Oriented silicon steel with uniform magnetic performance and laser nicking method thereof
By superimposing initial and compensating scoring lines on the surface of grain-oriented silicon steel sheets, the problem of uneven magnetic properties caused by uneven laser scoring was solved, resulting in more uniform magnetic properties and a higher iron loss improvement rate.
Patent Information
- Application Number
- CN202411012177.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Existing laser marking methods result in uneven magnetic properties on the surface of grain-oriented silicon steel sheets, mainly due to inconsistent energy density caused by changes in the angle between the laser beam and the sheet surface.
The method of superimposed scoring lines is adopted, including initial scoring lines and compensation scoring lines. The initial scoring lines decrease in energy from the center of the plate to the edge, and the compensation scoring lines gradually decrease in energy from the edge to the center. Two rows of lasers are used for energy compensation to form superimposed scoring lines perpendicular to the rolling direction.
It improves the uniformity of scoring energy on the surface of grain-oriented silicon steel sheets, enhances the uniformity of magnetic properties, improves iron loss by 11% to 13%, reduces magnetic induction loss by 0 to 0.01T, and reduces the difference in iron loss between the edge and the center by 0 to 1%.
Smart Images

Figure CN118910378A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the technical field of grain-oriented silicon steel manufacturing, and in particular to grain-oriented silicon steel with uniform magnetic properties and a laser marking method thereof. Background Technology
[0002] Today, green development and energy efficiency upgrades have become important development directions in the power industry. As a core device in the power transmission system, the transformer's losses affect the power transmission efficiency, and oriented silicon steel, as a key material in transformers, directly affects the transformer's energy efficiency and performance through its magnetic properties.
[0003] In related technologies, in order to reduce the iron loss of grain-oriented silicon steel, i.e., to improve the magnetic properties of grain-oriented silicon steel, the methods of increasing the grain orientation degree of grain-oriented silicon steel and reducing the plate thickness are usually adopted to reduce hysteresis loss and classical eddy current loss. However, with the continuous improvement of grain-oriented silicon steel manufacturing technology, the grain orientation degree of grain-oriented silicon steel has approached the ideal state. At the same time, further reducing the plate thickness will greatly increase the production difficulty. The loss reduction effect of traditional metallurgical methods is very limited. On the other hand, the magnetic domain refinement technology, which reduces anomalous eddy current loss by refining magnetic domains, has gradually become an important development direction. For example, patent CN102477484B discloses a method for rapid marking by simultaneously and interlacing highly focused continuous laser beams on the upper and lower surfaces of a steel strip, achieving an iron loss improvement rate of 10% to 16%. Patent CN102941413B discloses a method for controlling thermal diffusion and melting during laser marking by forming composite superimposed grooves on the surface of grain-oriented silicon steel using front and rear laser scanning, resulting in good stacking coefficient and surface coating adhesion, and preventing iron loss deterioration after stress-relief annealing. However, in the aforementioned laser marking methods, the angle between the laser beam and the plate changes as the laser beam sweeps from one side of the grain-oriented silicon steel sheet to the other, leading to inconsistent laser energy density. Specifically, the energy density at the edge of the plate width is much lower than that at the center, resulting in uneven marking and consequently, uneven magnetic properties across the entire grain-oriented silicon steel sheet. Summary of the Invention
[0004] Therefore, it is necessary to provide a grain-oriented silicon steel with uniform magnetic properties and a laser marking method to address the problem of uneven magnetic properties on the surface of grain-oriented silicon steel sheets caused by uneven laser marking.
[0005] In a first aspect, this application provides a grain-oriented silicon steel with superimposed scoring lines on its surface. The superimposed scoring lines extend perpendicularly to the rolling direction of the grain-oriented silicon steel. The superimposed scoring lines include an initial scoring line and two compensating scoring lines. The initial scoring line is a continuous scoring line that runs through the entire width direction of the grain-oriented silicon steel sheet. The laser energy received by the initial scoring line decreases from the center point of the width of the silicon steel sheet towards both sides of the edge. One compensating scoring line extends from one edge of the grain-oriented silicon steel sheet towards the center point of the width of the grain-oriented silicon steel sheet, and the other compensating scoring line extends from the other edge of the grain-oriented silicon steel sheet towards the center point of the width of the sheet. The laser energy received by the compensating scoring lines gradually decreases from the edge side of the grain-oriented silicon steel sheet to the center point of the width of the sheet.
