Double-sided high temperature resistant release film and preparation method thereof

By using a porous network structure of carbon doped boron carbide as the skeleton in the PET film and performing low-temperature plasma treatment, the thermal shrinkage and viscosity unevenness of the PET film under high temperature conditions is solved, and efficient release effect and resistance are achieved High temperature performance improves the toughness and application range of the membrane.

CN117507539BActive Publication Date: 2024-12-06SUZHOU AOBEIXIN MATERIAL TECH LTD CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311447891.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-02
Publication Date
2024-12-06
Estimated Expiration
2043-11-02

AI Technical Summary

Technical Problem

The existing PET release films have defects such as poor thermal shrinkage, uneven viscosity, and incomplete plasticization of materials or overheating during extrusion under high temperature conditions, resulting in defects on the film surface, affecting normal production and composite The film material has insufficient high temperature resistance and dispersion.

Method used

Using a porous network structure of carbon doped boron carbide as the skeleton, a single-layer high-temperature releasing film was prepared by electrospinning, and graft polymerization was performed in low-temperature plasma treatment to improve the adhesion performance with PET substrates and form multi-layers Strength to enhance toughness and bending resistance.

Benefits of technology

实现了在不添加离型剂的情况下,PET膜的良好离型效果,提高了耐高温性能和韧性,降低了废品率,增强了膜的应用范围。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004528020320000071
    Figure BDA0004528020320000071
  • Figure BDA0004528020320000091
    Figure BDA0004528020320000091
Patent Text Reader

Abstract

The present invention provides a double-sided high temperature resistant release film and a preparation method thereof. The method comprises the following steps: placing a carbon-doped boron carbide porous network structure in the center of a lower electrode of a low temperature plasma device for treatment to obtain the treated carbon-doped boron carbide porous network structure; laying it flat in a mold; drying PET in an oven, adding it to a single screw extruder, and casting it into a mold paved with the treated carbon-doped boron carbide porous network structure, wherein PET coats the treated carbon-doped boron carbide porous network structure. The present invention adopts a single-layer high temperature resistant release film prepared with a carbon-doped boron carbide porous network structure as a skeleton. Boron carbide has a strong covalent bond, a large resistance to grain boundary movement, and a very low surface tension. When it is added to a PET film, a very good release effect can be achieved without adding a release agent. At the same time, by adding boron carbide and carbon together to form a network skeleton structure, the problem of poor composite adhesion with PET and inability to have a good bonding effect with PET is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of release films, specifically to a double-sided high-temperature resistant release film and its preparation method. Background Technology

[0002] Release film, also known as release liner, peeling film, or separation film, is most commonly made of PET. The manufacturing process for PET release film involves vapor deposition, multiple coatings, lamination, and final peeling. This process is lengthy and involves many steps, with temperatures mostly between 120℃ and 150℃, and occasionally reaching as high as 190℃. Therefore, release film needs excellent high-temperature resistance. Currently, high-temperature resistant PET release films are mainly composite release film materials, typically with two structures: Structure 1: Release film layer / adhesive layer / high-temperature resistant resin layer (lamination sequence); Structure 2: Release film layer / high-temperature resistant resin layer. However, composite films have the following drawbacks: the release resin film layer and the substrate resin film layer materials differ in temperature resistance and crystallinity, ranging from highly crystalline to amorphous materials. The degree of molecular chain segment movement under high-temperature conditions also varies. To combine them while maintaining good appearance and dimensional stability, especially avoiding significant thermal shrinkage during use, is challenging. Furthermore, the polymer properties vary considerably depending on the crystallization temperature, casting speed ratio, and viscosity during extrusion plasticizing. The matching extrusion plasticizing system, particularly the extruder screw and die head, significantly impacts film performance. Therefore, controlling the two resins during the extrusion plasticizing process is crucial. Improper design can lead to incomplete plasticizing or shear overheating during extrusion, resulting in defects such as small black spots, white hard lumps, and focal spots on the film surface. More seriously, it can cause perforation during molding, hindering normal production and resulting in high scrap rates. Therefore, simplifying the process while providing a high-temperature resistant release film is an urgent problem to be solved. Summary of the Invention

