A lithium manganese iron phosphate battery electrolyte and battery thereof

By using electrolyte with additive A with specific molecular orbital characteristics and non-aqueous organic solvents in lithium manganese phosphate batteries, the problem of insufficient circulation and rate performance of lithium manganese phosphate batteries is solved, and a high conductivity Li+ and stable battery is achieved Performance, inhibits the dissolution of manganese ions and improves the overall performance of the battery.

CN117691183BActive Publication Date: 2024-11-19FARASIS TECH (GANZHOU) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311512538.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-14
Publication Date
2024-11-19
Estimated Expiration
2043-11-14

AI Technical Summary

Technical Problem

Lithium manganese ferrophosphate batteries have shortcomings in terms of circulation and rate performance. The low ratio of manganese ions affects the energy density and voltage platform, and too high will lead to lattice distortion and manganese dissolution, affecting stability.

Method used

Using a lithium manganese iron phosphate battery electrolyte including additive A, non-aqueous organic solvent and lithium salt, additive A has a low minimum unoccupied molecular orbital and a high maximum occupied molecular orbital, which can decompose Li3N and LiBO2 on the electrode surface. , improve Li+ conductivity and magnification performance, and inhibit manganese ions dissolution through binding energy with HF, improving cycling performance.

Benefits of technology

It significantly improves the circulation performance and rate performance of lithium manganese iron phosphate batteries, inhibits manganese ion dissolution, extends the cycle stability of the battery and improves the high rate performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0004547858150000011
    Figure BDA0004547858150000011
  • Figure BDA0004547858150000031
    Figure BDA0004547858150000031
Patent Text Reader

Abstract

The present invention discloses a lithium iron manganese phosphate battery electrolyte and a battery thereof, belonging to the technical field of lithium ion batteries. The lithium iron manganese phosphate battery electrolyte comprises a non-aqueous organic solvent, a lithium salt and an additive, wherein the additive comprises an additive A. The lithium iron manganese phosphate battery electrolyte provided by the present invention can form a high-conductivity Li+ electrolyte at the electrode interface through the action of the additive A. + At the same time, it can also effectively remove HF to inhibit the dissolution of manganese ions, so that the lithium manganese iron phosphate battery has excellent rate performance and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium manganese iron phosphate battery electrolyte and a battery thereof. Background Art

[0002] Compared with NCM, lithium iron phosphate and lithium iron manganese phosphate, the olivine structure lattice stability of lithium iron manganese phosphate material is better than the ternary layered structure, and it has better cycle performance; due to the synergistic effect of Mn and Fe in lithium iron manganese phosphate material, Fe and Mn can be dissolved in any ratio to form a solid solution. Combined with the stable electrochemical properties of lithium iron phosphate and the high voltage advantage of lithium manganese phosphate, lithium iron manganese phosphate has higher energy density and higher safety than lithium iron phosphate, and the voltage platform voltage can reach 4.1V.

[0003] In terms of application, lithium manganese iron phosphate has lower electronic conductivity and lithium ion diffusion rate than lithium iron phosphate materials, which affects the rate performance, and the electrochemical properties of the materials are different due to the different proportions of manganese ions in the materials. For example, if the proportion of manganese ions is too low, it will affect the improvement of energy density and voltage platform, and it will not be able to achieve ideal material performance. However, if the proportion is too high, it will easily promote the Jan-Taylor effect, resulting in material lattice distortion and manganese dissolution, which will affect the cycle stability. Therefore, it is necessary to develop a lithium manganese iron phosphate battery electrolyte that can improve the battery cycle and rate performance. Summary of the invention

[0004] In view of the above shortcomings of the prior art, the present invention provides a lithium manganese iron phosphate battery electrolyte, and the lithium manganese iron phosphate battery prepared using the electrolyte has excellent cycle performance and rate performance. It is specifically achieved through the following technologies.

