Liquid crystal composition and liquid crystal display element

By using specific compound compositions in liquid crystal display elements, the balance problem of liquid crystal display elements in temperature range, viscosity and stability is solved, and the effects of short response time, low threshold voltage and long life are achieved.

CN118909643APending Publication Date: 2024-11-08JIANGSU HECHENG DISPLAY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958932.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2016-03-25
Filing Date
2017-02-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing liquid crystal display elements have challenges in terms of temperature range, viscosity, dielectric anisotropy, contrast and stability, resulting in problems such as long response time, low voltage retention, insufficient contrast and short life.

Method used

A liquid crystal composition consisting of a specific compound, including a compound as a first and second component, having positive dielectric anisotropy and optimizing the composition by adjusting the proportion and additives of the compound Characteristics to meet high upper limit temperature, low lower limit temperature, appropriate optical anisotropy and high stability requirements.

Benefits of technology

The short response time, low threshold voltage, long life and high voltage retention rate of the liquid crystal display element are realized, improving the performance and stability of the element.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004949725650000021
    Figure BDA0004949725650000021
  • Figure BDA0004949725650000031
    Figure BDA0004949725650000031
  • Figure BDA0004949725650000041
    Figure BDA0004949725650000041
Patent Text Reader

Abstract

The invention provides a liquid crystal composition and a liquid crystal display element, the liquid crystal composition fully satisfies at least one of characteristics such as high upper limit temperature, low lower limit temperature, low viscosity, appropriate optical anisotropy, and large dielectric anisotropy, or has an appropriate balance between at least two characteristics. The liquid crystal composition contains a specific compound having a large positive dielectric anisotropy as a first component and a specific compound having a small viscosity as a second component. The liquid crystal composition may also contain, as a third component, a specific compound having a high upper limit temperature or a low viscosity, as a fourth component, a specific compound having positive dielectric anisotropy, or as a fifth component, a specific compound having negative dielectric anisotropy.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention is a divisional application of the invention patent application with application number 201780018966.X filed on February 13, 2017 and invention name “Liquid Crystal Composition and Liquid Crystal Display Element”. Technical Field

[0002] The present invention relates to a liquid crystal composition and a liquid crystal display element containing the composition, etc. In particular, the present invention relates to a liquid crystal composition with positive dielectric anisotropy and an active matrix (AM) element containing the composition and having twisted nematic (TN), optically compensated bend (OCB), in-plane switching (IPS), fringe field switching (FFS) or field-induced photoreactive alignment (FPA) mode. Background Art

[0003] In liquid crystal display elements, the operation mode of liquid crystal molecules is classified into phase change (PC), twisted nematic (TN), super twisted nematic (STN), electrically controlled birefringence (ECB), optically compensated bend (OCB), in-plane switching (IPS), vertical alignment (VA), fringe field switching (FFS), field-induced photo-reactive alignment (FPA) and other modes. The driving method of the element is classified into passive matrix (PM) and active matrix (AM). PM is classified into static and multiplex, etc., and AM is classified into thin film transistor (TFT), metal insulator metal (MIM), etc. TFT is classified into amorphous silicon and polycrystalline silicon. The latter is classified into a high temperature type and a low temperature type according to the manufacturing process. The latter is classified into a reflective type using natural light, a transmissive type using backlight, and a semi-transmissive type using both natural light and backlight according to the light source.

[0004] The liquid crystal display element contains a liquid crystal composition having a nematic phase. The composition has appropriate characteristics. By improving the characteristics of the composition, an AM element with good characteristics can be obtained. The correlation between the characteristics of the two is summarized in the following Table 1. The characteristics of the composition are further described based on commercially available AM ​​elements. The temperature range of the nematic phase is related to the temperature range in which the element can be used. The preferred upper limit temperature of the nematic phase is above about 70°C, and the preferred lower limit temperature of the nematic phase is below about -10°C. The viscosity of the composition is related to the response time of the element. In order to display dynamic images with the element, it is preferred that the response time is short. The ideal response time is shorter than 1 millisecond. Therefore, it is preferred that the viscosity of the composition is small. It is more preferred that the viscosity at low temperatures is small. The elastic constant of the composition is related to the contrast of the element. In order to improve the contrast in the element, it is more preferred that the elastic constant in the composition is large.

[0005] Table 1. Composition and characteristics of AM components

[0006]

[0007] The optical anisotropy of the composition is related to the contrast ratio of the element. Depending on the mode of the element, a large optical anisotropy or a small optical anisotropy, that is, an appropriate optical anisotropy, is required. The product (Δn×d) of the optical anisotropy (Δn) of the composition and the cell gap (d) of the element is designed to maximize the contrast ratio. The value of the appropriate product depends on the type of operation mode. In elements of modes such as TN, the appropriate value is about 0.45μm. In the above case, a composition with a large optical anisotropy is preferred for an element with a small cell gap. The large dielectric anisotropy of the composition contributes to a low threshold voltage, a small power consumption and a large contrast ratio in the element. Therefore, a large dielectric anisotropy is preferred. The large specific resistance of the composition contributes to a large voltage holding ratio and a large contrast ratio of the element. Therefore, a composition having a large specific resistance not only at room temperature but also at a temperature close to the upper limit temperature of the nematic phase in the initial stage is preferred. A composition having a large specific resistance not only at room temperature but also at a temperature close to the upper limit temperature of the nematic phase after long-term use is preferred. The stability of the composition to ultraviolet light and heat is related to the life of the liquid crystal display element. When these stabilities are high, the life of the element is long. Such properties are preferred for AM elements used in liquid crystal projectors, liquid crystal televisions, etc.

[0008] A composition having positive dielectric anisotropy is used in an AM element having a TN mode. A composition having negative dielectric anisotropy is used in an AM element having a VA mode. A composition having positive or negative dielectric anisotropy is used in an AM element having an IPS mode or an FFS mode. A composition having positive or negative dielectric anisotropy is used in an AM element of polymer sustained alignment (PSA) type. The compound contained in the first component of the present invention is disclosed in the following patent documents 1 and 2. The compound contained in the second component of the present application is disclosed in patent documents 3 to 6.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: International Publication No. 2004 / 48501

[0012] Patent Document 2: International Publication No. 1996 / 11897

[0013] Patent Document 3: Japanese Patent Laid-Open No. 09-077692

[0014] Patent Document 4: Japanese Patent Laid-Open No. 10-114690

[0015] Patent Document 5: Japanese Patent Application Publication No. 2010-275390

[0016] Patent Document 6: International Publication No. 2010 / 131594 Summary of the invention

[0017] Problems to be solved by the invention

[0018] One of the purposes of the present invention is a liquid crystal composition that fully satisfies at least one of the following characteristics: a high upper temperature limit of the nematic phase, a low lower temperature limit of the nematic phase, a low viscosity, an appropriate optical anisotropy, a large dielectric anisotropy, a large specific resistance, a high stability to ultraviolet rays, a high stability to heat, and a large elastic constant. Another purpose is a liquid crystal composition that has a proper balance between at least two characteristics. Another purpose is a liquid crystal display element containing such a composition. Yet another purpose is an AM element that has characteristics such as a short response time, a large voltage holding ratio, a low threshold voltage, a large contrast ratio, and a long life.

[0019] Technical means of solving problems

[0020] The present invention relates to a liquid crystal composition and a liquid crystal display element containing the composition, wherein the liquid crystal composition contains at least one compound selected from the group of compounds represented by formula (1) as a first component and at least one compound selected from the group of compounds represented by formula (2) as a second component, and has positive dielectric anisotropy.

[0021]

[0022] In formula (1) and formula (2), R 1 is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms; R 2 and R 3 are independently alkenyl groups having 2 to 12 carbon atoms; Ring A and Ring B are independently 1,4-cyclohexylene, 1,4-cyclohexenylene, 1,4-phenylene, 1,4-phenylene in which at least one hydrogen is substituted by fluorine or chlorine, tetrahydropyran-2,5-diyl, 1,3-dioxane-2,5-diyl, pyrimidine-2,5-diyl or pyridine-2,5-diyl, and at least one Ring A is tetrahydropyran-2,5-diyl or 1,3-dioxane-2,5-diyl; 1 and Z 2 X is independently a single bond, ethylene, vinylene, methyleneoxy, carbonyloxy or difluoromethyleneoxy; 1 and X 2 are independently hydrogen or fluorine; Y 1is fluorine, chlorine, an alkyl group having 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, an alkoxy group having 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, or an alkenyloxy group having 2 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine; a is 1, 2, 3 or 4; b is 0, 1, 2 or 3; and the sum of a and b is 4 or less.

[0023] Effects of the Invention

[0024] The advantages of the present invention are a liquid crystal composition which satisfies at least one of the following characteristics: a high upper temperature limit of the nematic phase, a low lower temperature limit of the nematic phase, low viscosity, appropriate optical anisotropy, large dielectric anisotropy, large specific resistance, high stability to ultraviolet rays, high stability to heat, and large elastic constant. Another advantage is a liquid crystal composition having a proper balance between at least two characteristics. Another advantage is a liquid crystal display element containing such a composition. Another advantage is an AM element having characteristics such as a short response time, a large voltage holding ratio, a low threshold voltage, a large contrast ratio, and a long life. DETAILED DESCRIPTION

[0025] The terms used in the specification are as follows. Sometimes the terms "liquid crystal composition" and "liquid crystal display element" are referred to as "composition" and "element", respectively. "Liquid crystal display element" is a general term for liquid crystal display panels and liquid crystal display modules. "Liquid crystal compound" is a compound having a liquid crystal phase such as a nematic phase and a smectic phase, and a general term for a compound that does not have a liquid crystal phase but is mixed in a composition for the purpose of adjusting the temperature range, viscosity, dielectric anisotropy and other properties of the nematic phase. The compound has a six-membered ring such as 1,4-cyclohexylene or 1,4-phenylene, and its molecular structure is rod-like. "Polymerizable compound" is a compound added for the purpose of generating a polymer in the composition. Sometimes at least one compound selected from the group of compounds represented by formula (1) is referred to as "compound (1)". "Compound (1)" refers to one compound or two or more compounds represented by formula (1). The same is true for compounds represented by other formulas. "At least one" related to "substitution" means that not only the position but also the number can be selected without restriction.

