A method for improving the dyeing levelness of PA56 / silk interwoven fabrics
By amino modification and degumming of PA56/silk interwoven, combined with low-temperature weak acid dye dye dye dye, the problem of poor color identity of silk/nylon interwoven dye is solved, and the color fastness and uniformity after dyeing is improved, and the color fastness and uniform dyeing after dyeing is achieved. Resource savings and energy efficiency.
Patent Information
- Application Number
- CN202310417318.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-13
AI Technical Summary
The silk/nylon interwoven fabric has poor color properties during the dyeing process, which leads to the unsatisfactory and uniform dyeing properties of the fabric after dyeing.
By performing amino modification treatment on the PA56/silk interwoven, the amino content on the fiber surface is increased by aqueous polyurethane emulsion and degummed to remove serous, followed by dyeing with a weak acid dye and a homogenizer under low temperature conditions.
It significantly improves the K/S value and uniformity after dyeing, reduces the unevenness rate, achieves better color fastness and dyeing uniformity, and saves resources and energy.
Smart Images

Figure CN116289259B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textile dyeing, in particular to a method for improving the dyeing levelness of a PA56 / silk interwoven fabric. Background Art
[0002] Silk, as a natural protein fiber, is favored by consumers for its many advantages such as non-toxicity, softness, comfort and elegance. The silk fabric prepared by it is famous for its lightness, comfort and breathability. Its skin-friendliness is unmatched by all other fabrics, and it has a pearl-like luster, soft luster, good skin-fitting, and is naturally degradable. It is often used in the development of high-end home clothing products. However, the defects of silk fabrics such as low strength, poor elasticity and easy yellowing affect its quality and consumption. The development of silk / synthetic fiber composite fiber can combine the advantages of silk and synthetic fiber and avoid their shortcomings. This is better than single silk or synthetic fiber in terms of comfort and functionality, and can meet the requirements of fabric diversification and personalization. However, due to the great differences between silk and synthetic fiber in heat resistance and dyeability, this also brings many defects when interweaving with ordinary synthetic fibers: for example, the interweaving of silk and ordinary synthetic fibers greatly reduces the degradability of silk fabrics. Therefore, the development of degradable synthetic fibers and silk for interweaving has become a topic of widespread concern in the textile and clothing industry.
[0003] Nylon, also known as polyamide fiber, is a type of synthetic fiber containing several amide repeating units in its molecular structure. Polyamide is divided into three categories: aliphatic polyamide, aromatic polyamide and aliphatic aromatic polyamide. Due to its excellent comprehensive performance, it has developed rapidly in different fields. At present, the main nylon products in my country are PA6 and PA66, accounting for more than 90% of the total polyamide production. Polyamide fiber is a type of synthetic fiber with organic diamine and diacid, amino acid or lactam as raw materials, and the main chain of the molecule is connected by amide bonds. The raw materials for the production of traditional polyamide fibers rely on petrochemical products and are not easy to degrade. This brings hidden dangers such as resource depletion and environmental pollution, and threatens the health and sustainable development of the environment and human beings; while biomass products are taken from nature and have good biodegradability. They are an effective way to achieve sustainable development of the textile industry and can bring huge economic value and environmental benefits. Biomass fiber polyamide 56 (PA56) is polymerized by pentamethylenediamine and adipic acid prepared by biological fermentation, in which pentamethylenediamine is prepared by biological fermentation process from renewable resources such as corn and wheat. Shanghai Kaisai Biotechnology Co., Ltd. uses bio-based pentamethylenediamine and petroleum-based adipic acid to polymerize PA56, which is a new type of biomass material independently developed by my country. It is an environmentally friendly and sustainable new type of nylon. Yassir A. et al. conducted relevant research on the mechanical properties and hygroscopic properties of bio-based nylon PA56; it was found that under the conditions of different stretching ratios, the mechanical properties of PA56 were slightly worse than those of PA6, but its moisture regain was significantly higher than that of PA6. Yu Weicai conducted relevant research on the physical properties and spinnability of PA56 and found that the saturated water absorption rate of PA56 was higher than that of PA66 and PA6, up to 14%, and its antistatic properties and comfort were greatly improved. Cong Honglian et al. applied bio-based nylon PA56 to the development of knitted fabrics. The study found that bio-based nylon PA56 has good properties such as softness, hygroscopicity, breathability, light weight, and wear resistance, which greatly improved the comfort and wearing performance of nylon; blending with wool, cotton, viscose and other fabrics not only improves the quality of fabrics, but also reduces the cost of fabrics. Zhang Chen et al. studied the performance of low-speed spun bio-based polypentamethylene adipate filaments and found that PA56 has good spinnability, good resilience and hydrophilicity, and its mechanical properties are similar to those of PA66, which has broad application prospects. Chinese patent CN200820040422.1 discloses a method for preparing a knitted nylon silk fabric, which is a two-layer composite structure consisting of a nylon layer and a silk layer. The nylon layer is the front of the fabric, and the silk layer is the inner surface of the fabric in contact with the human body. The nylon layer is a bright nylon layer. The front of the fabric of this new product uses a nylon layer, which has bright colors, high color fastness, wear resistance, and strong gloss, which is better than the gloss of silk; the inner surface uses silk, which has strong moisture absorption and good air permeability. When the fabric is made into clothes, the clothes that come into contact with the human body are silk, which is soft, smooth, comfortable to wear, and also has antibacterial effects.This fabric can be widely used in various T-shirts, sportswear, home textiles, etc.