[0003] Technical Problem to be Solved: To address the aforementioned technical problems, the purpose of this invention is to provide a double-sided high-temperature resistant release film and its preparation method. This invention provides a high-temperature resistant release film entirely different from composite layers, using a carbon-doped boron carbide porous network structure as the framework to prepare a single-layer high-temperature resistant release film. Boron carbide has strong covalent bonds, high grain boundary movement resistance, and very low surface tension. Adding it to PET film can achieve excellent release effects without the addition of a release agent. However, due to its low surface tension and low self-diffusion coefficient, it cannot be uniformly dispersed in PET. Furthermore, simply adding boron carbide results in poor adhesion to PET, failing to achieve good bonding. Therefore, this application uses boron carbide together with carbon to form a network framework structure, solving the problem of poor dispersibility and inability to uniformly disperse in PET materials.

[0004] Technical solution: A double-sided high-temperature resistant release film, which is a double-sided high-temperature resistant release film with a carbon-doped boron carbide porous network structure as the skeleton and PET coated on it. The carbon-doped boron carbide porous network structure itself has mesopores.

[0005] Furthermore, the preparation method of the carbon-doped boron carbide porous network structure is as follows:

[0006] S1: Dissolve polyacrylonitrile in N,N-dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 9-10%;

[0007] S2: Dissolve polymethyl methacrylate in N,N-dimethylformamide to obtain a polymethyl methacrylate solution with a mass fraction of 9-10%.

[0008] S3: Mix polyacrylonitrile solution and polymethyl methacrylate solution, add pretreated boron carbide nanoparticles, stir evenly, and use as electrospinning solution;

[0009] S4: Electrospinning is performed using an electrospinning device to obtain an electrospinned membrane;

[0010] S5: Place the electrospun film in an oven and dry it at 80℃, then heat it to 200-300℃ for pre-oxidation for 5-8 hours;

[0011] S6: After being removed, it is placed in a sintering furnace and sintered at a temperature of 900-1200℃ for 1-2 hours to obtain a carbon-doped boron carbide porous network as a framework structure.

[0012] Furthermore, the pore size of the carbon-doped boron carbide porous network structure is 6-15 μm, and the porosity is 30-43%.

[0013] Furthermore, the mass ratio of polyacrylonitrile to polymethyl methacrylate is (7:3)-(2:1); the mass ratio of polyacrylonitrile to nano boron carbide particles is 2:(7-12).

[0014] Furthermore, the pretreatment method for the boron carbide nanoparticles is as follows:

[0015] S31: Place boron carbide nanoparticles with a particle size of 100-500nm in an oven and dry them to obtain dried boron carbide nanoparticles;

[0016] S32: Dry boron carbide nanoparticles are pulverized a second time using an air jet mill;

[0017] S33: After collecting the boron carbide nanoparticles, use an ultrasonic instrument to sonicate them for 1-2 minutes to obtain the pretreated boron carbide nanoparticles.

[0018] Furthermore, the electrospinning conditions are as follows: spinning speed is 2.0 mL / h, spinning voltage is 25 kV, distance between needle and receiving plate is 15 cm, and ambient temperature is 25-37℃.

[0019] Furthermore, the classifying speed of the air jet mill is 2000 r / min.

[0020] The preparation method of the above-mentioned double-sided high-temperature resistant release film includes the following steps:

[0021] (1) The carbon-doped boron carbide porous network structure is placed in the center of the lower electrode of the low-temperature plasma device for processing to obtain the processed carbon-doped boron carbide porous network structure.

[0022] (2) The treated carbon-doped boron carbide porous network structure is laid flat in the mold;

[0023] (3) Dry the PET in an oven and add it to a single screw extruder. The temperatures of each section of the single screw extrusion are 180℃, 220℃, 250℃, 260℃ and 265℃. The PET is then cast into a mold with the treated carbon-doped boron carbide porous network structure. The PET then coats the treated carbon-doped boron carbide porous network structure to obtain the final product.

[0024] Furthermore, the low-temperature plasma treatment conditions are as follows: positive corona discharge is used, a stainless steel mesh is connected to the negative terminal of the power supply, the hollow nozzle electrode is connected to the positive terminal of the power supply, and the DC high-voltage power supply output power is 150W.

