good thermal stability and meets the requirements of green light materials for wide color gamut LED backlight display.
[0022] (3) The CsPbBr3 perovskite quantum dot glass with high optical stability and high thermal stability of the present invention contains Al2O3 in its glass matrix composition. By adjusting the content of Al2O3, the self-crystallization behavior can be adjusted so that the main emission peak of the quantum dot glass is located at 522 nm and the half-peak width is 25 nm, thereby improving applicability.
[0023] To achieve the second objective above, the present invention provides the following technical solutions:
[0024] A method for preparing CsPbBr3 perovskite quantum dot glass is provided, and the preparation method of the CsPbBr3 perovskite quantum dot glass comprises the following steps:
[0025] S1. Weigh the components of the formula and mix them thoroughly, melt the mixed components at a certain temperature, and then pour them into a graphite mold to obtain self-crystallized glass;
[0026] S2. The self-crystallized glass is transferred into a muffle furnace for annealing to eliminate internal stress and obtain CsPbBr3 perovskite quantum dot glass.
[0027] In some embodiments, in step S1, the melting temperature is 1000-1200 °C, and the melting time is 20-60 min.
[0028] In some embodiments, in step S2, the annealing temperature is 200-450 °C, and the annealing time is 3-20 h.
[0029] In some embodiments, after step S2, the annealed CsPbBr3 perovskite quantum dot glass is ground into powder to obtain a finished product.
[0030] The beneficial effects of the method for preparing CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability of the present invention are as follows:
[0031] (1) The method for preparing the CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability of the present invention only requires annealing after the components are melted at high temperature and formed, without the need for subsequent secondary heating and crystallization, thus saving energy and complying with the concept of green chemistry.
[0032] (2) The method for preparing the CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability of the present invention has readily available raw materials, a simple preparation process, strong repeatability and is easy to prepare on a large scale.
[0033] To achieve the third of the above objectives, the present invention provides the application of the above CsPbBr3 perovskite quantum dot glass in the field of wide color gamut LED backlight display, so that it can be used in a variety of different types of wide color gamut LED backlight display devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the XRD diagram of the CsPbBr3 perovskite quantum dot glass sample with high photostability and high thermal stability in Example 1.
[0035] Figure 2 This is the TEM image of the CsPbBr3 perovskite quantum dot glass with high photostability and high thermal stability in Example 1.
[0036] Figure 3 This is the emission spectrum of the CsPbBr3 perovskite quantum dot glass with high photostability and high thermal stability in Example 2.
[0037] Figure 4 It is the internal quantum efficiency of the CsPbBr3 perovskite quantum dot fluorescent glass with high photostability and high thermal stability in Example 3 under 455nm excitation.
[0038] Figure 5 This is a study on the cyclic thermal stability of the high light stability and high thermal stability CsPbBr3 perovskite quantum dot glass powder in Example 4.
[0039] Figure 6 This is the fluorescence lifetime decay curve of the CsPbBr3 perovskite quantum dot glass with high photostability and high thermal stability in Example 5.
[0040] Figure 7 This is a study on the photostability of the CsPbBr3 perovskite quantum dot glass powder with high photostability and high thermal stability in Example 5.
[0041] Figure 8 This is the application of the CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability in Example 6 in a vehicle-mounted wide color gamut LED display backlight device (7 inches).
[0042] Fig. 9 This is the application of CsPbBr3 perovskite quantum dots in wide color gamut display in Example 6. DETAILED DESCRIPTION
[0043] The preferred embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the preferred embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.
[0044] The terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The singular forms "a", "the" used in the present invention and the appended claims are intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.