[0005] The present invention provides a lithium manganese iron phosphate battery electrolyte, comprising an additive A, wherein the additive A is shown in structural formula I:

[0006]

[0007]

[0008] Wherein R1, R2, R3, and R4 are independently selected from one of C1-C4 unsubstituted or fluorinated straight chain or branched alkyl, fluorine atom, hydrogen atom, olefin group, alkynyl group, and silane group; R5 and R6 are independently selected from one of C1-C6 unsubstituted or fluorinated straight chain or branched alkyl, olefin group, silane group, and alkynyl group.

[0009] The lithium manganese iron phosphate battery electrolyte of the present invention further comprises a non-aqueous organic solvent and a lithium salt.

[0010] The mass of the additive A is 0.2-5% of the total mass of the lithium iron manganese phosphate battery electrolyte. More preferably, the mass of the additive A is 0.5-2% of the total mass of the lithium iron manganese phosphate battery electrolyte.

[0011] The lithium manganese iron phosphate battery electrolyte also includes other additives, namely additive B.

[0012] Optionally, the additive B is at least one of 1,3-propylene sultone, vinylene sulfate, lithium difluorophosphate, fluoroethylene carbonate, and vinylene carbonate.

[0013] Optionally, the non-aqueous organic solvent is at least two of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethyl acetate, propyl acetate, and propyl propionate.

[0014] Optionally, the lithium salt is at least one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium methanesulfonate.

[0015] The mass of the lithium salt is 10-15% of the total mass of the lithium iron manganese phosphate battery electrolyte. Preferably, the mass of the lithium salt is 13.5% of the total mass of the lithium iron manganese phosphate battery electrolyte.

[0016] The present invention also provides a lithium manganese iron phosphate battery, comprising a positive electrode material, a negative electrode material, a separator and an electrolyte, wherein the electrolyte is the lithium manganese iron phosphate battery electrolyte described above.

[0017] The positive electrode material may be LiMn a Fe (1-a) PO4, wherein 0<a<1. Preferably, a=0.6.

[0018] The negative electrode material may be at least one of natural graphite, artificial graphite, silicon-oxygen or silicon-carbon. Preferably, the negative electrode material is artificial graphite.

[0019] Compared with the prior art, the present invention is beneficial in that:

[0020] Compared with the non-aqueous carbonate solvent, the additive A has a lower LUMO (lowest unoccupied molecular orbital) and a higher HOMO (highest occupied molecular orbital), and can be preferentially decomposed on the electrode surface to form Li3N and LiBO2, so that the manganese iron phosphate lithium battery of the present invention has high Li conductivity. + and high rate performance; at the same time, additive A and HF have strong binding energy, which can remove HF in the electrolyte of lithium manganese iron phosphate battery, inhibit the dissolution of manganese ions, and improve the cycle performance of lithium manganese iron phosphate battery. DETAILED DESCRIPTION

[0021] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0022] The present invention provides a lithium manganese iron phosphate battery electrolyte, comprising a non-aqueous organic solvent, a lithium salt and an additive, wherein the additive comprises an additive A, and the additive A is shown in structural formula I:

[0023]

[0024] Wherein R1, R2, R3, and R4 are independently selected from one of C1-C4 unsubstituted or fluorinated straight chain or branched alkyl, fluorine atom, hydrogen atom, olefin group, alkynyl group, and silane group; R5 and R6 are independently selected from one of C1-C6 unsubstituted or fluorinated straight chain or branched alkyl, olefin group, silane group, and alkynyl group.

[0025] The additives also include other additives, namely, additive B.

[0026] The mass of the additive A is 0.2-5% of the total mass of the lithium iron manganese phosphate battery electrolyte. Further preferably, the mass of the additive A is 0.5-2% of the total mass of the lithium iron manganese phosphate battery electrolyte.

[0027] The mass of the lithium salt is generally 10-15% of the total mass of the lithium iron manganese phosphate battery electrolyte. For the convenience of comparison, the mass of the lithium salt in the following specific embodiments is uniformly selected to be 13.5% of the total mass of the lithium iron manganese phosphate battery electrolyte.

[0028] The additive B, non-aqueous organic solvent and lithium salt are all commonly used components in electrolytes used in the field of lithium batteries.

[0029] In some examples, the additive B may be selected from but not limited to at least one of 1,3-propylene sultone, vinylene sulfate, lithium difluorophosphate, fluoroethylene carbonate, and vinylene carbonate.