[0004] As mentioned above, nylon fabrics have a soft hand feel and good elasticity. After silk and nylon are interwoven, the shortcomings of silk fabrics, such as poor dimensional stability and easy wrinkling, can be overcome while maintaining the excellent properties of silk. However, acid dyes have a higher affinity for nylon than silk, resulting in a higher color yield of nylon than silk when dyed at low concentrations. The amino content of nylon is low, which makes the color yield of silk deeper than nylon when dyed at high concentrations. Silk has excellent dyeing properties and can be dyed with acidic, reactive, and direct dyes. However, in actual production, silk fibers are easily damaged under alkaline conditions, so acid dyes are generally selected for dyeing. The dyes and fibers are mainly bonded by hydrogen bonds and Van der Waals forces. When the pH value of the dye bath exceeds the isoelectric point of silk fibers (3.5-4.2), the negative charge of silk increases and its affinity for acid dyes decreases. Chen Yumei et al. found in their study of the dyeing temperature of silk that the higher the dyeing temperature, the lower the dyeing rate. If the temperature is too low, the diffusion coefficient of the dye in the fiber will also decrease, so the dyeing temperature is generally controlled at around 90°C. Nylon is a polyamide fiber, and its composition and structure are simpler than silk. Amino and carboxyl groups only exist at the ends of the molecular chain. The molecule contains long methylene chains and amide groups, and no side chains. There are not only strong Fann forces and hydrogen bonds between acid dye molecules and polyamide fibers, but also the dye anions can be combined with the terminal amino groups of nylon in the form of ionic bonds. The isoelectric point of nylon (5-6) is higher than that of silk, and the macromolecular chain contains a large number of methylene groups. Therefore, when acid dyes are used to dye nylon fabrics, the influence of pH value is relatively small compared to silk. In actual production, weak acid dyes are often used to dye nylon. However, the pH value cannot be too low during dyeing, otherwise the dye will undergo superequivalent adsorption, resulting in reduced color fastness. Therefore, the same color of silk / nylon interweaving is poor. At the same time, acid dyes can ionize dye anions in aqueous solution, because most of their acidic groups are sulfonic acid groups, which are very soluble in water.
[0005] In addition, the dyeing temperature of acid dyes for silk and nylon fabrics is mostly above 90°C, while the optimal same-color temperature of silk / nylon interwoven fabrics is 85°C. Lowering the temperature will inevitably affect the color fastness. Therefore, a suitable fixing agent should be selected after dyeing to improve the color fastness. The fixing agent for nylon is generally anionic, and the fixing agent for silk is generally cationic. Wang Rui et al.'s research shows that after nylon fabrics are dyed with acid dyes, they are first fixed with anionic fixing agents and then fixed with cationic fixing agents for a second time, which can effectively improve the color fastness of the fabric. Although there are reports on improving the same-color leveling properties through the screening of acid dyes, optimization of process parameters and application of same-color leveling agents, the results are still not ideal. Therefore, it is of great significance to study the same-color dyeing process of silk / nylon interwoven fabrics. Summary of the invention
[0006] The object of the present invention is to provide a method for improving the dyeing levelness of PA56 / silk interwoven fabrics, wherein after dyeing, the K / S of the fabric is significantly increased, the unevenness is low, and the dyeing levelness is better.