[0025] Furthermore, the volume ratio of the treated carbon-doped boron carbide porous network structure to PET is 1:(2.7-4.3).

[0026] Beneficial effects:

[0027] 1. This invention provides a high-temperature resistant release film that is completely different from composite layers. Instead, it is a single-layer high-temperature resistant release film prepared with a porous network structure of boron carbide doped with carbon as the skeleton. Boron carbide has strong covalent bonds, high resistance to grain boundary movement, and very low surface tension. When added to PET film, it can achieve a very good release effect without the addition of release agent. However, due to its low surface tension, it has a very low self-diffusion coefficient and cannot be uniformly dispersed in PET. At the same time, simply adding boron carbide to PET results in poor adhesion and no good bonding effect with PET. Therefore, this application makes it into a network skeleton structure together with carbon to solve the problem of poor dispersibility and inability to be uniformly dispersed in PET material.

[0028] 2. The carbon-doped boron carbide porous network structure of this invention is prepared by electrospinning and has a porous structure. At the same time, the network structure itself also has mesopores (due to the difference in surface tension between polyacrylonitrile and polymethyl methacrylate, polyacrylonitrile with low surface tension easily forms a continuous phase, while polymethyl methacrylate with high surface tension forms a dispersed phase. During heat treatment, the dispersed polymethyl methacrylate decomposes to form mesopores). On the one hand, it can increase the bonding force with the PET substrate. On the other hand, the two different pore structures also have multi-layered structure. This multi-layered structure allows the release film to release pressure when bent, improving the toughness of the release film.

[0029] 3. The porous network structure of boron carbide doped with carbon in this invention has also undergone low-temperature plasma treatment, which utilizes the active free radicals generated on the surface to initiate the grafting polymerization of olefin monomers on the surface of carbon materials in boron carbide doped with carbon, thereby improving the adhesion performance with PET substrate.

[0030] 4. The carbon-doped boron carbide porous network structure used in this invention not only enables the PET substrate to have release properties, but also improves the high temperature resistance of the PET substrate.

[0031] 5. In this invention, the boron carbide nanoparticles are subjected to secondary pulverization by an air jet mill before use. Air jet milling is carried out under the action of high-speed airflow. The boron carbide nanoparticles are impacted, sheared, and rubbed by the airflow through the collision between the particles themselves. This effectively solves the problem of easy agglomeration of boron carbide nanoparticles and also reduces their surface tension, resulting in a better release effect in the release film.

[0032] 6. The release film of the present invention has release effect on both sides, which can improve its application range. Detailed Implementation

[0033] This invention proposes a double-sided high-temperature resistant release film and its preparation method. To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the following will provide a more detailed description of the invention with reference to specific embodiments. It should be understood that the specific embodiments described herein are only for explaining the invention and are not intended to limit the invention.

[0034] Example 1

[0035] The pretreatment method for boron carbide nanoparticles is as follows:

[0036] S31: Place boron carbide nanoparticles with a particle size of 100-500nm in an oven and dry them to obtain dried boron carbide nanoparticles;

[0037] S32: Dry boron carbide nanoparticles are pulverized a second time using an air jet mill, with a classifying speed of 2000 r / min.

[0038] S33: After collecting the boron carbide nanoparticles, sonicate them for 2 minutes using an ultrasonic instrument to obtain the pretreated boron carbide nanoparticles.

[0039] Example 2

[0040] The preparation method of the carbon-doped boron carbide porous network structure is as follows:

[0041] S1: Dissolve polyacrylonitrile in N,N-dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 9%;

[0042] S2: Dissolve polymethyl methacrylate in N,N-dimethylformamide to obtain a polymethyl methacrylate solution with a mass fraction of 9%;

[0043] S3: Mix polyacrylonitrile solution and polymethyl methacrylate solution, with a mass ratio of polyacrylonitrile to polymethyl methacrylate of 7:3, add pretreated boron carbide nanoparticles, stir evenly, and use as electrospinning solution, wherein the mass ratio of polyacrylonitrile to boron carbide nanoparticles is 2:9.

