A Tm 3+ and Dy 3+ Co-doped Y2MgTiO6 phosphor and preparation method thereof
Through the preparation of Tm3+ and Dy3+ co-doped Y2MgTiO6 phosphor, the problem of excessive white fluorescent pink in existing white LEDs is solved, and the effect of color coordinates close to white light, low color temperature and high color purity is achieved, becoming an ideal material for white LEDs.
Patent Information
- Application Number
- CN202410417860.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-04-09
AI Technical Summary
The white fluorescent pink used in existing white LEDs is too high to achieve the 'white and bright' effect, and the color purity is not enough to meet the standard requirements.
Tm3+ and Dy3+ are used to co-dop Y2MgTiO6 phosphors, and through specific chemical composition and preparation methods, phosphors with excellent coordinates close to white light, color temperature and color purity are prepared. The specific steps include selecting appropriate Tm2O3, Dy2O3, Y2O3, MgO and TiO2 By proportion, grinding and sintering treatment, the chemical formula of the obtained phosphor is Y2MgTiO6: xTm3+, yDy3+, where 0
The color coordinates of the phosphor are close to standard white light, with low color temperature and color purity close to sunlight color temperature 5500K, avoiding the defect of excessive color temperature of commercial white LEDs and meeting the color purity requirements of white LEDs.
Smart Images

Figure CN118256242B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fluorescent powder, and in particular to a Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor and preparation method thereof. Background Art
[0002] Light Emitting Diode (LED) is a light-emitting device. It not only has the advantages of low power consumption, long life, low operating voltage, environmental protection, safety, fast response, high reliability, low maintenance, small size, light weight, etc., but also can emit blue light, green light, purple light or deep ultraviolet light, making LED produce white light a reality, which is the high-tech direction of my country's development. The color coordinates of white light (also known as CIE coordinates) are (0.3300, 0.3300), the daylight color temperature (CCT) is 5500K, and the color purity of white light is 0%. However, the white phosphors used in white light LEDs are not close enough to standard white light. The color temperature of these white phosphors is too high and cannot achieve the "white and bright" effect, thus failing to meet the requirements of white light LEDs. For example, LiMgBO 3 :0.03Tm 3+ ,0.05Dy 3+ The CIE coordinates of the phosphor are (0.334, 0.306). Gd2(MoO4) 3 :12%Dy 3+ ,12%Tm 3+ The CIE coordinates of the phosphor are (0.3388, 0.3293). 4 :5%Pr 3+ The color coordinates of the phosphor under ultraviolet excitation at 242nm are (0.3100, 0.3458), the color temperature (CCT) is as high as 6526K, and the color purity is even close to 10%.
[0003] Therefore, in view of the shortcomings of the prior art, a Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphors and methods for preparing the same are necessary to address the deficiencies of the prior art. Summary of the invention
[0004] The first object of the present invention is to avoid the shortcomings of the prior art and provide a Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor. The Tm 3+ and Dy3+ Co-doped Y 2 MgTiO 6 The color coordinates of phosphor are close to white light, and its color temperature and color purity are relatively low.
[0005] The above-mentioned purpose of the present invention is achieved by the following technical measures:
[0006] Provide a Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The chemical formula of phosphor is Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , where 0<x≤0.5, 0<y≤0.5.
[0007] 0.02<x≤0.1, 0.05≤y≤0.2.
[0008] x is 0.05 and y is 0.1.
[0009] Tm of the present invention 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor, color coordinates are (0.3316, 0.3261); correlated color temperature is 5538K; color purity is 2.74%.
[0010] Tm of the present invention 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor, Tm 3+ By Tm 2 O 3 Provided by Dy 3+ By Dy 2 O 3 Provide, Y 3+ By Y 2 O 3 Provided, Mg 2+ Provided by MgO, Ti 4+ TiO 2 supply.
[0011] The second object of the present invention is to avoid the shortcomings of the prior art and provide a Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Preparation method of phosphor. 3+ and Dy 3+ Co-doped Y 2MgTiO 6 The preparation method of phosphor powder prepared by Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The color coordinates of phosphor are close to white light, and its color temperature and color purity are relatively low.
[0012] The above-mentioned purpose of the present invention is achieved by the following technical measures:
[0013] Provide a Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The preparation method of the phosphor is obtained by the following steps:
[0014] S1. Weigh Tm according to the stoichiometric ratio 2 O 3 、Dy 2 O 3 , Y 2 O 3 , MgO and TiO 2 to a container;
[0015] S2, grinding to obtain a precursor;
[0016] S3, sintering the precursor to obtain a sintered product;
[0017] S4, cooling the sintered product, and then grinding it to obtain the Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor.
