Olefin polymerization catalyst component and preparation method thereof, olefin polymerization catalyst and application thereof
By using diether and methacrylate compounds as internal electron donors in olefin polymerization catalysts, combining magnesium halide and titanium compounds, the problem of rapid activity decay in existing catalysts is solved, and the activity life is extended and stereotactic orientation is achieved. Improved performance, meeting the need for multi-kettle series connection.
Patent Information
- Application Number
- CN202111256537.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-27
AI Technical Summary
The existing olefin polymerization catalyst based on diether compounds as internal electron donors has fast activity decayed and cannot meet the demand for industrial multi-kettle series connection.
Diether compounds and methacrylate compounds are used as internal electron donors, combined with magnesium halide and titanium compounds, and olefin polymerization catalyst components are formed through a specific preparation method to extend the active life of the catalyst.
It effectively slows down the activity attenuation rate of the catalyst, extends the activity life, improves stereotactic orientation, and meets the demand for industrial multi-kettle series connection.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of olefin polymerization catalysts, and in particular to an olefin polymerization catalyst component and a preparation method thereof, an olefin polymerization catalyst and an application thereof. Background Art
[0002] In order to achieve the diversification of polyolefin products, olefin polymerization units are increasingly adopting the method of multi-reactor series connection and bulk and gas combination, which is more conducive to the development of wide molecular weight distribution polyolefin grades and multi-olefin copolymer grades. In order to meet the needs of multi-reactor series connection of industrial units, the catalyst used needs to have a longer active life and slower activity decay.
[0003] European Patent EP1921093A1 uses an organosilicon compound containing an olefin group to treat an olefin polymerization catalyst component. The obtained catalyst has a slower activity decay, but the stereospecificity of the catalyst is not high.
[0004] Chinese patents CN102040691A and CN102453162A use an amine compound containing an allyl group in combination with a catalyst component containing magnesium, titanium, chlorine and an electron-donating compound to effectively slow down the decay of catalyst activity.
[0005] Chinese patent CN104558264A combines phenolic compounds with phthalic acid ester compounds to effectively improve the activity decay of olefin polymerization catalysts.
[0006] In 1990, Himont's patent US4971937 disclosed a catalyst with 1.3-diether as an internal electron donor. The catalyst of this system has the advantages of high activity and good stereospecificity. However, the activity of this type of catalyst decays quickly and the resulting molecular weight distribution is narrow. Therefore, a lot of work has been done to improve the performance of catalysts based on this type of electron donor. Patent CN108239191B uses an ether electron donor combined with a diphenol ester compound to broaden the molecular weight distribution of the product obtained by catalyst polymerization. Patent CN105440177A uses an ether compound combined with a glycol ester compound to improve the comprehensive performance of the catalyst. Patent CN106317275A uses an ether compound combined with a glycol ester compound on the basis of alkoxy magnesium to improve the comprehensive performance of the catalyst.
[0007] At present, the improvement of the activity decay of olefin polymerization catalysts based on diether compounds as internal electron donors has not achieved satisfactory results and cannot meet the needs of multiple reactors in series. Summary of the invention
[0008] In view of the above problems existing in the prior art, the present invention provides an olefin polymerization catalyst component, wherein the internal electron donor is a diether internal electron donor compound and a methacrylate internal electron donor compound, which can effectively slow down the activity decay of the catalyst, prolong the active life, and meet the requirements of multiple reactors in series in an industrial device. The present invention also provides a preparation method of the olefin polymerization catalyst component, an olefin polymerization catalyst, and its application.
[0009] The first aspect of the present invention provides an olefin polymerization catalyst component, comprising a magnesium halide, a titanium compound and an internal electron donor, wherein the internal electron donor comprises a diether internal electron donor compound and a methacrylate internal electron donor compound.
[0010] According to some embodiments of the present invention, the diether internal electron donor compound is selected from at least one of the diether compounds represented by formula (1);
[0011]
[0012] wherein R'1, R'2, R'3, R'4, R'5 and R'6 are the same or different and are independently selected from hydrogen, halogen, C1-C 20 Alkyl, C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Aralkyl, C2-C 20 Alkenyl and C2-C 20 Alkynyl; R'7 and R'8 are the same or different and are independently selected from C1-C 20 Straight or branched alkyl, C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Aralkyl, C7-C 20 Alkyl, C2-C 20 Alkenyl and C2-C 20 Alkynyl;
[0013] Wherein, any one of the alkyl, alkenyl, alkynyl, cycloalkyl, aryl, aralkyl and alkaryl groups is optionally substituted by one or more substituents; and / or, two or more of R'1, R'2, R'3, R'4, R'5 and R'6 are bonded to each other to form a saturated or unsaturated monocyclic or polycyclic ring.
[0014] According to some embodiments of the present invention, the one or more substituents are selected from hydroxyl (-OH), halogen, cyano (-CN), nitro (-NO2), amino (-NH2), mono-C1-C 10 Alkylamino, di-C1-C 10One or more of an alkylamino group, an aldehyde group (-CHO), a carboxyl group (-COOH) and a heteroatom.
[0015] According to some embodiments of the present invention, the heteroatom is selected from one or more of a carbon heteroatom, a nitrogen heteroatom, an oxygen heteroatom and a silicon heteroatom.
[0016] According to some embodiments of the present invention, the diether compound is a 1,3-diether compound.
