Polyvinyl chloride microspheres with rich pore structure and preparation method thereof
A one-step polymerization method using a double emulsion template stabilizes oil-in-water-in-oil droplets to create polyvinyl chloride microspheres with rich pore structures, addressing complexity and environmental issues in existing methods, enabling high surface area and plasticizer diffusion for industrial uses.
Patent Information
- Application Number
- CN202411170608.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Existing methods for preparing polyvinyl chloride microspheres with precise pore structures are complicated due to the need for harsh removal of hard templates and lack efficient, environmentally friendly processes for creating interconnected pores.
A one-step polymerization method using a double emulsion template with a stabilizer and emulsifier to stabilize oil-in-water-in-oil droplets, forming polyvinyl chloride microspheres with rich pore structures without the need for pore-forming agents, and utilizing water as a porogen for easy removal.
The method produces polyvinyl chloride microspheres with high specific surface area and rich pore structures, facilitating plasticizer diffusion, suitable for industrial applications in medical gloves, leather, and wallpaper, with a simple, environmentally friendly process.
Smart Images

Figure CN118684802B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer chemistry and polymer materials, and particularly relates to a polyvinyl chloride microsphere with a rich pore structure and a preparation method thereof. Background Art
[0002] Porous materials have special properties such as low density, high surface area and good permeation selectivity (Perego C, Millini R. Porous materials in catalysis: challenges for mesoporous materials[J]. Chemical Society Reviews, 2013, 42(9), 3956-3976). Due to these excellent properties, porous materials have attracted widespread attention in the scientific and technological community. In particular, porous polymer materials in the form of microspheres have great application potential in various fields such as polymer synthesis, adsorption, drug delivery and tissue engineering (Yang XY, Chen LH, Li Y, et al. Hierarchically porous materials: synthesis strategies and structure design[J]. Chemical Society Reviews, 2017, 46(2): 481-558.; Zhang K, Li Q, FanH, et al. Multi-layer dextran-decorated poly(glycidyl methacrylate)-co-divinyl benzene copolymer matrices enabling efficient protein chromatographic separation[J]. Reactive and Functional Polymers, 2017, 112: 45-52).
[0003] Porous microspheres usually contain a certain amount of pores in the system, and the pores are obtained by hard templates and soft templates. The former was once very popular because pores of precise size and porosity can be formed after etching away the densely packed solid particles embedded in the polymer spheres (Takami T, Murakami Y. Unexpected and successful "one-step" formation of porous polymeric particles only by mixing organic solvent and water under "low-energy-input" conditions [J]. Langmuir, 2014, 30 (12): 3329-3336). However, the removal of the hard template requires harsh conditions, which makes the manufacturing process more complicated. In contrast, the soft template composed of various diluents can be easily removed by simple extraction or evaporation. Double emulsion technology is widely used in the soft template method to prepare porous microspheres with interconnected morphologies. In general, double emulsions are formed by a two-step stirring emulsification process, using a combination of oil-soluble and water-soluble surfactants to stabilize the oil-water (O / W) and water-oil (W / O) interfaces, respectively. The multiple emulsion template method facilitates the preparation of porous microspheres with its unique structure. This method does not require the porogen of the suspension polymerization method, because the internal phase component of the emulsion droplets in the multiple emulsion itself is water, and the removal of water is simple and environmentally friendly and will form voids. In addition, the multiple emulsion template has many advantages: the raw material composition is simple in the preparation process, the cost is low, and it is easy to prepare; water is used as a porogen, and the product can be obtained by washing and drying in the later stage, which is environmentally friendly; the structure of the multiphase emulsion is conducive to the formation of multi-level pores, and the morphology of the microspheres is easy to control.
[0004] Polyvinyl chloride (PVC) resin is a thermoplastic polymer formed by the polymerization of vinyl chloride monomer. Due to the abundant raw material sources, low production cost and good comprehensive performance of PVC, it has high commercial application value and has become one of the most widely used plastics. According to the production method, PVC resin mainly includes suspension, bulk, emulsion and micro-suspension resins. Among them, emulsion and micro-suspension PVC resins are mainly used in the form of plasticized paste, so they are also called PVC paste resins. However, there are few reports on the preparation method of polyvinyl chloride microspheres. The porous microsphere-type polyvinyl chloride resin has a rich pore structure, which is conducive to the diffusion of plasticizers, so that it can be better swollen by plasticizers and reduce the amount of plasticizers used. Therefore, the present invention has important economic value. Summary of the invention
[0005] The purpose of the present invention is to provide a polyvinyl chloride microsphere with a rich pore structure and a preparation method thereof in view of the shortcomings of the current technology. The method reduces the water solubility of vinyl chloride by adding a stabilizer to inhibit the agglomeration of droplets, and uses an emulsifier to stabilize the emulsion, thereby preparing stable oil-in-water-in-oil droplets, and initiating polymerization to obtain a polyvinyl chloride microsphere material with a rich pore structure. The rich pore structure increases the specific surface area and is conducive to the diffusion of plasticizers in the pores. The polyvinyl chloride microsphere with a rich pore structure has potential uses in adsorption, catalysis and the preparation of polyvinyl chloride paste resins.
