Wear-resistant non-stick pan process
Through the combination of bamboo charcoal microcrystals and water-based coatings, the shortcomings of existing non-stick pans in temperature resistance, wear resistance and bacteriostatic resistance are solved, and safe use and efficient thermal conductivity on a variety of heating equipment are achieved to ensure that the product is not Sticky, lightweight and safe.
Patent Information
- Application Number
- CN202410947042.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-05
AI Technical Summary
The existing non-stick pans have average effects in temperature resistance, wear resistance and antibacterial resistance, and have sticking phenomena and safety hazards. They are of heavy quality and cannot be used on all heating equipment.
Using a pot body made of bamboo charcoal as the material and a non-stick coating with silicon as the main component, combined with far-infrared characteristics and electromagnetic wave absorption function, bamboo charcoal microcrystals are formed by calcining bamboo charcoal at high temperature, and mixed with adhesive to form and match with water properties. The coating is sprayed to form a stable non-stick coating, ensuring that the product is non-stick, wear-resistant, heat-conductive and safe.
It achieves non-stick performance at high temperatures, is easy to clean, is safe and free of fluorine, has good thermal conductivity, is suitable for a variety of heating equipment, and the product is lightweight, has far-infrared function to improve water quality and antibacterial effect.
Smart Images

Figure CN118892266A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cookers and relates to a wear-resistant non-stick pan process. Background Art
[0002] The cookware on the market is mainly made of the following materials: stainless steel, iron, aluminum, copper, ceramic, glass, etc. However, stainless steel and iron cookware have relatively poor thermal conductivity, heavy weight, and average non-stick properties. Aluminum cookware has good thermal conductivity, but there has always been controversy over its safety in the health field. Ceramic and glass cookware are heavy in weight and cannot be used in some areas, such as open flames and induction cookers.
[0003] At present, there are two main types of kitchenware coatings on the market: Teflon coating and ceramic coating:
[0004] 1. Teflon coating: The main component is polytetrafluoroethylene; this coating has ultra-low friction coefficient and high corrosion resistance, hardly reacts with any chemicals, and other substances are difficult to adhere to its surface; however, the operating temperature of Teflon coating cannot exceed 260°C, it cannot be dry-burned, and avoid using shovels, steel wool and other utensils that are easy to scratch the pot body. At the same time, problems such as washing hot pots with cold water should be avoided.
[0005] 2. Ceramic coating: The main component is ceramic; the coating has the characteristics of high hardness, wear resistance, high temperature resistance, and high appearance; however, the non-stick performance of the ceramic coating will decrease significantly during long-term use, and it may be damaged or cracked when subjected to severe impact or shock.
[0006] Existing non-stick pans have the problem of sticking when used, and the use of fluorine non-stick materials has potential safety hazards. Existing non-stick pans have average effects in terms of temperature resistance, wear resistance and antibacterial properties, and the product quality is relatively poor. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a wear-resistant non-stick pan process. The non-stick coating with silicon as the main component and the pan body with bamboo charcoal as the material can ensure that the product is non-stick and has far-infrared characteristics, electromagnetic wave absorption and other characteristics. This technology can ensure that the kitchenware products are non-stick, do not contain fluorine components, and can be used on heating equipment such as induction cookers, electric ceramic stoves, and open flames. Consumers do not need to consider the matching problem of heating equipment, which not only ensures the safety of consumers' use, but also the product is easy to clean, has high temperature tolerance, strong wear resistance, and light product quality.
[0008] The technical solution adopted by the present invention to achieve its purpose is as follows:
[0009] The bamboo stems are cut into sections, washed and dried, and then crushed into particles by a crushing device. The crushed bamboo particles are placed in a tubular furnace for calcination. When the calcination temperature is higher than 900°C, the bamboo charcoal will form a shiny metallic luster, which is the bamboo charcoal microcrystal.
[0010] It is a composite crystal formed by high-temperature calcination of iron, aluminum, copper, magnesium and other minerals naturally contained in bamboo. The bamboo charcoal microcrystals are crushed into charcoal powder.
[0011] Then, the crushed carbon powder and the binder are mixed evenly, with the weight percentage of carbon crystals being 80% to 90% and the binder being 10% to 20%, to obtain a prefabricated material. The prefabricated material is poured into a preheated mold under vacuum, the mold preheating temperature is 100 to 250°C, the mold is closed and pressurized, and then demolded to obtain a hard embryo; the obtained embryo is heated under vacuum and at a temperature of 700 to 1500°C to carbonize the binder (the binder is one or more of furan resin glue, furfural resin glue, furfuryl alcohol resin glue or phenolic resin glue), and then cooled for 8 to 10 hours to obtain a pot body.