[0044] S4: Electrospinning was performed using an electrospinning device. The electrospinning conditions were: spinning speed of 2.0 mL / h, spinning voltage of 25 kV, distance between needle and receiving plate of 15 cm, and ambient temperature of 30 °C to obtain an electrospinned membrane.

[0045] S5: Place the electrospun film in an oven and dry it at 80℃, then heat it to 250℃ for pre-oxidation for 7 hours;

[0046] S6: After removal, place in a sintering furnace and sinter at 1100℃ for 1.5 hours to obtain a carbon-doped boron carbide porous network as a framework structure. The carbon-doped boron carbide porous network framework structure itself has mesopores on its fibers.

[0047] Example 3

[0048] The preparation method of the carbon-doped boron carbide porous network structure is as follows:

[0049] S1: Dissolve polyacrylonitrile in N,N-dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 9%;

[0050] S2: Dissolve polymethyl methacrylate in N,N-dimethylformamide to obtain a polymethyl methacrylate solution with a mass fraction of 10%.

[0051] S3: Mix polyacrylonitrile solution and polymethyl methacrylate solution, with a mass ratio of polyacrylonitrile to polymethyl methacrylate of 7:3, add pretreated boron carbide nanoparticles, stir evenly, and use as electrospinning solution, wherein the mass ratio of polyacrylonitrile to boron carbide nanoparticles is 2:9.

[0052] S4: Electrospinning was performed using an electrospinning device. The electrospinning conditions were: spinning speed of 2.0 mL / h, spinning voltage of 25 kV, distance between needle and receiving plate of 15 cm, and ambient temperature of 30 °C to obtain an electrospinned membrane.

[0053] S5: Place the electrospun film in an oven and dry it at 80℃, then heat it to 250℃ for pre-oxidation for 7 hours;

[0054] S6: After removal, place in a sintering furnace and sinter at 1100℃ for 1.5 hours to obtain a carbon-doped boron carbide porous network as a framework structure. The carbon-doped boron carbide porous network framework structure itself has mesopores on its fibers.

[0055] Example 4

[0056] The preparation method of the carbon-doped boron carbide porous network structure is as follows:

[0057] S1: Dissolve polyacrylonitrile in N,N-dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 10%;

[0058] S2: Dissolve polymethyl methacrylate in N,N-dimethylformamide to obtain a polymethyl methacrylate solution with a mass fraction of 9%;

[0059] S3: Mix polyacrylonitrile solution and polymethyl methacrylate solution, with a mass ratio of polyacrylonitrile to polymethyl methacrylate of 7:3, add pretreated boron carbide nanoparticles, stir evenly, and use as electrospinning solution, wherein the mass ratio of polyacrylonitrile to boron carbide nanoparticles is 2:9.

[0060] S4: Electrospinning was performed using an electrospinning device. The electrospinning conditions were: spinning speed of 2.0 mL / h, spinning voltage of 25 kV, distance between needle and receiving plate of 15 cm, and ambient temperature of 30 °C to obtain an electrospinned membrane.

[0061] S5: Place the electrospun film in an oven and dry it at 80℃, then heat it to 250℃ for pre-oxidation for 7 hours;

[0062] S6: After removal, place in a sintering furnace and sinter at 1100℃ for 1.5 hours to obtain a carbon-doped boron carbide porous network as a framework structure. The carbon-doped boron carbide porous network framework structure itself has mesopores on its fibers.

[0063] Example 5

[0064] The preparation method of the carbon-doped boron carbide porous network structure is as follows:

[0065] S1: Dissolve polyacrylonitrile in N,N-dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 10%;

[0066] S2: Dissolve polymethyl methacrylate in N,N-dimethylformamide to obtain a polymethyl methacrylate solution with a mass fraction of 10%.

[0067] S3: Mix polyacrylonitrile solution and polymethyl methacrylate solution, with a mass ratio of polyacrylonitrile to polymethyl methacrylate of 7:3, add pretreated boron carbide nanoparticles, stir evenly, and use as electrospinning solution, wherein the mass ratio of polyacrylonitrile to boron carbide nanoparticles is 2:9.

