A multivariate optical coating material, preparation method and application thereof

By combining the formation of lanthanum niobate or lanthanum niobate aluminum optical coating materials under vacuum and high temperature, the problem of unstable components during the evaporation process of traditional coating materials is solved, and an optical film with high refractive index and stability is achieved. The design of the new film system requires and improves the efficiency of the evaporation process.

CN116282950BActive Publication Date: 2024-11-22GRINM RESOURCES & ENVIRONMENT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310272065.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-11-22
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

During the evaporation process, traditional high-refractive index optical coating materials are difficult to maintain component consistency due to differences in the physical and chemical properties of components, resulting in poor performance and stability of optical films, which cannot meet the demand for high-refractive index materials in the new film design.

Method used

Nb2O5, Al2O3, La2O3 and Nb powders are used to combine lanthanum niobate or aluminum lanthanum niobate as optical coating materials. Compounds are formed through high-temperature solid phase synthesis reactions to ensure the consistency of component stability and film performance.

Benefits of technology

An optical film with high refractive index (2.1-2.20) and good stability is achieved, which meets the demand for refractive index of film system design and improves the stability and efficiency of the evaporation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116282950B_ABST
    Figure CN116282950B_ABST
Patent Text Reader

Abstract

The present invention provides a multi-element optical coating material, a preparation method and an application thereof, wherein the optical coating material is composed of lanthanum niobate or lanthanum aluminum niobate (LaNb x Al y O z ), wherein the value of x is 0.65-1.0, the value of y is 0-0.22, and the value of z is 2.1-4. The density of the optical coating material is 5.8-6.1 g / cm 3 , melting point is 1800-1900℃, with the characteristics of high density and small closed porosity. The use of this optical coating material for evaporation has the advantages of small outgassing, stable evaporation process, easy control, and the material in the coating crucible does not need to be updated to maintain the refractive index of the film layer. The formed optical film has stable strength, no cracking, no spots, good uniformity during the film formation process, and a refractive index of 2.1-2.20 at 500nm, which is a high refractive index. In addition, the optical coating material is stable when placed in the air, without oxidation discoloration, the optical coating material has a wide transmission band, good evaporation characteristics, dense structure, and low absorption, and can be used for mass production of hard dielectric optical films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of optical coating technology, and in particular to a multi-element optical coating material, a preparation method and application thereof. Background Art

[0002] Traditional high-refractive-index optical coating materials are mainly composed of single oxides of titanium, zirconium, and hafnium or their mixtures. The coating materials formed by the mixture can change the refractive index of the single oxide optical film layer, thereby expanding the range of options for film system design. However, during the evaporation film formation process, due to the differences in the physical and chemical properties of the components, it is difficult to keep the components unchanged (consistency) at each stage of evaporation, resulting in poor performance consistency and stability of the formed optical film.

[0003] At the same time, the progress of optical technology has further increased the requirements for the optical and mechanical properties of optical films, and the international market and domestic users have put forward the demand for new materials in the design of optical film systems. In order to meet the needs of new film system design, this technical field urgently needs to develop new high refractive index materials. Summary of the invention

[0004] In view of the above problems existing in the prior art, the present invention provides a multi-element optical coating material, a preparation method and its application. The preparation method is based on the formation of a compound by combining Nb2O5, Al2O3, La2O3 and Nb powder under vacuum and high temperature. The compound is used as an optical coating material, which overcomes the deficiency of the coating material in the form of a mixture that changes in components at each stage of evaporation, and maintains the stability of the material components during the evaporation process and the consistency of the film performance. The density of the optical coating material is 5.8-6.1g / cm 3 The refractive index of the formed optical film at 500nm is 2.1-2.20, which has high refractive index and stability, meeting the requirements of film system design for refractive index materials in this area.

[0005] The specific content of the invention is as follows:

[0006] In a first aspect, the present invention provides a multivariate optical coating material, wherein the optical coating material is composed of lanthanum niobate or lanthanum aluminum niobate; wherein the chemical formula of the lanthanum niobate or lanthanum aluminum niobate is LaNb x Al y O z ; Among them, the value of x is 0.65~1.0, the value of y is 0~0.22, and the value of z is 2.1~4;

[0007] The density of the optical coating material is 5.8-6.1 g / cm 3 ;

[0008] The melting point of the optical coating material is 1800-1900°C;

[0009] The optical film layer formed by evaporation of the optical coating material has a refractive index of 2.1-2.20 at 500nm.

[0010] In a second aspect, the present invention provides a method for preparing the optical coating material according to the first aspect, the preparation method comprising the following steps:

[0011] S1. Using powders of Nb2O5, La2O3, Al2O3 and Nb as reaction raw materials, mechanically mixing to obtain a uniformly mixed powder;

[0012] S2, granulating or pressing the powder to obtain a granular material or a block material;

[0013] S3, placing the granular material or bulk material in a vacuum environment to perform a high-temperature solid-phase synthesis reaction to obtain the optical coating material.