[0026] The liquid crystal composition is prepared by mixing a plurality of liquid crystal compounds. Additives are added to the composition for the purpose of further adjusting physical properties. Additives such as optically active compounds, antioxidants, ultraviolet absorbers, pigments, defoamers, polymerizable compounds, polymerization initiators, polymerization inhibitors, polar compounds are added as needed. The liquid crystal compounds or additives are mixed in this order. Even in the case of adding additives, the proportion (content) of the liquid crystal compound is expressed by the weight percentage (wt%) based on the weight of the liquid crystal composition without additives. The proportion (addition amount) of the additive is expressed by the weight percentage (wt%) based on the weight of the liquid crystal composition without additives, similarly to the proportion of the liquid crystal compound. Parts per million (ppm) by weight is sometimes used. The proportion of the polymerization initiator and the polymerization inhibitor is expressed as an exception based on the weight of the polymerizable compound.

[0027] Sometimes the “upper limit temperature of the nematic phase” is simply referred to as the “upper limit temperature”. Sometimes the “lower limit temperature of the nematic phase” is simply referred to as the “lower limit temperature”. “High specific resistance” means that the composition has a high specific resistance not only at room temperature but also at a temperature close to the upper limit temperature of the nematic phase in the initial stage, and after long-term use, it has a high specific resistance not only at room temperature but also at a temperature close to the upper limit temperature of the nematic phase. “High voltage holding ratio” means that the element has a high voltage holding ratio not only at room temperature but also at a temperature close to the upper limit temperature of the nematic phase in the initial stage, and after long-term use, it has a high voltage holding ratio not only at room temperature but also at a temperature close to the upper limit temperature of the nematic phase.

[0028] The expression "at least one 'A' may be substituted with 'B'" means that the number of 'A' is arbitrary. When the number of 'A' is one, the position of 'A' is arbitrary, and when the number of 'A' is two or more, these positions can also be selected without limitation. The above rule also applies to the expression "at least one 'A' may be substituted with 'B'".

[0029] In the chemical formula of the component compound, the terminal group R 1 The symbol is used in many compounds. In these compounds, any two R 1 The two groups represented by may be the same or different. For example, R 1 is ethyl, and R of compound (1-1) 1 In the case of ethyl. There are also compounds (1) where R 1 is ethyl, and R of compound (1-1) 1 The above rule also applies to R 3In formula (1), when a is 2, there are two rings A. In the compound, the two rings represented by the two rings A may be the same or different. When a is greater than 2, the above rule also applies to any two rings A. The above rule also applies to Z 1 , ring C, etc.

[0030] 2-Fluoro-1,4-phenylene refers to the following two divalent groups. In the chemical formula, fluorine can be left-facing (L) or right-facing (R).

[0031] The same rule applies to asymmetric cyclic divalent radicals such as tetrahydropyran-2,5-diyl.

[0032]

[0033] The present invention includes the following items and the like.

[0034] Item 1. A liquid crystal composition comprising as a first component at least one compound selected from the group of compounds represented by formula (1) and as a second component at least one compound selected from the group of compounds represented by formula (2), and having positive dielectric anisotropy,

[0035]

[0036] In formula (1) and formula (2), R 1 is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms; R 2 and R 3 are independently alkenyl groups having 2 to 12 carbon atoms; Ring A and Ring B are independently 1,4-cyclohexylene, 1,4-cyclohexenylene, 1,4-phenylene, 1,4-phenylene in which at least one hydrogen is substituted by fluorine or chlorine, tetrahydropyran-2,5-diyl, 1,3-dioxane-2,5-diyl, pyrimidine-2,5-diyl or pyridine-2,5-diyl, and at least one Ring A is tetrahydropyran-2,5-diyl or 1,3-dioxane-2,5-diyl; 1 and Z 2 X is independently a single bond, ethylene, vinylene, methyleneoxy, carbonyloxy or difluoromethyleneoxy; 1 and X 2 are independently hydrogen or fluorine; Y 1 is fluorine, chlorine, an alkyl group having 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, an alkoxy group having 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, or an alkenyloxy group having 2 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine; a is 1, 2, 3 or 4; b is 0, 1, 2 or 3; and the sum of a and b is 4 or less.

[0037] Item 2. The liquid crystal composition according to Item 1, comprising as a first component at least one compound selected from the group of compounds represented by Formula (1-1) to Formula (1-12),

[0038]

[0039]

[0040]

[0041] In formula (1-1) to formula (1-12), R 1 is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms; X 1 , X 2 , X 3 , X 4 , X 5 , X 6 , X 7 , X 8 , X 9 , X 10 and X 11 are independently hydrogen or fluorine; Y 1 It is fluorine, chlorine, an alkyl group having 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, an alkoxy group having 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, or an alkenyloxy group having 2 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine.

[0042] Item 3. The liquid crystal composition according to Item 1 or Item 2, wherein the proportion of the first component is in the range of 5 wt % to 40 wt %, and the proportion of the second component is in the range of 10 wt % to 70 wt %, based on the weight of the liquid crystal composition.

[0043] Item 4. The liquid crystal composition according to any one of Items 1 to 3, comprising as a third component at least one compound selected from the group of compounds represented by formula (3),

[0044]

[0045] In formula (3), R 4 is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms in which at least one hydrogen atom is substituted by fluorine or chlorine; R 5 is an alkyl group having 1 to 12 carbon atoms or an alkoxy group having 1 to 12 carbon atoms; Ring C and Ring D are independently 1,4-cyclohexylene, 1,4-phenylene, 2-fluoro-1,4-phenylene or 2,5-difluoro-1,4-phenylene; Z 3 is a single bond, ethylene, carbonyloxy or methyleneoxy; c is 1, 2 or 3.

[0046] Item 5. The liquid crystal composition according to any one of Items 1 to 4, comprising as a third component at least one compound selected from the group of compounds represented by Formula (3-1) to Formula (3-13),

[0047]

[0048] In formula (3-1) to formula (3-13), R 4 is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms in which at least one hydrogen atom is substituted by fluorine or chlorine; R 5 It is an alkyl group having 1 to 12 carbon atoms or an alkoxy group having 1 to 12 carbon atoms.

[0049] Item 6. The liquid crystal composition according to Item 4 or Item 5, wherein a ratio of the third component is in a range of 10 wt % to 80 wt % based on the weight of the liquid crystal composition.

[0050] Item 7. The liquid crystal composition according to any one of Items 1 to 6, further comprising as a fourth component at least one compound selected from the group of compounds represented by formula (4),

[0051]

[0052] In formula (4), R 6 is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms; Ring E is 1,4-cyclohexylene, 1,4-phenylene, 2-fluoro-1,4-phenylene, 2,3-difluoro-1,4-phenylene, 2,6-difluoro-1,4-phenylene, tetrahydropyran-2,5-diyl, 1,3-dioxane-2,5-diyl, or pyrimidine-2,5-diyl; 4 is a single bond, ethylene, carbonyloxy or difluoromethyleneoxy; X 12 and X 13 are independently hydrogen or fluorine; Y 2 is fluorine, chlorine, an alkyl group with 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, an alkoxy group with 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, or an alkenyloxy group with 2 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine; d is 1, 2, 3 or 4; wherein, when Z 4 When it is a difluoromethyleneoxy group, ring E is 1,4-cyclohexylene, 1,4-phenylene, 2-fluoro-1,4-phenylene, 2,3-difluoro-1,4-phenylene, 2,6-difluoro-1,4-phenylene or pyrimidine-2,5-diyl.

[0053] Item 8. The liquid crystal composition according to any one of Items 1 to 7, comprising as a fourth component at least one compound selected from the group of compounds represented by Formula (4-1) to Formula (4-30),

[0054]

[0055]

[0056]

[0057]

[0058] In formula (4-1) to formula (4-30), R 6 It is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms.

[0059] Item 9. The liquid crystal composition according to Item 7 or Item 8, wherein a ratio of the fourth component is in a range of 2% by weight to 45% by weight based on the weight of the liquid crystal composition.

[0060] Item 10. The liquid crystal composition according to any one of Items 1 to 9, comprising as a fifth component at least one compound selected from the group of compounds represented by formula (5),

[0061]

[0062] In formula (5), R 7 and R 8 are independently alkyl having 1 to 12 carbon atoms, alkoxy having 1 to 12 carbon atoms, alkenyl having 2 to 12 carbon atoms, or alkenyloxy having 2 to 12 carbon atoms; Ring F and Ring I are independently 1,4-cyclohexylene, 1,4-cyclohexenylene, 1,4-phenylene, 1,4-phenylene in which at least one hydrogen is substituted by fluorine or chlorine, or tetrahydropyran-2,5-diyl; Ring G is 2,3-difluoro-1,4-phenylene, 2-chloro-3-fluoro-1,4-phenylene, 2,3-difluoro-5-methyl-1,4-phenylene, 3,4,5-trifluoronaphthalene-2,6-diyl, or 7,8-difluorochromane-2,6-diyl; 5 and Z 6 are independently a single bond, ethylene, carbonyloxy or methyleneoxy; e is 1, 2 or 3, f is 0 or 1; and the sum of e and f is 3 or less.

