Carbon dot modified platinum-palladium alloy nanosheet as well as preparation method and application thereof

The two-dimensional flexible porous Pt2Pd alloy nanosheet catalyst modified by carbon dots solves the problems of poor stability and toxicity in the ammonia oxidation reaction, and achieves efficient ammonia oxidation reaction and long-term cycle stability.

CN118925714APending Publication Date: 2024-11-12SUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411002097.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the ammonia oxidation reaction, the existing PtPd alloy catalysts have problems such as high precious metal content, small electrochemical active specific surface area, high oxidation peak potential and poor stability. In particular, the strong force of the Pt-N bond causes the catalyst to be easily toxic.

Method used

Two-dimensional flexible porous Pt2Pd alloy nanosheets modified with carbon dots are used as catalysts, and prepared by oxidation treatment and reduction reactions, combined with carbon dot calcination treatment, to improve the number of electrochemical reaction active sites and anti-toxicity properties of the catalyst.

Benefits of technology

It significantly improves the ammonia oxidation reaction activity and stability of the catalyst, reduces the starting potential of the oxidation peak, and improves the anti-toxicity performance of the catalyst. The mass activity can reach 175.5A·gPGM-1, and the cycle stability is better than that of commercial Pt/C. catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925714A_ABST
    Figure CN118925714A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon dot modified platinum-palladium alloy nanosheet and a preparation method and application thereof.The preparation method comprises the following steps that platinum salt, palladium salt and an alkaline substance are dissolved in an organic solvent to be mixed and heated to be oxidized to obtain platinum-palladium oxide, the platinum-palladium oxide and a reducing agent are dissolved in water, heating reduction is conducted to obtain the platinum-palladium alloy nanosheet, and the carbon dot modified platinum-palladium alloy nanosheet is obtained. And mixing the platinum-palladium alloy nanosheet with the carbon dots, and calcining in a mixed gas atmosphere of hydrogen and inert gas to obtain the platinum-palladium alloy nanosheet modified by the carbon dots. The carbon dots are adopted to modify the platinum-palladium alloy, rich functional groups on the surfaces of the carbon dots enable the carbon dots to be tightly combined with the platinum-palladium alloy, meanwhile, ammonia adsorption can be improved, the electrochemical activity specific surface area of the catalyst is increased, and the ammoxidation reaction catalytic activity of the catalyst is improved. In addition, by adopting the carbon dot modified two-dimensional flexible porous platinum-palladium alloy nanosheet, the content of noble metal in the catalyst can be reduced, the anti-poisoning performance of the catalyst is improved, and the stability of the catalyst is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of platinum-palladium alloy materials, and in particular to a carbon-dot-modified platinum-palladium alloy nanosheet and a preparation method and application thereof. Background Art

[0002] Ammonia (NH3) is a carbon-free fuel with low cost and high energy density (3000Wh·Kg -1 ), mature transportation and storage infrastructure, and is a cost-effective hydrogen carrier (its hydrogen capacity is as high as 17.6wt%, and its specific energy density is 50% higher than that of liquefied hydrogen per unit volume), which can be used in direct ammonia fuel cells. In addition, the electrocatalytic ammonia oxidation reaction (NH3OR) is a very important electrochemical process, and the exploration of electrocatalytic NH3OR is of great significance for the electrochemical removal of NH3 from wastewater and the development of emerging energy devices.

[0003] In NH3OR, the rate-determining step is NH x The main catalyst for NH3OR is Pt-based catalyst. However, the strong force of Pt-N bond makes Pt easily poisoned by nitrogen adsorbed intermediates. Existing reports show that PtPd alloy exhibits higher NH3OR catalytic activity than Pt alone, and the introduction of Pd can reduce the strength of Pt-N bond. However, the existing PtPd alloy catalysts are mostly nanoparticles with high precious metal content, small electrochemically active specific surface area, and high oxidation peak potential. At the same time, precious metal catalysts are easily poisoned and have poor stability. It is still challenging to prepare two-dimensional flexible porous alloy catalysts with large electrochemically active specific surface area and high catalytic activity. Summary of the invention

[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a carbon dot-modified platinum-palladium alloy nanosheet and a preparation method and application thereof.