[0007] The technical solution adopted by the present invention to solve its technical problem is:
[0008] A method for improving the dyeing levelness of PA56 / silk interwoven fabrics, comprising the following steps:
[0009] (1) Amino modification of PA56 / silk interwoven fabric
[0010] The PA56 / silk interwoven fabric is dyed and immersed in a water-based polyurethane emulsion at 60-70° C. for 1-1.5 hours, taken out, dried, and then placed in a steam oven at 100-105° C. for 1-1.5 hours to obtain a PA56 / silk amino-modified interwoven fabric;
[0011] (2) Degumming treatment
[0012] The PA56 / silk amino modified interwoven fabric is placed in a degumming solution for degumming treatment, washed with deionized water, and then dried in an oven;
[0013] (3) Dyeing
[0014] The degummed PA56 / silk amino modified interwoven fabric is immersed in dye solution, dyeing is started at 40°C, the temperature is increased to 70-80°C at a rate of 1-2°C / min, and then kept warm for 60-65min, followed by washing and drying.
[0015] The PA56 / silk interwoven fabric is modified by grafting the fabric surface with an aqueous polyurethane containing a large number of amino groups to increase the amino content on the surface of the PA56 fiber and improve the dimensional stability of the PA56 / silk fabric to facilitate the subsequent dyeing process; the degumming treatment is used to remove the sericin on the silk surface so that the amino content on the surface of PA56 and silk is close.
[0016] The aqueous polyurethane emulsion is prepared by the following steps:
[0017] a: Weigh diisocyanate and polyethylene glycol and react them at 75-80°C for 2-2.5 hours in the presence of nitrogen and a catalyst to generate a polyurethane prepolymer; add an organic solvent to control viscosity during the reaction;
[0018] b: Keep the temperature constant and add chain extender 1 to carry out chain extension reaction for 2-2.5h;
[0019] c: Keep the temperature constant and add chain extender 2 to continue the chain extension reaction for 2-2.5h;
[0020] d: Keep the temperature constant and add the end-capping agent 1 to carry out the end-capping reaction for 2-2.5 hours;
[0021] e: Cool down to 50-55°C, add end-capping agent 2 and carry out end-capping reaction for 1-1.5h;
[0022] f: After the reaction is completed, triethylamine in an amount equal to the molar amount of chain extender 1 is added for neutralization reaction, deionized water is added for high-speed emulsification for 20-30 minutes, and the organic solvent is removed by reduced pressure distillation at room temperature to finally obtain an aqueous polyurethane emulsion with a solid content of 15-30%.
[0023] The diisocyanate is one of hexamethylene diisocyanate and isophorone diisocyanate;
[0024] The polyethylene glycol is PEG 400 or PEG 600;
[0025] The chain extender 1 is 2,2-hydroxymethyl propionic acid or 2,2-hydroxymethyl butyric acid;
[0026] The chain extender 2 is tris(hydroxymethyl)aminomethane;
[0027] The end-capping agent 1 is one of diethylenetriamine, ethylenediamine, and diethyltoluenediamine;
[0028] The end-capping agent 2 is methyl ethyl ketone oxime;
[0029] The molar ratio of diisocyanate, polyethylene glycol, chain extender 1, chain extender 2, end capping agent 1, end capping agent 2 is 4: 1-1.2: 1.2-1.5: 0.4-0.6: 0.8-1: 0.4. The molar ratio is preferably 4: 1: 1.2: 0.6: 0.8: 0.4.
[0030] The catalyst is dibutyltin dilaurate, and its usage is 2% to 3% of the total weight of the two monomers of diisocyanate and polyethylene glycol.
[0031] The organic solvent is acetone or butanone, and the amount of the organic solvent used is 30-50 mL per 1 mol of polyethylene glycol.
[0032] In step (1), the amount of waterborne polyurethane used is 4-6% owf based on the weight of the fabric.
[0033] In step (2), the formula of the degumming solution is: 1.5-2.5wt% sodium carbonate, 0.8-1.5wt% soap powder, and the balance water.
[0034] The parameters of the degumming treatment are set as follows: bath ratio 1:20-50, degumming temperature 95-100°C, and time 2-2.5h.
[0035] In step (2), the dyeing parameters are set as follows: weak acid dye 2-4% owf, acid leveling agent 2-4% owf, pH value of dye solution controlled at 4-5, bath ratio 1:20-25.
[0036] The acid leveling agent is TY-YR005 or Goon302.