[0063] Item 11. The liquid crystal composition according to any one of Items 1 to 10, comprising as a fifth component at least one compound selected from the group of compounds represented by Formula (5-1) to Formula (5-22),

[0064]

[0065]

[0066] In formula (5-1) to formula (5-22), R 7 and R 8 They are independently alkyl having 1 to 12 carbon atoms, alkoxy having 1 to 12 carbon atoms, alkenyl having 2 to 12 carbon atoms, or alkenyloxy having 2 to 12 carbon atoms.

[0067] Item 12. The liquid crystal composition according to Item 10 or Item 11, wherein a proportion of the fifth component is in a range of 3 wt % to 30 wt % based on the weight of the liquid crystal composition.

[0068] Item 13. A liquid crystal composition according to any one of Items 1 to Item 12, wherein the upper limit temperature of the nematic phase is above 70°C, the optical anisotropy at a wavelength of 589 nm (measured at 25°C) is above 0.07, and the dielectric anisotropy at a frequency of 1 kHz (measured at 25°C) is above 2.

[0069] Item 14. A liquid crystal display element comprising the liquid crystal composition according to any one of Items 1 to 13.

[0070] Item 15. A liquid crystal display element according to Item 14, wherein an operation mode of the liquid crystal display element is a TN mode, an ECB mode, an OCB mode, an IPS mode, an FFS mode or an FPA mode, and a driving mode of the liquid crystal display element is an active matrix mode.

[0071] Item 16. Use of the liquid crystal composition according to any one of Items 1 to 13 in a liquid crystal display element.

[0072] The present invention also includes the following items. (a) The composition, which further contains at least one additive such as an optically active compound, an antioxidant, an ultraviolet absorber, a pigment, a defoaming agent, a polymerizable compound, a polymerization initiator, a polymerization inhibitor, a polar compound, etc. (b) An AM element, which contains the composition. (c) The composition and a polymer-stabilized alignment (PSA) type AM element containing the composition, wherein the composition further contains a polymerizable compound. (d) A polymer-stabilized alignment (PSA) type AM element, which contains the composition, and the polymerizable compound in the composition is polymerized. (e) An element, which contains the composition and has a mode of PC, TN, STN, ECB, OCB, IPS, VA, FFS or FPA. (f) A transmissive element, which contains the composition. (g) Use of the composition as a composition having a nematic phase. (h) Use of the composition as an optically active composition by adding an optically active compound to the composition.

[0073] The composition of the present invention is described in the following order. First, the composition of the component compounds in the composition is described. Second, the main characteristics of the component compounds and the main effects of the compounds on the composition are described. Third, the combination of the components in the composition, the preferred ratio of the components and the basis thereof are described. Fourth, the preferred form of the component compounds is described. Fifth, the preferred component compounds are shown. Sixth, the additives that can be added to the composition are described. Seventh, the synthesis method of the component compounds is described. Finally, the use of the composition is described.

[0074] First, the composition of the component compounds in the composition is described. The composition of the present invention is classified into composition A and composition B. In addition to containing a liquid crystal compound selected from compound (1), compound (2), compound (3), compound (4) and compound (5), composition A may also contain other liquid crystal compounds, additives, etc. "Other liquid crystal compounds" are liquid crystal compounds different from compound (1), compound (2), compound (3), compound (4) and compound (5). Such compounds are mixed in the composition for the purpose of further adjusting the properties. Additives are optically active compounds, antioxidants, ultraviolet absorbers, pigments, defoaming agents, polymerizable compounds, polymerization initiators, polymerization inhibitors, polar compounds, etc.

[0075] Composition B substantially contains only a liquid crystal compound selected from compound (1), compound (2), compound (3), compound (4) and compound (5). "Substantially" means that the composition may contain additives but does not contain other liquid crystal compounds. Compared with composition A, the number of components of composition B is small. From the perspective of reducing costs, composition B is better than composition A. From the perspective of being able to further adjust the characteristics by mixing other liquid crystal compounds, composition A is better than composition B.

[0076] Second, the main characteristics of the component compounds and the main effects of the compounds on the characteristics of the composition are described. Based on the effects of the present invention, the main characteristics of the component compounds are summarized in Table 2. In the symbols of Table 2, L means large or high, M means medium, and S means small or low. The symbols L, M, and S are classifications based on qualitative comparisons between the component compounds, and 0 (zero) means a value of zero, or a value of approximately zero.

[0077] Table 2. Properties of the compounds

[0078]

[0079] 1) The value of dielectric anisotropy is negative, and the sign indicates the magnitude of the absolute value

[0080] When the component compounds are mixed in the composition, the main effects of the component compounds on the properties of the composition are as follows. Compound (1) increases dielectric anisotropy. Compound (2) reduces viscosity. Compound (3) increases the upper limit temperature or reduces the lower limit temperature. Compound (4) reduces the lower limit temperature and increases dielectric anisotropy. Compound (5) increases dielectric anisotropy in the short axis direction.

[0081] Third, the combination of components in the composition, the preferred ratio of the component compounds and the basis thereof are described. The preferred combination of components in the composition is the first component + the second component, the first component + the second component + the third component, the first component + the second component + the fourth component, the first component + the second component + the fifth component, the first component + the second component + the third component + the fourth component, the first component + the second component + the third component + the fifth component, the first component + the second component + the fourth component + the fifth component or the first component + the second component + the third component + the fourth component + the fifth component. A further preferred combination is the first component + the second component + the third component + the fourth component.

[0082] In order to improve the dielectric anisotropy, the preferred ratio of the first component is about 5% by weight or more, and in order to reduce the lower limit temperature, the preferred ratio of the first component is about 40% by weight or less. A further preferred ratio is in the range of about 5% by weight to about 35% by weight. A particularly preferred ratio is in the range of about 5% by weight to about 30% by weight.

[0083] In order to reduce the viscosity, the preferred ratio of the second component is about 10% by weight or more, and in order to improve the dielectric anisotropy, the preferred ratio of the second component is about 70% by weight or less. A further preferred ratio is in the range of about 10% by weight to about 60% by weight. A particularly preferred ratio is in the range of about 15% by weight to about 50% by weight.

[0084] In order to increase the upper limit temperature or to reduce the viscosity, the preferred ratio of the third component is about 10% by weight or more, and in order to increase the dielectric anisotropy, the preferred ratio of the third component is about 80% by weight or less. A further preferred ratio is in the range of about 15% by weight to about 75% by weight. The specific ratio is in the range of about 20% by weight to about 70% by weight.

[0085] In order to improve the dielectric anisotropy, the preferred ratio of the fourth component is about 2 weight % or more, and in order to reduce the lower limit temperature, the preferred ratio of the fourth component is about 45 weight % or less. A further preferred ratio is in the range of about 2 weight % to about 40 weight %. A particularly preferred ratio is in the range of about 2 weight % to about 35 weight %.

[0086] In order to improve the dielectric anisotropy in the short axis direction, the preferred ratio of the fifth component is about 3 weight % or more, and in order to reduce the lower limit temperature, the preferred ratio of the fifth component is about 30 weight % or less. A further preferred ratio is in the range of about 3 weight % to about 20 weight %. A particularly preferred ratio is in the range of about 3 weight % to about 10 weight %.

[0087] Fourth, preferred forms of the component compounds are described. In formula (1), formula (2), formula (3), formula (4) and formula (5), R 1 and R 6 are independently an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms. In order to improve the stability to ultraviolet rays or heat, preferably R 1 or R 6 is an alkyl group having 1 to 12 carbon atoms. 2 and R 3 R is independently an alkenyl group having 2 to 12 carbon atoms. 4 is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms in which at least one hydrogen atom is substituted by fluorine or chlorine. In order to improve the stability to ultraviolet light or heat, preferably R 4 is an alkyl group with 1 to 12 carbon atoms. In order to reduce the lower temperature limit, preferably R 4 is an alkenyl group having 2 to 12 carbon atoms. 5 is an alkyl group having 1 to 12 carbon atoms or an alkoxy group having 1 to 12 carbon atoms. In order to improve the stability to ultraviolet rays or heat, R 5 is an alkyl group having 1 to 12 carbon atoms. 7 and R 8 are independently an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, or an alkenyloxy group having 2 to 12 carbon atoms. In order to improve the stability to ultraviolet rays or heat, preferably R 7 or R 8 is an alkyl group with 1 to 12 carbon atoms. In order to improve the dielectric anisotropy, preferably R 7 or R 8 It is an alkoxy group having 1 to 12 carbon atoms.

[0088] Preferred alkyl groups are methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl or octyl. In order to reduce the viscosity, further preferred alkyl groups are ethyl, propyl, butyl, pentyl or heptyl.

[0089] Preferred alkoxy groups are methoxy, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy or heptyloxy. In order to reduce the viscosity, further preferred alkoxy groups are methoxy or ethoxy.

[0090] Preferred alkenyl groups are vinyl, 1-propenyl, 2-propenyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, 1-hexenyl, 2-hexenyl, 3-hexenyl, 4-hexenyl or 5-hexenyl. In order to reduce viscosity, further preferred alkenyl groups are vinyl, 1-propenyl, 3-butenyl or 3-pentenyl. The preferred stereo configuration of -CH=CH- in these alkenyl groups depends on the position of the double bond. For reasons such as reducing viscosity, trans configuration is preferred in alkenyl groups such as 1-propenyl, 1-butenyl, 1-pentenyl, 1-hexenyl, 3-pentenyl and 3-hexenyl. Cis configuration is preferred in alkenyl groups such as 2-butenyl, 2-pentenyl and 2-hexenyl. Among these alkenyl groups, straight-chain alkenyl groups are preferred over branched alkenyl groups.

[0091] Preferred alkenyloxy groups are vinyloxy, allyloxy, 3-butenyloxy, 3-pentenyloxy or 4-pentenyloxy. In order to reduce the viscosity, further preferred alkenyloxy groups are allyloxy or 3-butenyloxy.