[0005] The above object of the present invention is achieved through the following technical solutions:

[0006] The first aspect of the present invention provides a method for preparing carbon dot-modified platinum-palladium alloy nanosheets, comprising the following steps:

[0007] (1) dissolving a platinum salt, a palladium salt and an alkaline substance in an organic solvent to obtain a mixed solution, and subjecting the mixed solution to oxidation treatment to obtain a platinum-palladium oxide;

[0008] (2) dissolving the platinum-palladium oxide obtained in step (1) and a reducing agent in water, and performing a reduction reaction at 60 to 80° C. to obtain platinum-palladium alloy nanosheets; the reducing agent is morpholine borane or dimethylformamide;

[0009] (3) The platinum-palladium alloy nanosheets obtained in step (2) are mixed with carbon dots and placed in a heating device for calcination in a mixed gas atmosphere of hydrogen and inert gas to obtain the carbon dot-modified platinum-palladium alloy nanosheets (Pt2Pd-CD).

[0010] The platinum-palladium alloy nanosheet provided by the present invention is a two-dimensional flexible porous Pt2Pd alloy nanosheet. As an NH3OR catalyst, ammonia is more easily in contact with the surface of the flexible porous catalyst, thereby increasing the number of electrochemical reaction active sites of the catalyst and improving the NH3OR activity of platinum. At the same time, the porous structure is conducive to the diffusion of ammonia.

[0011] In order to further improve the stability and conductivity of the catalyst, the present invention uses carbon dots (CD) to modify the Pt2Pd alloy. The rich functional groups on the surface of CD enable it to be tightly combined with the Pt2Pd alloy, and at the same time, it can also increase the adsorption of ammonia, increase the electrochemical active specific surface area of ​​the catalyst, and then reduce the starting potential of the oxidation peak, and improve the NH3OR catalytic activity of the catalyst. In addition, the use of CD to modify the Pt2Pd two-dimensional flexible porous nanosheet can also reduce the precious metal content in the catalyst, improve the anti-poisoning performance of the catalyst, and increase the stability of the catalyst.

[0012] Furthermore, in step (1), the platinum salt is platinum acetylacetonate, chloroplatinic acid or platinum tetrachloride.

[0013] Furthermore, in step (1), the palladium salt is palladium acetylacetonate or palladium chloride.

[0014] Furthermore, in step (1), the alkaline substance is potassium carbonate or potassium hydroxide, preferably potassium carbonate.

[0015] Furthermore, in step (1), the organic solvent is methanol or ethanol.

[0016] Furthermore, in step (1), the oxidation treatment is specifically as follows: placing the mixed solution in a heating device, first heating it to 100-150°C at a rate of 8-10°C / min and keeping it warm for 0.5-1h, and then heating it to 350-400°C at a rate of 8-10°C / min and keeping it warm for 1.5-2h.

[0017] Furthermore, in step (1), the molar ratio of the platinum salt to the palladium salt is 1:(0.5-2).

[0018] Furthermore, in step (2), the mass ratio of the platinum palladium oxide to the reducing agent is 1:(5-15).

[0019] Furthermore, in step (2), the platinum-palladium alloy nanosheets obtained by the reduction reaction at 60-80° C. have a more uniform morphology.

[0020] Furthermore, in step (3), the carbon dots are prepared by an electrochemical method, using graphite as a carbon source and water as an electrolyte.

[0021] In a specific embodiment, two graphite rods are placed in water, connected to the positive and negative electrodes of a DC power supply, respectively, and a voltage of 20 to 30 V is applied, and electrolysis is continued until the color of the electrolyte turns brown-black. The obtained brown-black solution is filtered, centrifuged, and dried to obtain carbon dots.

[0022] Furthermore, in step (3), the mass of the carbon dots is 1% to 10%, preferably 3% to 5%, of the mass of the platinum-palladium alloy nanosheets.

[0023] Furthermore, in step (3), the calcination treatment is carried out at 200-300°C.

[0024] Furthermore, in step (3), the volume ratio of hydrogen to inert gas is (2-8):(92-98).

[0025] Furthermore, in step (3), the inert gas is selected from one of argon, helium, krypton and xenon.