[0017] According to some embodiments of the present invention, the diether compound is selected from but not limited to 2-(2-ethylhexyl)-1,3-dimethoxypropane, 2-isopropyl-1,3-dimethoxypropane, 2-butyl-1,3-dimethoxypropane, 2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-1,3-dimethoxypropane, 2-phenyl-1,3-dimethoxypropane, 2-(2-phenylethyl)-1,3-dimethoxypropane, 2-(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-(p-chlorophenyl)-1,3-dimethoxypropane, 2-(diphenylmethyl)-1,3-dimethoxypropane, 2,2-dicyclohexyl-1 ,3-dimethoxypropane, 2,2-dicyclopentyl-1,3-dimethoxypropane, 2,2-diethyl-1,3-dimethoxypropane, 2,2-dipropyl-1,3-dimethoxypropane, 2,2-diisopropyl-1,3-dimethoxypropane, 2,2-dibutyl-1,3-dimethoxypropane, 2-methyl-2-propyl-1,3-dimethoxypropane, 2-methyl-2-benzyl-1,3-dimethoxypropane, 2-methyl-2-ethyl-1,3-dimethoxypropane, 2-methyl-2-isopropyl-1,3-dimethoxypropane, 2-methyl-2-phenyl-1,3-dimethoxypropane, 2-methyl-2-cyclohexyl-1,3-dimethoxypropane Oxypropane, 2,2-bis(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-methyl-2-isobutyl-1,3-dimethoxypropane, 2-methyl-2-(2-ethylhexyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2,2-diphenyl-1,3-dimethoxypropane, 2,2-dibenzyl-1,3-dimethoxypropane, 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane, 2-isobutyl-2-isopropyl-1,3-dimethoxypropane, 2-(1-methylbutyl)-2-isopropyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane One or more of methoxypropane, 2-phenyl-2-isopropyl-1,3-dimethoxypropane, 2-phenyl-2-sec-butyl-1,3-dimethoxypropane, 2-benzyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclohexyl-2-sec-butyl-1,3-dimethoxypropane, 2-isopropyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1,3-dimethoxypropane and 9,9-dimethoxymethylfluorene.
[0018] According to some specific embodiments of the present invention, the diether compound is 9,9-dimethoxymethylfluorene.
[0019] According to some specific embodiments of the present invention, the diether compound is 2-isopropyl-2-isopentyl-1,3-dimethoxypropane.
[0020] According to some embodiments of the present invention, the molar amount (dosage) of the diether internal electron donor compound is 0.01 to 1 mole, preferably 0.04 to 0.5 mole, per mole of magnesium halide.
[0021] According to some embodiments of the present invention, the methacrylate internal electron donor compound is one or more of the compound represented by formula (2), the compound represented by formula (3), (meth)acrylic acid alkyl ester polymers, (meth)acrylic acid alkyl ester copolymers, alcoholysis products of maleic anhydride polymers, and alcoholysis products of maleic anhydride copolymers;
[0022]
[0023] Wherein R' is selected from C1-C 50 Straight or branched chain alkanes, C3-C 50 Straight or branched cycloalkanes, C6-C 50 Straight-chain or branched aromatic hydrocarbons, C1-C 20 Straight-chain or branched-chain fatty ethers;
[0024] Wherein R" is selected from C1-C 20 Saturated or unsaturated straight or branched chain alkanes, C1-C 20 Saturated or unsaturated straight-chain or branched-chain fatty ethers, C6-C 50 Saturated or unsaturated straight-chain or branched aromatic hydrocarbons, C6-C 50 Cyclic bridged or non-cyclic bridged saturated cycloalkanes, C6-C 50 Cyclic bridged or non-cyclic bridged monocyclic or condensed ring aromatic hydrocarbons.
[0025] According to some embodiments of the present invention, R' is selected from C 13 -C 50 Straight or branched chain alkanes, C 13 -C 50 Straight or branched cycloalkanes, C 13 -C 50 Straight-chain or branched-chain aromatic hydrocarbons.
[0026] According to some embodiments of the present invention, R" is selected from C1-C 10 Straight or branched chain alkanes, C1-C 10 Straight-chain or branched-chain fatty ethers.
[0027] According to some embodiments of the present invention, the methacrylate internal electron donor compound is selected from one or more of tridecyl methacrylate, octadecyl methacrylate, behenyl methacrylate, tetradecyl methacrylate, hexadecyl methacrylate, octadecyl methacrylate, triacontyl methacrylate, tritriacontyl methacrylate, tetratriacontyl methacrylate, trihexacontyl methacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, butanediol dimethacrylate, (meth)acrylic acid alkyl ester polymers, (meth)acrylic acid alkyl ester copolymers, alcoholysis products of maleic anhydride polymers and alcoholysis products of maleic anhydride copolymers.
[0028] According to some embodiments of the present invention, the methacrylate internal electron donor compound is selected from octadecyl methacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, (meth)acrylic acid alkyl ester polymers and (meth)acrylic acid alkyl ester copolymers, alcoholysis products of maleic anhydride polymers and alcoholysis products of maleic anhydride copolymers.
[0029] According to some embodiments of the present invention, the amount of the methacrylate internal electron donor compound used is 0.01 to 1 mole, preferably 0.04 to 0.5 mole, per mole of magnesium halide.
[0030] According to some embodiments of the present invention, the general formula of the magnesium halide is MgX2, wherein X is a halogen. According to some embodiments of the present invention, X is chlorine, bromine or iodine.
[0031] According to some embodiments of the present invention, the magnesium halide is one or more of magnesium dichloride, magnesium dibromide and magnesium diiodide.
[0032] According to some specific embodiments of the present invention, the magnesium halide is magnesium dichloride.
[0033] The second aspect of the present invention provides a method for preparing the olefin polymerization catalyst component described in the first aspect, comprising the following steps:
[0034] A. dissolving a magnesium halide in a dissolving system, wherein the dissolving system contains an organic epoxy compound, an organic phosphorus compound and an organic solvent to obtain a solution;
[0035] B. In the presence of a precipitation aid, a methacrylate internal electron donor compound and an inert diluent, the solution obtained in step A is mixed with a titanium compound and heated to precipitate a solid component, which is filtered and washed to obtain a catalyst component;
[0036] The diether electron donor compound is added once or multiple times during the dissolving in step A and the heating or washing in step B.
[0037] According to some embodiments of the present invention, before step A, high-purity nitrogen is introduced into the reactor for repeated replacement.
[0038] According to some embodiments of the present invention, in the dissolution process of step A, the stirring speed is not particularly specified, and is based on sufficient dissolution. The stirring time is 10 to 180 minutes, preferably 30 to 120 minutes.
