Low-cement-amount concrete mix proportion design method based on glass powder
The reaction of glass powder with water to generate hydrolysate and adjust the substitution rate. Based on the activity index calculation, the optimal dosage amount is solved, and the problem of ASR risk and glass powder activity improvement is improved, concrete performance is improved and production costs are reduced.
Patent Information
- Application Number
- CN202411001487.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the application of glass powder in concrete has a risk of alkali-silicon reaction (ASR), which leads to structural expansion failure, and the problem of improving glass powder activity and determining optimal dosage is not completely solved.
The reaction of glass powder with water generates a hydrolysate of Si-O-H+, Ca2+, and Na+, and adjusts the glass powder substitution rate, and determines the optimal dosage based on the glass powder activity index calculation rules, reduces the risk of ASR, and improves the performance of concrete.
Effectively reduce ASR risks, improve the slump, density, compressive strength, bending strength and water absorption of concrete, simplify the process of glass powder incorporation, reduce production costs, and obtain glass according to different performance design requirements. Optimal amount of powder.
Smart Images

Figure CN118908657A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete, and in particular to a low-cement concrete mix design method based on glass powder. Background Art
[0002] With the rapid development of the construction industry, the consumption of cement is growing rapidly. The production of cement not only consumes a lot of natural resources, but also produces harmful substances such as dust, CO2, heavy metals, etc., which have an adverse impact on the environment. Using admixtures to replace part of cement in engineering construction and reducing the relative amount of cement is an effective way to solve the above problems. However, there are fewer types of mineral admixtures in concrete, and high-quality mineral admixtures such as fly ash, slag powder and silica fume are becoming increasingly scarce. It is particularly important to find natural minerals or solid waste as concrete admixtures and increase their utilization rate in concrete. Glass powder is an active material that has been studied more. It is simple, easy to obtain, and low in price. It is an important material in the development of low-cement concrete.
[0003] Wan Li et al. studied the effect of glass powder replacing cement on the performance of concrete. The results showed that replacing part of the cement with glass powder can help improve the workability of concrete and increase the slump of the mixture. The addition of glass powder has a certain effect on the early and late strength of concrete. Due to the volcanic ash effect of glass powder, the trend of the later compressive strength of concrete decreasing with the increase of glass powder content is slower than that of the early strength. The addition of glass powder to concrete can help improve the drying shrinkage of concrete, and the higher the content, the more obvious the effect. Glass powder can fill the internal pores of concrete and reduce the evaporation of internal water. The above results show that the activity of glass powder is related to the content, and it has strong volcanic ash activity in the later stage. The application of glass powder in concrete has certain benefits, but how to improve the activity of glass powder itself and conveniently derive the optimal content of glass stone powder based on different performance design requirements has not yet formed a unified conclusion, and the specific application needs further research.
[0004] Although glass powder has strong volcanic ash activity and can promote cement hydration and improve the performance of concrete, due to the high alkali activity of amorphous silica in glass, alkali-silicon reaction (ASR) will occur in concrete, causing expansion damage to the concrete structure. At present, the method of grinding waste glass to less than 100 microns or adding modified inorganic materials can effectively prevent concrete from expanding and damaging, but grinding to reduce the particle size of glass powder requires high energy consumption, increases production costs, and the improvement effect of adding modified inorganic materials is not obvious. Therefore, how to reduce the risk of ASR is also an urgent problem to be solved in the current application of glass powder in concrete. Summary of the invention
[0005] The problem to be solved by the present invention is to provide a low-cement concrete mix design method based on glass powder in view of the above-mentioned deficiencies in the prior art. By improving and simplifying the way of adding glass powder and proposing a technical parameter of glass powder activity index, the present invention can effectively reduce the ASR risk and improve the volcanic ash activity of glass powder in concrete, while conveniently deriving the optimal dosage of glass stone powder based on different performance design requirements.