[0006] Furthermore, the total energy density E at any point on the superimposed scribe line when subjected to two laser irradiations ranges from 100 to 300 mJ / mm². 2 .
[0007] Furthermore, after laser marking, the iron loss improvement rate of oriented silicon steel is between 11% and 13%, and the magnetic induction loss is between 0 and 0.01T.
[0008] Furthermore, the iron loss value of the grain-oriented silicon steel sheet varies between 0% and 1% at different locations along the width direction.
[0009] Secondly, this application provides a laser marking method suitable for preparing any type of oriented silicon steel with uniform magnetic properties provided in the first aspect, the laser marking method comprising:
[0010] The laser is controlled to etch from one side of the edge of the grain-oriented silicon steel to the other along the width direction of the plate to obtain the initial groove line;
[0011] Compensation marks are made on the initial score line from both ends toward the center of the width of the grain-oriented silicon steel, resulting in two compensation score lines superimposed on the initial score line. The compensation score line and the initial score line are superimposed to form a superimposed score line, and the extension direction of the superimposed score line is perpendicular to the rolling direction of the grain-oriented silicon steel.
[0012] Among them, the laser energy received by the two compensation scoring lines gradually decreases from the edge side of the oriented silicon steel at both ends of the initial scoring line to the center point of the plate width.
[0013] Furthermore, the first laser used for the initial scoring line and the second laser used for the compensation scoring line are at the same horizontal height and are arranged sequentially along the rolling direction of the grain-oriented silicon steel. The first laser is closer to the feeding side of the grain-oriented silicon steel than the second laser, and the first laser is located directly above the center line along the rolling direction of the grain-oriented silicon steel. There are two second lasers, one of which is located directly above one edge of the grain-oriented silicon steel and the other is located directly above the other edge of the grain-oriented silicon steel.
[0014] Furthermore, both the first and second lasers are continuous-type lasers.
[0015] Furthermore, the arrangement height h of the first laser and the second laser and the width L of the oriented silicon steel satisfy the following relationship: h ≥ 0.9L.
[0016] Furthermore, the two compensation notch lines overlap each other at the center of the width of the grain-oriented silicon steel sheet or have a gap along the width direction, and the overlap length is l. a The value range is (0, 3] mm, and the spacing is l. b The value range is [0, 5] mm.
[0017] The aforementioned grain-oriented silicon steel with uniform magnetic properties has superimposed scoring lines on its surface. The superimposed scoring lines extend perpendicularly to the rolling direction of the grain-oriented silicon steel. The superimposed scoring lines include an initial scoring line and two compensating scoring lines. The initial scoring line is a continuous scoring line that runs through the entire width of the grain-oriented silicon steel sheet. The laser energy received by the initial scoring line decreases from the center point of the width of the silicon steel sheet towards both sides of the edge. One compensating scoring line extends from one edge of the grain-oriented silicon steel sheet towards the center point of the width of the grain-oriented silicon steel sheet, and the other compensating scoring line extends from the other edge of the grain-oriented silicon steel sheet towards the center point of the width of the sheet. The laser energy received by the compensating scoring lines gradually decreases from the edge of the grain-oriented silicon steel sheet to the center point of the width of the sheet.
[0018] The beneficial effects of this application are as follows: The grain-oriented silicon steel of this application has a compensation score line superimposed on the initial score line, which makes the energy density difference when different positions along the width of the plate are irradiated by laser smaller. This helps to make the laser energy distribution at any position on the superimposed score line formed in the end more uniform, thereby helping to improve the score energy uniformity of the entire grain-oriented silicon steel plate and thus obtaining a grain-oriented silicon steel product with uniform magnetic properties. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of this application or the conventional technology, the drawings used in the description of the embodiments or the conventional technology will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0020] Figure 1 This is a schematic diagram showing the positional relationship between the laser beam and the plate surface during laser irradiation.