[0068] S4: Electrospinning was performed using an electrospinning device. The electrospinning conditions were: spinning speed of 2.0 mL / h, spinning voltage of 25 kV, distance between needle and receiving plate of 15 cm, and ambient temperature of 30 °C to obtain an electrospinned membrane.

[0069] S5: Place the electrospun film in an oven and dry it at 80℃, then heat it to 250℃ for pre-oxidation for 7 hours;

[0070] S6: After removal, place in a sintering furnace and sinter at 1100℃ for 1.5 hours to obtain a carbon-doped boron carbide porous network as a framework structure. The carbon-doped boron carbide porous network framework structure itself has mesopores on its fibers.

[0071] Example 6

[0072] The preparation method of the carbon-doped boron carbide porous network structure is as follows:

[0073] S1: Dissolve polyacrylonitrile in N,N-dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 9%;

[0074] S2: Dissolve polymethyl methacrylate in N,N-dimethylformamide to obtain a polymethyl methacrylate solution with a mass fraction of 9%;

[0075] S3: Mix polyacrylonitrile solution and polymethyl methacrylate solution, with a mass ratio of polyacrylonitrile to polymethyl methacrylate of 2:1, add pretreated boron carbide nanoparticles, stir evenly, and use as electrospinning solution, wherein the mass ratio of polyacrylonitrile to boron carbide nanoparticles is 2:9.

[0076] S4: Electrospinning was performed using an electrospinning device. The electrospinning conditions were: spinning speed of 2.0 mL / h, spinning voltage of 25 kV, distance between needle and receiving plate of 15 cm, and ambient temperature of 30 °C to obtain an electrospinned membrane.

[0077] S5: Place the electrospun film in an oven and dry it at 80℃, then heat it to 250℃ for pre-oxidation for 7 hours;

[0078] S6: After removal, place in a sintering furnace and sinter at 1100℃ for 1.5 hours to obtain a carbon-doped boron carbide porous network as a framework structure. The carbon-doped boron carbide porous network framework structure itself has mesopores on its fibers.

[0079] Example 7

[0080] The preparation method of the carbon-doped boron carbide porous network structure is as follows:

[0081] S1: Dissolve polyacrylonitrile in N,N-dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 9%;

[0082] S2: Dissolve polymethyl methacrylate in N,N-dimethylformamide to obtain a polymethyl methacrylate solution with a mass fraction of 9%;

[0083] S3: Mix polyacrylonitrile solution and polymethyl methacrylate solution, with a mass ratio of polyacrylonitrile to polymethyl methacrylate of 7:3, add pretreated boron carbide nanoparticles, stir evenly, and use as electrospinning solution, wherein the mass ratio of polyacrylonitrile to boron carbide nanoparticles is 2:7.

[0084] S4: Electrospinning was performed using an electrospinning device. The electrospinning conditions were: spinning speed of 2.0 mL / h, spinning voltage of 25 kV, distance between needle and receiving plate of 15 cm, and ambient temperature of 30 °C to obtain an electrospinned membrane.

[0085] S5: Place the electrospun film in an oven and dry it at 80℃, then heat it to 250℃ for pre-oxidation for 7 hours;

[0086] S6: After removal, place in a sintering furnace and sinter at 1100℃ for 1.5 hours to obtain a carbon-doped boron carbide porous network as a framework structure. The carbon-doped boron carbide porous network framework structure itself has mesopores on its fibers.

[0087] Example 8

[0088] The preparation method of the carbon-doped boron carbide porous network structure is as follows:

[0089] S1: Dissolve polyacrylonitrile in N,N-dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 9%;

[0090] S2: Dissolve polymethyl methacrylate in N,N-dimethylformamide to obtain a polymethyl methacrylate solution with a mass fraction of 9%;

[0091] S3: Mix polyacrylonitrile solution and polymethyl methacrylate solution, with a mass ratio of polyacrylonitrile to polymethyl methacrylate of 7:3, add pretreated boron carbide nanoparticles, stir evenly, and use as electrospinning solution, wherein the mass ratio of polyacrylonitrile to boron carbide nanoparticles is 2:12.