[0039] According to some embodiments of the present invention, the organic epoxy compound is selected from one or more of oxidation products of C2-C8 aliphatic olefins and oxidation products of C2-C8 halogenated aliphatic olefins.
[0040] According to some embodiments of the present invention, the organic epoxy compound is selected from one or more of ethylene oxide, propylene oxide, epichlorohydrin, epichlorohydrin, butylene oxide, butadiene oxide, butadiene dioxide, methyl glycidyl ether and diglycidyl ether.
[0041] According to some embodiments of the present invention, the organic epoxy compound is epichlorohydrin.
[0042] According to some embodiments of the present invention, the amount of the organic epoxy compound used is 0.1 to 10 moles, preferably 0.4 to 4 moles, per mole of magnesium halide.
[0043] According to some embodiments of the present invention, the organophosphorus compound is selected from one or more of the compounds described in formula (4) and formula (5);
[0044]
[0045] In formula (4) and formula (5), R1, R2, R3, R4, R5, and R6 are each independently selected from C1-C 20 A straight-chain or branched alkane, a cycloalkane or an aromatic hydrocarbon which may or may not have a substituent.
[0046] According to some embodiments of the present invention, the organophosphorus compound is selected from one or more of trimethyl phosphate, triethyl phosphate, tributyl phosphate, tripentyl phosphate, triphenyl phosphate, trimethyl phosphite, triethyl phosphite, tributyl phosphite and benzyl phosphite.
[0047] According to some embodiments of the present invention, the organophosphorus compound is tributyl phosphate and / or tripentyl phosphate.
[0048] The amount of the organic phosphorus compound used is 0.1 to 10 moles, preferably 0.4 to 5 moles, per mole of magnesium halide.
[0049] According to some embodiments of the present invention, the organic solvent is selected from one or more of aromatic hydrocarbon compounds and halogenated hydrocarbon compounds.
[0050] According to some embodiments of the present invention, the organic solvent is selected from one or more of toluene, ethylbenzene, benzene, xylene and chlorobenzene, preferably toluene.
[0051] According to some embodiments of the present invention, the amount of the organic solvent used is 0.5 to 40 moles, preferably 2 to 30 moles, per mole of magnesium halide.
[0052] According to some embodiments of the present invention, the precipitation aid is selected from one or more of organic acids, organic anhydrides, organic ethers and organic ketones.
[0053] According to some embodiments of the present invention, the precipitation aid is selected from one or more of acetic anhydride, phthalic anhydride, succinic anhydride, maleic anhydride, pyromellitic anhydride, acetic acid, propionic acid, butyric acid, acrylic acid, methacrylic acid, acetone, methyl ethyl ketone, benzophenone, methyl ether, ethyl ether, propyl ether, butyl ether and pentyl ether.
[0054] According to some embodiments of the present invention, the amount of the precipitation aid is 0.001 to 1 mole, preferably 0.04 to 0.4 mole, per mole of magnesium halide.
[0055] According to some embodiments of the present invention, the general formula of the titanium compound is TiX m (OR) 4-m , wherein X is a halogen, preferably chlorine, bromine or iodine, and R is C1-C 20 wherein m is an integer of 1 to 4.
[0056] According to some embodiments of the present invention, the titanium-containing compound is selected from one or more of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, tetrabutoxytitanium, tetraethoxytitanium, triethoxytitanium monochloride, diethoxytitanium dichloride and triethoxytitanium trichloride, preferably titanium tetrachloride.
[0057] According to some embodiments of the present invention, the amount of the titanium-containing compound is 0.5 to 25 moles, preferably 1 to 20 moles, per mole of magnesium halide.
[0058] According to some embodiments of the present invention, the inert reagent is selected from C6-C 20 One or more of straight-chain or branched alkanes, white oil, and silicone oil.
[0059] According to some embodiments of the present invention, the amount of the inert reagent is 0.5 to 100 moles, preferably 2 to 30 moles, per mole of magnesium halide.
[0060] According to some embodiments of the present invention, the mixing temperature is 30 to 120° C. and the mixing time is 10 to 180 min.
[0061] According to some embodiments of the present invention, the temperature raising conditions include: raising the temperature to 40-120° C. and maintaining it for 0.1-180 min.
[0062] According to some specific embodiments of the present invention, the specific method of step B can be: first add the precipitation aid to the solution, stir evenly, add the methacrylate internal electron donor compound and the inert diluent, and drop the titanium compound into the solution within 1 to 70 minutes. After the dropwise addition is completed, continue to maintain for 1 hour and gradually raise the temperature to 40 to 120°C.
[0063] According to some specific embodiments of the present invention, after the precipitation aid is added to the solution in step B, the solution is cooled to -30 to 30°C.
[0064] According to some specific embodiments of the present invention, the washing process of step B is: washing with an organic solvent for 2 to 3 times, then adding an organic solvent and a titanium compound to treat at 80 to 120° C. for 0.5 to 1 hour, removing the filtrate, repeating the addition of the organic solvent and the titanium compound once, and then repeating the washing with hexane for 4 to 5 times.
[0065] According to some specific embodiments of the present invention, the amount of hexane used is 150-220 mL.
[0066] According to some specific embodiments of the present invention, the diether internal electron donor compound is added once or multiple times during the dissolving in step A and the heating or washing in step B, wherein the multiple times are, for example but not limited to, 2 to 10 times, preferably 2 to 5 times.
[0067] The third aspect of the present invention provides an olefin polymerization catalyst, comprising:
[0068] 1) the olefin polymerization catalyst component described in the first aspect or the olefin polymerization catalyst component obtained by the preparation method described in the second aspect;
[0069] 2) Organic aluminum compounds;
[0070] 3) Optionally, an external electron donor compound.
[0071] According to some embodiments of the present invention, the molar ratio of aluminum in the organic aluminum to titanium in the catalyst component is 1 to 1500:1, preferably 10 to 1000:1.
[0072] According to some embodiments of the present invention, the molar ratio of the external electron donor compound to the titanium in the catalyst component is 0 to 500:1, more preferably 0 to 200:1.