[0092] Preferred examples of the alkyl group in which at least one hydrogen is substituted with fluorine or chlorine are fluoromethyl, 2-fluoroethyl, 3-fluoropropyl, 4-fluorobutyl, 5-fluoropentyl, 6-fluorohexyl, 7-fluoroheptyl or 8-fluorooctyl. In order to improve dielectric anisotropy, further preferred examples are 2-fluoroethyl, 3-fluoropropyl, 4-fluorobutyl or 5-fluoropentyl.

[0093] Preferred examples of alkenyl groups in which at least one hydrogen is substituted with fluorine or chlorine are 2,2-difluorovinyl, 3,3-difluoro-2-propenyl, 4,4-difluoro-3-butenyl, 5,5-difluoro-4-pentenyl or 6,6-difluoro-5-hexenyl. Further preferred examples are 2,2-difluorovinyl or 4,4-difluoro-3-butenyl in order to reduce the viscosity.

[0094] Ring A and Ring B are independently 1,4-cyclohexylene, 1,4-cyclohexenylene, 1,4-phenylene, 1,4-phenylene in which at least one hydrogen is substituted by fluorine or chlorine, tetrahydropyran-2,5-diyl, 1,3-dioxane-2,5-diyl, pyrimidine-2,5-diyl or pyridine-2,5-diyl, wherein at least one Ring A is tetrahydropyran-2,5-diyl or 1,3-dioxane-2,5-diyl. In order to improve the optical anisotropy, the preferred Ring A or Ring B is 1,4-phenylene, 2-fluoro-1,4-phenylene or 2,6-difluoro-1,4-phenylene, and in order to improve the dielectric anisotropy, the preferred Ring A or Ring B is tetrahydropyran-2,5-diyl or 1,3-dioxane-2,5-diyl. Ring C and Ring D are independently 1,4-cyclohexylene, 1,4-phenylene, 2-fluoro-1,4-phenylene or 2,5-difluoro-1,4-phenylene. In order to reduce the viscosity or to increase the upper limit temperature, the preferred ring C or ring D is 1,4-cyclohexylene, and in order to increase the optical anisotropy, the preferred ring C or ring D is 1,4-phenylene. Ring E is 1,4-cyclohexylene, 1,4-phenylene, 2-fluoro-1,4-phenylene, 2,3-difluoro-1,4-phenylene, 2,6-difluoro-1,4-phenylene, tetrahydropyran-2,5-diyl, 1,3-dioxane-2,5-diyl or pyrimidine-2,5-diyl, wherein when Z 4 When it is a difluoromethyleneoxy group, ring E is 1,4-cyclohexylene, 1,4-phenylene, 2-fluoro-1,4-phenylene, 2,3-difluoro-1,4-phenylene, 2,6-difluoro-1,4-phenylene or pyrimidine-2,5-diyl. In order to increase the optical anisotropy, ring E is preferably 1,4-phenylene or 2-fluoro-1,4-phenylene.

[0095] Ring F and Ring I are independently 1,4-cyclohexylene, 1,4-cyclohexenylene, 1,4-phenylene, 1,4-phenylene in which at least one hydrogen is replaced by fluorine or chlorine, or tetrahydropyran-2,5-diyl. Here, preferred examples of 1,4-phenylene in which at least one hydrogen is replaced by fluorine or chlorine are 2-fluoro-1,4-phenylene, 2,3-difluoro-1,4-phenylene or 2-chloro-3-fluoro-1,4-phenylene. In order to reduce viscosity, the preferred ring F or ring I is 1,4-cyclohexylene, in order to increase dielectric anisotropy, the preferred ring F or ring I is tetrahydropyran-2,5-diyl, and in order to increase optical anisotropy, the preferred ring F or ring I is 1,4-phenylene. Ring G is 2,3-difluoro-1,4-phenylene, 2-chloro-3-fluoro-1,4-phenylene, 2,3-difluoro-5-methyl-1,4-phenylene, 3,4,5-trifluoronaphthalene-2,6-diyl or 7,8-difluorochromane-2,6-diyl. In order to improve the dielectric anisotropy, the preferred ring G is 2,3-difluoro-1,4-phenylene. In order to increase the upper limit temperature, the trans configuration is better than the cis configuration for the stereo configuration related to 1,4-cyclohexylene. Tetrahydropyran-2,5-diyl is

[0096]

[0097] or

[0098]

[0099] , preferably

[0100]

[0101] Z 1 and Z 2 Z is independently a single bond, ethylene, vinyl, methyleneoxy, carbonyloxy or difluoromethyleneoxy. 1 or Z 2 Z is a single bond. 3 Z is a single bond, ethylene, carbonyloxy or methyleneoxy. 3 For a single bond, in order to reduce the lower limit temperature, the preferred Z 3 For ethylene, in order to increase the upper limit temperature, the preferred Z 3 Z is a carbonyl group. 4 Z is a single bond, ethylene, carbonyloxy or difluoromethyleneoxy. 4 is a single bond. In order to improve the dielectric anisotropy, the preferred Z 4 Z is difluoromethyleneoxy. 5 and Z 6 Z is independently a single bond, ethylene, carbonyloxy or methyleneoxy. 5or Z 6 For a single bond, in order to reduce the lower limit temperature, the preferred Z 5 or Z 6 For ethylene, in order to improve the dielectric anisotropy, the preferred Z 5 or Z 6 It is a methyleneoxy group.

[0102] X 1 , X 2 , X 3 , X 4 , X 5 , X 6 , X 7 , X 8 , X 9 , X 10 , X 11 , X 12 and X 13 In order to improve the dielectric anisotropy, the preferred X 1 , X 2 , X 3 , X 4 , X 5 , X 6 , X 7 , X 8 , X 9 , X 10 , X 11 , X 12 or X 13 For fluorine.

[0103] Y 1 and Y 2 is fluorine, chlorine, an alkyl group having 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, an alkoxy group having 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, or an alkenyloxy group having 2 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine. 1 or Y 2 For fluorine.

[0104] a is 1, 2, 3 or 4, b is 0, 1, 2 or 3, and the sum of a and b is 4 or less. In order to increase the dielectric anisotropy, a is preferably 2 or 3. In order to lower the lower limit temperature, b is preferably 0 or 1. c is 1, 2 or 3. In order to lower the viscosity, c is preferably 1, and in order to increase the upper limit temperature, c is preferably 2 or 3. d is 1, 2, 3 or 4. In order to lower the lower limit temperature, d is preferably 2, and in order to increase the dielectric anisotropy, d is preferably 3. e is 1, 2 or 3, f is 0 or 1, and the sum of e and f is 3 or less. In order to lower the viscosity, e is preferably 1, and in order to increase the upper limit temperature, e is preferably 2 or 3. In order to lower the viscosity, f is preferably 0, and in order to lower the lower limit temperature, f is preferably 1.

[0105] Preferred compound (1) is compound (1-1) to compound (1-12) described in item 2. Among these compounds, it is preferred that at least one of the first components is compound (1-2), compound (1-5), compound (1-7), compound (1-8) or compound (1-11). It is preferred that at least two of the first components are a combination of compound (1-2) and compound (1-5), compound (1-2) and compound (1-7), compound (1-2) and compound (1-8), compound (1-5) and compound (1-7), compound (1-5) and compound (1-8), or compound (1-7) and compound (1-8).

[0106] Preferred compound (3) is compound (3-1) to compound (3-13) described in item 5. Among these compounds, it is preferred that at least one of the third components is compound (3-1), compound (3-3), compound (3-5), compound (3-6), compound (3-8) or compound (3-13). It is preferred that at least two of the third components are a combination of compound (3-1) and compound (3-3), compound (3-1) and compound (3-5), compound (3-1) and compound (3-8) or compound (3-3) and compound (3-5).

[0107] Preferred compound (4) is compound (4-1) to compound (4-30) described in item 8. Among these compounds, it is preferred that at least one of the fourth components is compound (4-2), compound (4-8), compound (4-9), compound (4-11), compound (4-13), compound (4-14), compound (4-15), compound (4-16), compound (4-20), compound (4-21), compound (4-22), compound (4-24), compound (4-25) or compound (4-26). It is preferred that at least two of the fourth components are a combination of compound (4-9) and compound (4-13), compound (4-11) and compound (4-13), compound (4-13) and compound (4-14), compound (4-13) and compound (4-20), compound (4-21) and compound (4-24), or compound (4-22) and compound (4-24).

[0108] Preferred compound (5) is compound (5-1) to compound (5-22) described in item 11. Among these compounds, it is preferred that at least one of the fifth components is compound (5-1), compound (5-3), compound (5-4), compound (5-6), compound (5-8) or compound (5-10). It is preferred that at least two of the fifth components are a combination of compound (5-1) and compound (5-6), compound (5-1) and compound (5-10), compound (5-3) and compound (5-8), compound (5-4) and compound (5-6), compound (5-4) and compound (5-8), or compound (5-4) and compound (5-10).

[0109] Sixth, the additives that can be added to the composition are described. Such additives are optically active compounds, antioxidants, ultraviolet absorbers, pigments, defoamers, polymerizable compounds, polymerization initiators, polymerization inhibitors, polar compounds, etc. For the purpose of causing the helical structure of the liquid crystal to impart a torsion angle, the optically active compound is added to the composition. Examples of such compounds are compounds (6-1) to (6-5). The preferred ratio of the optically active compound is about 5% by weight or less. A further preferred ratio is in the range of about 0.01% by weight to about 2% by weight.

[0110]

[0111] An antioxidant is added to the composition in order to prevent a decrease in specific resistance due to heating in the atmosphere or to maintain a large voltage holding ratio not only at room temperature but also at a temperature close to the upper limit temperature after the element has been used for a long time.