[0006] The above-mentioned object of the present invention is achieved through the following technical solutions:
[0007] A method for designing a low-cement concrete mix ratio based on glass powder comprises the following steps:
[0008] S1 glass powder reacts with the first portion of water. After the reaction is completed, a Si-OH + , Ca 2+ 、Na + hydrolyzate;
[0009] S2 According to the preset mix ratio of cementitious materials, aggregates and water, the cementitious materials include cement and P GP % glass powder, and adjust the glass powder replacement rate P GP %, mixing cement, the hydrolyzate obtained in S1, aggregate and a second portion of water to obtain a concrete specimen;
[0010] S3 determines the concrete working performance under different glass powder replacement rates based on the calculation rules of glass powder activity, and determines the corresponding glass powder activity index, and then determines the glass powder replacement rate under the maximum glass powder activity index.
[0011] By adopting the above technical solution, glass powder will undergo hydrolysis reaction after mixing with water, and generate a large amount of Si-OH + , Ca 2+ 、Na + There is no need to pre-grind the glass powder to the 100-micron level. The activity of the glass powder can be greatly improved after the hydrolysis is completed, and then the volcanic ash reaction can continue to occur in concrete of different ages, and ultimately the slump, density, compressive strength, flexural strength, water absorption and other properties of the concrete can be improved simultaneously. In addition, the technical parameter of glass powder activity index is proposed, which can conveniently derive the optimal dosage of glass stone powder based on different performance design requirements, which has important guiding significance for actual production.
[0012] Furthermore, in S1, the particle size of the glass powder is controlled to be ≤75 mm. By means of hydrolysis pretreatment, the ASR risk caused by the high alkali activity of the original amorphous silica can be directly eliminated without grinding the glass powder to a particle size of 100 microns or adding modified inorganic materials, which is conducive to reducing production costs.
[0013] Furthermore, in S1, the reaction time is 8 to 10 hours. After 8 hours of hydrolysis, the glass powder completes most of the hydrolysis process to generate SiO2, CaO and Na2O.
[0014] Furthermore, in S1, the hydrolyzate includes SiO2, CaO and Na2O. After the amorphous silicon dioxide is hydrolyzed, SiO2, CaO and Na2O are in the form of Si-OH + , Ca 2+ 、Na + The presence of these forms in the hydrolyzate can significantly improve the activity of the glass powder while eliminating the ASR risk.
[0015] Furthermore, in S2, the glass powder replacement rate P is adjusted. GP % is 0~50wt%. The glass powder replacement rate can be specifically 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50wt%.
[0016] Furthermore, in S2, the raw materials of each cubic meter of the concrete include 270-330 kg of cementitious material, 1840-1880 kg of aggregate, and 70-75% of water accounting for the total weight of the cementitious material, the aggregate includes 595-605 kg of fine sand, 345-355 kg of small stone, 245-255 kg of medium stone and 655-665 kg of large stone, and the water includes a first part of water and 0-50 wt% of a second part of water.
[0017] Furthermore, in S2, the raw materials of each cubic meter of the concrete include 300 kg of cementitious material, 1860 kg of aggregate and 215 kg of water, the aggregate includes 600 kg of fine sand, 350 kg of small stone, 250 kg of medium stone and 660 kg of large stone, and the water includes a first part of water and 20 wt% of a second part of water.
[0018] Furthermore, in the S2, the cement is 42.5 ordinary Portland cement, the particle size range of fine sand is 0.1~0.8mm, the particle size range of small stone is 4~15mm, the particle size range of medium stone is 8~20mm, and the particle size range of large stone is 10~30mm.
[0019] Furthermore, in S3, the calculation rule of the glass powder activity is: glass powder activity index = 1-f0*P GP % / f GP ; Among them, f0 and f GP The glass powder replacement rate is 0% and P GPWhen the glass powder activity index is less than 0, it means that the glass powder is inactive and the compressive strength of the concrete decreases. When the glass powder activity index = 0, it means that the glass powder is not affected and the compressive strength of the concrete remains unchanged. When the glass powder activity index is greater than 0, it means that the glass powder is reactive and replacing the glass powder has a positive effect on the compressive strength of the concrete.