[0073] According to some embodiments of the present invention, the organoaluminum compound is an alkylaluminum compound.
[0074] According to some embodiments of the present invention, the chemical formula of the alkyl aluminum compound is AlR' n’ X' 3-n’ , wherein R' is a C1-C8 alkyl group or a halogenated alkyl group, X' is a halogen group, and n' is an integer of 1 to 3.
[0075] According to some embodiments of the present invention, X' is one or more of chlorine, bromine and iodine, more preferably chlorine.
[0076] According to some embodiments of the present invention, the alkyl aluminum compound is selected from triethylaluminum, tripropylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-n-hexylaluminum, tri-n-octylaluminum, triisobutylaluminum, diethylaluminum monohydrogen, diisobutylaluminum monohydrogen, diethylaluminum monochloride, diisobutylaluminum monochloride, ethylaluminum dichloride, Al(n-C6H 13 )3 and Al(n-C8H 17 )3 or more.
[0077] According to some embodiments of the present invention, the alkyl aluminum compound is triethyl aluminum and / or triisobutyl aluminum.
[0078] According to some embodiments of the present invention, the molar ratio of aluminum in the alkyl aluminum compound to titanium in the catalyst component is 1 to 1500:1, preferably 10 to 1000:1.
[0079] According to some embodiments of the present invention, the external electron donor compound is selected from one or more of carboxylic acids, carboxylic acid anhydrides, carboxylic acid esters, ketones, ethers, alcohols, lactones, organophosphorus compounds and organosilicon compounds.
[0080] According to some embodiments of the present invention, the external electron donor compound is an organosilicon compound having the chemical formula (R 13 )m'(R 14 )p'Si(OR 15 )q', where R 13 , R 14 and R 15 Each independently is C1-C 18 Hydrocarbyl, preferably C1-C 18The alkane optionally contains heteroatoms, wherein the heteroatoms are one or more of F, Cl, Br, N and I; m' and p' are each independently an integer of 0-2, q' is an integer of 1 to 3, and the sum of m', p' and q' is 4.
[0081] According to some embodiments of the present invention, R 13 and R 14 Each independently is C3-C 10 Alkyl, C3-C 10 Alkenyl, C3-C 10 Alkylene, C3-C 10 Substituted or unsubstituted cycloalkyl and C6-C 10 The present invention is one of substituted or unsubstituted aryl groups, optionally containing a heteroatom, wherein the heteroatom is one or more of F, Cl, Br, N and I.
[0082] According to some embodiments of the present invention, R 15 C1-C 10 Alkyl, more preferably C1-C6 alkyl, more preferably C1-C4 alkyl, more preferably methyl.
[0083] According to some embodiments of the present invention, the organosilicon compound is selected from one or more of cyclohexylmethyldimethoxysilane, diisopropyldimethoxysilane, di-n-butyldimethoxysilane, diisobutyldimethoxysilane, diphenyldimethoxysilane, methyl-tert-butyldimethoxysilane, dicyclopentyldimethoxysilane, cyclohexyltrimethoxysilane, tert-butyltrimethoxysilane, tert-hexyltrimethoxysilane and 2-ethylpiperidinyl-2-tert-butyldimethoxysilane.
[0084] According to some embodiments of the present invention, the external electron donor compound is cyclohexylmethyldimethoxysilane and / or dicyclopentyldimethoxysilane.
[0085] The fourth aspect of the present invention provides the use of the catalyst component described in the first aspect, the catalyst component prepared by the method described in the second aspect, and the catalyst described in the third aspect in olefin polymerization reactions.
[0086] According to some embodiments of the present invention, the olefin polymerization reaction is a homopolymerization reaction or a copolymerization reaction of multiple olefins.
[0087] According to some embodiments of the present invention, at least one of the olefins is an olefin represented by the formula CH2=CHR, wherein R is hydrogen or a C1-C6 alkyl group. Specific examples of the olefin represented by the formula CH2=CHR may include ethylene, propylene, 1-n-butene, 1-n-pentene, 1-n-hexene, 1-n-octene and 4-methyl-1-pentene.
[0088] According to some embodiments of the present invention, the olefin represented by the formula CH2=CHR is one or more of ethylene, propylene, 1-n-butene, 1-n-hexene and 4-methyl-1-pentene.
[0089] According to some embodiments of the present invention, the olefin represented by the formula CH2=CHR is propylene, or a copolymer of propylene and other olefins.
[0090] Compared with the prior art, the present invention has the following beneficial effects:
[0091] (1) The olefin polymerization catalyst component provided by the present invention uses a diether compound and a methacrylate compound as internal electron donors, which can effectively slow down the activity decay rate of the olefin polymerization catalyst;
[0092] (2) The olefin polymerization catalyst provided by the present invention has a long active life, high activity and good stereospecificity;
[0093] (3) The olefin polymer catalyst component and catalyst provided by the present invention are used in olefin polymerization reactions, and can meet the requirements of multiple reactors in series in industrial devices. DETAILED DESCRIPTION
[0094] In order to make the present invention more easily understood, the present invention will be described in detail below in conjunction with embodiments. These embodiments are only for illustration and are not intended to limit the application scope of the present invention.
[0095] The experimental method involved in the present invention is as follows:
[0096] (1) Propylene polymerization method
[0097] In a 5-liter autoclave, after nitrogen is fully replaced, 5 mL of triethylaluminum hexane solution (the concentration of triethylaluminum is 0.5 mmol / mL), 1 mL of cyclohexylmethyldimethoxysilane (CHMMS) hexane solution (the concentration of CHMMS is 0.1 mmol / mL), 10 mL of anhydrous hexane and 10 mg of catalyst components are added at room temperature. The autoclave is closed, and 1.2 L of hydrogen and 2.3 L of liquid propylene are added. The temperature is raised to 70°C, and the polymerization reaction is carried out at 70°C for 1 hour and 2 hours respectively. After the reaction is completed, the reactor is cooled and stirring is stopped to discharge the reaction product to obtain an olefin polymer.