[0026] The second aspect of the present invention provides a carbon dot-modified platinum-palladium alloy nanosheet prepared by the method described in the first aspect.

[0027] The third aspect of the present invention provides the use of the carbon dot-modified platinum-palladium alloy nanosheets described in the second aspect in an ammonia oxidation reaction.

[0028] The fourth aspect of the present invention provides a catalyst for an ammonia fuel cell, comprising the carbon-dot-modified platinum-palladium alloy nanosheets described in the second aspect.

[0029] Beneficial effects of the present invention:

[0030] 1. The platinum-palladium alloy nanosheet provided by the present invention is a two-dimensional flexible porous Pt2Pd alloy nanosheet. As an NH3OR catalyst, ammonia is more likely to contact the surface of the flexible porous catalyst, thereby increasing the number of reactive sites of the catalyst, improving the NH3OR activity of platinum, and the porous structure is conducive to the diffusion of ammonia. The present invention adopts CD to modify the Pt2Pd alloy. The rich functional groups on the surface of CD enable it to be closely combined with the Pt2Pd alloy, and at the same time, it can also increase the adsorption of ammonia, increase the electrochemical active specific surface area of ​​the catalyst, and then reduce the starting potential of the oxidation peak, and improve the NH3OR catalytic activity of the catalyst. In addition, the use of CD to modify the Pt2Pd two-dimensional flexible porous nanosheet can also reduce the precious metal content in the catalyst, improve the anti-poisoning performance of the catalyst, and increase the stability of the catalyst.

[0031] 2. The mass activity of the Pt2Pd-CD catalyst provided by the present invention when catalyzing NH3OR can reach 175.5A·g PGM -1 , which is 4 times that of commercial Pt / C catalyst. After 2000 cycles of CV, the mass activity only decreased by 8.29%, while the mass activity of Pt2Pd catalyst without CD decreased by 43.2%. After 6000s of constant potential test, the catalytic performance of commercial Pt / C was almost 0, while Pt2Pd-CD could still maintain 48.4% of mass activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 These are morphology characterization pictures of the Pt2Pd-3%CD prepared in Example 1; wherein, a is a scanning electron microscope (SEM) picture, b is a transmission electron microscope (TEM) picture, c is a high-resolution transmission electron microscope (HRTEM) picture, d is a local enlarged picture of c, e is a scanning transmission microscope (STEM) picture, f is a Pd elemental analysis (EDS) surface scan picture, g is a Pt elemental analysis (EDS) surface scan picture, and h is a C elemental analysis (EDS) surface scan picture.

[0033] Figure 2 This is the SEM image of Na-Pt2Pd-3%CD prepared in Comparative Example 1.

[0034] Figure 3 It is a structural characterization and binding energy test result diagram of Pt2Pd-3%CD prepared in Example 1; wherein, a is an X-ray powder diffraction pattern (XRD) diagram, b is a local enlarged diagram of a, c is a Raman spectrum (Raman) diagram, d is a Fourier transform infrared spectrum (FTIR) diagram, e is an X-ray photoelectron spectrum (XPS) diagram of Pd, and f is an X-ray photoelectron spectrum (XPS) diagram of Pt.

[0035] Figure 4 FTIR graphs of Pt2Pd-3%CD and Pt2Pd after adsorbing ammonia water.

[0036] Figure 5 Cyclic voltammetry (CV) curves of Pt2Pd-3%CD in 1M KOH and 1M KOH+0.5M NH3 electrolytes.

[0037] Figure 6 CV diagrams of Pt2Pd-3%CD, Na-Pt2Pd and Na-Pt2Pd-3%CD in 1M KOH+0.5M NH3 electrolyte.

[0038] Figure 7 CV diagrams of Pt2Pd-3%CD and P-Pt2Pd-3%CD in 1M KOH+0.5M NH3 electrolyte.