[0045] It should be understood that although the terms "first", "second", "third", etc. may be used to describe various information in the present invention, such information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of the present invention, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0046] Example 1
[0047] The chemical composition of the CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability in this embodiment is as follows: 68NH4H2PO4, 10SiO2, 5CaCO3, 3SrCO3, 7Al2O3, 9Cs2CO3, 18PbBr2 and 18NaBr
[0048] Table 1 Raw material composition of CsPbBr3 perovskite quantum dot glass in Example 1
[0049] ;
[0050] According to Table 1, accurately weigh analytically pure ammonium dihydrogen phosphate (NH4H2PO4), silicon dioxide (SiO2), calcium carbonate (CaCO3), strontium carbonate (SrCO3), aluminum oxide (Al2O3), cesium carbonate (Cs2CO3), lead bromide (PbBr2), and sodium bromide (NaBr). The accurately weighed raw materials were placed in an agate mortar and fully ground, mixed evenly, and placed in a corundum crucible, melted in a muffle furnace at 1150 °C for 15 min, and then the glass melt was taken out and quickly poured into a preheated graphite mold for molding, and then transferred to a muffle furnace at 350 °C for annealing for 3 h to eliminate internal stress. After grinding the self-crystallized glass, CsPbBr3 perovskite quantum dot glass powder was obtained. Figure 1 Shown is the XRD spectrum of the quantum dot glass powder sample. It can be seen from the figure that the diffraction peak is relatively obvious and matches the standard card of cubic phase CsPbBr3, confirming that the CsPbBr3 quantum dots are successfully precipitated in the glass system. Figure 2This is the TEM image of the quantum dot glass powder sample. From the image, it can be clearly observed that the quantum dots are evenly distributed in the glass matrix, and the average particle size is about 6nm.
[0051] Example 2
[0052] The chemical composition molar percentage (mol%) of the CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability in this embodiment is: 70NH4H2PO4, 13SiO2, 7CaCO3, 3SrCO3, 5Al2O3, 20CsBr, 15PbO, 15NaBr
[0053] Table 2 Raw material composition of CsPbBr3 perovskite quantum dot glass in Example 2
[0054] ;
[0055] According to Table 2, accurately weigh analytically pure ammonium dihydrogen phosphate (NH4H2PO4), silicon dioxide (SiO2), calcium carbonate (CaCO3), strontium carbonate (SrCO3), aluminum oxide (Al2O3), cesium bromide (CsBr), lead oxide (PbO), and sodium bromide (NaBr). The accurately weighed raw materials were fully ground in a ball mill, mixed evenly, and placed in a corundum crucible, melted in a muffle furnace at 1100 °C for 18 min, and then the glass melt was taken out and quickly poured into a preheated graphite mold for molding, and then transferred to a muffle furnace at 250 °C for annealing for 10 h to eliminate internal stress. After grinding the self-crystallized glass, CsPbBr3 perovskite quantum dot glass powder was obtained. Figure 3 Shown is the emission spectrum of the prepared CsPbBr3 perovskite quantum dot glass powder sample under 450 nm blue light excitation. It can be seen from the figure that the main luminescence peak of the quantum dot glass is at 522 nm, and the half-peak width is about 25 nm, indicating that the CsPbBr3 perovskite quantum dot glass is suitable for ultraviolet, near-ultraviolet and blue light LED chips. The luminescence characteristics are similar to the luminescence properties of traditional colloidal CsPbBr3 quantum dots, indicating that CsPbBr3 perovskite quantum dots are successfully precipitated in the glass.
[0056] Example 3
[0057] The chemical composition molar percentage (mol%) of the CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability in this embodiment is: 74NH4H2PO4, 10SiO2, 5CaCO3, 3SrCO3, 3Al2O3, 10Cs2CO3, 15PbBr2, 15NaBr
[0058] Table 3 Raw material composition of CsPbBr3 perovskite quantum dot glass in Example 3
[0059] ;
[0060] According to Table 3, accurately weigh analytically pure diammonium dihydrogen phosphate (NH4H2PO4), silicon dioxide (SiO2), calcium carbonate (CaCO3), strontium carbonate (SrCO3), aluminum oxide (Al2O3), cesium carbonate (Cs2CO3), lead bromide (PbBr2), and sodium bromide (NaBr). The accurately weighed raw materials are placed in an agate mortar and ground thoroughly. After mixing evenly, they are placed in a corundum crucible and melted in a muffle furnace at 1050 °C for 10 min. Then, the glass melt is taken out and quickly poured into a preheated graphite mold for molding, and then transferred to a muffle furnace at 370 °C for annealing for 5 h to eliminate internal stress. After grinding the self-crystallized glass, CsPbBr3 perovskite quantum dot glass powder is obtained. Figure 4 Shown is the quantum efficiency test result of the prepared CsPbBr3 perovskite quantum dot glass powder sample under 455 nm excitation. The internal quantum efficiency of the sample under 455 nm excitation is 36.85%.