[0098] (2) Method for determining the content of each component in the catalyst
[0099] The titanium content was determined colorimetrically using a UV-visible spectrophotometer Model 722;
[0100] The magnesium content was measured by complexometric titration of magnesium ions and EDTA;
[0101] The halogen content was measured by AgNO3-NH4CNS back titration method;
[0102] Determination of internal electron donor content in methacrylates: using chromatography, decomposing the catalyst powder with dilute acid, extracting the internal electron donor compound with an extractant, and determining it with a liquid chromatograph;
[0103] Determination of the content of electron donors in ethers: Agilent high-performance GC-MS was used for determination.
[0104] The isotacticity index (II) of propylene polymer is determined by the heptane extraction method: 2 grams of dried polymer sample is placed in an extractor and extracted with boiling heptane for 6 hours, and the residue is dried to constant weight. The ratio of the obtained polymer weight (g) to 2 (g) is the isotacticity.
[0105] Catalyst activity AC = (polymer weight) / (catalyst weight).
[0106] In the present invention, the organic raw materials involved were purchased from Bailingwei Chemical Reagent Co., Ltd., and the polymethacrylate compound used in some embodiments was pour point depressant T602, which was purchased from Liyang Wandefu Chemical Company.
[0107] Example 1
[0108] Preparation of olefin polymerization catalyst components.
[0109] In a reactor that has been repeatedly replaced with high-purity nitrogen, add 7.2g of anhydrous magnesium chloride, 60mL of toluene, 6.0mL of epichlorohydrin, 36mL of tributyl phosphate and 0.6mL of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane in sequence, and stir at 350rpm for 2 hours at 60°C. Then add 2.0g of phthalic anhydride and continue stirring at 60°C for 1 hour. Cool the solution to 5°C and increase the stirring to 400rpm. Add 0.7g of octadecyl methacrylate and 8g of food-grade No. 100 white oil (kinematic viscosity (40°C) at 100mm 2 / s), 73mL of titanium tetrachloride was dripped into the solution within 60min. After the addition was completed, it was maintained for 1 hour and the temperature was gradually raised to 80°C. During the heating process, 1.4mL of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane was added, and the temperature was raised to 85°C and maintained for 1 hour. After filtering the clear liquid, it was washed twice with 200mL of toluene. 120mL of toluene, 80mL of titanium tetrachloride, treated at 110°C for 0.5 hour, and the filtrate was removed. 120mL of toluene, 80mL of titanium tetrachloride, treated at 110°C for 0.5 hour, and the filtrate was removed. After repeated washing with 200mL of hexane 4 times, a solid olefin polymerization catalyst component was obtained. Catalyst physical property data are shown in Table 1.
[0110] Example 2
[0111] Preparation of olefin polymerization catalyst components.
[0112] In a reactor that has been repeatedly replaced with high-purity nitrogen, 7.2g of anhydrous magnesium chloride, 58mL of toluene, 6.0mL of epichlorohydrin, 30mL of tributyl phosphate and 0.5mL of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane were added in sequence, and stirred at 350rmp for 2 hours at a temperature of 60°C. Then 2.0g of phthalic anhydride was added, followed by 88mL of decane and 2g of pour point depressant T602, and stirring was continued at 60°C for 1 hour. The solution was cooled to 10°C. Stirring was increased to 400rmp. 73mL of titanium tetrachloride was dripped into the solution within 60min. After the addition was completed, it was continued for 1 hour and the temperature was gradually raised to 80°C. During the heating process, 1.5mL of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane was added, and the temperature was raised to 85°C and continued for 1 hour. After filtering the clear liquid, it was washed twice with 200mL of toluene. Add 120 mL toluene and 80 mL titanium tetrachloride, treat at 110°C for 0.5 hour, and remove the filtrate. Add 120 mL toluene and 80 mL titanium tetrachloride, treat at 110°C for 0.5 hour, and remove the filtrate. Repeat washing with 200 mL hexane for 4 times to obtain a solid olefin polymerization catalyst component. The catalyst physical property data are shown in Table 1.
[0113] Example 3
[0114] Preparation of olefin polymerization catalyst components.
[0115] The preparation method is the same as that of Example 1, except that 0.5 g and 2.0 g of 9,9-dimethoxymethylfluorene are used instead of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane. The catalyst properties are shown in Table 1.
[0116] Example 4
[0117] Preparation of olefin polymerization catalyst components.
[0118] The preparation method is the same as that of Example 2, except that 0.5 g and 2.0 g of 9,9-dimethoxymethylfluorene are used instead of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane. The catalyst properties are shown in Table 1.
[0119] Example 5
[0120] Preparation of olefin polymerization catalyst components.
[0121] In a reactor that has been repeatedly replaced with high-purity nitrogen, 7.2g of anhydrous magnesium chloride, 54mL of toluene, 6.0mL of epichlorohydrin, 30mL of tributyl phosphate and 0.6mL of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane were added in sequence, and stirred at 350rmp for 2 hours at a temperature of 60°C. Then 2.0g of phthalic anhydride was added, followed by 65mL of hexane and 0.5mL of diethylene glycol dimethacrylate, and stirring was continued at 60°C for 1 hour. The solution was cooled to 10°C. Stirring was increased to 400rmp. 76mL of titanium tetrachloride was dropped into the solution within 60min. After the addition was completed, it was continued for 1 hour and the temperature was gradually raised to 80°C. During the heating process, 1.4mL of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane was added, and the temperature was raised to 85°C and continued for 1 hour. After filtering the clear liquid, it was washed twice with 200mL of toluene. Add 120 mL toluene and 80 mL titanium tetrachloride, treat at 110°C for 0.5 hour, and remove the filtrate. Add 120 mL toluene and 80 mL titanium tetrachloride, treat at 110°C for 0.5 hour, and remove the filtrate. Repeat washing with 200 mL hexane for 4 times to obtain a solid olefin polymerization catalyst component. The catalyst physical property data are shown in Table 1.
[0122] Example 6
[0123] Preparation of olefin polymerization catalyst components.