[0092] S4: Electrospinning was performed using an electrospinning device. The electrospinning conditions were: spinning speed of 2.0 mL / h, spinning voltage of 25 kV, distance between needle and receiving plate of 15 cm, and ambient temperature of 30 °C to obtain an electrospinned membrane.

[0093] S5: Place the electrospun film in an oven and dry it at 80℃, then heat it to 250℃ for pre-oxidation for 7 hours;

[0094] S6: After removal, place in a sintering furnace and sinter at 1100℃ for 1.5 hours to obtain a carbon-doped boron carbide porous network as a framework structure. The carbon-doped boron carbide porous network framework structure itself has mesopores on its fibers.

[0095] The porosity, network pore size, and mesopore size of the fibers in the carbon-doped boron carbide porous network structure were determined.

[0096] Comparative Example 1

[0097] The difference between this embodiment and Embodiment 2 is that a polymethyl methacrylate solution is not used; instead, a polyacrylonitrile solution is used alone. Specifically:

[0098] The preparation method of the carbon-doped boron carbide porous network structure is as follows:

[0099] S1: Dissolve polyacrylonitrile in N,N-dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 9%;

[0100] S2: Add the pretreated boron carbide nanoparticles and stir evenly to make an electrospinning solution, wherein the mass ratio of polyacrylonitrile to boron carbide nanoparticles is 2:9.

[0101] S3: Electrospinning was performed using an electrospinning device. The electrospinning conditions were: spinning speed of 2.0 mL / h, spinning voltage of 25 kV, distance between needle and receiving plate of 15 cm, and ambient temperature of 30 °C to obtain an electrospinned membrane.

[0102] S4: Place the electrospun film in an oven and dry it at 80℃, then heat it to 250℃ for pre-oxidation for 7 hours;

[0103] S5: After removal, place in a sintering furnace and sinter at 1100℃ for 1.5 hours to obtain a carbon-doped boron carbide porous network as a framework structure. The carbon-doped boron carbide porous network as a framework structure itself has almost no mesopores on its fibers.

[0104] Table 1 Performance indicators of the carbon-doped boron carbide porous network structure

[0105]

[0106] Based on a comprehensive comparison of the data in Table 1, the carbon-doped boron carbide porous network structures prepared in Examples 2 and 8 were selected for subsequent experiments.

[0107] Example 9

[0108] A method for preparing a double-sided high-temperature resistant release film includes the following steps:

[0109] (1) The carbon-doped boron carbide porous network structure was placed in the center of the lower electrode of the low-temperature plasma device for treatment. The low-temperature plasma treatment conditions were: positive corona discharge was used, the stainless steel mesh was connected to the negative terminal of the power supply, the hollow nozzle electrode was connected to the positive terminal of the power supply, and the DC high voltage power supply output power was 150W. The treated carbon-doped boron carbide porous network structure was obtained.

[0110] (2) The treated carbon-doped boron carbide porous network structure is laid flat in the mold;

[0111] (3) Dry the PET in an oven and add it to a single-screw extruder. The temperatures of each section of the single-screw extrusion are 180℃, 220℃, 250℃, 260℃ and 265℃. The PET is then cast into a mold with the treated boron carbide porous network structure. The PET coats the treated boron carbide porous network structure to obtain the final product. The volume ratio of the treated boron carbide porous network structure to the PET is 1:2.7.

[0112] Example 10

[0113] A method for preparing a double-sided high-temperature resistant release film includes the following steps:

[0114] (1) The carbon-doped boron carbide porous network structure was placed in the center of the lower electrode of the low-temperature plasma device for treatment. The low-temperature plasma treatment conditions were: positive corona discharge was used, the stainless steel mesh was connected to the negative terminal of the power supply, the hollow nozzle electrode was connected to the positive terminal of the power supply, and the DC high voltage power supply output power was 150W. The treated carbon-doped boron carbide porous network structure was obtained.

[0115] (2) The treated carbon-doped boron carbide porous network structure is laid flat in the mold;

[0116] (3) Dry the PET in an oven and add it to a single-screw extruder. The temperatures of each section of the single-screw extrusion are 180℃, 220℃, 250℃, 260℃ and 265℃. The PET is then cast into a mold with the treated boron carbide porous network structure. The PET coats the treated boron carbide porous network structure to obtain the final product. The volume ratio of the treated boron carbide porous network structure to the PET is 1:3.5.