[0020] Furthermore, in S3, the concrete working performance includes one or more of compressive strength, flexural strength, bulk density, water absorption, slump expansion, expansion time, and J-ring expansion.
[0021] In summary, the beneficial technical effect of the present invention is as follows: by improving and simplifying the method of adding glass powder and proposing a technical parameter of glass powder activity index, the ASR risk can be effectively reduced and the volcanic ash activity of glass powder in concrete can be increased. At the same time, the optimal amount of glass stone powder can be conveniently obtained based on different performance design requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the aggregate screening curve diagram of Example 2 of the present invention.
[0023] Figure 2 4 is a graph showing the relationship between the concrete slump and the glass powder replacement rate of Example 6 of the present invention.
[0024] Figure 3 3 is a graph showing the relationship between the density of concrete at different ages and the replacement rate of glass powder in Example 6 of the present invention.
[0025] Figure 4 1 is a graph showing the relationship between the density of concrete at different ages and the replacement rate of glass powder under the dry mixing method and the wet mixing method in Example 6 of the present invention.
[0026] Figure 5 3 is a graph showing the relationship between the compressive strength of concrete at different ages and the replacement rate of glass powder according to Example 6 of the present invention.
[0027] Figure 6 3 is a graph showing the relationship between the compressive strength of concrete at different ages and the replacement rate of glass powder under the dry mixing method and the wet mixing method in Example 6 of the present invention.
[0028] Figure 7 3 is a graph showing the relationship between the water absorption rate of concrete at different ages and the replacement rate of glass powder in Example 6 of the present invention.
[0029] Figure 8 3 is a graph showing the relationship between the water absorption rate of concrete at different ages and the replacement rate of glass powder under the dry mixing method and the wet mixing method in Example 6 of the present invention. DETAILED DESCRIPTION
[0030] In order to make the technical means, creative features, objectives and functions achieved by the present invention clearer and easier to understand, the present invention is further explained below in conjunction with the accompanying drawings and specific implementation methods.
[0031] Embodiment 1: A method for designing a low-cement concrete mix ratio based on glass powder disclosed in the present invention comprises the following steps:
[0032] The glass powder with a particle size of S1 ≤ 75 mm reacts with the first portion of water. After 8 hours of hydrolysis, the glass powder completes most of the hydrolysis process to generate SiO2, CaO and Na2O. + , Ca 2+ 、Na + hydrolyzate;
[0033] S2 According to the preset mix ratio of cementitious materials, aggregates and water, the cementitious materials include cement and P GP % glass powder, and adjust the glass powder replacement rate P GP %, firstly mix cement and aggregate to form a solid mixture, then add the hydrolyzate obtained in S1 and the second portion of water, and stir and shape by wet mixing or dry mixing to obtain a concrete specimen;
[0034] S3 determines the concrete working performance under different glass powder replacement rates based on the calculation rules of glass powder activity, and determines the corresponding glass powder activity index, and then determines the glass powder replacement rate under the maximum glass powder activity index.
[0035] Example 2: A low cement content concrete mix design method based on glass powder disclosed in the present invention is different from Example 1 in that, in S2, the screening curves of the components in the aggregate are as follows: Figure 1 As shown, the cement is 42.5 ordinary Portland cement, the particle size range of fine sand (sand) is 0.1~0.8mm, the particle size range of small stone (small-size coarse aggregate) is 4~15mm, the particle size range of medium stone (medium-size coarse aggregate) is 8~20mm, and the particle size range of large stone (large-size coarse aggregate) is 10~30mm.
[0036] Example 3: A method for designing a concrete mix ratio with low cement content based on glass powder disclosed in the present invention. The difference from Example 4 is that in S2, concrete mix ratios with different glass powder replacement rates are specifically shown in Table 1.