[0012] Use special water-based paint, liquid A and liquid B with a mass ratio of 100:15. Liquid A contains 60% silicon dioxide, 20% titanium dioxide, 15% water, 3% aluminum oxide, and 2% ethanol by weight, and does not contain fluorine element; liquid B is silicone oil; place liquid A in a drum, roll at a speed of 90-100rpm for 30 minutes, then add liquid B to liquid A, continue rolling for 3 hours, and control the temperature at 22-28℃ throughout the process to complete the maturation.
[0013] Preheat the workpiece surface to 40-50℃, and use an air gun to blow away the dust on the workpiece surface; the nozzle size is 0.8-1.5mm in diameter, and the spraying pressure is 3-4Kgf / cm ^2 , the paint is filtered through 350 mesh. The product is sprayed. The paint must be stirred during the spraying process (the paint spraying process must be stirred to avoid precipitation), and then the product is cured, allowing the non-stick coating to cure under certain temperature and humidity conditions to form a stable coating.
[0014] The beneficial effects of the present invention are
[0015] 1. Ensure the non-stick performance of the product when in contact with food at high temperature;
[0016] 2. Solve the problem of difficult cleaning of products after use;
[0017] 3. The product does not contain fluorine and can pass national standard testing to ensure food safety and hygiene;
[0018] 4. The carbon substrate has good thermal conductivity and wear resistance. Carbon is one of the most high-temperature resistant materials known so far. Its melting point is 3850℃±50℃ and its boiling point is 4250℃.
[0019] 5. With far-infrared function, the product has high thermal efficiency and is safe and antibacterial. Through the far-infrared characteristics of bamboo charcoal, the product has certain effects of improving water quality and safe antibacterial.
[0020] 6. This product can turn water into weak alkaline water after boiling. The weak far infrared rays of the bamboo charcoal pot can change the structure of water molecules, turning water molecules into small molecules of water to increase the oxygen storage capacity and make the water weakly alkaline;
[0021] 7. The product has faster electrical and thermal conductivity than metal kitchen utensils, and is suitable for open flames or induction cookers to save energy and heat quickly;
[0022] 8. This product is not picky about stoves, it can be used with electric ceramic stoves, induction cookers, open flames, etc.
[0023] 9. The product quality is lighter than other materials and the user experience is better. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the process flow of the present invention.
[0025] Figure 2 This is an infrared detection diagram of the non-stick pan inner pot of the present invention. DETAILED DESCRIPTION
[0026] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work should belong to the scope of protection of the present invention.
[0027] Example 1
[0028] S1. Preparation of pot body: Cut bamboo stems into segments, wash and dry them, and then crush them into particles by a crushing device. Place the crushed bamboo particles in a tubular furnace for calcination at 900°C or above for 60 hours to obtain bamboo charcoal microcrystals, which are crushed into charcoal powder; when the calcination temperature is higher than 900°C, the bamboo charcoal will form a shiny metallic luster, which is the bamboo charcoal microcrystal, which is a composite crystal formed by high-temperature calcination of minerals such as iron, aluminum, copper, and magnesium naturally contained in bamboo, and the bamboo charcoal microcrystals are crushed into charcoal powder;
[0029] Then the crushed carbon powder and the adhesive are mixed evenly in the weight percentage of 85% carbon powder and 15% adhesive to obtain a prefabricated material, and the prefabricated material is poured into a preheated mold with a preheating temperature of 200°C. The mold is closed and pressurized, and then demolded to obtain a hard embryo. The embryo is heated in a vacuum state of -0.02MPa to -0.001MPa and a temperature of 1000±50°C to carbonize the adhesive furan resin glue, and then cooled for 9 hours to obtain a pot body.
[0030] S2. Paint preparation: Use special water-based paint, including liquid A and liquid B with a mass ratio of 100:15. Liquid A is prepared by weight percentage of 60% silicon dioxide, 20% titanium dioxide, 15% water, 3% aluminum oxide, and 2% ethanol; liquid B is silicone oil; place liquid A in a drum, roll at a speed of 100 rpm for 30 minutes, then add liquid B to liquid A, continue rolling for 3 hours, and control the temperature at 25°C throughout the process to complete the aging (the aging paint should be used up within 24 hours after the aging is completed).