[0014] Optionally, in step S1, the mass ratio of each component in the reaction raw material is:

[0015] Nb2O5: 27-37wt.%;

[0016] La2O3: 50~70wt.%;

[0017] Al2O3: 0~5wt.%;

[0018] Nb powder: 5~11wt.%.

[0019] Optionally, in step S1, the mass ratio of each component in the reaction raw material is:

[0020] Nb2O5: 30-37wt.%;

[0021] La2O3: 56~60wt.%;

[0022] Al2O3: 1-4wt.%;

[0023] Nb powder: 6~10wt.%.

[0024] Optionally, in step S1, the mechanical mixing is ball milling mixing or stirring mixing, and the time of the ball milling mixing or stirring mixing is 4 to 24 hours.

[0025] Optionally, in step S2, the pressure used in the granulation or pressing process is 300-800 N / cm 2 .

[0026] Optionally, in step S2, the pressure used in the granulation or pressing process is 500-600 N / cm 2.

[0027] Optionally, in step S3, the reaction temperature of the high-temperature solid phase synthesis reaction of the granular material is 1400-1700° C., the heating rate is 5-15° C. / min, and the reaction time is 4-20 h.

[0028] Optionally, in step S3, the bulk material is subjected to a high-temperature solid phase synthesis reaction in a two-stage gradient temperature increase manner, comprising:

[0029] The temperature is 1400-1700°C; the heating rate is 5-15°C / min, and the time is 6-12h;

[0030] Raise the temperature to 1700-1900°C at a rate of 7-12°C / min and maintain for 2-4 hours.

[0031] In a third aspect, the present invention provides an application of the optical coating material described in the first aspect in preparing a hard dielectric optical film, comprising:

[0032] The optical coating material is melted at 2000° C. to form a molten optical coating material;

[0033] Evaporating the molten optical coating material;

[0034] Wherein, the evaporation is performed using electron beam evaporation equipment; the process parameters of the evaporation include:

[0035] The vacuum degree is 1.5×10 -4 torr;

[0036] Evaporation temperature is 1900-2100℃;

[0037] The evaporation rate is 3A / sec;

[0038] The substrate temperature was 100°C.

[0039] Compared with the prior art, the present invention has the following advantages:

[0040] (1) The present invention provides a multivariate optical coating material, which is composed of lanthanum niobate or lanthanum aluminum niobate and has a density of 5.8-6.1 g / cm 3 The melting point is 1800-1900℃. The optical film formed by evaporation with this material has stable strength, no cracking, no spots, good uniformity in the film forming process, and a refractive index of 2.1-2.20 at 500nm, which is high in refractive index. In addition, the material is stable when placed in the air, without oxidation discoloration, wide transmission band, good evaporation characteristics, dense structure, small absorption, and can be used for mass production of hard medium optical films.

[0041] (2) The present invention provides a method for preparing a multinary optical coating material, which is based on the chemical reaction of Nb2O5, Al2O3, La2O3 and Nb powder under vacuum and high temperature to form a compound lanthanum aluminum niobate, and uses this compound as a new optical coating material. This overcomes the asynchronous changes in the components of the coating material in the form of a mixture at each stage of evaporation, and maintains the stability of the material components during the evaporation process and the consistency of the film performance.

[0042] In addition, the lanthanum aluminum niobate optical coating material obtained by the preparation method provided by the present invention can be a pre-melted material, that is, it has undergone a melting process before evaporating to prepare the optical film. Therefore, the material has the characteristics of high density and small closed porosity after condensation. Based on these characteristics, when evaporating to prepare the optical film, the material has the advantages of small outgassing, stable evaporation process, easy control, and the material in the coating crucible does not need to be updated to maintain the refractive index of the film layer. In addition, since the pre-melted material has a high density and good material filling, the lanthanum aluminum niobate optical coating material provided by the embodiment of the present invention can be evaporated multiple times after one melting, which is beneficial to improve the efficiency of the coating equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0044] Figure 1 The figure shows the appearance of the multivariate optical coating material prepared by the embodiment of the present invention;

[0045] Figure 2 The figure shows the appearance of a multivariate optical coating material prepared according to another embodiment of the present invention;

[0046] Figure 3 A flow chart of a method for preparing a multivariate optical coating material provided by an embodiment of the present invention is shown;

[0047] Figure 4 The infrared absorption spectrum and transmittance spectrum of the optical film obtained after the multi-element optical coating material prepared in Example 1 of the present invention is evaporated are shown;

[0048] Figure 5 The refractive index curve of the optical film obtained after evaporation of the multi-element optical coating material prepared in Example 1 of the present invention is shown;

[0049] Figure 6 The figure shows the appearance of the multivariate optical coating material prepared in the comparative example of the present invention. DETAILED DESCRIPTION

[0050] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0051] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the prior art can be used. The reagents and other instruments used without specifying the manufacturer are all conventional reagent products that can be purchased commercially.