[0006] The method for preparing polyvinyl chloride microspheres with a rich pore structure described in the present invention comprises the following steps:
[0007] (1) Add stabilizer, vinyl chloride monomer, emulsifier and oil-soluble initiator into the reactor, stir at room temperature for 5 to 30 minutes, and dissolve and mix them evenly to obtain an oil phase;
[0008] Among them, the mass ratio of stabilizer, vinyl chloride monomer, emulsifier and oil-soluble initiator is 14~22:100:8~12:1.2~2.6;
[0009] The stabilizer is one or more of tridecane, hexadecane, octadecane and hexadecanol;
[0010] The emulsifier is one or more of block polyether F127, Tween 80, Span 80, Tween 20, Span 20, Span60, glyceryl monostearate, polyoxyethylene alkyl ether, emulsifier OP-10, polyoxyethylene monolaurate, and fatty alcohol polyoxyethylene ether;
[0011] The oil-soluble initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, azobisisovaleronitrile, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, methyl ethyl ketone peroxide, cyclohexanone peroxide, tert-butyl perbenzoate, tert-butyl peroxyvalerate, di-tert-butyl peroxide, tert-butyl hydroperoxide, benzoyl peroxide, and lauroyl peroxide;
[0012] (2) mixing a soluble metal salt and deionized water and dissolving them uniformly to obtain an aqueous phase;
[0013] The mass ratio of the soluble metal salt to deionized water is 1-1.6:50-70; the soluble metal salt is one or more of sodium chloride, potassium chloride, sodium sulfate, potassium sulfate, calcium chloride, and magnesium chloride;
[0014] (3) mixing the aqueous phase obtained in step (2) with the oil phase obtained in step (1), stirring at room temperature and 2000-4000 rpm for 2-6 min to obtain a white emulsion; wherein, in the mixed system of the aqueous phase and the oil phase, the volume percentage of the aqueous phase is 73-86%, and the rest is the oil phase;
[0015] (4) Add 1.2 to 2.4 times the total volume of deionized water to the white emulsion obtained in step (3), let it stand for 30 to 60 min, and then rotate at 100 to 200 rpm and 85 to 95 o C for 4-6 h to obtain a white emulsion; then centrifuge at 600-1000 rpm to obtain a white product. The white product is ultrasonically washed and centrifuged at 50-80 o C, thereby obtaining polyvinyl chloride microspheres with rich pore structures;
[0016] The detergent used for washing is deionized water, methanol or ethanol; the ultrasonic power is 100-150W, and the ultrasonic treatment time is 30-60 minutes.
[0017] The polyvinyl chloride microspheres with rich pore structure described in the present invention are prepared by the above method.
[0018] The essential features of the present invention are:
[0019] Among the methods for preparing organic porous microspheres reported in the literature before, some prepare porous microspheres by adding pore-forming agents to monomers by suspension polymerization, and some prepare porous polymer microspheres by seed swelling method, but both have certain disadvantages. The method described in the present invention does not require the pore-forming agent of the suspension polymerization method, because the internal phase component of the emulsion droplets inside the multiple emulsion itself is water, and the removal of water is simple and environmentally friendly and will form voids; at the same time, it does not require long-term swelling like the seed swelling method, and there is no risk of generating new colloid particles; water is used as a pore-forming agent, which is environmentally friendly; the structure of the multiphase emulsion is conducive to the generation of multi-level pores, and the morphology of the microspheres is easy to control. The present invention adopts a one-step polymerization method to prepare polyvinyl chloride microspheres with rich pore structures, and its rich pore structure is conducive to the diffusion of plasticizers therein, and polyvinyl chloride paste resin can be prepared for the preparation of medical gloves, wallpaper, and leather. Therefore, this method is the simplest and most effective, and it can be said that it has opened up a new way to prepare polyvinyl chloride paste resin.