[0039] Figure 8 The graphs are the test results of the ammonia oxidation performance of catalysts with different Pt and Pd ratios and different CD contents in 1M KOH+0.5M NH3 electrolyte; wherein, a is the CV graph of Pt, PtPd, PtPd2, Pt2Pd and Pd, b is the CV graph of Pt2Pd, Pt2Pd-1%CD, Pt2Pd-3%CD, Pt2Pd-5%CD, Pt2Pd-10%CD and commercial Pt / C, c is the mass activity graph of Pt, PtPd, PtPd2, Pt2Pd and Pd, d is the mass activity diagram of Pt2Pd, Pt2Pd-1%CD, Pt2Pd-3%CD, Pt2Pd-5%CD, Pt2Pd-10%CD and commercial Pt / C; e is the peak mass activity bar chart of Pt, PtPd2, PtPd, Pt2Pd, Pt2Pd-1%CD, Pt2Pd-3%CD, Pt2Pd-5%CD, Pt2Pd-10%CD and commercial Pt / C.

[0040] Fig. 9 These are stability data graphs of Pt2Pd, Pt2Pd-1%CD, Pt2Pd-3%CD, Pt2Pd-5%CD, Pt2Pd-10%CD and commercial Pt / C; wherein, a is a mass activity graph of Pt2Pd before and after 2000 CV cycles, b is a mass activity graph of Pt2Pd-1%CD before and after 2000 CV cycles, c is a mass activity graph of Pt2Pd-3%CD before and after 2000 CV cycles, d is a mass activity graph of Pt2Pd-5%CD before and after 2000 CV cycles, e is a mass activity graph of Pt2Pd-10%CD before and after 2000 CV cycles, and f is a time-mass activity curve graph of Pt2Pd, Pt2Pd-1%CD, Pt2Pd-3%CD, Pt2Pd-5%CD, Pt2Pd-10%CD and commercial Pt / C tested with constant potential. DETAILED DESCRIPTION

[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0042] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0043] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.

[0044] In the following example, CD was obtained by electrolysis. The preparation method included the following steps: placing two cleaned graphite rods in deionized water, keeping a certain distance between the two graphite rods, connecting the two graphite rods to the positive and negative electrodes of a DC power supply, respectively, applying a voltage of 30 V, and continuing the electrolysis process for several days until the overall color of the solution is brown-black, filtering the obtained brown-black solution three times with qualitative filter paper to remove large-sized graphite oxide particles, and obtaining a CD solution (with a size of less than 10 nm) after centrifugation at 16,000 rpm, and obtaining CD powder after freeze-drying.

[0045] Example 1

[0046] A method for preparing carbon dot-modified platinum-palladium alloy nanosheets (Pt2Pd-3%CD), comprising the following steps:

[0047] (1) 35 mg of platinum acetylacetonate, 10 mg of palladium acetylacetonate and 1.8 g of potassium carbonate were dissolved in 20 mL of anhydrous ethanol, placed in a plastic beaker and ultrasonicated for 30 min to obtain a mixed solution, the mixed solution was transferred to a corundum crucible and placed in a muffle furnace, first heated to 100°C at a rate of 10°C / min and kept warm for 0.5 h, then heated to 400°C at a rate of 10°C / min and kept warm for 2 h, and the muffle furnace was cooled to room temperature, the product was washed with anhydrous ethanol and ultrapure water and dried to obtain platinum palladium oxide.

[0048] (2) 20 mg of platinum-palladium oxide and 200 mg of morpholine borane were dissolved in 20 mL of ultrapure water, reacted in a water bath at 70° C. for 2 h, and then centrifuged and freeze-dried to obtain platinum-palladium alloy nanosheets Pt2Pd.

[0049] (3) 0.6 mg CD and 20 mg Pt2Pd were mixed and placed in a crucible, which was then placed in a tubular furnace and calcined at 200°C for 1 h under the protection of a mixed gas of 5% H2 / 95% Ar to obtain carbon-dot-modified platinum-palladium alloy nanosheets (Pt2Pd-3%CD, 3% means that the mass of the carbon dots is 3% of the mass of the platinum-palladium alloy nanosheets).

[0050] Example 2

[0051] A method for preparing carbon dot-modified platinum-palladium alloy nanosheets (Pt2Pd-1%CD) is basically the same as Example 1, except that in step (3), 0.2 mg CD and 20 mg Pt2Pd are mixed.