[0037] The beneficial effects of the present invention are:
[0038] 1. The present invention uses waterborne polyurethane with a large number of amino groups to carry out amino grafting modification on the surface of PA56 fabric. The main mechanism is as follows:
[0039] Through structural design, tris(hydroxymethyl)aminomethane) is used to extend the chain, the waterborne polyurethane is designed into a hyperbranched structure, and chemical substances containing diamine structure are used for end-capping, so that a large number of amino groups are introduced into the prepared waterborne polyurethane structural chain segments. At the same time, methyl ethyl ketone oxime is used for the second end-capping of the waterborne polyurethane. Taking advantage of the easy unblocking of methyl ethyl ketone oxime at 100-105°C, the NCO active group is exposed and grafted with the amino group on the surface of PA56, so that the surface of PA56 fabric is modified with amino groups. Compared with traditional physical modifications such as plasma modification or ultraviolet light irradiation; its modification process is more thorough and efficient, and the amino content of the modified fabric will be significantly increased.
[0040] 2. In the present invention, steaming treatment at 100-105°C is used in the process of amino grafting modification on the surface of PA56 fabric. As we know, during steam treatment, on the one hand, it can have a shaping effect on the fabric, improve the dimensional stability of the fabric, thereby improving the dyeing stability and preventing wrinkles that are difficult to eliminate during dyeing. On the other hand, under the conditions of wet heat shaping, the amino content at the end of the nylon will also increase to a certain extent, and the dyeing rate of the dye will also be significantly improved.
[0041] 3. In the present invention, the PA56 / silk interwoven fabric is firstly subjected to amino modification so that a large number of amino groups are grafted onto the surfaces of PA56 and silk sericin. In the next step, the PA56 / silk fabric is degummed so that the sericin on the silk surface is removed, so that the amino content on the surfaces of silk and PA56 is not much different, thereby improving the dyeing uniformity of the interwoven fabric.
[0042] 4. In the present invention, since the PA56 / silk interwoven fabric is modified by amino grafting, the amino content on the surface of the PA56 fiber is increased. At the same time, the silk surface itself has a high content of amino groups. Therefore, a small bath ratio and low temperature are used in the dyeing process. Compared with the traditional large bath ratio and high temperature dyeing, the modified interwoven fabric can obtain a good level dyeing effect and save resources and energy. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a physical picture of the dyed fabrics of Example 2 and Comparative Example 2.
[0044] Figure 2 It is the infrared spectrum of waterborne polyurethane. DETAILED DESCRIPTION
[0045] The technical solution of the present invention is further described in detail below through specific embodiments.
[0046] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the following embodiments, unless otherwise specified, are all conventional methods in the art.
[0047] Embodiment 1:
[0048] (1) Amino modification of PA56 / silk interwoven fabric
[0049] According to the calculation of the molar ratio of diisocyanate, polyethylene glycol, chain extender 1, chain extender 2, end capping agent 1, end capping agent 2 (the molar ratio of the six monomers is 4:1:1.2:0.6:0.8:0.4, 1 mol of polyethylene glycol 400 was added to a three-necked flask equipped with a stirrer and a reflux condenser, the three-necked flask was fixed in an oil bath, the temperature was raised to 120°C and vacuum dehydrated for 1h, then the temperature was lowered to 75°C, 4 mol of isophorone diisocyanate and 2% of the total weight of dibutyltin dilaurate of the above two monomers were added, nitrogen was passed for 5min, and the reaction was carried out for 2h to generate a polyurethane prepolymer, 50mL of acetone was added during the reaction to control the viscosity; keeping the temperature constant, 1.2mol 2,2-hydroxymethylbutyric acid was subjected to chain extension reaction for 2h; at the same temperature, 0.6mol tris(hydroxymethyl)aminomethane was added to continue the chain extension reaction for 2h; at the same temperature, 0.8mol diethylenetriamine was added to react for 1h, the temperature was lowered to 50°C, and 0.4mol methyl ethyl ketone oxime was added to cap the reaction for 1h; after the reaction, 1.2mol triethylamine was added to carry out neutralization reaction for 1h, an appropriate amount of deionized water was added for high-speed emulsification for 20min, the rotation speed was 1000r / min, and the acetone was removed by reduced pressure distillation at room temperature to obtain a water-based polyurethane with a solid content of 15%.