[0124] The preparation method is the same as that of Example 5, except that 0.8 mL of triethylene glycol dimethacrylate is used instead of diethylene glycol dimethacrylate. The catalyst property data are shown in Table 1.
[0125] Example 7
[0126] Preparation of olefin polymerization catalyst components.
[0127] The preparation method is the same as that of Example 2, except that 2-isopropyl-2-isopentyl-1,3-dimethoxypropane is added at once during the heating process. The catalyst properties are shown in Table 1.
[0128] Example 8
[0129] Preparation of olefin polymerization catalyst components.
[0130] The preparation method is the same as that of Example 2, except that 2-isopropyl-2-isopentyl-1,3-dimethoxypropane is added once during the toluene washing process. The catalyst properties are shown in Table 1.
[0131] Example 9
[0132] Preparation of olefin polymerization catalyst components.
[0133] The preparation method is the same as that of Example 2, except that no external electron donor compound is used during the polymerization process.
[0134] Catalyst physical properties data are shown in Table 1
[0135] Comparative Example 1
[0136] Preparation of olefin polymerization catalyst components.
[0137] In a reactor that has been repeatedly replaced with high-purity nitrogen, 7.2g of anhydrous magnesium chloride, 66mL of toluene, 6.0mL of epichlorohydrin, and 30mL of tributyl phosphate are added in sequence, and stirred at 350rmp for 2 hours at 60°C. Then 2.0g of phthalic anhydride and 88mL of decane are added, and stirring is continued at 60°C for 1 hour. The solution is cooled to 10°C. Stirring is increased to 400rmp. 73mL of titanium tetrachloride is dripped into the solution within 60min. After the addition is completed, continue to maintain for 1 hour and gradually increase the temperature to 80°C. During the heating process, 2.0mL of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane is added, and the temperature is increased to 85°C and continued for 1 hour. After filtering the clear liquid, wash it twice with 200mL of toluene. Add 120mL of toluene and 80mL of titanium tetrachloride, treat at 110°C for 0.5 hours, and remove the filtrate. 120 mL of toluene and 80 mL of titanium tetrachloride were added, and the mixture was treated at 110°C for 0.5 hours, and the filtrate was removed. The mixture was washed with 200 mL of hexane for 4 times to obtain a solid olefin polymerization catalyst component. The catalyst properties are shown in Table 1.
[0138] Comparative Example 2
[0139] Preparation of olefin polymerization catalyst components.
[0140] The preparation method is the same as that of Comparative Example 1, except that 2.5 g of 9,9-bis(methoxymethyl)fluorene is used instead of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane. The catalyst property data are shown in Table 1.
[0141] Comparative Example 3
[0142] Preparation of olefin polymerization catalyst components.
[0143] The preparation method is the same as that of Example 8, except that octadecyl methacrylate is not used. The catalyst property data are shown in Table 1.
[0144] Comparative Example 4
[0145] Preparation of olefin polymerization catalyst components.
[0146] The preparation method is the same as that of Comparative Example 1, except that no external electron donor is used during polymerization. The catalyst property data are shown in Table 1.
[0147] Test Example 1
[0148] The catalysts prepared in Examples 1 to 9 and Comparative Examples 1 to 4 were used for propylene polymerization, respectively. The obtained polymerization data and polymer data are shown in Table 1.
[0149] Table 1 Test results
[0150]
[0151] In Table 1, "AC, kgPP / gCat.hr" indicates the catalyst activity after 1 hour of reaction; "AC, kgPP / gCat.2hr" indicates the catalyst activity after 2 hours of reaction; "AC 2hr / AC 1hr " represents the ratio of the catalyst activity after 2 hours of reaction to the catalyst activity after 1 hour of reaction.
[0152] According to the test results in Table 1, the AC of the catalyst components prepared in Examples 1 to 9 is 2hr / AC 1hr The test results are significantly greater than those of Comparative Examples 1 to 4, indicating that using a diether internal electron donor compound and a methacrylate internal electron donor compound together as an internal electron donor can effectively slow down the activity decay of the catalyst, especially when 2-isopropyl-2-isopentyl-1,3-dimethoxypropane is used as the internal electron donor, the effect of delaying the activity decay is the best.
[0153] In summary, the olefin polymer catalyst component provided by the present invention uses diether compounds and methacrylate compounds as internal electron donor compounds, which effectively delays the activity decay of the catalyst, and the prepared catalyst can meet the needs of multiple reactors in series in an industrial device.
[0154] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this field, under the technical enlightenment provided by the present invention, as common knowledge in the field, other equivalent variations and improvements can also be made, which should also be regarded as the protection scope of the present invention.
Claims
1. An olefin polymerization catalyst component, It is characterized in that The method comprises a magnesium halide, a titanium compound and an internal electron donor, wherein the internal electron donor comprises a diether internal electron donor compound and a methacrylate internal electron donor compound; The molar amount of the diether internal electron donor compound is 0.01 to 1 mole per mole of magnesium halide; The molar amount of the methacrylate internal electron donor compound is 0.01 to 1 mole per mole of magnesium halide; The titanium compound is used in an amount of 0.5 to 25 moles per mole of magnesium halide; The methacrylate internal electron donor compound is a compound represented by formula (2), a compound represented by formula (3), an alkyl (meth)acrylate polymer, or an alkyl (meth)acrylate copolymer; Where R' is selected from C 13 -C 50 Straight or branched chain alkanes, C 13 -C 50 Straight or branched cycloalkanes, C 13 -C 50 Straight-chain or branched-chain aromatic hydrocarbons; wherein R" is selected from C1-C20 saturated or unsaturated straight or branched alkanes, C1-C20 saturated or unsaturated straight or branched fatty ethers, C6-C50 saturated or unsaturated straight or branched aromatic hydrocarbons, C6-C50 cyclic bridged or non-cyclic bridged saturated cycloalkanes, C6-C50 cyclic bridged or non-cyclic bridged monocyclic or condensed aromatic hydrocarbons; The diether internal electron donor compound is selected from at least one of the diether compounds represented by formula (1); Formula (1), Among them, R' 1 , R' 2 , R' 3 , R' 4 , R' 5 and R' 6 are the same or different and are independently selected from hydrogen, halogen, C 1 -C 20 Alkyl, C 3 -C 20 Cycloalkyl, C 6 -C 20 Aryl, C 7 -C 20 Aralkyl, C 7 -C 20 Alkyl, C 2 -C 20 Alkenyl and C 2 -C 20 Alkynyl; R' 7 and R' 8 The same or different, each independently selected from C 1 -C 20 Straight or branched alkyl, C 3 -C 20 Cycloalkyl, C 6 -C 20 Aryl, C 7 -C 20 Aralkyl, C 7 -C 20 Alkyl, C 2 -C 20 Alkenyl and C 2 -C 20 Alkynyl; Wherein, any one of the alkyl, alkenyl, alkynyl, cycloalkyl, aryl, aralkyl and alkaryl groups is optionally substituted by one or more substituents.