[0018] Preferably, the above S3 specifically comprises heating the precursor to 1200° C. to 1350° C. and then maintaining the temperature for 8 h to 10 h to obtain a sintered product.
[0019] Preferably, the above S4 is specifically to cool the sintered product to 750°C to 850°C, and then naturally cool it to room temperature and grind it into powder to obtain the Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor.
[0020] Preferably, the above S3 specifically comprises heating the precursor to 1300° C. at a heating rate of 5° C. / min and then maintaining the temperature for 9 hours to obtain a sintered product.
[0021] Preferably, the above S4 is specifically to cool the sintered product to 800°C at a cooling rate of 2.5°C / min, and then naturally cool it to room temperature and grind it into powder to obtain the Tm3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor.
[0022] The present invention provides a Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor and its preparation method and application, wherein Tm 3+ and Dy 3 + Co-doped Y 2 MgTiO 6 Chemical formula of phosphor Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , where 0<x≤0.5, 0<y≤0.5. The color coordinates of the phosphor are very close to the standard white light, and it can be an ideal candidate material for white light LED. Compared with the white phosphor in the prior art, the Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The color coordinates of the phosphor are close to white light, and the color temperature and color purity are both low, avoiding the defect of commercial white light having too high color temperature, and the color purity of the phosphor is close to the color purity of standard white light. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention is further described with reference to the accompanying drawings, but the contents in the accompanying drawings do not constitute any limitation to the present invention.
[0024] Figure 1 Tm 3+ Single doped Y 2 MgTiO 6 PLE spectrum and PL spectrum of phosphor.
[0025] Figure 2 Tm 3+ Single doped Y 2 MgTiO 6 CIE coordinate diagram of phosphor.
[0026] Figure 3 For Dy 3+ Single doped Y 2 MgTiO 6 PLE spectrum of phosphor.
[0027] Figure 4 For Dy 3+ Single doped Y 2 MgTiO 6PL spectrum of phosphor.
[0028] Figure 5 For Dy 3+ Single doped Y 2 MgTiO 6 CIE coordinate diagram of phosphor.
[0029] Figure 6 Tm 3+ Single doped Y 2 MgTiO 6 Phosphor and Dy 3+ Single doped Y 2 MgTiO 6 PLE spectrum of phosphor.
[0030] Figure 7 is the Tm of the present invention 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor in λ ex =PL spectrum at 360nm.
[0031] Figure 8 is the Tm of the present invention 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor in λ ex =PL spectrum at 353 nm.
[0032] Fig. 9 is the Tm of the present invention 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 CIE coordinate diagram of phosphor.
[0033] Fig.10 is the Tm of the present invention 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor decay curve. DETAILED DESCRIPTION
[0034] The technical solution of the present invention is further described in conjunction with the following examples. Unless otherwise specified, the raw materials used in the following examples are all commercially available products. 2 O 3 ,MgO,TiO 2 、Tm 2 O 3 、Dy 2 O 3All were purchased from Shanghai Aladdin Co., Ltd.
[0035] Example 1
[0036] A Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Chemical formula of phosphor Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , where 0<x≤0.5, 0<y≤0.5. Where Tm 3+ By Tm 2 O 3 Provided by Dy 3+ By Dy 2 O 3 Provide, Y 3+ By Y 2 O 3 Provided, Mg 2+ Provided by MgO, Ti 4+ TiO 2 supply.
[0037] Among them, Y 2 O 3 ,MgO,TiO 2 、Tm 2 O 3 and Dy 2 O 3 The purity is greater than 99.99%.
[0038] Tm of the present invention 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The phosphor is obtained by the following steps:
[0039] S1. Weigh Tm according to the stoichiometric ratio 2 O 3 、Dy 2 O 3 , Y 2 O 3 , MgO and TiO 2 to a container;
[0040] S2, grinding to obtain a precursor;
[0041] S3, heating the precursor to 1300°C at a heating rate of 5°C / min and maintaining the temperature for 9 hours to obtain a sintered product;
[0042] S4, cooling the sintered product to 800°C at a cooling rate of 2.5°C / min, then naturally cooling it to room temperature and grinding it into powder to obtain the Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor.