[0050] The PA56 / silk interwoven fabric was dyed and immersed in an emulsion containing waterborne polyurethane (wherein the content of waterborne polyurethane was 4% owf of the weight of the fabric), immersed at 60°C for 1 hour, taken out, and dried. The obtained PA56 / silk interwoven fabric was placed in a steam oven at 100°C for 1 hour to obtain a PA56 / silk amino grafted modified interwoven fabric.
[0051] (2) Degumming treatment of PA56 / silk interwoven fabric
[0052] Degumming formula:
[0053] Sodium carbonate 2%
[0054] Soap powder 1%
[0055] Bath ratio 1:20
[0056] Temperature 95℃
[0057] The PA56 / silk amino modified interwoven fabric prepared in step (1) is placed in a degumming solution for degumming. After boiling for 2 hours, the degummed PA56 / silk interwoven fabric is taken out, repeatedly washed with deionized water at about 40° C., and then dried in an oven to check the degree of degumming until the degumming is complete.
[0058] (3) Dyeing of PA56 / silk interwoven fabric
[0059] The PA56 / silk amino grafted modified interwoven fabric prepared in (2) was dyed with weak acid dyes. The dyeing process is as follows: weak acid dye blue C-GR 2% (owf)
[0060] pH 5 (adjusted with 1 mol / L HCl)
[0061] Acid leveling agent TY-YR005 2% (owf) (Dongguan Taiyang Textile Products Co., Ltd., model: TY-YR005) bath ratio 1:20.
[0062] The PA56 / silk amino grafted modified cross-woven fabric was immersed in the dye solution. The dyeing started at 40℃, and the temperature was raised to 70℃ at a rate of 1℃ / min, and then kept warm for 60min, followed by washing and drying. The K / S value and unevenness of the dyed fabric were tested.
[0063] The K / S value of the dyed fabric was tested using a datacolor colorimeter, and the color properties (L*, a*, b*, C*) were recorded. The light source was D65 and the viewing angle was 10°.
[0064] Randomly select 10 points on the PVC colored coated fabric and measure the K / S value of the dyed fabric at the maximum absorption wavelength. According to formula (1), calculate the unevenness U of the PVC coated colored fabric. The smaller the unevenness, the better the levelness.
[0065] Wherein, (K / S)i is the apparent color depth of the fabric measured for the ith time, and n is the number of measurements.
[0066] Embodiment 2:
[0067] (1) Amino modification of PA56 / silk interwoven fabric
[0068] According to the molar ratio of diisocyanate, polyethylene glycol, chain extender 1, chain extender 2, end capping agent 1 and end capping agent 2 being 4:1:1.5:0.4:1:0.4, 1 mol of polyethylene glycol 400 was added to a three-necked flask equipped with a stirrer and a reflux condenser, the three-necked flask was fixed in an oil bath, the temperature was raised to 120°C and vacuum dehydrated for 1 hour, then the temperature was lowered to 75°C, 4 mol of isophorone diisocyanate and 2% of dibutyltin dilaurate of the above two monomers were added, nitrogen was passed for 5 minutes, and the reaction was carried out for 2.5 hours to generate a polyurethane prepolymer, 50 mL of acetone was added during the reaction to control the viscosity; keeping the temperature constant, 1.5 mol of 2,2-hydroxymethylbutyric acid was subjected to chain extension reaction for 2.5h; at the same temperature, 0.4mol tris(hydroxymethyl)aminomethane was added to continue the chain extension reaction for 2.5h; at the same temperature, 1mol ethylenediamine was added to react for 2.5h, the temperature was lowered to 50°C, and 0.4mol methyl ethyl ketone oxime was added to cap the reaction for 1.5h; after the reaction, 1.5mol triethylamine was added to carry out neutralization reaction for 1h, an appropriate amount of deionized water was added for high-speed emulsification for 20min, the rotation speed was 1000r, and the acetone was removed by reduced pressure distillation at room temperature to obtain a water-based polyurethane with a solid content of 20%.
[0069] The PA56 / silk interwoven fabric was dyed and immersed in an emulsion containing waterborne polyurethane (wherein the content of waterborne polyurethane was 6% owf of the weight of the fabric), immersed at 70°C for 1.5 hours, taken out, and dried. The obtained PA56 / silk interwoven fabric was placed in a steam oven at 105°C for 1.5 hours to obtain a PA56 / silk amino-modified interwoven fabric.