[0112] Preferred examples of the antioxidant include compound (7) wherein t is an integer of 1 to 9, and the like.

[0113]

[0114] In compound (7), preferably t is 1, 3, 5, 7 or 9. More preferably, t is 7. Compound (7) in which t is 7 has low volatility and is effective for maintaining a large voltage holding ratio not only at room temperature but also at a temperature close to the upper limit temperature after the element is used for a long time. In order to obtain the above effect, the preferred ratio of the antioxidant is about 50 ppm or more, and in order not to reduce the upper limit temperature or to increase the lower limit temperature, the preferred ratio of the antioxidant is about 600 ppm or less. More preferably, the ratio is in the range of about 100 ppm to about 300 ppm.

[0115] Preferred examples of ultraviolet absorbers include benzophenone derivatives, benzoate derivatives, triazole derivatives, and the like. In addition, light stabilizers such as sterically hindered amines are also preferred. In order to obtain the above-mentioned effects, the preferred ratio of these absorbers or stabilizers is about 50 ppm or more, and in order not to lower the upper limit temperature or to not increase the lower limit temperature, the preferred ratio of these absorbers or stabilizers is about 10,000 ppm or less. A further preferred ratio is in the range of about 100 ppm to about 10,000 ppm.

[0116] In order to be suitable for the elements of the guest host (GH) mode, dichroic dyes such as azo pigments and anthraquinone pigments are added to the composition. The preferred ratio of the pigment is in the range of about 0.01% by weight to about 10% by weight. In order to prevent foaming, defoamers such as dimethyl silicone oil and methylphenyl silicone oil are added to the composition. In order to obtain the above effect, the preferred ratio of the defoamer is about 1ppm or more, and in order to prevent poor display, the preferred ratio of the defoamer is about 1000ppm or less. Furthermore, the preferred ratio is in the range of about 1ppm to about 500ppm.

[0117] In order to be suitable for polymer stable orientation (PSA) type elements, polymerizable compounds are added to the composition. Preferred examples of polymerizable compounds are compounds having polymerizable groups such as acrylates, methacrylates, vinyl compounds, vinyloxy compounds, allyl ethers, epoxy compounds (oxirane, oxetane), vinyl ketones, etc. Preferred examples are derivatives of acrylates or methacrylates. In order to obtain the above effect, the preferred ratio of the polymerizable compound is about 0.05% by weight or more, and in order to prevent poor display, the preferred ratio of the polymerizable compound is about 10% by weight or less. The preferred ratio is in the range of about 0.1% by weight to about 2% by weight. The polymerizable compound is polymerized by ultraviolet irradiation. It can also be polymerized in the presence of an initiator such as a photopolymerization initiator. The appropriate conditions for polymerization, the appropriate type of initiator, and the appropriate amount are known to those skilled in the art and are recorded in the literature. For example, Irgacure 651 (registered trademark; BASF), Irgacure 184 (registered trademark; BASF), or Darocur 1173 (registered trademark; BASF) as a photopolymerization initiator is suitable for free radical polymerization. The preferred ratio of the photopolymerization initiator is in the range of about 0.1 wt % to about 5 wt % based on the weight of the polymerizable compound. A further preferred ratio is in the range of about 1 wt % to about 3 wt %.

[0118] When storing the polymerizable compound, a polymerization inhibitor may be added to prevent polymerization. The polymerizable compound is usually added to the composition without removing the polymerization inhibitor. Examples of the polymerization inhibitor are hydroquinone, hydroquinone derivatives such as methyl hydroquinone, 4-tert-butylcatechol, 4-methoxyphenol, phenothiazine, etc.

[0119] Seventh, the synthesis method of the component compounds is described. These compounds can be synthesized using known methods. Example synthesis methods. Compound (1-4) is synthesized using the method described in the International Publication No. 98-17664 Handbook. Compound (2) is synthesized using the method described in the Japanese Patent Publication No. 59-176221. Compound (3-3) is synthesized using the method described in the Japanese Patent Publication No. 52-53783. Compound (4-2) and compound (4-8) are synthesized using the method described in the Japanese Patent Publication No. 2-233626. Compound (5-1) and compound (5-6) are synthesized using the method described in the Japanese Patent Publication No. 2-503441. Antioxidants are commercially available. The compound in which t is 1 in formula (7) can be obtained from Sigma-Aldrich Corporation. Compound (7) wherein t is 7 and the like are synthesized by the method described in the specification of US Pat. No. 3,660,505.

[0120] Compounds for which no synthesis method is described can be synthesized by methods described in the following books: Organic Syntheses (John Wiley & Sons, Inc.), Organic Reactions (John Wiley & Sons, Inc.), Comprehensive Organic Synthesis (Pergamon Press), New Experimental Chemistry Lectures (Maruzen), etc. The composition is prepared by a known method from the compound obtained in the above manner. For example, the component compounds are mixed and then dissolved in each other by heating.

[0121] Finally, the use of the composition is described. The composition of the present invention mainly has a lower limit temperature of about -10°C or less, an upper limit temperature of about 70°C or more, and an optical anisotropy in the range of about 0.07 to about 0.20. The element containing the composition has a large voltage holding ratio. The composition is suitable for AM elements. The composition is particularly suitable for transmissive AM elements. It is also possible to prepare a composition having an optical anisotropy in the range of about 0.08 to about 0.25 by controlling the ratio of the component compounds or by mixing other liquid crystal compounds, and further prepare a composition having an optical anisotropy in the range of about 0.10 to about 0.30. The composition can be used as a composition having a nematic phase, and can be used as an optically active composition by adding an optically active compound.

[0122] The composition can be used for AM elements. Furthermore, it can also be used for PM elements. The composition can be used for AM elements and PM elements having modes such as PC, TN, STN, ECB, OCB, IPS, FFS, VA, and FPA. It is particularly preferably used for AM elements having TN mode, OCB mode, IPS mode, or FFS mode. In AM elements having IPS mode or FFS mode, when no voltage is applied, the arrangement of liquid crystal molecules can be parallel to the glass substrate, or can also be vertical. These elements can be reflective, transmissive, or semi-transmissive. It is preferably used for transmissive elements. It can also be used for amorphous silicon-TFT elements or polycrystalline silicon-TFT elements. It can also be used for nematic curvilinear aligned phase (NCAP) type elements made by microencapsulating the composition or polymer dispersed (PD) type elements in which a three-dimensional network polymer is formed in the composition.

[0123] Example

[0124] The present invention is further described in detail by examples. The present invention is not limited by these examples. The present invention includes a mixture of the composition of Example 1 and the composition of Example 2. The present invention also includes a mixture of at least two of the compositions of the examples. The synthesized compound is identified by nuclear magnetic resonance (NMR) analysis and other methods. The properties of the compound and the composition are measured by the methods described below.

[0125] NMR analysis: DRX-500 manufactured by Bruker BioSpin was used for the measurement. 1In the H-NMR measurement, the sample is dissolved in a deuterated solvent such as CDCl3, and the measurement is performed at room temperature, 500 MHz, and the number of integrations is 16. Tetramethylsilane is used as an internal standard. 19 In the determination of F-NMR, CFCl3 was used as an internal standard and the cumulative number of measurements was 24. In the description of the nuclear magnetic resonance spectrum, s refers to a singlet, d refers to a doublet, t refers to a triplet, q refers to a quartet, quin refers to a quintet, sex refers to a sextet, m refers to a multiplet, and br refers to a broad peak.

[0126] Gas chromatography analysis: A GC-14B gas chromatograph manufactured by Shimadzu Corporation was used for the measurement. The carrier gas was helium (2 mL / min). The sample vaporization chamber was set to 280°C, and the detector (flame ionization detector (FID)) was set to 300°C. When separating the component compounds, a capillary column DB-1 (length 30 m, inner diameter 0.32 mm, film thickness 0.25 μm; stationary liquid phase was dimethyl polysiloxane; non-polar) manufactured by Agilent Technologies Inc. was used. The column was kept at 200°C for 2 minutes and then heated to 280°C at a rate of 5°C / min. After the sample was prepared as an acetone solution (0.1 wt%), 1 μL of it was injected into the sample vaporization chamber. The recorder was a C-R5A chromatograph assembly (Chromatopac) manufactured by Shimadzu Corporation or its equivalent. The obtained gas chromatogram shows the retention time and peak area of ​​the peak corresponding to the component compounds.

[0127] The solvent used to dilute the sample can be chloroform, hexane, etc. In order to separate the component compounds, the following capillary columns can be used. HP-1 (length 30m, inner diameter 0.32mm, film thickness 0.25μm) manufactured by Agilent Technologies, Rtx-1 (length 30m, inner diameter 0.32mm, film thickness 0.25μm) manufactured by Restek Corporation, BP-1 (length 30m, inner diameter 0.32mm, film thickness 0.25μm) manufactured by SGE International Pty. Ltd. of Australia. For the purpose of preventing the overlap of compound peaks, the capillary column CBP1-M50-025 (length 50m, inner diameter 0.25mm, film thickness 0.25μm) manufactured by Shimadzu Corporation can be used.

[0128] The ratio of the liquid crystal compound contained in the composition can be calculated using the method described below. A mixture of liquid crystal compounds is detected using a gas chromatograph (FID). The area ratio of the peaks in the gas chromatogram is equivalent to the ratio (weight ratio) of the liquid crystal compounds. When using the capillary column described above, the correction coefficient of each liquid crystal compound can be regarded as 1. Therefore, the ratio (weight %) of the liquid crystal compound can be calculated based on the area ratio of the peaks.