[0043] Example 2
[0044] A Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Chemical formula of phosphor Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Example 1, wherein x is 0.05 and Y is 0.01. Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Preparation process of phosphor:
[0045] Tm of the present invention 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The phosphor is obtained by the following steps:
[0046] S1. Weigh Tm according to the stoichiometric ratio 2 O 3 、Dy 2 O 3 , Y 2 O 3 , MgO and TiO 2 to the agate mortar;
[0047] S2, grinding the above raw materials in an agate mortar for 30 minutes to obtain a precursor;
[0048] S3, heating the precursor to 1300°C at a heating rate of 5°C / min and maintaining the temperature for 9 hours to obtain a sintered product;
[0049] S4, cooling the sintered product to 800°C at a cooling rate of 2.5°C / min, then naturally cooling it to room temperature and grinding it into powder to obtain the Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor.
[0050] Example 3
[0051] A Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Chemical formula of phosphor Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those in Example 2, wherein x is 0.05 and Y is 0.02.
[0052] Example 4
[0053] A Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The chemical formula of phosphor is Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those in Example 2, wherein x is 0.05 and Y is 0.05.
[0054] Example 5
[0055] A Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The chemical formula of phosphor is Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those in Example 2, wherein x is 0.05 and Y is 0.10.
[0056] Example 6
[0057] A Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The chemical formula of phosphor is Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those in Example 2, wherein x is 0.05 and Y is 0.20.
[0058] Example 7
[0059] A Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The chemical formula of phosphor is Y 2 MgTiO6 :xTm 3+ ,yDy 3+ , other features are the same as those in Example 2, wherein x is 0.05 and Y is 0.50.
[0060] Example 8
[0061] A Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The chemical formula of phosphor is Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those in Example 2, where x is 0.10 and Y is 0.10.
[0062] Tm of this example 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The phosphor is obtained by the following steps:
[0063] S1. Weigh Tm according to the stoichiometric ratio 2 O 3 、Dy 2 O 3 , Y 2 O 3 , MgO and TiO 2 to the agate mortar;
[0064] S2, grinding the above raw materials in an agate mortar for 30 minutes to obtain a precursor;
[0065] S3, heating the precursor to 1200°C at a heating rate of 5°C / min and maintaining the temperature for 10 hours to obtain a sintered product;
[0066] S4, the sintered product is cooled to 750°C at a cooling rate of 2.5°C / min, and then naturally cooled to room temperature and ground into powder to obtain the Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor.
[0067] Example 9
[0068] A Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The chemical formula of phosphor is Y 2 MgTiO 6 :xTm3+ ,yDy 3+ , other features are the same as those in Example 2, wherein x is 0.02 and Y is 0.10.
[0069] Tm of this example 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The phosphor is obtained by the following steps:
[0070] S1. Weigh Tm according to the stoichiometric ratio 2 O 3 、Dy 2 O 3 , Y 2 O 3 , MgO and TiO 2 to the agate mortar;
[0071] S2, grinding the above raw materials in an agate mortar for 30 minutes to obtain a precursor;
[0072] S3, heating the precursor to 1350°C at a heating rate of 5°C / min and maintaining the temperature for 8 hours to obtain a sintered product;
[0073] S4, the sintered product is cooled to 850°C at a cooling rate of 2.5°C / min, and then naturally cooled to room temperature and ground into powder to obtain the Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor.
[0074] Example 10
[0075] A Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The chemical formula of phosphor is Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Example 8, wherein x is 0.10 and Y is 0.10.
[0076] Embodiment 11
[0077] A Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The chemical formula of phosphor is Y 2 MgTiO 6 :xTm 3+ ,yDy3+ , other features are the same as those of Example 8, wherein x is 0.20 and Y is 0.10.
[0078] Example 12
[0079] A Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The chemical formula of phosphor is Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Example 9, wherein x is 0.50 and Y is 0.10.
[0080] Comparative Example 1
[0081] A Tm 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Example 2, except that: x is 0.005, y is 0. Where Tm 3+ By Tm 2 O 3 Provided by Y 2 O 3 Provided by, Mg is provided by MgO, Ti is provided by TiO 2 supply.
[0082] The following steps are obtained:
[0083] S1. Weigh Tm according to the stoichiometric ratio 2 O 3 , Y 2 O 3 , MgO and TiO 2 to a container;
[0084] S2, grinding to obtain a precursor;
[0085] S3, heating the precursor to 1300°C at a heating rate of 5°C / min and maintaining the temperature for 9 hours to obtain a sintered product;
[0086] S4, cooling the sintered product to 800° C. at a cooling rate of 2.5° C. / min, and then naturally cooling it to room temperature and grinding it into powder to obtain the phosphor of Comparative Example 1.