[0052] The present invention is based on the fact that the refractive index of the optical film formed by vapor deposition of traditional optical coating materials does not meet the market demand, and in traditional high-refractive-index coating materials, the coating materials formed by mixing oxides of titanium, zirconium and hafnium have differences in physical and chemical properties between the components, so it is difficult to maintain the consistency of component changes during the vapor deposition process, resulting in poor performance consistency and stability of the formed optical film. Based on this, the present invention hopes to develop a high-refractive-index multivariate optical coating material to solve the change in optical film performance (optical properties and mechanical properties) caused by the change in coating material components during the vapor deposition process of the mixture coating material, and further expand the range of choices for film system design. The specific implementation content is as follows:

[0053] In a first aspect, the present invention provides a multivariate optical coating material, wherein the optical coating material is composed of lanthanum niobate or lanthanum aluminum niobate; wherein the chemical formula of the lanthanum aluminum niobate is LaNb x Al y O z ; wherein, the value of x is 0.65-1.0, the value of y is 0-0.22, and the value of z is 2.1-4; the refractive index of the optical film layer formed by evaporation of the optical coating material is 2.1-2.20 at 500nm; the density of the optical coating material is 5.8-6.1g / cm 3 ; The melting point of the optical coating material is 1800-1900℃.

[0054] In specific implementation, the composition of the multivariate optical coating material provided by the present invention is specifically lanthanum niobate or lanthanum aluminum niobate. The present invention selects Nb2O5, La2O3 and Al2O3, or Nb2O5 and La2O3 as the raw materials for preparing the multivariate optical coating material, and generates a new compound through a high-temperature solid-phase synthesis reaction, whose chemical formula is LaNb x Al y O z; Wherein, the value of x is 0.65~1.0, the value of y is 0~0.22, and the value of z is 2.1~4. It can be seen that when the value of y is 0, the composition of the optical coating material is lanthanum niobate. The refractive index of the optical film obtained by evaporation of the optical coating material is 2.1-2.20 at 500nm, which is higher than the refractive index of traditional optical film layers of lanthanum oxide La2O3 (1.88) or aluminum oxide Al2O3 (1.7), and slightly lower than the refractive index of traditional optical film layers of niobium oxide Nb2O5 (2.3). Moreover, its optical film performance (optical properties and mechanical properties) is greatly improved compared with traditional optical film layers of lanthanum oxide La2O3, niobium oxide Nb2O5 or aluminum oxide Al2O3.

[0055] Figure 1 The figure shows the appearance of the multivariate optical coating material provided by the embodiment of the present invention, Figure 2 FIG. 4 shows an appearance diagram of a multivariate optical coating material provided by another embodiment of the present invention. Figure 1 The multivariate optical coating material shown is a sintered granular material, such as Figure 2 The multivariate optical coating material shown is a pre-melted granular material. The multivariate optical coating material provided by the present invention has a density of 5.8-6.1 g / cm 3 The melting point of the material is 1800-1900℃. The optical film formed by evaporation using this material has stable strength, no cracking, no spots, good uniformity in the film forming process, and a refractive index of 2.1-2.20 at 500nm, which is high in refractive index. In addition, the material is stable when placed in the air, without oxidation discoloration, wide transmission band, good evaporation characteristics, dense structure, small absorption, and can be used for mass production of hard medium optical films.

[0056] In some embodiments, the optical film layer formed by evaporation of the optical coating material has a refractive index of 2.17 at 500 nm and a density of 6.1 g / cm 3 ; The melting point is 1800-1900℃; the closed porosity of the optical coating material tested by mercury intrusion method is 0.99%.

[0057] The second object of the present invention is to provide a method for preparing the optical coating material described in the first aspect. Figure 2 FIG. 1 shows a flow chart of a method for preparing a multivariate optical coating material provided by an embodiment of the present invention. Figure 2 As shown, the preparation method comprises the following steps:

[0058] S1. Using powders of Nb2O5, La2O3, Al2O3 and Nb as reaction raw materials, mechanically mixing to obtain a uniformly mixed powder;

[0059] In the specific implementation, this step uses Nb2O5, La2O3 and Al2O3 as raw materials for preparing the multivariate optical coating material of the present invention, and adds an appropriate amount of Nb powder thereto, and performs mechanical mixing to make the reaction raw materials fully and evenly mixed. The addition of Nb powder can improve the solid effect of the reaction raw materials in the subsequent high-temperature sintering to obtain the finished multivariate optical coating material, and avoid the material pulverization and instability.