[0052] Example 3

[0053] A method for preparing carbon dot-modified platinum-palladium alloy nanosheets (Pt2Pd-5%CD) is basically the same as Example 1, except that in step (3), 1 mg CD and 20 mg Pt2Pd are mixed.

[0054] Example 4

[0055] A method for preparing carbon dot-modified platinum-palladium alloy nanosheets (Pt2Pd-10%CD) is basically the same as that of Example 1, except that in step (3), 2 mg CD and 20 mg Pt2Pd are mixed.

[0056] Comparative Example 1

[0057] A method for preparing carbon dot-modified platinum-palladium alloy nanoparticles (Na-Pt2Pd-3%CD) is basically the same as that of Example 1, except that in step (2), morpholine borane is replaced by sodium borohydride.

[0058] Comparative Example 2

[0059] A method for preparing carbon dot-modified platinum-palladium alloy nanosheets (P-Pt2Pd-3%CD) is basically the same as Example 1, except that in step (2), 0.6 mg CD and 20 mg Pt2Pd are directly mixed to obtain carbon dot-modified platinum-palladium alloy nanosheets (P-Pt2Pd-3%CD).

[0060] The morphology of the Pt2Pd-3%CD prepared in Example 1 and the Na-Pt2Pd-3%CD prepared in Comparative Example 1 was characterized. The characterization results are shown in FIG. Figure 1 and Figure 2 shown. Figure 1 The morphology characterization diagram of Pt2Pd-3%CD prepared in Example 1; wherein, a is a scanning electron microscope (SEM) diagram, b is a transmission electron microscope (TEM) diagram, c is a high-resolution transmission electron microscope (HRTEM) diagram, d is a local enlarged diagram of c, e is a scanning transmission microscope (STEM) diagram, f is a Pd elemental analysis (EDS) surface scan diagram, g is a Pt elemental analysis (EDS) surface scan diagram, and h is a C elemental analysis (EDS) surface scan diagram. Figure 1 As can be seen from a and b, Pt2Pd-3%CD presents a porous nanosheet structure; Figure 1 In c and d, the lattice fringes of the (111) surface of Pt2Pt and the lattice fringes of the (200) surface of CD can be clearly seen; Figure 1 As can be seen from images e, f, g and h, Pd, Pt and C elements are uniformly distributed in Pt2Pd-3%CD. Figure 2 This is the SEM image of Na-Pt2Pd-3%CD prepared in Comparative Example 1. Figure 2It can be seen that the morphology of Na-Pt2Pd-3%CD is nanoparticles.

[0061] The structure of Pt2Pd-3%CD prepared in Example 1 was characterized and its binding energy was tested. The characterization results are as follows: Figure 3 As shown, Figure 3 The structure characterization and binding energy test results of Pt2Pd-3%CD prepared in Example 1 are shown in the figure; wherein, a is an X-ray powder diffraction pattern (XRD) diagram, b is a local enlarged diagram of a, c is a Raman spectrum (Raman) diagram, d is a Fourier transform infrared spectrum (FTIR) diagram, e is an X-ray photoelectron spectrum (XPS) diagram of Pd, and f is an X-ray photoelectron spectrum (XPS) diagram of Pt. Figure 3 As can be seen in a and b, Pt2Pd has only one set of lattice fringes, no phase separation, and the peak position of Pt2Pd is between pure Pt and pure Pd, proving the successful synthesis of the alloy. After adding CD, the XRD peak of Pt2Pd did not shift, indicating that the introduction of CD does not change the phase structure of the Pt2Pd alloy. Figure 3 The characteristic peaks of CD were observed in both c and d, and the combined SEM and TEM images showed that CD was successfully loaded on the surface of Pt2Pd alloy.