[0021] Figure 2 This is a schematic diagram showing the change of the laser spot when a laser beam with a circular cross-section is used to scan and scribble a line.
[0022] Figure 3This is a schematic diagram of the laser spot moving on the surface of a silicon steel plate during laser scanning.
[0023] Figure 4 This is a schematic diagram of the laser structure layout.
[0024] Figure 5 This is a diagram showing the energy density distribution at different locations along the scribe line when irradiated by a laser.
[0025] Figure 6 This is a schematic diagram of the sampling location during magnetic property testing.
[0026] Figure 7 This is a schematic diagram showing the intersection of two compensation groove lines at the center of the plate width.
[0027] Explanation of icon numbers:
[0028] 10. Grain-oriented silicon steel; 21. First laser; 22. Second laser; 31. Initial scribe line; 32. First compensation scribe line; 33. Second compensation scribe line; 34. Superimposed scribe line. Detailed Implementation
[0029] To make the above-mentioned objectives, features, and advantages of this application more apparent and understandable, the specific embodiments of this application are described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of this application. However, this application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of this application. Therefore, this application is not limited to the specific embodiments disclosed below.
[0030] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.
[0031] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.
[0032] The terms “vertical,” “horizontal,” “up,” “down,” “left,” “right,” and similar expressions used in this document are for illustrative purposes only and do not represent the only possible implementation.
[0033] Currently, the most widely used laser marking scheme typically involves keeping the laser stationary and, through a well-designed optical path, ensuring the focal point remains on the surface of the grain-oriented silicon steel sheet. During laser scanning, the laser beam rotates approximately around a point at a constant angular velocity, thus achieving rapid scanning and marking of the entire surface of the grain-oriented silicon steel sheet. However, this scheme neglects the impact of changes in the angle between the laser beam and the sheet surface on the laser energy density at different locations along the marking line.
[0034] Specifically, refer to Figure 1 , Figure 1 This diagram illustrates the positional relationship between the laser beam and the surface of the grain-oriented silicon steel sheet during laser scanning. The angle between the laser beam and the grain-oriented silicon steel sheet changes during the laser scanning and marking process, thus affecting the shape and size of the laser spot illuminating the sheet. (Refer to...) Figure 2 , Figure 2 The difference in spot shape between the edge and center of a plate is illustrated using a circular laser beam as an example. Additionally, refer to... Figure 3 When the laser beam rotates at a constant speed through two identical angles θ, the time taken is equal. However, at this time, the distances AP and PB of the laser spot are obviously not equal, which indicates that the speed at which the laser spot moves on the surface of the grain-oriented silicon steel plate is different.
[0035] Taking the laser located at the center of the width of the grain-oriented silicon steel plate as an example, the study found that during the process of the laser beam sweeping from one side of the grain-oriented silicon steel plate to the other, the changes in the spot area and the spot moving speed conform to the following rules: the spot area first decreases and then increases; the spot moving speed on the grain-oriented silicon steel plate first decreases and then increases.
[0036] It should be noted that the above-mentioned spot area S and spot movement speed v s The calculation is performed using the following formula:
[0037]
[0038] Where, a is the length of the laser spot along the scanning direction when the laser beam is perpendicularly irradiated on the plate surface, in mm, which is affected by the angle α between the laser beam and the grain-oriented silicon steel plate surface; b is the length of the laser spot perpendicular to the scanning direction, in mm, which is not affected by the angle α between the laser beam and the grain-oriented silicon steel plate surface; ω is the angular velocity of the laser beam as it sweeps across the grain-oriented silicon steel plate surface; h is the arrangement height of the laser.
[0039] The formula for calculating the energy density e of a laser beam irradiating a plate surface is:
[0040]
[0041] Where P is the laser output power, in W; t s The duration of laser beam irradiation on a single point of a grain-oriented silicon steel sheet, measured in milliseconds, can be determined by... The calculation yielded the result.