[0087] Comparative Example 2
[0088] A Tm 3+ Single doped phosphor, its chemical formula can be expressed as Y2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Comparative Example 1, except that: x is 0.01 and y is 0.
[0089] Comparative Example 3
[0090] A Tm 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Comparative Example 1, except that: x is 0.02 and y is 0.
[0091] Comparative Example 4
[0092] A Tm 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Comparative Example 1, except that: x is 0.05 and y is 0.
[0093] Comparative Example 5
[0094] A Tm 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Comparative Example 1, except that: x is 0.1 and y is 0.
[0095] Comparative Example 6
[0096] A Tm 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Comparative Example 1, except that: x is 0.2 and y is 0.
[0097] Comparative Example 7
[0098] A Tm 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+ ,yDy 3+, other features are the same as those of Comparative Example 1, except that: x is 0.5 and y is 0.
[0099] Comparative Example 8
[0100] A kind of Dy 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Example 2, except that: x is 0, y is 0.005. 3+ By Dy 2 O 3 Provided by Y 2 O 3 Provided by, Mg is provided by MgO, Ti is provided by TiO 2 supply.
[0101] The following steps are obtained:
[0102] S1. Weigh Dy according to the stoichiometric ratio 2 O 3 , Y 2 O 3 , MgO and TiO 2 to a container;
[0103] S2, grinding to obtain a precursor;
[0104] S3, heating the precursor to 1300°C at a heating rate of 5°C / min and maintaining the temperature for 9 hours to obtain a sintered product;
[0105] S4. Cooling the sintered product to 800° C. at a cooling rate of 2.5° C. / min, and then naturally cooling it to room temperature and grinding it into powder to obtain the phosphor of Comparative Example 8.
[0106] Comparative Example 9
[0107] A kind of Dy 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Comparative Example 8, except that: x is 0 and y is 0.01.
[0108] Comparative Example 10
[0109] A kind of Dy 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+,yDy 3+ , other features are the same as those of Comparative Example 8, except that: x is 0 and y is 0.02.
[0110] Comparative Example 11
[0111] A kind of Dy 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Comparative Example 8, except that: x is 0 and y is 0.05.
[0112] Comparative Example 12
[0113] A kind of Dy 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Comparative Example 8, except that: x is 0 and y is 0.1.
[0114] Comparative Example 13
[0115] A kind of Dy 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Comparative Example 8, except that: x is 0 and y is 0.2.
[0116] Comparative Example 13
[0117] A kind of Dy 3+ Single doped phosphor, its chemical formula can be expressed as Y 2 MgTiO 6 :xTm 3+ ,yDy 3+ , other features are the same as those of Comparative Example 8, except that: x is 0 and y is 0.5.
[0118] Effect example
[0119] 1. Luminescence characteristics of single-doped phosphors
[0120] 1.1、Tm 3+ Single doped phosphor PLE spectrum and PL spectrum test
[0121] The Tm of Comparative Examples 1 to 7 3+ Single doped phosphors were tested for PLE spectrum and spectrum, and the results were Figure 1 .
[0122] from Figure 1 It can be seen that Tm 3+ Single doped phosphor at 458nm ( 1 D 2 → 3 F 4 ) and determined the Tm 3+ The optimal doping concentration is x = 0.05. And Tm 3+ The CIE coordinates of single-doped phosphors are all in the blue region, such as Figure 2 shown.
[0123] 1.2、Dy 3+ PLE spectrum and PL spectrum test of single doped phosphor
[0124] The Dy of Comparative Examples 8 to 13 was 3+ The single-doped phosphor was tested for PLE spectrum and PL spectrum, and the results were Figure 3 and Figure 4 , and get Tm 3+ The color coordinates of single-doped phosphors, such as Figure 5 .
[0125] from Figure 3-Figure 5 It can be seen that Dy 3+ Single doped phosphor at 484nm ( 4 F 9 / 2 → 6 H 15 / 2 ) and 579nm( 4 F 9 / 2 → 6 H 13 / 2 ) emit cyan and yellow light respectively, among which Dy 3+ The optimal doping concentration is y=0.2.