[0030] In some examples, the non-aqueous organic solvent may be selected from but not limited to two or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.

[0031] In some examples, the lithium salt may be selected from but not limited to at least one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium methanesulfonate.

[0032] The lithium manganese iron phosphate battery prepared using the above electrolyte generally also includes a positive electrode material, a negative electrode material and a separator. The positive electrode material, the negative electrode material and the separator can all be made of materials commonly used in the art.

[0033] Some examples, the positive electrode material can be selected but not limited to LiMn a Fe (1-a) PO4, wherein 0<a<1, the positive electrode material used in the following specific embodiments and comparative examples is LiMn 0.6 Fe 0.4 PO4.

[0034] In some examples, the negative electrode material may be selected from but not limited to at least one of natural graphite, artificial graphite, silicon oxygen or silicon carbon.

[0035] As some examples, the membrane may be selected from but not limited to at least one of polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyimide, polyacrylonitrile, polyamide, polyester and natural fibers.

[0036] The technical solution of the present invention will be described clearly and completely below. For example, Examples 1 to 5 in Table 1 list the proportions of the electrolyte components. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative labor are within the scope of protection of the present invention.

[0037] Table 1 The proportion of electrolyte components used in Examples 1 to 5 and Comparative Examples 1 to 4

[0038] Group <![CDATA[LiPF6]]> Additive A PST VC FEC <![CDATA[LiPO2F2]]> Example 1 13.5% 0.5% 0.3% 1% 2% 0.8% Example 2 13.5% 1% 0.3% 1% 2% 0.8% Example 3 13.5% 2% 0.3% 1% 2% 0.8% Example 4 13.5% 0.2% 0.3% 1% 2% 0.8% Example 5 13.5% 5% 0.3% 1% 2% 0.8% Comparative Example 1 13.5% / 0.3% 1% 2% 0.8% Comparative Example 2 13.5% 0.5% TMSP 0.3% 1% 2% 0.8%

[0039] In the electrolytes of the above embodiments and comparative examples, except for the components listed in the table, the rest are organic solvents.

[0040] The organic solvents described above are at least two of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethyl acetate, propyl acetate, and propyl propionate. In this embodiment and the comparative example, the organic solvents selected are EC and EMC, and the mass ratio of EC:EMC is 3:7.

[0041] The mass ratio of solvent and mass fraction of lithium salt used in preparing the electrolytes of Examples 1 to 5 are substantially the same, and the only difference is the amount of additive A. The electrolyte of Comparative Example 1 does not contain additive A. The electrolyte of Comparative Example 2 replaces additive A with an equal amount of tris(trimethylsilyl)phosphate (TMSP).

[0042] The preparation method of the electrolyte of Examples 1 to 5 and Comparative Examples 1 to 4 comprises the following steps:

[0043] Operating in a helium atmosphere glove box, the organic solvents ethylene carbonate (EC) and ethyl methyl carbonate were first mixed evenly in a mass ratio of 3:7, and then additives were added, including additive A, 1,3-propylene sultone (PST), vinylene carbonate (VC), fluoroethylene carbonate (FEC) and lithium difluorophosphate (LiPO2F2), and finally lithium hexafluorophosphate (LiPF6) was added, stirred and mixed evenly to obtain a lithium iron manganese phosphate battery electrolyte.

[0044] Among them, when R1, R2, R3, and R4 in the additive A are independently selected from one of C1-C4 unsubstituted or fluorinated straight or branched alkyl, fluorine atom, hydrogen atom, olefin group, alkyne group, and silane group; and R5 and R6 are independently selected from one of C1-C6 unsubstituted or fluorinated straight or branched alkyl, olefin group, silane group, and alkyne group, the effect is very good. Therefore, for the convenience of explanation, the additive A used in the embodiment of Table 1 above is preferably as shown in structural formula II:

[0045]

[0046] Preparation of lithium manganese iron phosphate battery:

[0047] Preparation of positive electrode sheet: LiMn 0.6 Fe 0.4 PO4, conductive agent SP, and binder PVDF are added to NMP solvent in a mass ratio of 97.2:1.6:1.2, and after being fully stirred and mixed, a positive electrode slurry is obtained. The positive electrode slurry is coated on the positive electrode current collector aluminum foil, and then after baking, rolling, and punching, a positive electrode sheet of a lithium manganese iron phosphate battery is obtained, wherein the thickness of the aluminum foil is 12 μm, and the thickness of the active material layer on the positive electrode sheet is 110 μm;

[0048] Preparation of negative electrode sheet: Add artificial graphite, conductive agent SP, thickener CMC and dispersing agent SBR as negative electrode material active material into deionized water in a mass ratio of 94.95:1.05:1:3, stir well to obtain negative electrode slurry, apply the negative electrode slurry on the negative electrode current collector copper foil, and then obtain the negative electrode sheet of lithium battery after baking, rolling and punching, wherein the thickness of the copper foil is 8 μm, and the thickness of the active material layer on the negative electrode sheet is 100 μm;

[0049] The separator is polypropylene, a porous polymer film with a thickness of 20 μm;

[0050] The positive electrode sheet, the separator, and the negative electrode sheet are stacked into a roll core in the order of the positive electrode sheet, the separator serves as an isolation between the positive and negative electrode sheets, and then the tabs are welded and packaged to obtain a soft-packaged dry cell. Four soft-packaged dry cells are prepared in the same manner, and the four soft-packaged dry cells are respectively injected into the electrolytes prepared in Examples 1 to 3 and Comparative Example 1, and then after activation, formation, and aging processes, a lithium manganese iron phosphate battery prepared by the electrolytes of Examples 1 to 3 and Comparative Example 1 is obtained.

[0051] Battery performance test:

[0052] The lithium manganese iron phosphate batteries prepared with the electrolytes of Examples 1 to 5 and Comparative Examples 1 to 4 were subjected to the following verification tests:

[0053] (1) Cycle performance:

[0054] Under the test thermostat at 25℃ or 45℃, the test steps are as follows:

[0055] S1, 1C constant current charge to 4.2V, then constant voltage charge to cut-off current 0.05C, let stand for 30 minutes;

[0056] S2, 1C constant current discharge to 2.5V, stand for 30 minutes;

[0057] S3, loop steps S1 and S2 for 500 cycles.

[0058] The cycle test results are shown in Table 2.

[0059] Table 2 Cyclic test results

[0060]

[0061] From the cycle test results in Table 2, under the conditions of 25°C or 45°C, the capacity retention rates of Examples 4 to 5 are inferior to those of Examples 1 to 3, and the DCR growth rates of Examples 1 to 3 are relatively lower, which indicates that the amount of additive A added is insufficient or excessive, and the improvement effect is poor; compared with Example 1, the battery capacity retention rate of Comparative Example 1 without using additive A is significantly reduced under the conditions of 25°C or 45°C, and the cycle DCR growth rate is significantly increased, which indicates that additive A can inhibit the growth of cycle DCR and improve the cycle performance. Compared with Comparative Example 1, the capacity retention rates of Comparative Examples 3 and 4 decrease, and the cycle DCR growth rate increases, and the battery capacity retention rate of Comparative Example 2 increases, and the cycle DCR growth rate decreases; but compared with Example 1, the battery capacity retention rate of Comparative Example 2 still decreases significantly, and the cycle DCR growth rate still increases significantly, because although TMSP can also improve the cycle and inhibit the growth of DCR, its improvement effect is weaker than that of additive A.

[0062] (2) Ratio test:

[0063] Under the test thermostat at 25°C, the test steps are as follows:

[0064] S1, 0.33C constant current and constant voltage charge to 4.2V, cut-off current 0.05C, stand for 60 minutes;

[0065] S2. Discharge at different rates (0.33C, 1C, 2C, 3C) to 2.5V and let stand for 60 minutes.

[0066] The capacity retention rate results of the rate test are shown in Table 3.