[0129] Determination of sample: When measuring the properties of the composition, the composition is directly used as a sample. When measuring the properties of the compound, the sample for measurement is prepared by mixing the compound (15 wt%) in the mother liquid crystal (85 wt%). Based on the value obtained by the measurement, the characteristic value of the compound is calculated by extrapolation. (Extrapolated value) = {(measured value of the sample) - 0.85 × (measured value of the mother liquid crystal)} / 0.15. When the smectic phase (or crystal) precipitates at 25°C under the said ratio, the ratio of the compound to the mother liquid crystal is changed in the order of 10 wt%: 90 wt%, 5 wt%: 95 wt%, 1 wt%: 99 wt%. The extrapolation method is used to obtain the values ​​of the upper limit temperature, optical anisotropy, viscosity and dielectric anisotropy related to the compound.

[0130] The following mother liquid crystals were used. The ratios of the component compounds are expressed in % by weight.

[0131]

[0132] Measurement method: The characteristics were measured using the following methods. Most of these methods are methods described in the JEITA standard (JEITA ED-2521B) reviewed and established by the Japan Electronics and Information Technology Industries Association (hereinafter referred to as JEITA) or modified methods. The TN element used for the measurement does not have a thin film transistor (TFT) mounted on it.

[0133] (1) Upper limit temperature of nematic phase (NI; °C): Place the sample on a hot plate of a melting point measuring device equipped with a polarizing microscope and heat at a rate of 1 °C / min. Measure the temperature at which a portion of the sample changes from the nematic phase to an isotropic liquid.

[0134] (2) The lower limit temperature of the nematic phase (T C; ℃): Place a sample with a nematic phase in a glass bottle and store it in a freezer at 0℃, -10℃, -20℃, -30℃ and -40℃ for 10 days, and then observe the liquid crystal phase. For example, if the sample is in a nematic phase at -20℃ and changes to a crystalline or smectic phase at -30℃, the T C Recorded as <-20°C.

[0135] (3) Viscosity (bulk viscosity; η; measured at 20°C; mPa·s): An E-type rotational viscometer manufactured by Tokyo Keiki Co., Ltd. was used for measurement.

[0136] (4) Viscosity (rotational viscosity; γ1; measured at 25°C; mPa·s): Measured according to the method described in M. Imai et al., Molecular Crystals and Liquid Crystals, Vol. 259, p. 37 (1995). A sample was placed in a TN device having a twist angle of 0° and a distance between two glass substrates (cell gap) of 5 μm. A voltage was applied to the device in steps of 0.5 V in the range of 16 V to 19.5 V. After no voltage was applied for 0.2 seconds, the voltage was repeatedly applied under the conditions of applying only one rectangular wave (rectangular pulse; 0.2 seconds) and no voltage (2 seconds). The peak current and peak time of the transient current generated by the application were measured. The rotational viscosity value was obtained from these measured values ​​and the calculation formula (8) described on p. 40 of the paper by M. Imai et al. The value of dielectric anisotropy required for the calculation is obtained by the method described below using the element for measuring the rotational viscosity.

[0137] (5) Optical anisotropy (refractive index anisotropy; Δn; measured at 25°C): Measured using light of a wavelength of 589 nm using an Abbe refractometer with a polarizing plate mounted on the eyepiece. After rubbing the surface of the main prism in one direction, drop the sample onto the main prism. The refractive index n∥ is measured when the direction of polarization is parallel to the direction of rubbing. The refractive index n⊥ is measured when the direction of polarization is perpendicular to the direction of rubbing. The value of optical anisotropy is calculated based on the formula Δn = n∥ - n⊥.

[0138] (6) Dielectric anisotropy (Δε; measured at 25°C): A sample was placed in a TN device in which the distance between two glass substrates (cell gap) was 9 μm and the twist angle was 80 degrees. A sine wave (10 V, 1 kHz) was applied to the device, and after 2 seconds, the dielectric constant (ε∥) in the long axis direction of the liquid crystal molecules was measured. A sine wave (0.5 V, 1 kHz) was applied to the device, and after 2 seconds, the dielectric constant (ε⊥) in the short axis direction of the liquid crystal molecules was measured. The value of dielectric anisotropy was calculated based on the formula Δε=ε∥-ε⊥.

[0139] (7) Threshold voltage (Vth; measured at 25°C; V): The measurement was performed using an LCD5100 luminance meter manufactured by Otsuka Electronics Co., Ltd. The light source was a halogen lamp. The sample was placed in a normally white mode TN element in which the distance between the two glass substrates (cell gap) was 0.45 / Δn (μm) and the twist angle was 80 degrees. The voltage applied to the element (32 Hz, rectangular wave) was increased stepwise from 0 V to 10 V in units of 0.02 V. At this time, light was irradiated to the element from a vertical direction, and the amount of light passing through the element was measured. A voltage-transmittance curve was prepared in which the transmittance was 100% when the light amount reached a maximum, and the transmittance was 0% when the light amount was a minimum. The threshold voltage is represented by the voltage when the transmittance reaches 90%.

[0140] (8) Voltage holding ratio (VHR-1; measured at 25°C; %): The TN element used in the measurement has a polyimide orientation film, and the interval between the two glass substrates (cell gap) is 5 μm. After the sample is added, the element is sealed with an adhesive that cures with ultraviolet light. A pulse voltage (5 V, 60 microseconds) is applied to the TN element for charging. The attenuated voltage is measured during 16.7 milliseconds using a high-speed voltmeter, and the area A between the voltage curve and the horizontal axis in a unit period is calculated. Area B is the area when there is no attenuation. The voltage holding ratio is expressed as a percentage of area A relative to area B.

[0141] (9) Voltage Holding Ratio (VHR-2; measured at 80°C; %): The voltage holding ratio was measured in the same manner as described above, except that the measurement was conducted at 80°C instead of 25°C. The obtained value is represented as VHR-2.

[0142] (10) Voltage holding ratio (VHR-3; measured at 25°C; %): After irradiation with ultraviolet rays, the voltage holding ratio is measured to evaluate the stability against ultraviolet rays. The TN element used in the measurement has a polyimide orientation film and a cell gap of 5 μm. The sample is injected into the element and irradiated with light for 20 minutes. The light source is an ultra-high pressure mercury lamp USH-500D (manufactured by USHIO Electric), and the distance between the element and the light source is 20 cm. In the measurement of VHR-3, the attenuated voltage is measured during 16.7 milliseconds. A composition having a large VHR-3 has a large stability against ultraviolet rays. VHR-3 is preferably 90% or more, more preferably 95% or more.

[0143] (11) Voltage holding ratio (VHR-4; measured at 25°C; %): After heating the TN device injected with the sample in a thermostatic chamber at 80°C for 500 hours, the voltage holding ratio was measured to evaluate the thermal stability. In the measurement of VHR-4, the voltage decayed during 16.7 milliseconds was measured. A composition having a large VHR-4 has a high thermal stability.

[0144] (12) Response time (τ; measured at 25°C; ms): The measurement was performed using an LCD5100 luminance meter manufactured by Otsuka Electronics Co., Ltd. The light source was a halogen lamp. The low-pass filter was set to 5 kHz. A sample was placed in a normally white mode TN element in which the distance between two glass substrates (cell gap) was 5.0 μm and the twist angle was 80 degrees. A rectangular wave (60 Hz, 5 V, 0.5 seconds) was applied to the element. At this time, light was irradiated to the element from a vertical direction, and the amount of light passing through the element was measured. When the amount of light reached a maximum, the transmittance was considered to be 100%, and when the amount of light reached a minimum, the transmittance was considered to be 0%. The rise time (τr: rise time; milliseconds) is the time required for the transmittance to change from 90% to 10%. The fall time (τf: fall time; milliseconds) is the time required for the transmittance to change from 10% to 90%. The response time is represented by the sum of the rise time and fall time calculated in the above manner.

[0145] (13) Elastic constant (K; measured at 25°C; pN): The measurement was performed using an HP4284A LCR tester manufactured by Yokogawa Hewlett-Packard Co., Ltd. A sample was placed in a horizontally oriented element with a spacing (cell gap) of 20 μm between two glass substrates. A charge of 0 volts to 20 volts was applied to the element, and the electrostatic capacitance and applied voltage were measured. Using equations (2.98) and (2.101) on page 75 of the Liquid Crystal Device Handbook (Nikkan Kogyo Shimbun Co., Ltd.), the measured electrostatic capacitance (C) and the applied voltage (V) values ​​were fitted, and the values ​​of K11 and K33 were obtained according to equation (2.99). K22 was then calculated using the previously determined values ​​of K11 and K33 in equation (3.18) on page 171 of the Liquid Crystal Device Handbook (Nikkan Kogyo Shimbun Co., Ltd.). The elastic constant is represented by the average value of K11, K22, and K33 determined in the above manner.

[0146] (14) Specific resistance (ρ; measured at 25°C; Ωcm): 1.0 mL of a sample is injected into a container equipped with electrodes. A DC voltage (10 V) is applied to the container, and the DC current is measured after 10 seconds. The specific resistance is calculated according to the following formula: (Specific resistance) = {(voltage) × (capacitance of container)} / {(DC current) × (dielectric constant of vacuum)}.

[0147] (15) Helical pitch (P; measured at room temperature; μm): The helical pitch is measured using the wedge method. Refer to "Liquid Crystal Handbook" page 196 (published in 2000, Maruzen). The sample is injected into the wedge unit and allowed to stand at room temperature for 2 hours. The spacing (d2-d1) of the disclination lines is then observed using a polarizing microscope (Nikon Co., Ltd., trade name MM40 / 60 series). The helical pitch (P) is calculated using the following formula where the angle of the wedge unit is represented by θ. P = 2×(d2-d1)×tanθ.

[0148] (16) Dielectric constant in the short axis direction (ε⊥; measured at 25°C): A sample was placed in a TN device with a distance between two glass substrates (cell gap) of 9 μm and a twist angle of 80 degrees. A sine wave (0.5 V, 1 kHz) was applied to the device, and after 2 seconds, the dielectric constant (ε⊥) in the short axis direction of the liquid crystal molecules was measured.