[0126] To evaluate Tm 3+ and Dy 3+ The possibility of energy transfer during co-doping is based on the Forster–Dexter theory, which takes the overlap of their excitation and emission spectra as an important criterion. 3+ PL spectra of single-doped phosphors and Dy 3+ The PLE spectra of single-doped phosphors are put into the same figure for comparison, such as Figure 6 As shown. Figure 6 As can be seen, Y 2 MgTiO 6 :0.05Tm 3+ The emission spectrum of Y 2 MgTiO 6 :0.2Dy3+ There is a lot of overlap in the excitation spectra of the two species, and the overlapping region is 449nm to 470nm, which almost includes Tm 3+ This is the entire emission band of Tm when the two ions are co-doped in the host lattice. 3+ To Dy 3+ The energy transfer of Dy provides conditions. 3+ Single-doped phosphors lack blue emission, so Dy 3+ The color coordinates of the single-doped phosphor cannot reach the standard white light area, and the overall trend is to move from the blue-purple area across the standard white light area to the yellow light area.
[0127] 2. Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Luminescence properties of phosphors
[0128] The Dy prepared in Comparative Example 4 3+ Single doping Y 2 MgTiO 6 The phosphor and the Tm prepared in Examples 2 to 7 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphor in λ ex =360nm and λ ex = 353nm, and the PL spectrum was tested. Figure 7 and Figure 8 , and get Tm 3+ The color coordinates of single-doped phosphors, such as Fig. 9 .
[0129] pass Figure 7-Figure 9 It can be seen that the present invention has been 3+ The doping concentration was optimized and the Y 2 MgTiO 6 :0.05Tm 3+ ,yDy 3+ Series of phosphors, under 360nm excitation, Tm 3+ The emission peak plays a leading role, and the emission color moves from the blue region to the blue-violet region; under 353nm excitation, Dy 3+ The emission peak plays a leading role. The emission color moves from the blue-violet region to the white light region through the CIE coordinate diagram.
[0130] Therefore, the Tm of the present invention 3+ and Dy 3+ Co-doped Y 2 MgTiO 6The color coordinates, color temperature and color purity of the phosphors prove that the color coordinates of the prepared phosphors are very close to the standard white light, the correlated color temperature is low, and it is more in line with the requirements of the color purity value of white light. 2 MgTiO 6 :0.05Tm 3+ ,0.1Dy 3+ The color coordinates of the phosphor are (0.3316, 0.3261), the correlated color temperature is 5538K, and the color purity is 2.74%. Fig. 9 It avoids the defect of too high color temperature of commercial WLED and is closer to daylight (5500K), meeting the requirements of white light for color purity. 2 MgTiO 6 :0.05Tm 3+ ,0.1Dy 3+ Phosphors can be ideal candidate materials for white light LEDs.
[0131] 3. Fluorescence lifetime test
[0132] The Dy prepared in Comparative Example 4 3+ Single doping Y 2 MgTiO 6 Phosphor, and Tm prepared in Example 2, Example 4 and Example 5 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The fluorescence lifetime curve and energy level transition test of the phosphor were carried out to obtain Fig. 9 .
[0133] from Fig.10 It has been proved that in Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Tm exists in phosphor 3+ →Dy 3+ The maximum energy transfer efficiency was 92.55%, which proved that Tm 3+ To Dy 3+ The energy transfer mechanism of the present invention is dipole-dipole interaction. 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 Phosphors can be ideal candidate materials for white light LEDs.
[0134] It should also be noted that according to Figure 6 Y 2 MgTiO 6 :0.05Tm3+ The emission spectrum of Y 2 MgTiO 6 :0.2Dy 3+ The overlap of the excitation spectra of the two ions in the host lattice proves that the Tm 3+ To Dy3+ provides the conditions for energy transfer. Figure 7 and Figure 8 As shown, Y 2 MgTiO 6 :0.05Tm 3+ ,yDy 3+ PL spectra at different excitation wavelengths. 3+ The increase in content, Tm 3+ The blue light emission intensity at 458 nm gradually weakens, while the Dy 3+ Feature Transition 4 F 9 / 2 → 6 H J / 2 The cyan (484 nm) and yellow (579 nm) emission intensities caused by (J=15,13) gradually increased and reached a maximum at x=0.2, and then gradually weakened due to concentration quenching. 3+ and Dy 3+ The emission intensity of the co-activated phosphor increases with the 3+ The variation trend of doping concentration is as follows Figure 8 As shown in the illustration. 3+ To Dy 3+ There is concrete evidence of energy transfer between them. Fig.10 The fluorescence lifetime curves of YMT:0.05Tm3+,yDy3+(y=0,0.01,0.05,0.10) samples were tested under 360nm excitation and 458nm monitoring. All decay curves were consistent with the three-exponential decay relationship. It was noted that with the increase of Dy3+ ion doping concentration, Tm 3+ The average lifetime decreases monotonically from 52.64 ns to 3.92 ns. These results clearly confirm that Y 2 MgTiO 6 :0.05Tm 3+ ,yDy 3+ Tm exists in phosphor 3+ →Dy 3+ Therefore, the energy transfer determination of the present invention is: 1. Tm 3+ Emission spectra of single-doped phosphors and Dy 3+ The excitation spectra of single-doped phosphors overlap; 2. 3+ and Dy 3+ Co-doped Y 2 MgTiO6 In phosphor, when 0.05Tm 3+ ,yDy 3+ When Dy 3+ With the increase of concentration, Tm 3+ The intensity gradually decreases; 3. Tm 3+ The fluorescence lifetime decreases gradually.