[0117] Example 11

[0118] A method for preparing a double-sided high-temperature resistant release film includes the following steps:

[0119] (1) The carbon-doped boron carbide porous network structure was placed in the center of the lower electrode of the low-temperature plasma device for treatment. The low-temperature plasma treatment conditions were: positive corona discharge was used, the stainless steel mesh was connected to the negative terminal of the power supply, the hollow nozzle electrode was connected to the positive terminal of the power supply, and the DC high voltage power supply output power was 150W. The treated carbon-doped boron carbide porous network structure was obtained.

[0120] (2) The treated carbon-doped boron carbide porous network structure is laid flat in the mold;

[0121] (3) Dry the PET in an oven and add it to a single-screw extruder. The temperatures of each section of the single-screw extrusion are 180℃, 220℃, 250℃, 260℃ and 265℃. The PET is then cast into a mold with the treated boron carbide porous network structure. The PET coats the treated boron carbide porous network structure to obtain the final product. The volume ratio of the treated boron carbide porous network structure to the PET is 1:4.3.

[0122] Comparative Example 2

[0123] The difference between this embodiment and Embodiment 10 is that an equal amount of nano-boron carbide particles are directly added, specifically:

[0124] A method for preparing a double-sided high-temperature resistant release film includes the following steps:

[0125] (1) Mix boron carbide nanoparticles with PET substrate and granulate them by extrusion through a twin-screw extruder to obtain composite PET material; (2) Dry in an oven and add to a single-screw extruder. The temperatures of each section of the single-screw extrusion are 180℃, 220℃, 250℃, 260℃ and 265℃. The composite PET material is cast into a film.

[0126] Comparative Example 3

[0127] The difference between this embodiment and Example 10 is that the carbon-doped boron carbide porous network structure prepared in Comparative Example 1 is used.

[0128] Comparative Example 4

[0129] The difference between this embodiment and Embodiment 10 is that the carbon-doped boron carbide porous network structure is not treated with a low-temperature plasma device. Specifically:

[0130] A method for preparing a double-sided high-temperature resistant release film includes the following steps:

[0131] (1) Lay the carbon-doped boron carbide porous network structure flat in the mold;

[0132] (2) The PET was dried in an oven and then fed into a single-screw extruder. The extrusion temperatures of each section of the single screw were 180℃, 220℃, 250℃, 260℃, and 265℃. The PET was then cast into a mold with a boron carbide porous network structure. The PET coated the boron carbide porous network structure to obtain the final product. The volume ratio of the boron carbide porous network structure to the PET was 1:3.5. The glass transition temperature Tg (℃) and initial decomposition temperature Ts (℃) of the double-sided high-temperature release film were tested using a DSC thermal analyzer.

[0133] Test bending strength according to GB / T9341-2008.

[0134] The release force of the release film was tested according to ASTM D3330 / D3330M-04(2018), and the results are shown in Table 2:

[0135] Table 2 Performance Indicators of Double-Sided High-Temperature Resistant Release Film

[0136]

[0137] As shown in Table 1, the double-sided high-temperature resistant release film prepared by this invention exhibits high-temperature resistance, with an initial decomposition temperature (Ts) reaching 410.8℃. Simultaneously, its flexural strength reaches 66.1 MPa, demonstrating excellent toughness. As a release film, its release force is between 3.6-4.1 g / 2.5 mm, fully meeting the requirements for release films. Compared to Comparative Example 2, Example 10 shows significantly better heat resistance, flexural strength, and release effect. This is mainly because directly adding an equal amount of nano-boron carbide particles cannot achieve uniform mixing in the PET substrate. Furthermore, it cannot obtain the bending resistance of the structure in Example 10. The carbon-doped boron carbide porous network structure possesses multi-layered characteristics. This multi-layered structure allows the release film to release pressure during bending, improving its toughness. Comparative Example 3, lacking a polymethyl methacrylate solution, cannot form mesopores on the network structure fibers, thus failing to provide good bending resistance. In contrast, Comparative Example 4, which was not treated with a low-temperature plasma device, could not utilize the active free radicals generated on the surface to initiate the grafting polymerization of olefin monomers on the carbon material surface of the carbon-doped boron carbide. As a result, the adhesion between the porous network structure of the carbon-doped boron carbide and the PET substrate was relatively poor, leading to a decline in its various properties.