[0062] from Figure 3 In Figures e and f, it can be found that the binding energy of Pd in ​​Pt2Pd-3%CD is 0.1eV higher than that of pure Pd, while the binding energy of Pt is 0.1eV lower than that of pure Pt, indicating that some electrons are transferred from Pt to Pd. Compared with Pt2Pd, the degree of electron transfer is slightly reduced after the addition of CD, indicating that CD also has the function of regulating the electronic structure. In the NH3OR process, the Pt surface is easily poisoned. This is because when ammonia is oxidized on the surface of the Pt catalyst, intermediates N*, NH* and NH2* are formed. These intermediates are very stable at a specific potential and easily accumulate on the catalyst surface, causing the catalyst to deactivate. At the same time, at a higher potential, oxides and adsorbed hydroxides (*OH) are generated on the catalyst surface. These substances will further promote the dehydrogenation reaction of the intermediates, but will also cause poisoning and deactivation of the catalyst surface. The introduction of CD and Pd can regulate the electronic structure of Pt, thereby changing the adsorption characteristics of the catalyst surface to the intermediates. The change in XPS binding energy indicates that CD and Pd weaken the adsorption strength of nitrogen (*N) and nitrogen hydride (*NHx) on the Pt surface, thereby reducing irreversible adsorption and reducing the poisoning of Pt during ammonia oxidation. The introduction of CD can increase the adsorption and activity of *OH on the catalyst surface, which has a positive effect on the dehydrogenation reaction of the intermediate. The presence of *OH helps to avoid excessive stability of the intermediate on the catalyst surface, thereby reducing the poisoning phenomenon.

[0063] Figure 4The FTIR images of Pt2Pd-3%CD and Pt2Pd after adsorption of ammonia water are shown in Figure 1. 0.1M ammonia water was mixed with Pt2Pd-3%CD and Pt2Pd for 1 min, washed with water, centrifuged and dried, and then tested with FTIR. The test results are shown in Figure 1. Figure 4 As shown, a peak at 3128 cm -1 The NH bond peak is located at 1393 cm -1 The peak intensity of Pt2Pd-3%CD increased compared to that without adding ammonia water, corresponding to the CC / CN peak, indicating that the addition of CD significantly increased the adsorption of the catalyst to the reactant NH3, which is beneficial to the subsequent performance improvement.

[0064] Test Example 1

[0065] The ammonia oxidation performance of Pt2Pd-3%CD prepared in Example 1, Na-Pt2Pd-3%CD prepared in Comparative Example 1 and P-Pt2Pd-3%CD prepared in Comparative Example 2 were tested.

[0066] The test method is as follows: 4 mg of Pt2Pd-3% CD is dispersed in 900 μL of isopropanol aqueous solution (the volume ratio of water to isopropanol is 5:1) and 100 μL of 0.5 wt% naphthol and mixed solution, and ultrasonicated to form a uniform dispersion. 4 μL of the dispersion is dropped on the surface of the glassy carbon electrode and air-dried naturally. The catalyst loading on the electrode is 226 μg cm -2 The test adopted a three-electrode system, with Hg / HgO electrode as the reference electrode, platinum wire electrode as the counter electrode, and catalyst-loaded glassy carbon electrode as the working electrode. 1M KOH+0.5M NH3 electrolyte was prepared by adding 1 volume of 1M ammonia water to 1 volume of 2M KOH.

[0067] Figure 5 The cyclic voltammetry (CV) curves of Pt2Pd-3%CD in 1M KOH and 1M KOH+0.5M NH3 electrolytes are shown in Figure 1. Figure 5 As shown, an obvious ammonia oxidation peak was observed at 0.76 V vs RHE, indicating that the catalyst has the ability to catalyze ammonia oxidation.

[0068] Figure 6 CV diagrams of Pt2Pd-3%CD, Na-Pt2Pd and Na-Pt2Pd-3%CD in 1M KOH+0.5M NH3 electrolyte. Figure 6 It can be seen that Pt2Pd-3%CD (59.8 mA cm -2 ) is Na-Pt2Pd-3%CD (32.3 mA cm -2), indicating that the layer morphology helps improve the performance. At the same time, the peak current of Na-Pt2Pd is 22.0 mA cm -2 After adding CD, the performance increased by 1.47 times. After adding CD to Pt2Pd, the performance increased by 1.79 times, indicating that the introduction of CD has a higher performance improvement effect on the layered catalyst.