[0070] (2) Degumming treatment of PA56 / silk interwoven fabric
[0071] Degumming formula:
[0072] Sodium carbonate 2%
[0073] Soap powder 1%
[0074] Bath ratio 1:50
[0075] Temperature 100℃
[0076] The PA56 / silk amino modified interwoven fabric prepared in step (1) is placed in a degumming solution for degumming, and after boiling for 2.5 hours, the degummed PA56 / silk interwoven fabric is taken out, repeatedly washed with deionized water at about 40° C., and then dried in an oven to check the degree of degumming until the degumming is complete.
[0077] (3) Dyeing of PA56 / silk interwoven fabric
[0078] The PA56 / silk amino grafted modified interwoven fabric prepared in (2) was dyed with weak acid dyes. The dyeing process is as follows: Weak acid dye blue C-GR 4% (owf) (Wuxi Fino Dye Chemical Co., Ltd.)
[0079] pH 4 (adjusted with 1 mol / L HCl)
[0080] Acid leveling agent Goon302 4% (owf) (Dongguan Jiahong Technology Co., Ltd., model: Goon302)
[0081] Bath ratio 1:20.
[0082] The PA56 / silk amino grafted modified interwoven fabric was immersed in the dye solution. The dyeing started at 40℃, and the temperature was raised to 80℃ at a rate of 1℃ / min, and then kept at that temperature for 60min, followed by washing and drying. The test conditions were the same as above.
[0083] Embodiment 3:
[0084] (1) Amino modification of PA56 / silk interwoven fabric
[0085] According to the molar ratio of diisocyanate, polyethylene glycol, chain extender 1, chain extender 2, end capping agent 1, and end capping agent 2 being 4:1:1.3:0.5:1:0.4, 1 mol of polyethylene glycol 600 was added to a three-necked flask equipped with a stirrer and a reflux condenser, the three-necked flask was fixed in an oil bath, the temperature was raised to 120°C and vacuum dehydrated for 1 hour, then the temperature was lowered to 75°C, 4 mol of hexamethylene diisocyanate and 3% of dibutyltin dilaurate of the above two monomers were added, nitrogen was passed through for 5 minutes, and the reaction was carried out for 2.3 hours to generate a polyurethane prepolymer, and 50 mL of butanone was added during the reaction to control viscosity. ; Keeping the temperature constant, add 1.3 mol of chain extender 2,2-hydroxymethylpropionic acid to carry out chain extension reaction for 2.3 hours; at the same temperature, add 0.5 mol of tris(hydroxymethyl)aminomethane to continue chain extension reaction for 2.3 hours; at the same temperature, add 1 mol of diethyltoluenediamine to react for 2.5 hours, cool to 50°C, add 0.4 mol of methyl ethyl ketone oxime to cap the reaction for 1.3 hours; after the reaction, add 1.3 mol of triethylamine to carry out neutralization reaction for 1 hour, add appropriate amount of deionized water for high-speed emulsification for 20 minutes, the rotation speed is 1000r, and remove acetone by reduced pressure distillation at room temperature to obtain a water-based polyurethane with a solid content of 30%.
[0086] The PA56 / silk interwoven fabric was dyed and immersed in an emulsion containing waterborne polyurethane (wherein the content of waterborne polyurethane was 5% owf of the weight of the fabric), immersed at 65°C for 1.3 hours, taken out, and dried. The obtained PA56 / silk interwoven fabric was placed in a steam oven at 103°C for 1.3 hours to obtain a PA56 / silk amino-modified interwoven fabric.
[0087] (2) Degumming treatment of PA56 / silk interwoven fabric
[0088] Degumming formula:
[0089] Sodium carbonate 2%
[0090] Soap powder 1%
[0091] Bath ratio 1:30
[0092] Temperature 98℃
[0093] The PA56 / silk amino modified interwoven fabric prepared in step (1) is placed in a degumming solution for degumming. After boiling for 2.3 hours, the degummed PA56 / silk interwoven fabric is taken out and repeatedly washed with deionized water at about 40° C., and then dried in an oven to check the degree of degumming until the degumming is complete.
[0094] (3) Dyeing of PA56 / silk interwoven fabric
[0095] The PA56 / silk amino grafted modified interwoven fabric prepared in (2) was dyed with weak acid dyes. The dyeing process is as follows: weak acid dye blue C-GR 3% (owf)
[0096] pH 4.5 (adjusted with 1 mol / L HCl)
[0097] Acid leveling agent TY-YR005 3% (owf) (Dongguan Taiyang Textile Products Co., Ltd., model: TY-YR005) bath ratio 1:20.