[0149] The compounds in the examples are represented by symbols based on the definitions in Table 3 below. In Table 3, the stereo configuration associated with 1,4-cyclohexylene is trans configuration. The numbers in the brackets after the symbols correspond to the numbers of the compounds. The symbol (-) refers to other liquid crystal compounds. The ratio (percentage) of liquid crystal compounds is the weight percentage (wt%) based on the weight of the liquid crystal composition. Finally, the characteristic values ​​of the composition are summarized.

[0150] Table 3. Method of expressing compounds using symbols

[0151] R-(A1)-Z1-……-Z n -(A n )-R'

[0152]

[0153] [Comparative Example 1]

[0154] Composition Example 30 was selected from the compositions disclosed in the brochure of International Publication No. 2004-48501. The reason for this is that the composition contains compound (1-5) and has the lowest rotational viscosity. The components and properties of the composition are as follows.

[0155]

[0156] NI=75.5℃; Tc<-20℃; Δn=0.0975; Δε=8.4; Vth=1.28V; γ1=67.0mPa·s.

[0157] [Example 1]

[0158] For comparison, according to Comparative Example 1, a composition obtained by replacing the fourth component compound (3-1), which is a similar compound to compound (2), with the second component compound (2) was designated as Example 1.

[0159]

[0160] NI=72.0℃; Tc<-20℃; Δn=0.101; Δε=6.5; Vth=1.46V; η=11.6mPa·s; γ1=56.8mPa·s.

[0161] [Comparative Example 2]

[0162] Composition Example 2 was selected from the compositions disclosed in Japanese Patent Laid-Open No. 2010-275390. The reason for this is that the composition contains compound (2) and has the largest dielectric anisotropy. The components and properties of the composition are as follows.

[0163]

[0164]

[0165] NI=75.1℃; Tc<-20℃; Δn=0.091; Δε=3.2; Vth=2.38V; eta=11.8mPa·s; γ1=46.8mPa·s.

[0166] [Example 2]

[0167] For comparison, according to Comparative Example 2, similar compounds of compound (1), namely, the fourth component compound (4-16), compound (4-22), and compound (4) are replaced with the first component compound (1-1) and compound (1-5), and the resulting composition is set as Example 2.

[0168]

[0169] NI=73.4℃; Tc<-20℃; Δn=0.086; Δε=3.9; Vth=2.04V; η=14.1mPa·s; γ1=52.0mPa·s.

[0170] [Example 3]

[0171] For comparison, according to Comparative Example 2, similar compounds of compound (1), namely, the fourth component compound (4-16), compound (4-22), and compound (4) are replaced with the first component compound (1-2) and compound (1-8), and the resulting composition is set as Example 3.

[0172]

[0173]

[0174] NI=73.3℃; Tc<-20℃; Δn=0.089; Δε=6.0; Vth=1.57V; eta=14.1mPa·s; γ1=55.7mPa·s.

[0175] [Comparative Example 3]

[0176] Composition Example 10 was selected from the compositions disclosed in the pamphlet of International Publication No. 2010-131594. The reason for this is that the composition contains compound (2) and has the largest dielectric anisotropy. The components and properties of the composition are as follows.

[0177]

[0178] NI=80.3℃; Tc<-20℃; Δn=0.118; Δε=6.0; Vth=1.60V; η=14.3mPa·s; γ1=67.9mPa·s.

[0179] [Example 4]

[0180] For comparison, according to Comparative Example 3, the fourth component compound (4-8) was replaced with the first component compound (1-1), and the resulting composition was designated as Example 4.

[0181]

[0182] NI=74.6℃; Tc<-20℃; Δn=0.110; Δε=7.1; Vth=1.42V; η=12.4mPa·s; γ1=58.0mPa·s.

[0183] [Example 5]

[0184] For comparison, according to Comparative Example 3, the fourth component compound (4-8) was replaced with the first component compound (1-2), and the obtained composition was designated as Example 5.

[0185]

[0186] NI=75.4℃; Tc<-20℃; Δn=0.111; Δε=9.3; Vth=1.30V; eta=12.3mPa·s; γ1=57.6mPa·s.

[0187] [Example 6]

[0188]

[0189] NI=71.2℃; Tc<-20℃; Δn=0.101; Δε=5.6; Vth=1.54V; η=13.4mPa·s; γ1=64.7mPa·s.

[0190] [Example 7]

[0191]

[0192] NI=80.8℃; Tc<-20℃; Δn=0.126; Δε=3.6; Vth=1.87V; η=14.2mPa·s; γ1=68.3mPa·s. [Example 8]

[0193]

[0194] NI=82.8℃; Tc<-20℃; Δn=0.097; Δε=4.9; Vth=1.72V; η=14.0mPa·s; γ1=67.3mPa·s. [Example 9]

[0195]

[0196] NI77.6°CTc<-20°Δn60.097Δε65.9Vth61.52Vη613.6mPa·sγ165.7mPa·s.

[0197]

[0198]

[0199] NI678.5°Tc<-20°Δn60.113Δε65.4Vth61.57Vη613.9mPa·sγ166.9mPa·s.

[0200]

[0201] NI680.0°Tc<-20°Δn60.116Δε65.9Vth61.50Vη614.1mPa·sγ168.1mPa·s.

[0202]

[0203] NI691.5°Tc<-20°Δn60.108Δε6.3Vth1.46Vη613.9mPa·sγ167.3mPa·s.

[0204]

[0205] NI670.3°Tc<-20°Δn60.103Δε6.7Vth1.43Vη612.4mPa·sγ1659.8mPa·s.

[0206]

[0207] NI675.5°Tc<-20°Δn60.102Δε65.3:Vth61.59Vη613.5mPa·sγ164.9mPa·s.

[0208]

[0209]

[0210] NI690.3°CTc<-20°Δn60.106Δε64.0Vth61.80Vη613.5mPa·sγ165.2mPa·s.

[0211]

[0212] NI=72.9℃; Tc<-20℃; Δn=0.118; Δε=6.5; Vth=1.44V; η=14.0mPa·s; γ1=67.7mPa·s. [Example 17]

[0213]

[0214] NI=74.5℃; Tc<-20℃; Δn=0.094; Δε=5.7; Vth=1.53V; η=13.2mPa·s; γ1=63.6mPa·s. [Example 18]

[0215]

[0216] NI=86.6℃; Tc<-20℃; Δn=0.109; Δε=6.2; Vth=1.47V; η=13.9mPa·s; γ1=66.9mPa·s. [Example 19]

[0217]

[0218]

[0219] NI=86.6℃; Tc<-20℃; Δn=0.098; Δε=5.0; Vth=1.72V; η=13.0mPa·s; γ1=62.4mPa·s.

[0220] [Example 20]

[0221]

[0222] NI=77.7℃; Tc<-20℃; Δn=0.105; Δε=5.0; Vth=1.68V; eta=10.8mPa·s; γ1=53.1mPa·s.

[0223] The composition of Example 1 has a smaller rotational viscosity than the composition of Comparative Example 1. The compositions of Examples 2 and 3 have a larger dielectric anisotropy than the composition of Comparative Example 2, and the compositions of Examples 4 and 5 have a larger dielectric anisotropy than the composition of Comparative Example 3. Therefore, it can be concluded that the liquid crystal composition of the present invention has excellent characteristics.

[0224] Industrial Applicability

[0225] The liquid crystal composition of the present invention fully satisfies at least one characteristic or has a proper balance with respect to at least two characteristics among the characteristics of high upper limit temperature, low lower limit temperature, low viscosity, appropriate optical anisotropy, large dielectric anisotropy, large specific resistance, high stability to ultraviolet rays, high stability to heat, and large elastic constant. The liquid crystal display element containing the composition has the characteristics of short response time, large voltage holding ratio, large contrast ratio, long life, etc., and can therefore be used in liquid crystal projectors, liquid crystal televisions, etc.

Claims

1. A liquid crystal composition comprising as a first component at least one compound selected from the compounds represented by formula (1) and as a second component at least one compound selected from the compounds represented by formula (2), and having positive dielectric anisotropy, In formula (1) and formula (2), R 1 is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms; R 2 and R 3 are independently alkenyl groups having 2 to 12 carbon atoms; Ring A and Ring B are independently 1,4-cyclohexylene, 1,4-cyclohexenylene, 1,4-phenylene, 1,4-phenylene in which at least one hydrogen is substituted by fluorine or chlorine, tetrahydropyran-2,5-diyl, 1,3-dioxane-2,5-diyl, pyrimidine-2,5-diyl or pyridine-2,5-diyl, and at least one Ring A is tetrahydropyran-2,5-diyl or 1,3-dioxane-2,5-diyl; 1 and Z 2 X is independently a single bond, ethylene, vinylene, methyleneoxy, carbonyloxy or difluoromethyleneoxy; 1 and X 2 are independently hydrogen or fluorine; Y 1 is fluorine, chlorine, an alkyl group having 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, an alkoxy group having 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, or an alkenyloxy group having 2 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine; a is 1, 2, 3 or 4; b is 0, 1, 2 or 3; and the sum of a and b is 4 or less.

2. The liquid crystal composition according to claim 1, comprising as a first component at least one compound selected from the group consisting of compounds represented by formula (1-1) to formula (1-12), In formula (1-1) to formula (1-12), R 1 is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms; X 1 , X 2 , X 3 , X 4 , X 5 , X 6 , X 7 , X 8 , X 9 , X 10 and X 11 are independently hydrogen or fluorine; Y 1It is fluorine, chlorine, an alkyl group having 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, an alkoxy group having 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, or an alkenyloxy group having 2 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine. 3 . The liquid crystal composition according to claim 1 , wherein the proportion of the first component is in the range of 5 wt % to 40 wt %, and the proportion of the second component is in the range of 10 wt % to 70 wt %, based on the weight of the liquid crystal composition.