Claims

1. A double-sided high temperature resistant release film, characterized in that: A double-sided high-temperature resistant release film with a carbon-doped boron carbide porous network structure as a skeleton and coated with PET, wherein the carbon-doped boron carbide porous network structure itself has mesopores; The preparation method of the carbon-doped boron carbide porous network structure is: S1: dissolving polyacrylonitrile in N,N-dimethylformamide to obtain a polyacrylonitrile solution with a mass fraction of 9-10%; S2: dissolving polymethyl methacrylate in N,N-dimethylformamide to obtain a polymethyl methacrylate solution with a mass fraction of 9-10%; S3: mixing the polyacrylonitrile solution and the polymethyl methacrylate solution, adding the pretreated nano boron carbide particles, and stirring evenly to prepare the electrospinning solution; S4: performing electrospinning using an electrospinning device to obtain an electrospinning membrane; S5: placing the electrospun membrane in an oven, drying it at 80°C, and heating it to 200-300°C for pre-oxidation for 5-8h; S6: After being taken out, the solid is placed in a sintering furnace and sintered at a temperature of 900-1200° C. for 1-2 hours to obtain a carbon-doped boron carbide porous network as a skeleton structure; The preparation method of the double-sided high temperature resistant release film comprises the following steps: (1) placing the carbon-doped boron carbide porous network structure in the center of the lower electrode of a low-temperature plasma device for treatment to obtain a treated carbon-doped boron carbide porous network structure; (2) Laying the treated carbon-doped boron carbide porous network structure flat in a mold; (3) Drying PET in an oven, adding it into a single-screw extruder, and extruding the single-screw at different temperatures of 180°C, 220°C, 250°C, 260°C and 265°C. Casting PET into a mold covered with the treated carbon-doped boron carbide porous network structure, and coating the treated carbon-doped boron carbide porous network structure with PET.

2. A double-sided high temperature resistant release film according to claim 1, characterized in that: The carbon-doped boron carbide porous network structure has a pore size of 6-15 μm and a porosity of 30-43%.

3. A double-sided high temperature resistant release film according to claim 1, characterized in that: The mass ratio of polyacrylonitrile to polymethyl methacrylate is (7:3)-(2:1); the mass ratio of polyacrylonitrile to nano boron carbide particles is 2:(7-12).

4. A double-sided high temperature resistant release film according to claim 1, characterized in that: The pretreatment method of the nano boron carbide particles is: S31: placing the nano-boron carbide with a particle size of 100-500 nm in an oven for drying to obtain dry nano-boron carbide; S32: using a jet mill to perform secondary crushing on the dried nano boron carbide; S33: After collecting the nano-boron carbide, an ultrasonic instrument is used to perform ultrasonic treatment for 1-2 minutes to obtain pretreated nano-boron carbide particles.

5. The double-sided high temperature resistant release film according to claim 1, characterized in that: The electrospinning conditions are as follows: spinning speed is 2.0 mL / h, spinning voltage is 25 kV, the distance between the needle and the receiving plate is 15 cm, and the ambient temperature is 25-37°C.

6. A double-sided high temperature resistant release film according to claim 4, characterized in that: The classifying speed of the air jet mill is 2000 r / min.

7. The double-sided high temperature resistant release film according to claim 1, characterized in that: The low-temperature plasma treatment conditions are: positive corona discharge is adopted, the stainless steel mesh is connected to the negative electrode of the power supply, the hollow nozzle electrode is connected to the positive electrode of the power supply, and the output power of the DC high-voltage power supply is 150W.

8. The double-sided high temperature resistant release film according to claim 1, characterized in that: The volume ratio of the treated carbon-doped boron carbide porous network structure to PET is 1: (2.7-4.3).