[0042] According to the above calculation formula, both the spot area and the spot movement speed are closely related to the energy density of the laser irradiation on the surface of the grain-oriented silicon steel sheet, and are directly affected by the angle α between the laser beam and the grain-oriented silicon steel sheet surface. This causes the following problem: as the spot moves on the surface of the grain-oriented silicon steel sheet, the energy density of the laser irradiation along a groove line will show a trend of first increasing and then decreasing from one side of the grain-oriented silicon steel sheet surface to the other. That is, the energy density at the wide edge of the grain-oriented silicon steel sheet is much lower than that at the center of the sheet width, resulting in poor uniformity of magnetic properties across the entire grain-oriented silicon steel sheet surface.
[0043] In response to the above issues, refer to Figure 4 , Figure 4 This application provides a schematic diagram of a laser structure arrangement. In the diagram, the RD arrow indicates the rolling direction of the grain-oriented silicon steel 10, which is also the length direction and feeding direction of the grain-oriented silicon steel. The TD arrow indicates the width direction of the grain-oriented silicon steel 10. In some embodiments, based on the arrangement of a first laser 21 at the center of the first row of plates, a second laser 22 is added to each of the two edges of the second row of plates. The first laser 21 and the second laser 22 are at the same horizontal height, and the first laser 21 and the second laser 22 are arranged sequentially along the rolling direction of the grain-oriented silicon steel 10. The first laser 21 is closer to the feeding side of the grain-oriented silicon steel 10 than the second laser 22. The first laser 21 is used to etch the initial score line 31, and the second laser 22 is used to etch the compensation score line. Accordingly, this application provides a laser marking method applicable to grain-oriented silicon steel 10. The method includes: using a compensation marking method to perform energy compensation on the initial marking line 31 on the grain-oriented silicon steel 10 plate surface, that is, superimposing a compensation marking line on the initial marking line 31 to form a superimposed marking line 34 perpendicular to the rolling direction of the grain-oriented silicon steel 10. The initial marking line 31 is a continuous marking line that runs through the entire grain-oriented silicon steel 10 plate surface. One compensation marking line extends from the edge of one side of the grain-oriented silicon steel towards the center point of the plate width of the grain-oriented silicon steel plate surface, and another compensation marking line extends from the edge of the other side of the grain-oriented silicon steel towards the center point of the plate width of the grain-oriented silicon steel plate surface. The two compensation marking lines are a first compensation marking line 32 and a second compensation marking line 33, respectively.
[0044] The initial scribe line 31 and the compensation scribe line are both parallel to the width direction of the grain-oriented silicon steel 10, that is, perpendicular to the rolling direction of the grain-oriented silicon steel 10. The two second lasers 22 are located on both sides of the width of the grain-oriented silicon steel 10, and the second lasers 22 are located directly above the edge of the width of the grain-oriented silicon steel 10.
[0045] Specifically, during the laser marking process of the grain-oriented silicon steel 10, the first laser 21 first performs preliminary marking on the grain-oriented silicon steel 10 plate from left to right or from right to left along the width direction of the plate, obtaining an initial marking line 31. The laser energy received by the initial marking line 31 decreases from the center point of the grain-oriented silicon steel 10 plate width towards both sides of the plate width edge. After the initial marking line 31 moves with the grain-oriented silicon steel 10 to directly below the second laser 22, both second lasers 22 start etching from the edge of the grain-oriented silicon steel 10 plate surface until they reach the center position of the plate width, so as to complete the compensation marking of the initial marking line 31 and obtain the superimposed marking line 34. One of the second lasers 22 is used to etch the first compensation marking line 32, and the other second laser 22 is used to etch the second compensation marking line 33. The laser energy received by the first compensation marking line 32 and the second compensation marking line 33 decreases from both ends of the initial marking line 31 towards the center of the plate width. Since the angle between the laser beam of the second laser 22 and the surface of the grain-oriented silicon steel 10 is the smallest at the center of the plate width and the largest at the edge of the plate width, the energy density of a scoring line irradiated by the compensating scoring laser will show a trend of first decreasing and then increasing from one side of the plate to the other. This is exactly the opposite of the energy density distribution after the initial scoring laser scanning irradiation. As a result, the energy density of the superimposed scoring line 34 located at the edge of the grain-oriented silicon steel 10 plate width can be made consistent with the energy density of the superimposed scoring line 34 located at the center of the grain-oriented silicon steel 10 plate width.