2. The catalyst component according to claim 1, It is characterized in that R' 1 , R' 2 , R' 3 , R' 4 , R' 5 and R' 6 Two or more of them are bonded to each other to form a saturated or unsaturated monocyclic or polycyclic ring.
3. The catalyst component according to claim 1, It is characterized in that The one or more substituents are selected from hydroxy, halogen, cyano, nitro, amino, mono-C 1 -C 10 Alkylamino, bis-C 1 -C 10 One or more of an alkylamino group, an aldehyde group, a carboxyl group and a heteroatom.
4. The catalyst component according to claim 3, It is characterized in that The heteroatom is selected from one or more of a carbon heteroatom, a nitrogen heteroatom, an oxygen heteroatom and a silicon heteroatom.
5. The catalyst component according to any one of claims 2 to 4, It is characterized in that The diether internal electron donor compound is selected from 2-(2-ethylhexyl)-1,3-dimethoxypropane, 2-isopropyl-1,3-dimethoxypropane, 2-butyl-1,3-dimethoxypropane, 2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-1,3-dimethoxypropane, 2-phenyl-1,3-dimethoxypropane, 2-(2-phenylethyl)-1,3-dimethoxypropane, 2-(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-(p-chlorophenyl)-1,3-dimethoxypropane, 2-(diphenylmethyl)-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxypropane 2,2-dicyclopentyl-1,3-dimethoxypropane, 2,2-diethyl-1,3-dimethoxypropane, 2,2-dipropyl-1,3-dimethoxypropane, 2,2-diisopropyl-1,3-dimethoxypropane, 2,2-dibutyl-1,3-dimethoxypropane, 2-methyl-2-propyl-1,3-dimethoxypropane, 2-methyl-2-benzyl-1,3-dimethoxypropane, 2-methyl-2-ethyl-1,3-dimethoxypropane, 2-methyl-2-isopropyl-1,3-dimethoxypropane, 2-methyl-2-phenyl-1,3-dimethoxypropane, 2-methyl-2-cyclohexyl-1,3-dimethoxypropane alkane, 2,2-bis(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-methyl-2-isobutyl-1,3-dimethoxypropane, 2-methyl-2-(2-ethylhexyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2,2-diphenyl-1,3-dimethoxypropane, 2,2-dibenzyl-1,3-dimethoxypropane, 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane, 2-isobutyl-2-isopropyl-1,3-dimethoxypropane, 2-(1-methylbutyl)-2-isopropyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3 -dimethoxypropane, 2-phenyl-2-isopropyl-1,3-dimethoxypropane, 2-phenyl-2-sec-butyl-1,3-dimethoxypropane, 2-benzyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclohexyl-2-sec-butyl-1,3-dimethoxypropane, 2-isopropyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1,3-dimethoxypropane, 9,9-dimethoxymethylfluorene.
6. The catalyst component according to claim 5, It is characterized in that The diether internal electron donor compound is selected from one or more of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane and 9,9-dimethoxymethylfluorene.
7. The catalyst component according to any one of claims 2 to 4, It is characterized in that The molar amount of the diether internal electron donor compound is 0.04 to 0.5 mole per mole of magnesium halide.
8. The catalyst component according to claim 1, It is characterized in that R" is selected from C 1 -C 10 Straight or branched chain alkanes, C 1 -C 10 Straight-chain or branched-chain fatty ethers.
9. The catalyst component according to claim 1 or 8, It is characterized in that The methacrylate internal electron donor compound is selected from one or more of tridecyl methacrylate, octadecyl methacrylate, behenyl methacrylate, tetracosyl methacrylate, hexacosyl methacrylate, octacosyl methacrylate, triacontyl methacrylate, tritriacontyl methacrylate, tetratriacontyl methacrylate, hexatriacontyl methacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, butanediol dimethacrylate, (meth)acrylic acid alkyl ester polymers, and (meth)acrylic acid alkyl ester copolymers.
10. The catalyst component according to claim 9, It is characterized in that The methacrylate internal electron donor compound is selected from octadecyl methacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, and polymethacrylate.
11. The catalyst component according to claim 1, It is characterized in that The molar amount of the methacrylate internal electron donor compound is 0.04 to 0.5 mole per mole of magnesium halide.
12. The catalyst component according to any one of claims 1 to 4, It is characterized in that The general formula of the magnesium halide is MgX 2 , wherein X is a halogen.
13. The catalyst component according to claim 11, It is characterized in that The magnesium halide is one or more of magnesium dichloride, magnesium dibromide and magnesium diiodide.
14. The catalyst component according to claim 13, It is characterized in that The magnesium halide is magnesium dichloride.
15. A method for preparing an olefin polymerization catalyst component according to any one of claims 1 to 14, It is characterized in that The following steps are involved: A. dissolving a magnesium halide in a dissolving system, wherein the dissolving system contains an organic epoxy compound, an organic phosphorus compound and an organic solvent to obtain a solution; B. In the presence of a precipitation aid, a methacrylate internal electron donor compound and an inert diluent, the solution obtained in step A is mixed with a titanium compound and heated to precipitate a solid component, which is filtered and washed to obtain a catalyst component; The diether internal electron donor compound is added once or multiple times during the dissolving in step A and the heating or washing in step B.