[0020] Beneficial effects of the present invention:
[0021] (1) The polyvinyl chloride microspheres with rich pore structures prepared by the present invention can be used in the production of medical gloves, leather, wallpaper, and labor protection gloves;
[0022] (2) The polyvinyl chloride microspheres with rich pore structures described in the present invention have a simple preparation process, do not use organic solvents in the preparation process, are environmentally friendly, and are conducive to industrial scale-up;
[0023] (3) The polyvinyl chloride microspheres with rich pore structure described in the present invention have rich pore structure and large specific surface area, which can reach 11.34 m 2 / g. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 : Optical microscope photograph of the oil-in-water-in-oil emulsion obtained in step (3) of Example 1, magnified 50 times;
[0025] Figure 2 : SEM photo of polyvinyl chloride microspheres with rich pore structure obtained in step (4) of Example 1;
[0026] Figure 3 : BET N2 adsorption-desorption isotherm curve of the polyvinyl chloride microspheres with rich pore structure obtained in step (4) of Example 1;
[0027] Figure 4 : The pore size distribution curve of the polyvinyl chloride microspheres with rich pore structure obtained in step (4) of Example 1. DETAILED DESCRIPTION
[0028] The method of the present invention mainly comprises: (1) utilizing the self-assembly of the oil phase and the water phase under the stabilizing effect of the stabilizer and the surfactant, and generating a stable water-in-oil emulsion by adding water as the external phase; (2) transferring the emulsion to a flask and polymerizing it under stirring to obtain polyvinyl chloride microspheres with a rich pore structure. The technical solution of the present invention is described clearly and completely below in conjunction with the embodiments and the accompanying drawings. Example 1
[0029] The method for preparing polyvinyl chloride microspheres with rich pore structures by double emulsion template method comprises the following steps:
[0030] (1) Add stabilizer hexadecane (16 g), vinyl chloride monomer (100 g), emulsifier Span 80 (10 g), and oil-soluble initiator azobisisobutyronitrile (1.4 g) into a 5 L kettle and stir at room temperature for 15 minutes to obtain an oil phase after dissolving and mixing evenly;
[0031] (2) Mix soluble metal salt sodium chloride (NaCl, 10 g) and deionized water 400 mL and dissolve them evenly to obtain an aqueous phase;
[0032] (3) mixing the aqueous phase obtained in step (2) with the oil phase obtained in step (1), stirring at room temperature and 2500 rpm for 3 min to obtain a white milky liquid;
[0033] (4) Add 800 mL of deionized water to the emulsion obtained in step (3), let it stand for 40 min, and then o The mixture was stirred at 40 °C for 5 h to obtain a white emulsion. The white product was then centrifuged at 800 rpm to obtain a white product. The product was washed with deionized water by ultrasonic (120 W) and centrifuged at 60 °C. o C to obtain polyvinyl chloride microspheres with rich pore structure, with a product mass of 90 g.
[0034] Figure 1 This is an optical photograph of a W / O / W emulsion prepared by a two-step method. From the photograph, it can be seen that it is in the form of oil-in-water-in-oil droplets.
[0035] Figure 2 This is a photo of polyvinyl chloride microspheres scanned with a FEI Nano SEM 450 scanning electron microscope. From the photo, it can be seen that the material has a rich pore structure. The microspheres are in the micron level and show a rich nanoscale pore structure.
[0036] Figure 3 The surface area and porosity analyzer model ASAP 2020M+C was used. In the N2 adsorption / desorption isotherm at 77 K, obvious hysteresis loops were visible in the pressure range of 0.8~1.0 P / P0 for polyvinyl chloride microspheres at relatively low pressure, indicating that the sample was a type IV isotherm.
[0037] Figure 4 The pore size distribution of polyvinyl chloride microspheres shows that there are micropores (<2 nm), mesopores (2-50 nm) and macropores (>50 nm) in the material. The specific surface area of the material is 11.34 m 2 / g, micropore volume 0.23 cm 3 / g, the average pore size is 25.49 nm, and the pore sizes are mainly concentrated at about 1.5 and 27.1 nm. These results show that the prepared polyvinyl chloride microspheres have a high specific surface area and pore size, which generally helps to promote the diffusion of plasticizers inside the microspheres and is beneficial to the swelling of the microspheres by plasticizers. Example 2
[0038] The other steps are the same as those in Example 1, except that in step (1), the composition of the organic phase is replaced by hexadecane (16 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g) with hexadecane (22 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g). Example 3
[0039] The other steps are the same as those in Example 1, except that in step (1), the organic phase composition is replaced by hexadecane (16 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g) with hexadecane (20 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g). Example 4
[0040] The other steps are the same as those in Example 1, except that in step (1), the organic phase composition is replaced by hexadecane (16 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g) with hexadecane (18 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g). Example 5
[0041] The other steps are the same as those in Example 1, except that in step (1), the organic phase composition is replaced by hexadecane (16 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g) with hexadecanol (16 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g). Example 6
[0042] The other steps are the same as those in Example 1, except that in step (1), the composition of the organic phase is replaced by octadecane (16 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g) with octadecane (16 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g). Example 7
[0043] The other steps are the same as those in Example 1, except that in step (1), the organic phase composition is replaced by hexadecane (16 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g) with hexadecane (16 g), Span 20 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g). Example 8
[0044] The other steps are the same as those in Example 1, except that in step (1), the composition of the organic phase is replaced by hexadecane (16 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g) with hexadecane (16 g), Tween 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g). Example 9
[0045] The other steps are the same as those in Example 1, except that in step (1), the composition of the organic phase is replaced by hexadecane (16 g), Span 80 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g) with hexadecane (16 g), Tween 20 (10 g), azobisisobutyronitrile (1.4 g), and vinyl chloride (100 g). Example 10
[0046] The other steps were the same as those in Example 1, except that in step (1), the aqueous phase composition was replaced by sodium chloride (12 g) and deionized water 400 mL instead of sodium chloride (10 g) and deionized water 400 mL. Embodiment 11
[0047] The other steps are the same as those in Example 1, except that in step (1), the aqueous phase composition is replaced by sodium sulfate (10 g) and 400 mL of deionized water instead of sodium chloride (10 g) and 400 mL of deionized water. Example 12
[0048] The other steps are the same as those in Example 1, except that in step (1), the aqueous phase composition is replaced by potassium chloride (10 g) and 400 mL of deionized water instead of sodium chloride (10 g) and 400 mL of deionized water.