4. The liquid crystal composition according to claim 1, comprising as a third component at least one compound selected from the group consisting of compounds represented by formula (3), In formula (3), R 4 is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms in which at least one hydrogen atom is substituted by fluorine or chlorine; R 5 is an alkyl group having 1 to 12 carbon atoms or an alkoxy group having 1 to 12 carbon atoms; Ring C and Ring D are independently 1,4-cyclohexylene, 1,4-phenylene, 2-fluoro-1,4-phenylene or 2,5-difluoro-1,4-phenylene; Z 3 is a single bond, ethylene, carbonyloxy or methyleneoxy; c is 1, 2 or 3.

5. The liquid crystal composition according to claim 4, comprising as a third component at least one compound selected from the group consisting of compounds represented by formula (3-1) to formula (3-13), In formula (3-1) to formula (3-13), R 4 is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms in which at least one hydrogen atom is substituted by fluorine or chlorine; R 5 It is an alkyl group having 1 to 12 carbon atoms or an alkoxy group having 1 to 12 carbon atoms. 6 . The liquid crystal composition according to claim 4 , wherein a ratio of the third component is in a range of 10 wt % to 80 wt % based on the weight of the liquid crystal composition.

7. The liquid crystal composition according to claim 1, further comprising as a fourth component at least one compound selected from the group consisting of compounds represented by formula (4), In formula (4), R 6is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms; Ring E is 1,4-cyclohexylene, 1,4-phenylene, 2-fluoro-1,4-phenylene, 2,3-difluoro-1,4-phenylene, 2,6-difluoro-1,4-phenylene, tetrahydropyran-2,5-diyl, 1,3-dioxane-2,5-diyl, or pyrimidine-2,5-diyl; 4 is a single bond, ethylene, carbonyloxy or difluoromethyleneoxy; X 12 and X 13 are independently hydrogen or fluorine; Y 2 is fluorine, chlorine, an alkyl group with 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, an alkoxy group with 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, or an alkenyloxy group with 2 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine; d is 1, 2, 3 or 4; wherein, When Z 4 When it is a difluoromethyleneoxy group, ring E is 1,4-cyclohexylene, 1,4-phenylene, 2-fluoro-1,4-phenylene, 2,3-difluoro-1,4-phenylene, 2,6-difluoro-1,4-phenylene or pyrimidine-2,5-diyl.

8. The liquid crystal composition according to claim 7, comprising as a fourth component at least one compound selected from the group consisting of compounds represented by formula (4-1) to formula (4-30), In formula (4-1) to formula (4-30), R 6 It is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms. 9 . The liquid crystal composition according to claim 7 , wherein a ratio of the fourth component is in a range of 2 wt % to 45 wt % based on the weight of the liquid crystal composition.

10. The liquid crystal composition according to claim 4, further comprising as a fourth component at least one compound selected from the group consisting of compounds represented by formula (4), In formula (4), R 6 is an alkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, or an alkenyl group having 2 to 12 carbon atoms; Ring E is 1,4-cyclohexylene, 1,4-phenylene, 2-fluoro-1,4-phenylene, 2,3-difluoro-1,4-phenylene, 2,6-difluoro-1,4-phenylene, tetrahydropyran-2,5-diyl, 1,3-dioxane-2,5-diyl, or pyrimidine-2,5-diyl; 4 is a single bond, ethylene, carbonyloxy or difluoromethyleneoxy; X 12 and X 13 are independently hydrogen or fluorine; Y 2is fluorine, chlorine, an alkyl group with 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, an alkoxy group with 1 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine, or an alkenyloxy group with 2 to 12 carbon atoms in which at least one hydrogen is replaced by fluorine or chlorine; d is 1, 2, 3 or 4; wherein, When Z 4 When it is a difluoromethyleneoxy group, ring E is 1,4-cyclohexylene, 1,4-phenylene, 2-fluoro-1,4-phenylene, 2,3-difluoro-1,4-phenylene, 2,6-difluoro-1,4-phenylene or pyrimidine-2,5-diyl.

11. The liquid crystal composition according to claim 1, comprising as a fifth component at least one compound selected from the group consisting of compounds represented by formula (5), In formula (5), R 7 and R 8 are independently alkyl having 1 to 12 carbon atoms, alkoxy having 1 to 12 carbon atoms, alkenyl having 2 to 12 carbon atoms, or alkenyloxy having 2 to 12 carbon atoms; Ring F and Ring I are independently 1,4-cyclohexylene, 1,4-cyclohexenylene, 1,4-phenylene, 1,4-phenylene in which at least one hydrogen is substituted by fluorine or chlorine, or tetrahydropyran-2,5-diyl; Ring G is 2,3-difluoro-1,4-phenylene, 2-chloro-3-fluoro-1,4-phenylene, 2,3-difluoro-5-methyl-1,4-phenylene, 3,4,5-trifluoronaphthalene-2,6-diyl, or 7,8-difluorochromane-2,6-diyl; 5 and Z 6 are independently a single bond, ethylene, carbonyloxy or methyleneoxy; e is 1, 2 or 3, f is 0 or 1; and the sum of e and f is 3 or less.

12. The liquid crystal composition according to claim 11, comprising as a fifth component at least one compound selected from the group consisting of compounds represented by formula (5-1) to formula (5-22), In formula (5-1) to formula (5-22), R 7 and R 8 They are independently alkyl having 1 to 12 carbon atoms, alkoxy having 1 to 12 carbon atoms, alkenyl having 2 to 12 carbon atoms, or alkenyloxy having 2 to 12 carbon atoms. 13 . The liquid crystal composition according to claim 11 , wherein a ratio of the fifth component is in a range of 3 wt % to 30 wt % based on the weight of the liquid crystal composition.

14. The liquid crystal composition according to claim 4, comprising as a fifth component at least one compound selected from the group consisting of compounds represented by formula (5), In formula (5), R 7 and R 8are independently alkyl having 1 to 12 carbon atoms, alkoxy having 1 to 12 carbon atoms, alkenyl having 2 to 12 carbon atoms, or alkenyloxy having 2 to 12 carbon atoms; Ring F and Ring I are independently 1,4-cyclohexylene, 1,4-cyclohexenylene, 1,4-phenylene, 1,4-phenylene in which at least one hydrogen is substituted by fluorine or chlorine, or tetrahydropyran-2,5-diyl; Ring G is 2,3-difluoro-1,4-phenylene, 2-chloro-3-fluoro-1,4-phenylene, 2,3-difluoro-5-methyl-1,4-phenylene, 3,4,5-trifluoronaphthalene-2,6-diyl, or 7,8-difluorochromane-2,6-diyl; 5 and Z 6 are independently a single bond, ethylene, carbonyloxy or methyleneoxy; e is 1, 2 or 3, f is 0 or 1; and the sum of e and f is 3 or less.

15. The liquid crystal composition according to claim 7, comprising as a fifth component at least one compound selected from the group consisting of compounds represented by formula (5), In formula (5), R 7 and R 8 are independently alkyl having 1 to 12 carbon atoms, alkoxy having 1 to 12 carbon atoms, alkenyl having 2 to 12 carbon atoms, or alkenyloxy having 2 to 12 carbon atoms; Ring F and Ring I are independently 1,4-cyclohexylene, 1,4-cyclohexenylene, 1,4-phenylene, 1,4-phenylene in which at least one hydrogen is substituted by fluorine or chlorine, or tetrahydropyran-2,5-diyl; Ring G is 2,3-difluoro-1,4-phenylene, 2-chloro-3-fluoro-1,4-phenylene, 2,3-difluoro-5-methyl-1,4-phenylene, 3,4,5-trifluoronaphthalene-2,6-diyl, or 7,8-difluorochromane-2,6-diyl; 5 and Z 6 are independently a single bond, ethylene, carbonyloxy or methyleneoxy; e is 1, 2 or 3, f is 0 or 1; and the sum of e and f is 3 or less.

16. The liquid crystal composition according to claim 10, comprising as a fifth component at least one compound selected from the group consisting of compounds represented by formula (5), In formula (5), R 7 and R 8are independently alkyl having 1 to 12 carbon atoms, alkoxy having 1 to 12 carbon atoms, alkenyl having 2 to 12 carbon atoms, or alkenyloxy having 2 to 12 carbon atoms; Ring F and Ring I are independently 1,4-cyclohexylene, 1,4-cyclohexenylene, 1,4-phenylene, 1,4-phenylene in which at least one hydrogen is substituted by fluorine or chlorine, or tetrahydropyran-2,5-diyl; Ring G is 2,3-difluoro-1,4-phenylene, 2-chloro-3-fluoro-1,4-phenylene, 2,3-difluoro-5-methyl-1,4-phenylene, 3,4,5-trifluoronaphthalene-2,6-diyl, or 7,8-difluorochromane-2,6-diyl; 5 and Z 6 are independently a single bond, ethylene, carbonyloxy or methyleneoxy; e is 1, 2 or 3, f is 0 or 1; and the sum of e and f is 3 or less.

17. The liquid crystal composition according to claim 1, wherein the upper limit temperature of the nematic phase is above 70°C, the optical anisotropy at a wavelength of 589 nm measured at 25°C is above 0.07, and the dielectric anisotropy at a frequency of 1 kHz measured at 25°C is above 2.

18. A liquid crystal display element comprising the liquid crystal composition according to claim 1.

19. The liquid crystal display element according to claim 18, wherein the operation mode of the liquid crystal display element is a twisted nematic mode, an electrically controlled birefringence mode, an optically compensated bending mode, an in-plane switching mode, a fringe field switching mode or an electric field induced photoreactive orientation mode, and the driving mode of the liquid crystal display element is an active matrix mode.