[0060] In some embodiments, the mass ratio of each component in the reaction raw material of this step can be: Nb2O5: 27-37wt.%; La2O3: 50-70wt.%; Al2O3: 0-5wt.%; Nb powder: 5-11wt.%.

[0061] As a preferred raw material, the mass ratio of each component can be further controlled as follows: Nb2O5: 30-37wt.%; La2O3: 56-60wt.%; Al2O3: 1-4wt.%; Nb powder: 6-10wt.%.

[0062] More preferably, the mass ratio of each component in the raw material can be further controlled to: Nb2O5: 30wt.%; La2O3: 60wt.%; Al2O3: 4wt.%; Nb powder: 6wt.%.

[0063] In some embodiments, in order to ensure the uniformity of powder mixing and improve production efficiency, the specific method of mechanical mixing in this step can be ball milling or stirring, and the time of ball milling or stirring is maintained at 8 to 12 hours. Preferably, the time of ball milling or stirring is maintained at 4 to 24 hours.

[0064] S2, granulating or pressing the powder to obtain a granular material or a block material;

[0065] During specific implementation, since the subsequent high-temperature solid-phase synthesis process requires vacuum treatment of the reaction environment, the vacuum process will cause the loss of powdered reaction raw materials, resulting in the powder flying around and affecting the reaction results. On the other hand, pressing or granulation treatment can also increase the contact area between powders of different components, which is helpful for the full progress of the solid-phase reaction. In view of the above reasons, this step further granulates or presses the powder that is evenly mixed by ball milling. The pressing or granulation treatment can be carried out on equipment such as hydraulic presses, isostatic presses, and granulators. The pressure used for granulation or pressing treatment is 300 to 800 N / cm 2 The preferred pressure is 500-600 N / cm 2 .

[0066] Furthermore, in this step, the ball-milled and uniformly mixed powder is further granulated or pressed. The selection of granulation or pressing means also depends on the specific requirements for the grade of the optical coating material. When the granular material obtained by granulation is subjected to the subsequent high-temperature solid-phase synthesis reaction, the reaction temperature will be controlled so that the formed lanthanum aluminum niobate optical coating material is a sintered material. The material maintains the original particle shape. Before the optical coating material is used for evaporation, it needs to be pre-melted. When the bulk material obtained by pressing is subjected to the subsequent high-temperature solid-phase synthesis, the reaction temperature will be adjusted so that after the reaction raw materials are sintered, the temperature is further increased to form a molten lanthanum aluminum niobate optical coating material.

[0067] It should be noted that, when preparing lanthanum aluminum niobate, whether to make it into a sintered material or a molten material can be determined based on comprehensive considerations of actual needs and industrial factors. In this embodiment, this is not limited. The main purpose of this embodiment is to provide a multivariate optical coating material; secondly, in order to ensure the optical stability of the film made of the material and reduce the problems of splashing in the film making process, it is preferably made into a molten material during the preparation process.

[0068] S3, placing the granular material or bulk material in a vacuum environment to perform a high-temperature solid-phase synthesis reaction to obtain the optical coating material.

[0069] In specific implementation, the high-temperature solid-phase synthesis equipment can be a medium-frequency furnace, a carbon tube furnace, a hot press furnace or other high-temperature vacuum equipment. When a hot press furnace is used, there is no need to press or granulate first, and pressurization and solid-phase synthesis can be carried out simultaneously; the vacuum degree of the solid-phase synthesis reaction environment is 10Pa to 1×10 -3 Pa; the preferred vacuum degree is 2×10 -1 Pa~5×10 -2 Pa.

[0070] In specific implementation, step S3 is a key step in obtaining optical coating materials, and the phase composition and material density obtained at different synthesis temperatures will be different. If the granular material is obtained by granulation treatment in the previous step for high-temperature solid-phase synthesis reaction, the reaction temperature of the solid-phase synthesis reaction in this step needs to be controlled to 1400-1700°C; the heating rate is 5-15°C / min, and the reaction time is 4-20h; the Nb2O5 (niobium pentoxide), Al2O3 (aluminum oxide), La2O3 (lanthanum trioxide), and Nb (metal niobium) reaction raw materials contained in the granular material are sintered within this temperature range to form a new compound lanthanum aluminum niobate.