[0098] The PA56 / silk amino grafted modified interwoven fabric was immersed in the dye solution. The dyeing started at 40℃, and the temperature was raised to 75℃ at a rate of 1℃ / min, and then kept at that temperature for 60min, followed by washing and drying. The test conditions were the same as above.
[0099] Comparative Example 1:
[0100] (1) Degumming treatment of PA56 / silk interwoven fabric
[0101] Degumming formula:
[0102] Sodium carbonate 2%
[0103] Soap powder 1%
[0104] Bath ratio 1:20
[0105] Temperature 100℃
[0106] The PA56 / silk interwoven fabric was degummed in a solution of 2% sodium carbonate and 1% soap powder at a bath ratio of 1:20, 100°C, and by mass. After boiling for 2.5 hours, the degummed PA56 / silk interwoven fabric was taken out and repeatedly washed with deionized water at about 40°C, and then dried in an oven to check the degree of degumming until the degumming was complete.
[0107] (2) Dyeing of PA56 / silk interwoven fabric
[0108] The PA56 / silk interwoven fabric prepared in (1) is dyed with a weak acid dye. The dyeing process is as follows:
[0109] Weakly Acid Dye Blue C-GR 3% (owf)
[0110] pH 4.5 (adjusted with 1 mol / L HCl)
[0111] Acid leveling agent TY-YR005 3% (owf) (Dongguan Taiyang Textile Products Co., Ltd., model: TY-YR005) bath ratio 1:20.
[0112] The PA56 / silk interwoven fabric was immersed in the dye solution. The dyeing started at 40℃, and the temperature was raised to 75℃ at a rate of 1℃ / min, and then kept at that temperature for 60min, followed by washing and drying. The test conditions were the same as above.
[0113] Comparative Example 2:
[0114] (1) Degumming treatment of PA56 / silk interwoven fabric
[0115] Degumming formula:
[0116] Sodium carbonate 2%
[0117] Soap powder 1%
[0118] Bath ratio 1:20
[0119] Temperature 100℃
[0120] The PA56 / silk interwoven fabric was degummed in a solution of 2% sodium carbonate and 1% soap powder at a bath ratio of 1:20, 100°C, and by mass. After boiling for 2.5 hours, the degummed PA56 / silk interwoven fabric was taken out and repeatedly washed with deionized water at about 40°C, and then dried in an oven to check the degree of degumming until the degumming was complete.
[0121] (2) Dyeing of PA56 / silk interwoven fabric
[0122] The PA56 / silk interwoven fabric prepared in (1) is dyed with a weak acid dye. The dyeing process is as follows:
[0123] Weakly Acid Dye Blue C-GR 3% (owf)
[0124] pH 4.5 (adjusted with 1 mol / L HCl)
[0125] Acid leveling agent TY-YR005 3% (owf) (Dongguan Taiyang Textile Products Co., Ltd., model: TY-YR005) bath ratio 1:100.
[0126] PA56 / silk interwoven fabric was immersed in dye solution. Dyeing started at 40℃, and the temperature was raised to 100℃ at a rate of 1℃ / min, and then kept at that temperature for 60min, followed by washing and drying. The test conditions were the same as above.
[0127] Table 1 Example 1-Comparative Example 2 PA56 amino grafted modified / silk interwoven fabric dyeing K / S and unevenness
[0128]
[0129]
[0130] from Figure 1 It can be seen that compared with the traditional PA56 dyeing temperature at 100℃ and the dyeing bath ratio of 1:100, the amino-grafted modified PA56 / silk interwoven fabric can achieve a good level dyeing effect under the low temperature dyeing conditions of 70-80℃ and a small bath ratio of 1:20, while saving resources and energy.
[0131] from Figure 2 It can be seen that 1360cm -1 Corresponding to CH characteristic absorption peak; 1540~1560cm -1 The peak at 1700-1710 cm-1 corresponds to the mixed peak of CC, CN and NH characteristic vibrations; the absorption peak of carbamate structure and carbonyl (-C=O) in DMBA appears at 1700-1710 cm-1 -1 The CH stretching vibration peak is located at 2960-2970cm -1 3370cm -1 The peak at 40° is attributed to NH stretching vibration. The appearance of these characteristic absorption peaks can prove the successful synthesis of waterborne polyurethane.