[0067] Table 3 Capacity retention results of rate test

[0068] Group 0.33C 0.5C 1C 2C Example 1 100% 98.36% 93.15% 85.12% Example 2 100% 98.64% 93.98% 85.79% Example 3 100% 98.56% 93.56% 85.09% Example 4 100% 98.29% 92.12% 84.23% Example 5 100% 98.32% 91.12% 83.56% Comparative Example 1 100% 98.13% 89.26% 81.98% Comparative Example 2 100% 98.45% 90.98% 83.12%

[0069] From the rate test results in Table 3, the rate discharge capacity retention rates of Comparative Example 1 and Comparative Example 2 are basically the same, indicating that the additive TMSP does not improve the rate performance.

[0070] At a low rate of 0.5C, the capacity retention rates of Examples 1 to 5 and Comparative Examples 1 to 4 at rate discharge are not much different and are basically consistent; however, at 1C and 2C rate discharge, Examples 1 to 3 are better than Examples 4 to 5. The possible reason is that the amount of additive A added is too small, forming a high-conductivity Li + The interface film has few components, which is not conducive to Li + Migration, if the addition amount is too high, the interface impedance will be high, which is not conducive to Li + Migration; Compared with Comparative Example 1, Comparative Example 3 and Comparative Example 4, the capacity retention rate at 0.5C is not much different, and the capacity retention rate at 1C and 2C rate discharge is relatively better in Comparative Example 1; Compared with Comparative Examples 1-2, the batteries of Examples 1-5 still have significantly higher capacity retention rates, indicating that the addition of additive A can make the lithium manganese iron phosphate battery have better rate discharge performance. After analysis, the possible reason why additive A improves the cycle performance and rate of lithium manganese iron phosphate batteries is that additive A can preferentially participate in the interface film formation by oxidation and reduction, forming a stable high-conductivity Li + SEI or CEI film.

[0071] The above specific embodiments describe the implementation of the present invention in detail, but the present invention is not limited to the specific details in the above embodiments. Within the scope of the claims and technical concept of the present invention, the technical solution of the present invention can be modified and changed in many simple ways, and these simple modifications all belong to the protection scope of the present invention.

Claims

1. A lithium manganese iron phosphate battery, characterized in that: It includes a lithium iron manganese phosphate battery electrolyte, wherein the lithium iron manganese phosphate battery electrolyte includes an additive A, and the additive A is shown in the following structural formula I: Structural Formula I Wherein R1, R2, R3, and R4 are independently selected from one of C1-C4 unsubstituted or fluorinated straight chain or branched alkyl, fluorine atom, hydrogen atom, olefin group, alkynyl group, and silane group; R5 and R6 are independently selected from one of C1-C6 unsubstituted or fluorinated straight chain or branched alkyl, olefin group, silane group, and alkynyl group.

2. The lithium manganese iron phosphate battery according to claim 1, characterized in that: The mass of the additive A is 0.2-5% of the total mass of the lithium manganese iron phosphate battery electrolyte.

3. The lithium manganese iron phosphate battery according to claim 2, characterized in that: The mass of the additive A is 0.5-2% of the total mass of the lithium manganese iron phosphate battery electrolyte.

4. The lithium manganese iron phosphate battery according to claim 1, characterized in that: The invention also includes an additive B, wherein the additive B is at least one of 1,3-propylene sultone, vinylene sulfate, lithium difluorophosphate, fluoroethylene carbonate, and vinylene carbonate.

5. The lithium manganese iron phosphate battery according to claim 1, characterized in that: The invention also comprises an organic solvent, wherein the organic solvent is at least two of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethyl acetate, propyl acetate and propyl propionate.

6. The lithium manganese iron phosphate battery according to claim 1, characterized in that: The invention also includes a lithium salt, wherein the lithium salt is at least one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide and lithium methanesulfonate.

7. The lithium manganese iron phosphate battery according to claim 6, characterized in that: The mass of the lithium salt is 10-15% of the total mass of the lithium manganese iron phosphate battery electrolyte.

8. The lithium manganese iron phosphate battery according to any one of claims 1 to 7, characterized in that: Also includes a positive electrode material, the positive electrode material is LiMn a Fe (1-a) PO4, where 0<a<1.