16. The method according to claim 15, It is characterized in that The organic epoxy compound is selected from C 2 -C 8 Oxidation products of aliphatic olefins, C 2 -C 8 One or more of the oxidation products of halogenated aliphatic olefins.
17. The method according to claim 16, It is characterized in that The organic epoxy compound is selected from one or more of ethylene oxide, propylene oxide, ethylene oxide, epichlorohydrin, butylene oxide, butadiene oxide, methyl glycidyl ether and diglycidyl ether.
18. The method according to claim 17, It is characterized in that The organic epoxy compound is epichlorohydrin.
19. The method according to any one of claims 16 to 18, It is characterized in that The amount of the organic epoxy compound used is 0.1 to 10 moles per mole of magnesium halide.
20. The method according to claim 19, It is characterized in that The amount of the organic epoxy compound used is 0.4 to 4 moles per mole of magnesium halide.
21. The method according to claim 15, It is characterized in that The organic phosphorus compound is selected from one or more compounds described in formula (4) and formula (5); In formula (4) and formula (5), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 Each independently selected from C 1 -C 20 A straight-chain or branched alkane, a cycloalkane or an aromatic hydrocarbon which may or may not have a substituent.
22. The method according to claim 21, It is characterized in that The organophosphorus compound is selected from one or more of trimethyl phosphate, triethyl phosphate, tributyl phosphate, tripentyl phosphate, triphenyl phosphate, trimethyl phosphite, triethyl phosphite, tributyl phosphite and benzyl phosphite.
23. The method according to claim 22, It is characterized in that The organic phosphorus compound is tributyl phosphate and / or tripentyl phosphate.
24. The method according to any one of claims 21 to 23, It is characterized in that The amount of the organic phosphorus compound used is 0.1 to 10 moles per mole of magnesium halide.
25. The method according to claim 24, It is characterized in that The amount of the organic phosphorus compound used is 0.4 to 5 moles per mole of magnesium halide.
26. The method according to claim 15, It is characterized in that The organic solvent is selected from one or more of aromatic hydrocarbon compounds and halogenated hydrocarbon compounds.
27. The method according to claim 26, It is characterized in that The organic solvent is selected from one or more of toluene, ethylbenzene, benzene, xylene and chlorobenzene.
28. The method according to claim 27, It is characterized in that The organic solvent is toluene.
29. The method according to any one of claims 26 to 28, It is characterized in that The amount of the organic solvent used is 0.5 to 40 moles per mole of magnesium halide.
30. The method according to claim 29, It is characterized in that The amount of the organic solvent used is 2 to 30 moles per mole of magnesium halide.
31. The method according to claim 15, It is characterized in that The precipitation aid is selected from one or more of organic acids, organic acid anhydrides, organic ethers and organic ketones.
32. The method according to claim 31, It is characterized in that The precipitation aid is selected from one or more of acetic anhydride, phthalic anhydride, succinic anhydride, maleic anhydride, pyromellitic anhydride, acetic acid, propionic acid, butyric acid, acrylic acid, methacrylic acid, acetone, methyl ethyl ketone, benzophenone, methyl ether, ethyl ether, propyl ether, butyl ether and pentyl ether.
33. The method according to claim 31 or 32, It is characterized in that The amount of the precipitation aid used is 0.001 to 1 mole per mole of magnesium halide.
34. The method according to claim 33, It is characterized in that The amount of the precipitation aid used is 0.04 to 0.4 mole per mole of magnesium halide.
35. The method according to claim 15, It is characterized in that The general formula of the titanium compound is TiXm(OR) 4-m , where X is halogen and R is C 1 -C 20 wherein m is an integer of 1 to 4.
36. The method according to claim 35, It is characterized in that The titanium compound is selected from one or more of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, titanium tetrabutoxide, titanium tetraethoxide, titanium triethoxide monochloride, titanium diethoxide dichloride and titanium triethoxide monochloride.
37. The method according to claim 36, It is characterized in that The titanium compound is titanium tetrachloride.
38. The method according to any one of claims 35 to 37, It is characterized in that The titanium compound is used in an amount of 1 to 20 moles per mole of magnesium halide.
39. The method according to claim 15, It is characterized in that The inert diluent is selected from one or more of C6-C20 straight-chain or branched alkanes, white oil, and silicone oil.
40. The method according to claim 39, It is characterized in that The amount of the inert diluent used is 0.5 to 100 moles per mole of magnesium halide.
41. The method according to claim 40, It is characterized in that The inert diluent is used in an amount of 2 to 30 moles per mole of magnesium halide.
42. The method according to claim 15, It is characterized in that The mixing temperature is 30-80° C. and the mixing time is 10-180 min; and / or the heating condition includes: heating to 40-120° C. and maintaining for 0.1-180 min.
43. An olefin polymerization catalyst, It is characterized in that include: 1) The olefin polymerization catalyst component according to any one of claims 1 to 14 or the olefin polymerization catalyst component obtained by the preparation method according to any one of claims 15 to 42; 2) Organic aluminum compounds; 3) optionally, an external electron donor compound; The molar ratio of aluminum in the organic aluminum to titanium in the catalyst component is 1 to 1500:1; The molar ratio of the external electron donor compound to the titanium in the catalyst component is 0 to 500:
1.
44. The catalyst according to claim 43, It is characterized in that The molar ratio of aluminum in the organic aluminum to titanium in the catalyst component is 10 to 1000:
1.
45. The catalyst according to claim 43, It is characterized in that The molar ratio of the external electron donor compound to the titanium in the catalyst component is 0 to 200:
1.
46. Use of the catalyst component according to any one of claims 1 to 14, the catalyst component prepared by the method according to any one of claims 15 to 42, and the catalyst according to any one of claims 43 to 45 in olefin polymerization reactions.
47. The use according to claim 46, It is characterized in that The olefin polymerization reaction is a homopolymerization reaction or a copolymerization reaction of multiple olefins.