[0071] If the block material is obtained by briquetting in the previous step for high-temperature solid-phase synthesis reaction, the solid-phase synthesis reaction in this step can be carried out by gradient heating, specifically: the reaction temperature is controlled to 1400-1700°C; the heating rate is 5-15°C / min, and the reaction is carried out for 6-12h. The Nb2O5 (niobium pentoxide), Al2O3 (aluminum oxide), La2O3 (lanthanum trioxide), and Nb (metallic niobium) reaction raw materials contained in the block material are sintered within this temperature range to form a new compound lanthanum aluminum niobate. Then the temperature is further set to 1700-1900°C, the heating rate is 7-12°C / min, and it is maintained for 2-4h. Since the temperature exceeds the melting point of the compound lanthanum aluminum niobate, the optical coating material finally obtained is a pre-melted material. Based on the characteristics of pre-melting, the optical coating material provided by the present invention has the advantage of small closed porosity, reduces the degassing of the optical coating material during pre-melting, shortens the material pre-melting time, and improves the use efficiency of the coating equipment. Taking electron beam evaporation equipment for evaporation as an example, since electron beam evaporation equipment evaporates materials onto a substrate under high temperature, the material ejected from the electron beam evaporation equipment is in a molten state. However, the existing optical coating materials are granular sintered materials. Since the sintered particles are not molten materials obtained after melting, when the sintered materials are converted into a molten state in the electron beam evaporation equipment, there are problems such as incomplete reaction, spraying, and unstable physical and chemical properties. The lanthanum aluminum niobate optical coating material provided in the embodiment of the present invention can be a pre-melted material, so there is no process of converting the sintered particles into a molten state in the evaporation equipment, which improves the evaporation efficiency while avoiding the problems of incomplete reaction, spraying, and unstable physical and chemical properties in the existing optical coating materials.

[0072] In specific implementation, the optical coating material obtained in this step can be broken into particles of a preset particle size according to actual needs, which can be used for preparing thin films later.

[0073] The preparation method of the multi-element optical coating material provided by the present invention is based on the existing optical coating monomer materials, and by adjusting the mixing ratio, Nb2O5 (niobium pentoxide), Al2O3 (aluminum oxide), and La2O3 (lanthanum trioxide) are converted into a new compound form (lanthanum aluminum niobate) with a consistent phase structure through high-temperature solid phase synthesis. On the one hand, there are no impurities or mixed phases in the lanthanum aluminum niobate optical coating material, which ensures the performance stability (optical properties and mechanical properties) of the optical film subsequently prepared from the lanthanum aluminum niobate optical coating material. On the other hand, compared with the asynchrony of component changes caused by differences in physical and chemical properties in the coating material in the form of a simple mixture at each stage of evaporation, the compound optical coating material with a consistent phase structure provided by the present invention can maintain the stability of the components in the evaporation process and the consistency of the film performance. In addition, the preparation method has the characteristics of simple process flow, short cycle, low cost, and environmental friendliness, is suitable for industrial production, and has broad prospects for industrial application.

[0074] In addition, the lanthanum aluminum niobate optical coating material prepared by the method provided by the present invention can be a pre-melted material, that is, it has undergone a melting process before evaporating to prepare the optical film. Therefore, the material has the characteristics of high density and small closed porosity after condensation. Based on these characteristics, when evaporating to prepare the optical film, the material has the advantages of small outgassing, stable evaporation process, easy control, and the material in the coating crucible does not need to be updated to maintain the refractive index of the film layer. In addition, since the pre-melted material has a high density and good material filling, the lanthanum aluminum niobate optical coating material provided in the embodiment of the present invention can be evaporated multiple times after one melting, which is beneficial to improve the efficiency of the coating equipment.

[0075] Furthermore, since Nb2O5, La2O3 and Al2O3 are conventional optical coating materials (with refractive indices of 2.3, 1.88 and 1.7 respectively), the present invention adjusts the mixing ratio and converts Nb2O5 (niobium pentoxide), Al2O3 (aluminum oxide) and La2O3 (lanthanum trioxide) into a new compound form (lanthanum aluminum niobate) through high-temperature solid phase synthesis, so that its refractive index is distributed in the range of 2.0-2.2, thereby meeting the requirements of the film system design for the refractive index material in this region.

[0076] The third object of the present invention is to provide an application of the optical coating material provided in the first aspect in preparing a hard dielectric optical film, comprising:

[0077] The optical coating material is melted at 2000° C. to form a molten optical coating material;

[0078] Evaporating the molten optical coating material;

[0079] Wherein, the evaporation is performed using electron beam evaporation equipment; the process parameters of the evaporation include:

[0080] The vacuum degree is 1.5×10 -4 torr;

[0081] Evaporation temperature is 1900-2100℃;

[0082] The evaporation rate is 3A / sec;

[0083] The substrate temperature was 100°C.

[0084] In specific implementation, the preparation of hard dielectric optical film can be selected as follows: first, the lanthanum aluminum niobate optical coating material (pre-melted type) obtained by the present invention is fully pre-melted. The specific pre-melting method is: the lanthanum aluminum niobate molten material is placed in an oxygen-free copper crucible with a diameter of 30×15mm for pre-melting, and the pre-melting temperature is 2000°C to obtain lanthanum aluminum niobate in a molten state.