[0132] As can be seen from Table 1, the surface of the PA56 / silk interwoven fabric is modified by amino grafting with water-based polyurethane containing a large amount of amino groups, so that the amino content on the surface of the PA56 / silk interwoven fabric is increased, and the sericin on the silk surface is removed by alkali desizing, so that the difference in the amino content on the surface of PA56 and silk is small. Therefore, the K / S of the PA56 / silk interwoven fabric is significantly increased after dyeing, and the levelness of the fabric after dyeing is also improved, and the unevenness is small.
[0133] The above-described embodiment is only a preferred solution of the present invention and does not limit the present invention in any form. There are other variations and modifications without exceeding the technical solution described in the claims.
Claims
1. A method for improving the dyeing levelness of PA56 / silk interwoven fabrics. It is characterized in that The following steps are involved: (1) Amino modification of PA56 / silk interwoven fabric The PA56 / silk interwoven fabric is immersed in an aqueous polyurethane emulsion at 60-70° C. for 1-1.5 hours, taken out, dried, and then placed in a steam oven at 100-105° C. for 1-1.5 hours to obtain a PA56 / silk amino-modified interwoven fabric; (2) Degumming treatment The PA56 / silk amino modified interwoven fabric is placed in a degumming solution for degumming treatment, washed with deionized water, and then dried in an oven; (3) Dyeing The degummed PA56 / silk amino modified interwoven fabric is immersed in the dye solution, dyed at 40°C, heated to 70-80°C at a rate of 1-2°C / min, and kept warm for 60-65min, then washed and dried; The aqueous polyurethane emulsion is prepared by the following steps: a: Weigh diisocyanate and polyethylene glycol and react them at 75-80°C for 2-2.5 hours in the presence of nitrogen and a catalyst to generate a polyurethane prepolymer; add an organic solvent to control viscosity during the reaction; b: Keep the temperature constant and add chain extender 1 to carry out chain extension reaction for 2-2.5 h; c: Keep the temperature constant and add chain extender 2 to continue the chain extension reaction for 2-2.5 h; d: Keep the temperature constant and add the end-capping agent 1 to carry out the end-capping reaction for 2-2.5 h; e: Cool down to 50-55 °C, add end-capping agent 2 and carry out end-capping reaction for 1-1.5 h; f: After the reaction is completed, triethylamine in an amount equal to the molar amount of the chain extender 1 is added for neutralization reaction, deionized water is added for high-speed emulsification for 20-30 min, and the organic solvent is removed by reduced pressure distillation at room temperature to finally obtain an aqueous polyurethane emulsion with a solid content of 15-30%; The chain extender 1 is 2,2-hydroxymethylpropionic acid or 2,2-hydroxymethylbutyric acid; the chain extender 2 is trishydroxymethylaminomethane; the end capping agent 1 is one of diethylenetriamine, ethylenediamine, and diethyltoluenediamine; and the end capping agent 2 is methyl ethyl ketone oxime.
2. The method according to claim 1, It is characterized in that The diisocyanate is one of hexamethylene diisocyanate and isophorone diisocyanate; The polyethylene glycol is PEG 400 or PEG 600; The molar ratio of diisocyanate, polyethylene glycol, chain extender 1, chain extender 2, end capping agent 1, and end capping agent 2 is 4:1-1.2:1.2-1.5:0.4-0.6:0.8-1:0.
4.
3. The method according to claim 1, It is characterized in that The catalyst is dibutyltin dilaurate, and its usage is 2% to 3% of the total weight of the two monomers of diisocyanate and polyethylene glycol.
4. The method according to claim 1, It is characterized in that The organic solvent is acetone or butanone, and the amount of the organic solvent used is 30-50 mL per 1 mol of polyethylene glycol.
5. The method according to claim 1, It is characterized in that In step (1), the amount of waterborne polyurethane used is 4-6% owf based on the weight of the fabric.
6. The method according to claim 1, It is characterized in that In step (2), the formula of the degumming solution is: 1.5-2.5wt% sodium carbonate, 0.8-1.5wt% soap powder, and the balance water.
7. The method according to claim 6, It is characterized in that The parameters of the degumming treatment are set as follows: bath ratio 1:20-50, degumming temperature 95-100°C, and time 2-2.5 h.
8. The method according to claim 1, It is characterized in that In step (3), the dyeing parameters are set as follows: weak acid dye 2-4% owf, acid leveling agent 2-4% owf, pH value of dye solution controlled at 4-5, bath ratio 1:20-25.
9. The method according to claim 8, It is characterized in that The acid leveling agent is TY-YR005 or Goon302.