[0061] Example 4
[0062] The chemical composition molar percentage (mol%) of the CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability in this embodiment is: 75NH4H2PO4, 12SiO2, 8CaCO3, 5SrCO3, 4Al2O3, 10Cs2CO3, 15PbO, 15KBr
[0063] Table 4 Raw material composition of CsPbBr3 perovskite quantum dot glass in Example 4
[0064] ;
[0065] According to Table 4, accurately weigh analytically pure ammonium dihydrogen phosphate (NH4H2PO4), silicon dioxide (SiO2), calcium carbonate (CaCO3), strontium carbonate (SrCO3), aluminum oxide (Al2O3), cesium carbonate (Cs2CO3), lead oxide (PbO), and potassium bromide (KBr). The accurately weighed raw materials were placed in a ball mill and fully ground, mixed evenly, and placed in a corundum crucible, melted in a muffle furnace at 1200 °C for 25 min, and then the glass melt was taken out and quickly poured into a preheated graphite mold for molding, and then transferred to a muffle furnace at 400 °C for annealing for 6 h to eliminate internal stress. After grinding the self-crystallized glass, CsPbBr3 perovskite quantum dot glass powder was obtained. Figure 5The figure shows the study of the spectral performance of the prepared sample at room temperature to 140 °C. It can be seen from the figure that as the temperature increases, the luminous intensity decreases, and when the temperature returns to room temperature, the luminous intensity can be restored to its initial value at room temperature. After multiple cycle tests, this phenomenon can be maintained, and at 100 °C, it can still maintain 64% of its room temperature luminous intensity.
[0066] Example 5
[0067] The chemical composition molar percentage (mol%) of the CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability in this embodiment is: 70NH4H2PO4, 13SiO2, 8CaCO3, 3SrCO3, 4Al2O3, 10Cs2CO3, 15PbBr2, 15KBr
[0068] Table 5 Raw material composition of CsPbBr3 perovskite quantum dot glass in Example 5
[0069] ;
[0070] According to Table 5, accurately weigh analytically pure ammonium dihydrogen phosphate (NH4H2PO4), silicon dioxide (SiO2), calcium carbonate (CaCO3), strontium carbonate (SrCO3), aluminum oxide (Al2O3), cesium carbonate (Cs2CO3), lead bromide (PbBr2), and potassium bromide (KBr). The accurately weighed raw materials were placed in a ball mill and fully ground, mixed evenly, and placed in a corundum crucible, melted in a muffle furnace at 1000 °C for 30 min, and then the glass melt was taken out and quickly poured into a preheated graphite mold for molding, and then transferred to a muffle furnace at 400 °C for annealing for 8 h to eliminate internal stress. After grinding the self-crystallized glass, CsPbBr3 perovskite quantum dot glass powder was obtained. Figure 6 Shown is the fluorescence decay curve of the CsPbBr3 perovskite quantum dot glass powder sample under 450 nm excitation. Its lifetime is calculated to be 24 ns, which is the characteristic lifetime of CsPbBr3 perovskite quantum dots. Figure 7 The figure shows the light stability test results of the prepared sample on the blue LED chip (20V 20mA). It can be seen from the figure that after running on the blue LED chip for 60 days, its luminous intensity is basically not attenuated.