[0085] Then, the coating was performed based on the pre-melted lanthanum aluminum niobate. The substrate used for the coating was a quartz substrate, and the deposition was performed using an electron beam evaporation device with a vacuum degree of 1.5×10 -4 torr, substrate temperature is 100°C, evaporation temperature is about 2000°C, and evaporation rate is 3A / sec. Based on these evaporation conditions, coating is performed to obtain an optical thin film layer.

[0086] The lanthanum aluminum niobate optical coating material (pre-melted type) provided in the embodiment of the present invention is used for evaporation, and the optical film formed has stable strength, small closed porosity, no cracking, no spots, good uniformity during the film formation process, and a refractive index of 2.1-2.20 at 500nm, which is a high refractive index. In addition, the material is stable when placed in the air, and there is no oxidation discoloration. The material has a wide transmission band, good evaporation characteristics, a dense structure, and low absorption, and can be used for the mass production of hard medium optical films. Therefore, the optical film made based on this material has the advantages of dense and firm film layer, good chemical stability, and stable refractive index.

[0087] In order to enable those skilled in the art to understand the present application more clearly, the multivariate optical coating material, preparation method and application thereof described in the present application are now described in detail through the following embodiments.

[0088] Embodiment 1:

[0089] The raw material ratio of Nb2O5 34% (wt.), La2O3 60% (wt.), and Nb 6% (wt.) was accurately weighed and mechanically mixed for 8 hours using a stirring mixer. The mixed powder was then crushed by a hydraulic press at 400N / cm 2 The briquettes were pressed under pressure and loaded into the furnace. The furnace temperature was raised at a rate of 5°C / min under vacuum. At a temperature of 1700°C and a vacuum of 2×10 -1Pa, the solid phase synthesis reaction was carried out for 8 hours and cooled to room temperature under vacuum. The material prepared by this method is a black granular material, as shown in the figure Figure 1 The material density tested by the drainage method is 6.1g / cm 3 The closed porosity of the material tested by mercury intrusion injection method is 0.99%.

[0090] When using, the material is fully pre-melted first, and the material is pre-melted in a water-cooled oxygen-free copper crucible. The pre-melting temperature is 2000℃. There is no splashing during the pre-melting process. The surface of the material is molten after pre-melting. The substrate for coating is a quartz substrate, and the material is evaporated using an electron beam evaporation coating equipment. The vacuum degree is 1.5×10 -2 Pa, the substrate temperature is 200°C, the evaporation temperature is about 2000°C, and the evaporation rate is 3A / sec.

[0091] Figure 4 The infrared absorption spectrum and transmittance spectrum of the optical film obtained after the multivariate optical coating material prepared in Example 1 of the present invention is shown. Figure 4 It can be seen that the material has a wide transmission band and low absorption in the near ultraviolet to near infrared band. Figure 5 The refractive index curve of the optical film obtained after evaporation of the multivariate optical coating material prepared in Example 1 of the present invention is shown. Figure 5 It can be seen that the refractive index of the lanthanum niobate optical film provided in this embodiment is 2.17 at 500 nm.

[0092] The adhesion of the film was tested by the cross-cut method using 3M tape and was found to be level 0. The film did not fall off after being soaked in water for 24 hours, and the film layer was firm and dense.

[0093] Embodiment 2:

[0094] The raw material ratio of Nb2O5 30% (wt.), La2O3 60% (wt.), Al2O3 4% (wt.), and Nb 6% (wt.) was accurately weighed and mechanically mixed by a stirring mixer for 8 hours. The mixed powder was then crushed by a hydraulic press at 400 N / cm 2 The briquettes were pressed under pressure and loaded into the furnace. The furnace temperature was raised at a rate of 5°C / min under vacuum. At a temperature of 1750°C and a vacuum of 2×10 -1 Pa, the solid phase synthesis reaction was carried out for 8 hours, and then cooled to room temperature under vacuum. The material prepared by this method is a black molten material, and its appearance is shown in the figure Figure 2 As shown, the material density tested by the drainage method is 6.1g / cm 3 The closed porosity of the material tested by mercury intrusion injection method is 0.99%.

[0095] When using, the material is fully pre-melted first, and the material is pre-melted in a water-cooled oxygen-free copper crucible. The pre-melting temperature is 2000℃. There is no splashing during the pre-melting process. The surface of the material is molten after pre-melting. The substrate for coating is a quartz substrate, and the material is evaporated using an electron beam evaporation coating equipment. The vacuum degree is 1.5×10 -2 Pa, substrate temperature is 100℃, evaporation temperature is about 2000℃, and evaporation rate is 3A / sec. The refractive index of the coating layer at 500nm is 2.12, the film layer is firm and dense, and has low absorption in the near ultraviolet to near infrared band.