[0031] S3. Substrate preparation: Workpieces suitable for spraying: Bamboo charcoal pot;
[0032] Degreasing: fully remove grease or other hydrophobic substances that may be attached to the surface of the substrate;
[0033] Sandblasting: A. Sand (aluminum, iron) 80# brown corundum
[0034] Sand (stainless steel) 60# brown corundum
[0035] B. Air pressure 4-6Kgf / cm ^2
[0036] C. Sandblasting roughness (important, sandblasting increases the adhesion of the coating) 2-3μm
[0037] S4. Product spraying: Preheat the surface temperature of the bamboo charcoal pot to 45℃, and use an air gun to blow away the dust on the surface of the workpiece; use a nozzle diameter of 0.8-1.5mm, and a spray pressure of 3-4Kgf / cm ^2 , the paint is filtered through 350 mesh. The product is sprayed, and the paint must be stirred during the spraying process (the paint spraying process must be stirred to avoid precipitation). After spraying, it is placed in a tunnel kiln and cured at 220°C for 1 hour to form a stable coating to obtain a wear-resistant non-stick pan.
[0038] Example 2
[0039] S1. Preparation of pot body: Cut bamboo stems into segments, wash and dry them, and then crush them into particles by a crushing device. Place the crushed bamboo particles in a tubular furnace for calcination at 900°C or above for 58 hours to obtain bamboo charcoal microcrystals, which are crushed into charcoal powder; when the calcination temperature is higher than 900°C, the bamboo charcoal will form a shiny metallic luster, which is the bamboo charcoal microcrystal, which is a composite crystal formed by high-temperature calcination of minerals such as iron, aluminum, copper, and magnesium naturally contained in bamboo, and the bamboo charcoal microcrystals are crushed into charcoal powder;
[0040] Then the crushed carbon powder and the adhesive are mixed evenly in a weight percentage of 80% carbon powder and 20% adhesive to obtain a prefabricated material, and the prefabricated material is poured into a preheated mold with a preheating temperature of 180°C. The mold is closed and pressurized to form, and then demolded to obtain a hard embryo. The embryo is heated in a vacuum state of -0.02MPa to -0.001MPa and a temperature of 1200±50°C to carbonize the adhesive furan resin glue, and then cooled for 10 hours to obtain a pot body.
[0041] S2. Paint preparation: Use special water-based paint, including liquid A and liquid B with a mass ratio of 100:15. Liquid A is prepared by weight percentage of 60% silicon dioxide, 20% titanium dioxide, 15% water, 3% aluminum oxide, and 2% ethanol; liquid B is silicone oil; put liquid A in a drum, roll at a speed of 90rpm for 30 minutes, then add liquid B to liquid A, and continue rolling for 3 hours. Control the temperature at 28℃ throughout the process to complete the aging (the aging paint should be used up within 24 hours after the aging is completed).
[0042] S3. Substrate preparation: Workpieces suitable for spraying: Bamboo charcoal pot;
[0043] Degreasing: fully remove grease or other hydrophobic substances that may be attached to the surface of the substrate;
[0044] Sandblasting: A. Sand (aluminum, iron) 80# brown corundum
[0045] Sand (stainless steel) 60# brown corundum
[0046] B. Air pressure 4-6Kgf / cm ^2
[0047] C. Sandblasting roughness (important, sandblasting increases the adhesion of the coating) 2-3μm
[0048] S4. Product spraying: Preheat the surface temperature of the bamboo charcoal pot to 45℃, and use an air gun to blow away the dust on the surface of the workpiece; use a nozzle diameter of 0.8-1.5mm, and a spray pressure of 3-4Kgf / cm ^2, the paint is filtered through 350 mesh. The product is sprayed, and the paint must be stirred during the spraying process (the paint spraying process must be stirred to avoid precipitation). After spraying, it is placed in a tunnel kiln and cured at 220°C for 1 hour to form a stable coating to obtain a wear-resistant non-stick pan.
[0049] Example 3
[0050] S1. Preparation of pot body: Cut bamboo stems into segments, wash and dry them, and then crush them into particles by a crushing device. Place the crushed bamboo particles in a tubular furnace for calcination at above 900°C for 65 hours to obtain bamboo charcoal microcrystals, which are crushed into charcoal powder; when the calcination temperature is higher than 900°C, the bamboo charcoal will form a shiny metallic luster, which is the bamboo charcoal microcrystal, which is a composite crystal formed by high-temperature calcination of minerals such as iron, aluminum, copper, and magnesium naturally contained in bamboo, and the bamboo charcoal microcrystals are crushed into charcoal powder;
[0051] Then the crushed carbon powder and the adhesive are mixed evenly in the weight percentage of 90% carbon powder and 10% adhesive to obtain a prefabricated material, and the prefabricated material is poured into a preheated mold with a preheating temperature of 210°C. The mold is closed and pressurized, and then demolded to obtain a hard embryo. The embryo is heated in a vacuum state of -0.02MPa to -0.001MPa and a temperature of 1100±50°C to carbonize the adhesive furan resin glue, and then cooled for 8 hours to obtain a pot body.