[0049] The polyvinyl chloride microspheres obtained from the formulations of Examples 2 to 12 all exhibited a rich pore structure, which is conducive to the diffusion of the plasticizer in the pores.
[0050] Matters not covered in the present invention are all known technologies.
Claims
1. A method for preparing polyvinyl chloride microspheres with rich pore structure, characterized in that: The steps of the preparation method are as follows, (1) Add stabilizer, vinyl chloride monomer, emulsifier and oil-soluble initiator into the reactor, stir at room temperature for 5 to 30 minutes, and dissolve and mix them evenly to obtain an oil phase; The mass ratio of stabilizer, vinyl chloride monomer, emulsifier and oil-soluble initiator is 14~22:100:8~12:1.2~2.6; the stabilizer is one or more of tridecane, hexadecane, octadecane and hexadecanol; (2) Mixing the soluble metal salt and deionized water, and dissolving them uniformly to obtain a water phase; the mass ratio of the soluble metal salt to the deionized water is 1-1.6:50-70; (3) mixing the aqueous phase obtained in step (2) with the oil phase obtained in step (1), stirring at room temperature and 2000-4000 rpm for 2-6 min to obtain a white emulsion; wherein, in the mixed system of the aqueous phase and the oil phase, the volume percentage of the aqueous phase is 73-86%, and the rest is the oil phase; (4) Add deionized water in an amount of 1.2 to 2.4 times the total volume of the white emulsion obtained in step (3), let the mixture stand for 30 to 60 minutes, and then stir the mixture at 100 to 200 rpm and 85 to 95°C for 4 to 6 hours to obtain a white emulsion; then centrifuge the mixture at 600 to 1000 rpm to obtain a white product, wash the white product by ultrasonic washing, centrifuge the product, and then dry the product at 50 to 80°C to obtain polyvinyl chloride microspheres having a rich pore structure.
2. The method for preparing polyvinyl chloride microspheres having a rich pore structure according to claim 1, characterized in that: The emulsifier described in step (1) is one or more of block polyether F127, Tween 80, Span 80, Tween 20, Span 20, Span 60, glyceryl monostearate, polyoxyethylene alkyl ether, emulsifier OP-10, polyoxyethylene monolaurate, and fatty alcohol polyoxyethylene ether.
3. The method for preparing polyvinyl chloride microspheres having a rich pore structure according to claim 1, characterized in that: The oil-soluble initiator in step (1) is one or more of azobisisobutyronitrile, azobisisoheptylnitrile, azobisisovaleronitrile, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, methyl ethyl ketone peroxide, cyclohexanone peroxide, tert-butyl perbenzoate, tert-butyl peroxyvalerate, di-tert-butyl peroxide, tert-butyl hydroperoxide, benzoyl peroxide, and lauroyl peroxide.
4. The method for preparing polyvinyl chloride microspheres having a rich pore structure according to claim 1, characterized in that: The soluble metal salt in step (2) is one or more of sodium chloride, potassium chloride, sodium sulfate, potassium sulfate, calcium chloride and magnesium chloride.
5. The method for preparing polyvinyl chloride microspheres having a rich pore structure according to claim 1, characterized in that: The detergent used for washing in step (4) is deionized water, methanol or ethanol; the ultrasonic power is 100-150 W, and the ultrasonic treatment time is 30-60 minutes.
6. A polyvinyl chloride microsphere with a rich pore structure, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 5.