[0046] For example, refer to Figure 4 and Figure 5 , Figure 5 Taking an arrangement height h of 1080mm for the first laser 21 and the second laser 22, and a width L of 1200mm for the grain-oriented silicon steel 10 as an example, the energy density distribution pattern at different positions on the scribe line under laser irradiation is illustrated. The first laser 21 and the second laser 22 have the same output power. Taking the position with the highest energy density on the scribe line as 100%, according to the calculation formula for the energy density of the laser beam irradiating the grain-oriented silicon steel 10 surface, without compensation for the initial scribe line 31, the maximum energy density difference at different positions along the width direction of the grain-oriented silicon steel 10 on the initial scribe line 31 is 23.58%. After compensating for the superimposed energy of the scribe line, the energy density difference at different positions along the width direction of the superimposed scribe line 34 is 4.99%. Therefore, by compensating for the scribe line, the energy density difference at different positions along the width direction under laser irradiation can be effectively reduced.
[0047] Furthermore, both the first laser 21 and the second laser 22 are continuous lasers, which ensures that the first laser 21 and the second laser 22 can output laser energy stably and continuously without frequent switching and restarting, thereby achieving efficient marking operations and ensuring production efficiency.
[0048] Select unmarked grain-oriented silicon steel coils with uniform magnetic properties across the entire surface, and perform laser marking according to the scheme in Table 1. Before and after marking, follow the... Figure 6 At the sampling locations shown, single samples of 500×100mm were cut out for magnetic performance testing. The results of the magnetic performance testing are shown in Table 2.
[0049] Table 1
[0050]
[0051] Note: Since Comparative Example 1 did not have a compensated etch, the "total energy density E when any position on the superimposed etch line is irradiated by two lasers" refers to the energy density irradiated by the initial etch laser (first laser 21).
[0052] Table 2
[0054]
[0055] According to Example 1 and Comparative Example 1, using the non-compensated scoring scheme, the maximum difference in iron loss value at different positions along the width of the plate after scoring exceeds 0.06 W / kg. However, after using the compensated scoring scheme, the iron loss value at different positions along the width of the plate tends to be consistent. This indicates that the compensated scoring can greatly reduce the difference in loss reduction effect at different positions on the plate surface and can effectively improve the uniformity of magnetic properties on the plate surface.
[0056] Reference Figure 4 In some embodiments, the arrangement height h of the first laser 21 and the width L of the oriented silicon steel 10 satisfy the following relationship: h ≥ 0.9L.
[0057] Since the arrangement height of the first laser 21 is the same as that of the second laser 22, the arrangement height of the second laser 22 and the width of the oriented silicon steel 10 also satisfy the above relationship.
[0058] Specifically, according to Example 2 and Comparative Example 2 in Table 1 above, and Table 2, the spacing l between the two compensation notch lines along the width direction of the plate is... b When the total energy density E is the same as that of two laser irradiations at any position on the superimposed scribe line 34, when At the same time, similar loss reduction effects can be obtained at different positions along the width of the plate, the magnetic properties of the plate surface are well uniform, and it can ensure that the laser can completely cover the entire surface of the grain-oriented silicon steel plate 10, avoiding the problem of incomplete marking or uneven coverage due to insufficient laser height, thereby improving the uniformity and stability of the overall magnetic properties of the grain-oriented silicon steel 10; in addition, it can also improve the consistency of marking, reduce the adjustment and correction coefficients in the generation process, thereby improving production efficiency; and when At that time, the iron loss reduction of oriented silicon steel 10 varied significantly at different locations along the width direction, resulting in poor uniformity of the magnetic properties on the plate surface. Therefore, the laser height h and plate width L must satisfy the following condition. The relationship.
[0059] Reference Figure 7 In some embodiments, the two compensation notch lines overlap at the center of the width of the grain-oriented silicon steel 10 plate, and the overlap length is l. a The value range is (0, 3] mm.