[0052] S2. Paint preparation: Use special water-based paint, including liquid A and liquid B with a mass ratio of 100:15. Liquid A is prepared by weight percentage of 60% silicon dioxide, 20% titanium dioxide, 15% water, 3% aluminum oxide, and 2% ethanol; liquid B is silicone oil; put liquid A in a drum, roll at a speed of 95rpm for 30 minutes, then add liquid B to liquid A, continue rolling for 3 hours, and control the temperature at 25℃ throughout the process to complete the aging (the aging paint should be used up within 24 hours after the aging is completed).
[0053] S3. Substrate preparation: Workpieces suitable for spraying: Bamboo charcoal pot;
[0054] Degreasing: fully remove grease or other hydrophobic substances that may be attached to the surface of the substrate;
[0055] Sandblasting: A. Sand (aluminum, iron) 80# brown corundum
[0056] Sand (stainless steel) 60# brown corundum
[0057] B. Air pressure 4-6Kgf / cm ^2
[0058] C. Sandblasting roughness (important, sandblasting increases the adhesion of the coating) 2-3μm
[0059] S4. Product spraying: Preheat the surface temperature of the bamboo charcoal pot to 40-50℃, and use an air gun to blow away the dust on the surface of the workpiece; use a nozzle diameter of 0.8-1.5mm, and a spray pressure of 3-4Kgf / cm ^2 , the paint is filtered through 350 mesh. The product is sprayed, and the paint must be stirred during the spraying process (the paint spraying process must be stirred to avoid precipitation). After spraying, it is placed in a tunnel kiln and cured at 220°C for 1 hour to form a stable coating to obtain a wear-resistant non-stick pan.
[0060] Performance Testing
[0061] 1. Coating characteristics
[0062] The wear-resistant non-stick pan obtained in the above embodiment was tested for pencil hardness, glossiness and adhesion, and the results all reached the performance shown in Table 1.
[0063] Table 1
[0064]
[0065]
[0066] 2. Non-stick pan characteristics
[0067] The wear-resistant non-stick pan obtained in the above embodiment was tested for water pH value, high and low temperature stability, wear resistance, and temperature tolerance, and the results all reached the performance shown in Table 2.
[0068] Table 2
[0069]
[0070] 3. Antibacterial properties
[0071] The wear-resistant non-stick pans obtained in the above examples were tested for antibacterial properties, and the results all achieved the performance shown in Table 3.
[0072] Table 3
[0073]
[0074]
Claims
1. A wear-resistant non-stick pan process, characterized in that: The following steps are involved: S1. Preparation of pot body: crushing bamboo stems into particles, calcining, obtaining bamboo charcoal microcrystals, and crushing into carbon powder; then mixing 80% to 90% by weight of carbon powder and 10% to 20% by weight of binder to obtain a preform, pouring the preform into a preheated mold, the mold preheating temperature is 100 to 250 ° C, closing the mold and pressing, and then demolding to obtain an embryo; then in a vacuum state of -0.02MPa to -0.001MPa and 700 to 1500 ° C, the obtained embryo is heated to carbonize the binder, and then cooled for 8-10h to obtain a pot body; S2. Prepare water-based coating: including liquid A and liquid B with a mass ratio of 100:15, wherein liquid A is prepared by weight percentage of 60% silicon dioxide, 20% titanium dioxide, 15% water, 3% aluminum oxide, and 2% ethanol; liquid B is silicone oil; Place liquid A in a drum and roll at a speed of 90-100 rpm for 30 minutes, then add liquid B to liquid A and continue rolling for 3 hours, controlling the temperature at 22-28°C throughout the process to complete the maturation; S3. Spraying: Preheat the surface temperature of the bamboo charcoal pot to 40-50℃, and use an air gun to blow away the dust on the surface; the nozzle size is 0.8-1.5mm in diameter, and the spraying pressure is 3-4Kgf / cm ^2 , the paint is filtered through 350 mesh, and then the product is sprayed. The paint must be stirred during the spraying process, and then cured after spraying to form a coating, thereby obtaining a wear-resistant non-stick pan.
2. A wear-resistant non-stick pan process according to claim 1, characterized in that: The calcination condition in step S1 is above 900° C. and calcination for 48-72 hours.
3. A wear-resistant non-stick pan process according to claim 1, characterized in that: In step S1, the adhesive is one or more of furan resin glue, furfural resin glue, furfuryl alcohol resin glue or phenolic resin glue.
4. A wear-resistant non-stick pan process according to claim 1, characterized in that: The curing condition in step S1 is to put the material into a tunnel kiln after spraying and cure it at 220° C. for 1 hour.