[0037] Table 1
[0038] Group Glass powder replacement rate / % Cement content / kg Glass powder dosage / kg Water content / kg Fine sand dosage / kg Small stone dosage / kg Medium stone content / kg Dashi content / kg 0%GP 0 300 0 215 600 350 250 660 10% GP 10 270 30 215 600 350 250 660 20% GP 20 240 60 215 600 350 250 660 30% GP 30 210 90 215 600 350 250 660
[0039] Example 4: A method for designing a low-cement concrete mix ratio based on glass powder disclosed in the present invention. The difference from Example 3 is that in S3, the activity index of glass powder = 1-f0*P GP % / f GP ; Among them, f0 and f GP The glass powder replacement rate is 0% and P GP %; when the glass powder activity index is less than 0, it means that the glass powder is inactive and the compressive strength of the concrete decreases. When the glass powder activity index = 0, it means that the glass powder is not affected and the compressive strength of the concrete remains unchanged. When the glass powder activity index is greater than 0, it means that the glass powder is reactive and replacing the glass powder has a positive effect on the compressive strength of the concrete.
[0040] Example 5: This is a method for designing a low-cement concrete mix ratio based on glass powder disclosed in the present invention. The difference from Example 4 is that in S3, the compressive strength of concrete with different glass powder replacement rates at different ages is measured, and the results are shown in Table 2.
[0041] Table 2
[0042] Group 2d compressive strength / MPa 7d compressive strength / MPa 28d compressive strength / MPa 90d compressive strength / MPa 0%GP 13.4 16.9 26.3 27.1 10% GP (dry mix method) 11.4 15.9 24.4 27.9 10% GP (wet mixing method) 16.9 20.2 28.2 34.3 30% GP (dry mix method) 8.1 10.3 17.8 20.0 30% GP (wet mixing method) 14.7 18.0 20.8 25.0
[0043] It can be seen from Table 2 that according to the compressive strength performance index, the glass powder replacement rate under the maximum glass powder activity index is determined to be 10wt%, and compared with the commonly used dry mixing method, the strength of concrete prepared by the wet mixing method is significantly higher than that of the dry mixing method.
[0044] Example 6: A method for designing a low-cement concrete mix ratio based on glass powder disclosed in the present invention. The difference from Example 4 is that in S3, the slump, density, compressive strength, flexural strength and water absorption of concrete with different glass powder replacement rates are measured. The results are as follows: Figures 2 to 8 shown.
[0045] from Figures 2 to 8 It can be seen that
[0046] (1) As the glass powder content increases, the slump gradually increases (the hydrolyzed glass powder contains more water);
[0047] (2) After 90 days, the density of concrete with 10% and 20% glass powder content was greater than that of the control group without glass powder, indicating that the pozzolanic reaction of glass powder was more intense and more hydrate products were formed;
[0048] (3) The density of concrete mixed with hydrolyzed glass powder is much higher than that of untreated glass powder. During the formation of CSH gel, the free ions of glass powder can produce more and denser hydration products;
[0049] (4) The compressive strength decreased with the increase of GP dosage until 28 days. Subsequently, at 90 days, an increase in compressive strength was obtained under 10% and 20% GP, which was higher than that of the control group. This is because the pozzolanic reaction that occurred in the later period affected the interface transition zone between cement paste, aggregate and pores, and the pores in the interface transition zone became finer;
[0050] (5) After using hydrolyzed glass powder, the compressive strength of concrete was significantly improved. The highest compressive strength was obtained at 10% replacement. The dissolution of glass powder led to an increase in the early (2 and 7 days) compressive strength, which was due to the formation of more free ions by hydrolysis. After 90 days, the volcanic ash reaction proceeded further, and the compressive strength was higher;
[0051] (6) Flexural strength at 28 days: 4.5 MPa for the control group, 5 MPa for 10% admixture, 5.5 MPa for 20% admixture, and 5 MPa for 30% admixture;
[0052] (7) The water absorption of the glass powder surface is insufficient, which affects the total absorption rate of the concrete prepared with glass powder. The water absorption rate is related to the degree of hydration. As the age increases, the water absorption rate decreases. The water absorption rate of concrete with a 30% admixture is the highest because there are a large number of unhydrated solids and a large number of pores;
[0053] (8) The absorption rate of the mixture prepared by hydrolysis of glass powder is significantly reduced, which is related to the degree of hydration and the structure of the hydration product.