[0060] Specifically, according to Examples 3-5 in Table 1, Comparative Examples 3-4, and Table 2 above, in When the ratio and the total energy density E at any position on the superimposed notch line 34 are the same under two laser irradiations, the two compensation notch lines overlap at the center of the plate width. When the overlap length l a When the value range is (0, 3] mm, the edge and center of the plate width can achieve similar loss reduction effects, and the magnetic properties of the plate surface are well uniform; while when the overlap length l of the two compensation notch lines at the center of the plate width of the grain-oriented silicon steel 10 plate is... a When the thickness is greater than 3mm, the difference in damage reduction between the center and edge of the board width is significant. Therefore, when making compensation grooves, the overlap length of the two compensation groove lines should be controlled within a reasonable range.
[0061] Alternatively, in other embodiments, the two compensation notch lines are spaced l apart along the width direction at the center position of the width of the grain-oriented silicon steel 10 plate. b The value range is [0, 5] mm.
[0062] Specifically, according to Examples 3-5 in Table 1, Comparative Examples 3-4, and Table 2 above, in When the ratio and the total energy density E at any position on the superimposed notch line 34 are the same under two laser irradiations, the two compensation notch lines have a gap along the width direction at the center of the plate width. When the gap l b When the value range is [0, 5] mm, the edge and center of the plate width can achieve similar loss reduction effects, and the magnetic properties of the plate surface are well uniform; however, when there is a gap along the plate width direction but l bWhen the thickness is greater than 5mm, the difference in loss reduction between the center and edge of the plate width is significant, and it is impossible to obtain oriented silicon steel products with uniform magnetic properties. Therefore, when performing compensation scoring, the spacing between the two compensation scoring lines along the plate width direction must be controlled within a reasonable range.
[0063] In some embodiments, the total energy density at any position on the superimposed scribe line 34 when subjected to two laser irradiations ranges from 100 to 300 mJ / mm². 2 .
[0064] Specifically, according to Example 6 in Table 1, Comparative Examples 5-6, and Table 2 above, in The ratio and the spacing l between the two compensation notch lines along the width of the plate b Under the same conditions, when any position on the superimposed scribe line 34 is subjected to two laser irradiations, the total energy density E is between 100 and 300 mJ / mm². 2 When E < 100 mJ / mm, the difference in iron loss reduction at different locations along the width of the plate is small, and the uniformity of magnetic properties on the plate surface is good; however, when E < 100 mJ / mm 2 At that time, although the difference in iron loss reduction effect at different positions along the width direction of grain-oriented silicon steel 10 was not significant, the effect of scoring on iron loss reduction was greatly weakened; when E>300mJ / mm 2 At that time, compared with before scoring, the iron loss increased after scoring, and the magnetic induction decreased significantly. This is because the excessive energy caused severe deformation of the grain-oriented silicon steel sheet surface. Therefore, the total energy density when any position on the superimposed scoring line is subjected to two laser irradiations must satisfy 100≤E≤300mJ / mm². 2 .
[0065] The laser marking method of this application compensates for the energy of the initial marking line, which can effectively reduce the difference in energy density when irradiated by laser at different positions along the width of the plate, thereby helping to improve the uniformity of marking energy on the entire grain-oriented silicon steel 10 plate and thus obtaining a grain-oriented silicon steel product with uniform magnetic properties.
[0066] In addition, one embodiment of this application provides an oriented silicon steel, which is produced by any of the above-mentioned laser marking methods. After laser marking compensation, the iron loss improvement rate of the oriented silicon steel plate is between 11% and 13%, the magnetic induction loss is between 0 and 0.01T, and the difference between the iron loss value at the two edges of the oriented silicon steel plate and the iron loss value at the center of the plate is between 0 and 1%.
[0067] Specifically, the grain-oriented silicon steel products produced by the laser marking method described above have higher energy density consistency on the final superimposed marking lines due to the energy compensation of the initial marking lines by the second laser, which helps to improve the uniformity of the markings. This makes the magnetic properties of the entire grain-oriented silicon steel plate more uniform, resulting in uniform magnetic properties of the final grain-oriented silicon steel product and good performance of the applicable transformer.
[0068] In the description of this specification, references to terms such as "some embodiments," "other embodiments," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative descriptions of the above terms do not necessarily refer to the same embodiments or examples.
[0069] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0070] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.