[0071] Example 6
[0072] The chemical composition molar percentage (mol%) of the CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability in this embodiment is: 80NH4H2PO4, 8SiO2, 10CaCO3, 3SrCO3, 3Al2O3, 10Cs2CO3, 15PbBr2, 15KBr
[0073] Table 6 Raw material composition of CsPbBr3 perovskite quantum dot glass in Example 6
[0074] ;
[0075] According to Table 6, accurately weigh analytically pure ammonium dihydrogen phosphate (NH4H2PO4), silicon dioxide (SiO2), calcium carbonate (CaCO3), strontium carbonate (SrCO3), aluminum oxide (Al2O3), cesium carbonate (Cs2CO3), lead bromide (PbBr2), and potassium bromide (KBr). The accurately weighed raw materials were placed in an agate mortar and fully ground, mixed evenly, placed in a corundum crucible, and melted in a muffle furnace at 1150 °C for 45 min. Then, the glass melt was taken out and quickly poured into a preheated graphite mold for molding, and then transferred to a muffle furnace at 270 °C for annealing for 2 h to eliminate internal stress. After grinding the self-crystallized glass, CsPbBr3 perovskite quantum dot glass powder was obtained. Figure 8 Shown is CsPbBr3 perovskite quantum dot glass powder combined with K2SiF6:Mn 4+ The electrospectral diagram of the wide color gamut LED backlight display made of red phosphor and blue LED chip shows that the color gamut area of the device is greater than 100% NTSC. Fig. 9 The figure shows the preparation of CsPbBr3 perovskite quantum dot glass powder combined with K2SiF6:Mn 4+ The display effect of the backlight strip made of red phosphor and blue LED chip when used on a wide color gamut LED backlight display is obvious, with good color reproduction and reproducibility.
[0076] Example 7
[0077] The difference between this embodiment and Example 1 is that the high photostability and high thermal stability CsPbBr3 perovskite quantum dot glass includes the following components in molar percentage: 55 mol% NH4H2PO4, 5 mol% SiO2, 3 mol% CaCO3, 1 mol% SrCO3, 1 mol% Al2O3, 5 mol% PbBr2, 5 mol% NaBr, 5mol% Cs2CO3 or 10mol% CsBr.
[0078] Example 8
[0079] The difference between this embodiment and embodiment 1 is that the high light stability and high thermal stability CsPbBr3 perovskite quantum dot glass includes the following components in molar percentage: 75 mol% NH4H2PO4, 20 mol% SiO2, 15 mol% CaCO3, 7 mol% SrCO 3、7 mol%Al2O3, 20 mol% PbBr2 or PbO, 20 mol% NaBr or KBr, 20mol%Cs2CO3.
[0080] Example 9
[0081] The difference between this embodiment and embodiment 1 is that the high light stability and high thermal stability CsPbBr3 perovskite quantum dot glass includes the following components in molar percentage: 60 mol% NH4H2PO4, 15 mol% SiO2, 10 mol% CaCO3, 5 mol% SrCO3, 5 mol% Al2O3, 14 mol% PbBr2 or PbO, 14 mol% NaBr or KBr, and 15mol% CsBr.
[0082] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values of the parts and steps set forth in these embodiments do not limit the scope of the present application. At the same time, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to the actual proportional relationship. The technology, method and equipment known to those of ordinary skill in the relevant field may not be discussed in detail, but in appropriate cases, the technology, method and equipment should be considered as a part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so that once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.
[0083] In the description of the present application, it should be understood that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings, and are only for the convenience of describing the present application and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific direction or be constructed and operated in a specific direction, and therefore cannot be understood as limiting the scope of protection of the present application; the directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.
[0084] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.
[0085] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of this application.
[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability, characterized by: The following steps are involved: The following components are included in mole percentage: NH4H2PO4 55~75 mol% SiO2 5~20 mol% CaCO3 3~15 mol% SrCO3 1~7 mol% Al2O3 1~7 mol% Pb compound 5~20 mol% Bromide 5~20 mol% Cs2CO3 5~20 mol%; Pb compounds are PbBr2 or PbO, The bromide is NaBr or KBr; S1. Weigh the components of the formula and mix them thoroughly, melt the mixed components at a certain temperature, and then pour them into a graphite mold to obtain self-crystallized glass; S2. The self-crystallized glass is transferred into a muffle furnace for annealing to eliminate internal stress and obtain CsPbBr3 perovskite quantum dot glass; In step S1, the melting temperature is 1000-1200°C, and the melting time is 20-60 min; In step S2, the annealing temperature is 200-450 °C, and the annealing time is 3-20 h.
2. The method for preparing the CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability according to claim 1, characterized in that: After step S2, the annealed CsPbBr3 perovskite quantum dot glass is ground into powder to obtain a finished product.
3. A CsPbBr3 perovskite quantum dot glass with high light stability and high thermal stability prepared by the preparation method according to any one of claims 1 to 2 is used in the field of wide color gamut LED backlight display.