[0054] Examples 7 to 10 are a method for designing a low-cement concrete mix ratio based on glass powder disclosed in the present invention. The difference from Example 4 is that in S1, the hydrolysis time is controlled to be 8.5, 9.1, 9.5, and 10.0 h.
[0055] After testing, the glass powder replacement rate is 10wt%, the slump of concrete under different hydrolysis times is ≥19cm, the density at 28d age is ≥2390kg / m3, the compressive strength is ≥28MPa, the flexural strength is ≥4.6MPa, and the water absorption rate is ≥4.3%. Moreover, with the increase of hydrolysis time, these concrete performance indicators show irregular changes, and when it exceeds 10.0h, these concrete performance indicators will drop significantly.
[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A low-cement concrete mix design method based on glass powder, characterized in that: The following steps are included: S1 glass powder reacts with the first portion of water. After the reaction is completed, a Si-OH + , Ca 2+ 、Na + hydrolyzate; S2 According to the preset mix ratio of cementitious materials, aggregates and water, the cementitious materials include cement and P GP % glass powder, and adjust the glass powder replacement rate P GP %, mixing cement, the hydrolyzate obtained in S1, aggregate and a second portion of water to obtain a concrete specimen; S3 determines the concrete working performance under different glass powder replacement rates based on the calculation rules of glass powder activity, and determines the corresponding glass powder activity index, and then determines the glass powder replacement rate under the maximum glass powder activity index.
2. The method for designing a low-cement concrete mix ratio based on glass powder according to claim 1, characterized in that: In the step S1, the particle size of the glass powder is controlled to be ≤75 mm.
3. The method for designing a low-cement concrete mix ratio based on glass powder according to claim 1, characterized in that: In the S1, the reaction time is 8 to 10 hours.
4. The method for designing a low-cement concrete mix ratio based on glass powder according to claim 1, characterized in that: In S1, the hydrolyzate includes SiO2, CaO and Na2O.
5. The method for designing a low-cement concrete mix ratio based on glass powder according to claim 1, characterized in that: In S2, the glass powder replacement rate P is adjusted. GP % is 0~50wt%.
6. The method for designing a low-cement concrete mix ratio based on glass powder according to claim 5, characterized in that: In S2, the raw materials of the concrete per cubic meter include 270-330 kg of cementitious material, 1840-1880 kg of aggregate, and 70-75% of water accounting for the total weight of the cementitious material, the aggregate includes 595-605 kg of fine sand, 345-355 kg of small stone, 245-255 kg of medium stone and 655-665 kg of large stone, and the water includes a first part of water and 0-50 wt% of a second part of water.
7. The method for designing a low-cement concrete mix ratio based on glass powder according to claim 6, characterized in that: In S2, the raw materials of each cubic meter of the concrete include 300 kg of cementitious material, 1860 kg of aggregate and 215 kg of water, the aggregate includes 600 kg of fine sand, 350 kg of small stone, 250 kg of medium stone and 660 kg of large stone, and the water includes a first part of water and 20 wt% of a second part of water.
8. The method for designing a low-cement concrete mix ratio based on glass powder according to claim 1, characterized in that: In the S2, the cement is 42.5 ordinary Portland cement, the particle size range of fine sand is 0.1~0.8mm, the particle size range of small stone is 4~15mm, the particle size range of medium stone is 8~20mm, and the particle size range of large stone is 10~30mm.
9. The method for designing a low-cement concrete mix ratio based on glass powder according to claim 1, characterized in that: In S3, the calculation rule of glass powder activity is: glass powder activity index = 1-f0*P GP % / f GP ; Among them, f0 and f GP The glass powder replacement rate is 0% and P GP % concrete compressive strength.
10. The method for designing a low-cement concrete mix ratio based on glass powder according to claim 1, characterized in that: In S3, the concrete working performance includes one or more of compressive strength, flexural strength, bulk density, water absorption, slump expansion, expansion time, and J-ring expansion.