Claims
1. A oriented silicon steel with uniform magnetic properties, It is characterized in that The plate surface of the oriented silicon steel is provided with superimposed scoring lines, the extension direction of the superimposed scoring lines is perpendicular to the rolling direction of the oriented silicon steel, the superimposed scoring lines include an initial scoring line and two compensating scoring lines, the initial scoring line is a continuous scoring line running through the entire width direction of the oriented silicon steel plate surface, the laser energy received by the initial scoring line decreases from the plate width center point of the silicon steel plate surface toward both sides of the edge, one of the compensating scoring lines extends from the edge of one side of the oriented silicon steel toward the plate width center point of the oriented silicon steel plate surface, and the other compensating scoring line extends from the edge of the other side of the oriented silicon steel toward the plate width center point, and the laser energy received by the compensating scoring lines when they are formed gradually decreases from the edge side of the oriented silicon steel to the plate width center point.
2. The oriented silicon steel with uniform magnetic properties according to claim 1, It is characterized in that The total energy density E of any position on the superimposed scoring line when subjected to two laser irradiations is in the range of 100 to 300 mJ / mm 2 .
3. The oriented silicon steel with uniform magnetic properties according to claim 1, It is characterized in that After laser notching, the iron loss improvement rate of the oriented silicon steel is between 11% and 13%, and the magnetic induction loss is between 0 and 0.01T.
4. The oriented silicon steel with uniform magnetic properties according to claim 1, It is characterized in that The difference in iron loss values of the oriented silicon steel at different positions along the plate width direction is between 0% and 1%.
5. A laser scoring method, suitable for preparing oriented silicon steel with uniform magnetic properties as claimed in any one of claims 1 to 4, It is characterized in that include: Controlling the laser to etch along the width direction of the oriented silicon steel from one side of the plate width edge to the other side to obtain an initial scoring line; Performing compensatory scoring on the initial score line from both ends of the initial score line along the initial score line toward the center point of the plate width of the oriented silicon steel to obtain two compensatory score lines superimposed on the initial score line, wherein the compensatory score lines and the initial score line are superimposed to form superimposed score lines, and the extending direction of the superimposed score lines is perpendicular to the rolling direction of the oriented silicon steel; The laser energy received by the two compensating scoring lines gradually decreases from the edge sides of the oriented silicon steel located at both ends of the initial scoring lines to the center point of the plate width.
6. The laser scoring method according to claim 5, It is characterized in that The first laser used for the initial scoring line and the second laser used for the compensation scoring line have the same horizontal height, and are arranged in rows in sequence along the rolling direction of the oriented silicon steel. The first laser is closer to the feeding side of the oriented silicon steel than the second laser, and the first laser is located directly above the center line along the rolling direction of the oriented silicon steel. There are two second lasers, one of which is located directly above the edge of one side of the oriented silicon steel, and the other second laser is located directly above the edge of the other side of the oriented silicon steel.
7. The laser scoring method according to claim 6, It is characterized in that The first laser and the second laser are both continuous lasers.
8. The laser scoring method according to claim 6, It is characterized in that The arrangement height h of the first laser and the second laser and the width L of the oriented silicon steel satisfy the following relationship: h≥0.9L.
9. The laser scoring method for oriented silicon steel according to claim 5 or 6, It is characterized in that The two compensation score lines overlap each other at the center of the width of the oriented silicon steel plate, and the overlap length is l a The value range is (0, 3] mm.
10. The laser scoring method for oriented silicon steel according to claim 5 or 6, It is characterized in that The two compensation score lines are spaced apart along the width direction at the center of the width of the oriented silicon steel sheet, and the spacing l b The value range is [0, 5] mm.
Citation Information
Patent Citations
Magnetic steel sheet with oriented grain and method for producing the same
BR112014025281A2
Method and device for miniaturizing magnetic domains of directional electric steel plate
CN108495940A
Manufacturing method for low-iron loss oriented silicon steel resistant to stress-relief annealing
CN110093486A
Nick-oriented silicon steel resistant to stress-relief annealing and manufacturing method for nick-oriented silicon steel
CN113584279A
Method for forming linear groove, device for forming linear groove, and method for manufacturing grain-oriented electrical steel sheet
CN114207157A