[0096] The infrared absorption spectrum of the multivariate optical coating material prepared in this embodiment is the same as the infrared absorption spectrum of the film layer prepared in Example 1, and will not be repeated in this embodiment.

[0097] The adhesion of the film was tested by the cross-cut method using 3M tape and was still level 0. The film did not fall off after 24 hours of water immersion test.

[0098] Embodiment 3:

[0099] The raw material ratio of Nb2O5 31% (wt.), La2O3 57% (wt.), Al2O3 2% (wt.), and Nb 10% (wt.) was accurately weighed and mechanically mixed for 6 hours using a stirring mixer. The mixed powder was then crushed by a hydraulic press at 400 N / cm 2 The briquettes were pressed under pressure and loaded into the furnace. The furnace temperature was raised at a rate of 5°C / min under vacuum. At a temperature of 1650°C and a vacuum of 2×10 -1 Pa, the solid phase synthesis reaction was carried out for 6 hours and cooled to room temperature under vacuum. The material prepared by this method was a black material, and the density of the material tested by the drainage method was 6.0g / cm 3 The closed porosity of the material tested by mercury intrusion injection method is 1.73%.

[0100] When using, the material is fully pre-melted first, and the material is pre-melted in a water-cooled oxygen-free copper crucible. The pre-melting temperature is 2000℃. There is no splashing during the pre-melting process. The surface of the material is molten after pre-melting. The substrate for coating is a quartz substrate, and the material is evaporated using an electron beam evaporation coating equipment. The vacuum degree is 1.5×10 -2 Pa, substrate temperature is 300℃, evaporation temperature is about 2000℃, and evaporation rate is 3A / sec. The refractive index of the coating layer at 500nm is 2.15, the film layer is firm and dense, and has low absorption in the near ultraviolet to near infrared band.

[0101] The infrared absorption spectrum of the multivariate optical coating material prepared in this embodiment is the same as the infrared absorption spectrum of the film layer prepared in Example 1, and will not be repeated in this embodiment.

[0102] The adhesion of the film was tested by the cross-cut method using 3M tape and was still level 0. The film did not fall off after 24 hours of water immersion test.

[0103] Example 4

[0104] The raw materials were accurately weighed according to their mass ratio: Nb2O5 27% (wt.), La2O3 66% (wt.), Nb 6% (wt.), and Al2O3 1% (wt.), and mechanically mixed for 8 h using a stirring mixer. The mixed powder was then crushed by a hydraulic press at 400 N / cm 2 The briquettes were pressed under pressure and loaded into the furnace. The furnace temperature was raised at a rate of 5°C / min under vacuum. At a temperature of 1750°C and a vacuum of 2×10 -1 Pa, the solid phase synthesis reaction was carried out for 8 hours, and the material was broken into particles after cooling to room temperature under vacuum. The density of the material tested by the drainage method was 6.1g / cm 3 The closed porosity of the material tested by mercury injection method is 0.96%.

[0105] When using, the material is fully pre-melted first, and the material is pre-melted in a water-cooled oxygen-free copper crucible. The pre-melting temperature is 2000℃. There is no splashing during the pre-melting process. The surface of the material is molten after pre-melting. The substrate for coating is a quartz substrate, and the material is evaporated using an electron beam evaporation coating equipment. The vacuum degree is 1.5×10 -2 Pa, substrate temperature is 200℃, evaporation temperature is about 2000℃, evaporation rate is 3A / sec. The refractive index of the coating layer at 500nm is 2.12, the film layer is firm and dense, and has low absorption in the near ultraviolet to near infrared band.

[0106] The adhesion of the film was tested by the cross-cut method using 3M tape and was found to be level 0. The film did not fall off after being soaked in water for 24 hours, and the film layer was firm and dense.

[0107] Example 5

[0108] According to the raw material mass ratio, Nb2O5 36.9% (wt.), La2O3 56.6% (wt.), Nb 6.5% (wt.), accurately weighed, mechanically mixed with a stirring mixer for 7 hours, and the mixed powder was pressed with an oil press at 400N / cm 2 The briquettes were pressed under pressure and loaded into the furnace. The furnace temperature was raised at a rate of 5°C / min under vacuum. At a temperature of 1780°C and a vacuum degree of 2×10 -1 Pa, the solid phase synthesis reaction was carried out for 8 hours, and the material was broken into particles after cooling to room temperature under vacuum. The density of the material tested by the drainage method was 6.1g / cm 3 The closed porosity of the material tested by mercury injection method is 0.98%.