[0135] In summary, the color coordinates of the phosphor are very close to the standard white light, and it can be an ideal candidate material for white light LED. Compared with the white phosphor in the prior art, the Tm 3+ and Dy 3+ Co-doped Y 2 MgTiO 6 The color temperature of the phosphor is lower and close to the color temperature of daylight, avoiding the defect of too high color temperature of commercial white light. The color purity of the phosphor is close to the color purity of standard white light.
[0136] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A Tm 3+ and Dy 3+ Co-doped Y2MgTiO6 phosphor, characterized by: The chemical formula is Y2MgTiO6:xTm 3+ ,yDy 3+ , where 0<x≤0.5, 0<y≤0.
5.
2. Tm according to claim 1 3+ and Dy 3+ Co-doped Y2MgTiO6 phosphor, characterized by: 0.02<x≤0.1, 0.05≤y≤0.
2.
3. Tm according to claim 1 3+ and Dy 3+ Co-doped Y2MgTiO6 phosphor, characterized by: x is 0.05 and y is 0.
1.
4. Tm according to claim 1 3+ and Dy 3+ Co-doped Y2MgTiO6 phosphor, characterized by: The color coordinates are (0.3316, 0.3261); The correlated color temperature is 5538K; The color purity is 2.74%.
5. The Tm according to any one of claims 1 to 4 3+ and Dy 3+ Co-doped Y2MgTiO6 phosphor, characterized by: Tm 3+ Provided by Tm2O3, Dy 3+ Provided by Dy2O3, Y 3+ Provided by Y2O3, Mg 2+ Provided by MgO, Ti 4+ Provided by TiO2.
6. A Tm according to claim 5 3+ and Dy 3+ The method for preparing co-doped Y2MgTiO6 phosphor is characterized in that: Obtained by the following steps: S1. Weigh Tm2O3, Dy2O3, Y2O3, MgO and TiO2 into a container according to the stoichiometric ratio; S2, grinding to obtain a precursor; S3, sintering the precursor to obtain a sintered product; S4, cooling the sintered product, and then grinding it to obtain the Tm 3+ and Dy 3+ Co-doped Y2MgTiO6 phosphor.
7. The preparation method according to claim 6, characterized in that: The S3 is specifically to heat the precursor to 1200° C. to 1350° C. and then maintain the temperature for 8 h to 10 h to obtain a sintered product.
8. The preparation method according to claim 6, characterized in that: The S4 is specifically to cool the sintered product to 750°C to 850°C, and then naturally cool it to room temperature and grind it into powder to obtain the Tm 3+ and Dy 3+ Co-doped Y2MgTiO6 phosphor.
9. The preparation method according to claim 7, characterized in that: The S3 is specifically to heat the precursor to 1300° C. at a heating rate of 5° C. / min and then maintain the temperature for 9 hours to obtain a sintered product.
10. The preparation method according to claim 8, characterized in that: Specifically, the S4 comprises cooling the sintered product to 800°C at a cooling rate of 2.5°C / min, and then naturally cooling the sintered product to room temperature and grinding the sintered product into powder to obtain the Tm 3+ and Dy 3+ Co-doped Y2MgTiO6 phosphor.
Citation Information
Patent Citations
Europium dysprosium co-doped tungstate red fluorescent powder for white light LED and preparation method of europium dysprosium co-doped tungstate red fluorescent powder
CN113462391A
Eu2+ doped tantalate red phosphor and preparation method therefor
WO2023104217A1