[0109] When using, the material is fully pre-melted first, and the material is pre-melted in a water-cooled oxygen-free copper crucible. The pre-melting temperature is 2000℃. There is no splashing during the pre-melting process. The surface of the material is molten after pre-melting. The substrate for coating is a quartz substrate, and the material is evaporated using an electron beam evaporation coating equipment. The vacuum degree is 1.5×10 -2 Pa, substrate temperature is 200℃, evaporation temperature is about 2000℃, evaporation rate is 3A / sec. The refractive index of the coating layer at 500nm is 2.12, the film layer is firm and dense, and has low absorption in the near ultraviolet to near infrared band.

[0110] The adhesion of the film was tested by the cross-cut method using 3M tape and was found to be level 0. The film did not fall off after being soaked in water for 24 hours, and the film layer was firm and dense.

[0111] Comparative Example 1: According to the raw material ratio of Nb2O5 43% (wt.), La2O3 55% (wt.), Al2O3 2% (wt.), the raw materials were accurately weighed, and mechanically mixed by a stirring mixer for 6 hours. The mixed powder was pressed by an oil press at 400N / cm 2 The briquettes were pressed under pressure and loaded into the furnace. The furnace temperature was raised at a rate of 5°C / min under vacuum. At a temperature of 1730°C and a vacuum of 2×10 -1 Pa, the solid phase synthesis reaction was carried out for 6 hours, and then cooled to room temperature under vacuum. The material prepared by this method is a black material. After being placed at room temperature for a period of time, the material turns into powder, and its appearance is shown in the figure Figure 6 shown.

[0112] The above is a detailed introduction to a multivariate optical coating material, a preparation method and a preparation method of a hard dielectric optical film provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present invention.

Claims

1. A multivariate optical coating material, characterized in that: The optical coating material is composed of lanthanum niobate or lanthanum aluminum niobate; wherein the chemical formula of the lanthanum niobate or lanthanum aluminum niobate is LaNb x Al y O z ; Among them, the value of x is 0.65~1.0, the value of y is 0~0.22, and the value of z is 2.1~4; The density of the optical coating material is 5.8-6.1 g / cm 3 ; The melting point of the optical coating material is 1800-1900°C; The refractive index of the optical film layer formed by evaporation of the optical coating material at 500nm is 2.1-2.20; The method for preparing the multivariate optical coating material comprises the following steps: S1. Using powders of Nb2O5, La2O3, Al2O3 and Nb as reaction raw materials, mechanically mixing to obtain a uniformly mixed powder; S2, granulating or pressing the powder to obtain a granular material or a block material; S3, placing the granular material or bulk material in a vacuum environment to perform a high-temperature solid-phase synthesis reaction to obtain the optical coating material; The mass ratio of each component in the reaction raw material is: Nb2O5: 27~37wt.%; La2O3: 50~70wt.%; Al2O3: 0~5wt.%; Nb powder: 5~11wt.%; The total mass ratio of each component in the reaction raw material is 100%.

2. The multivariate optical coating material according to claim 1, characterized in that: In step S1, the mass ratio of each component in the reaction raw material is: Nb2O5: 30~37wt.%; La2O3: 56~60wt.%; Al2O3: 1~4wt.%; Nb powder: 6~10wt.%.

3. The multivariate optical coating material according to claim 1, characterized in that: In step S1, the mechanical mixing is ball milling mixing or stirring mixing, and the time of the ball milling mixing or stirring mixing is 4 to 24 hours.

4. The multivariate optical coating material according to claim 1, characterized in that: In step S2, the pressure used in the granulation or pressing process is 300-800 N / cm 2 .

5. The multivariate optical coating material according to claim 1, characterized in that: In step S2, the pressure used in the granulation or pressing process is 500-600 N / cm 2 .

6. The multivariate optical coating material according to claim 1, characterized in that: In step S3, the reaction temperature of the high-temperature solid phase synthesis reaction of the granular material is 1400-1700° C., the heating rate is 5-15° C. / min, and the reaction time is 4-20 hours.

7. The multivariate optical coating material according to claim 1, characterized in that: In step S3, the bulk material is subjected to a high-temperature solid phase synthesis reaction in a two-stage gradient temperature increase manner, comprising: The temperature is 1400-1700℃; the heating rate is 5-15℃ / min, and the time is 6-12h; Raise the temperature to 1700-1900°C at a rate of 7-12°C / min and maintain for 2-4 hours.

8. An application of the multivariate optical coating material according to claim 1 in preparing a hard dielectric optical film, characterized in that: include: The optical coating material is melted at 2000° C. to form a molten optical coating material; Evaporating the molten optical coating material; Wherein, the evaporation is performed using electron beam evaporation equipment; the process parameters of the evaporation include: The vacuum degree is 1.5×10 -4 torr; Evaporation temperature is 1900-2100℃; The evaporation rate is 3A / sec; The substrate temperature was 100°C.