[0069] Figure 7 The CV graphs of Pt2Pd-3%CD and P-Pt2Pd-3%CD in 1M KOH+0.5M NH3 electrolyte. In the Pt2Pd-3%CD provided by the present invention, CD is added to Pt2Pd by H2 / Ar heat treatment. It is found that the performance of directly mixing CD and Pt2Pd (peak current 42.3mA cm -2 ) is also lower than Pt2Pd-3%CD.

[0070] Test Example 2

[0071] Comparison of the ammonia oxidation performance of catalysts with different Pt and Pd ratios and different CD contents. The test results are as follows: Figure 8 As shown, Figure 8 Figure 1 is a graph showing the test results of the ammonia oxidation performance of catalysts with different Pt and Pd ratios and different CD contents in 1M KOH + 0.5M NH3 electrolyte; wherein, a is the CV graph of Pt, PtPd, PtPd2, Pt2Pd and Pd, b is the CV graph of Pt2Pd, Pt2Pd-1%CD, Pt2Pd-3%CD, Pt2Pd-5%CD, Pt2Pd-10%CD and commercial Pt / C, c is the mass activity graph of Pt, PtPd, PtPd2, Pt2Pd and Pd, d is the mass activity diagram of Pt2Pd, Pt2Pd-1%CD, Pt2Pd-3%CD, Pt2Pd-5%CD, Pt2Pd-10%CD and commercial Pt / C; e is the peak mass activity bar chart of Pt, PtPd2, PtPd, Pt2Pd, Pt2Pd-1%CD, Pt2Pd-3%CD, Pt2Pd-5%CD, Pt2Pd-10%CD and commercial Pt / C.

[0072] Figure 8 Figure a shows that pure Pd has almost no ammonia oxidation performance, while the current density of the alloy Pt2Pd reaches 33.4 mA cm -2 , showing a higher performance than pure Pt (8.0 mA·cm -2 ), PtPd(23.7mA·cm -2 ) and PtPd2 (19.4 mA cm -2 ) have higher catalytic activity, which are 4.2, 1.4 and 1.7 times of the current density of Pt, PtPd and PtPd2, respectively. Figure 8 Figure b shows that adding 3% CD has the best effect on improving the performance of Pt2Pd, and the current density can reach 59.8 mA cm -2 ; Continuing to increase the content of CD, the performance actually decreases because the active sites are covered by CD. The mass activity of the catalyst is calculated according to the content of precious metal (PGM), such as Figure 8 As shown in c, d, and e, Pt2Pd-3%CD has the highest mass activity, reaching 175.5 A·g PGM -1 .

[0073] Test Example 3

[0074] Stability tests were conducted on Pt2Pd, Pt2Pd-1%CD, Pt2Pd-3%CD, Pt2Pd-5%CD, Pt2Pd-10%CD and commercial Pt / C. The test results are as follows: Fig. 9 As shown, Fig. 9 Figure 2 is a stability data diagram of Pt2Pd, Pt2Pd-1%CD, Pt2Pd-3%CD, Pt2Pd-5%CD, Pt2Pd-10%CD and commercial Pt / C; wherein, a is the mass activity diagram of Pt2Pd before and after 2000 CV cycles, b is the mass activity diagram of Pt2Pd-1%CD before and after 2000 CV cycles, c is the mass activity diagram of Pt2Pd-3%CD before and after 2000 CV cycles, d is the mass activity diagram of Pt2Pd-5%CD before and after 2000 CV cycles, e is the mass activity diagram of Pt2Pd-10%CD before and after 2000 CV cycles, and f is the constant potential test of Pt2Pd, Pt2Pd-1%CD, Pt2Pd-3%CD, Pt2Pd-5%CD, Pt2Pd-10%CD and commercial Pt / C (test potential is 0.72V vs Time-mass activity curve obtained by RHE.

[0075] from Fig. 9 As can be seen in Figure c, the mass activity of Pt2Pd-3%CD only decreased by 8.3%. Fig. 9 As can be seen in figure f, in the constant potential test, after 6000s, the performance of Pt2Pd-3%CD can still maintain 48.4% of the original, indicating that the stability of this catalyst is better than other catalysts and even better than commercial Pt / C.

[0076] In summary, the two-dimensional porous nanomaterial Pt2Pd-CD provided by the present invention has higher catalytic activity and stability for ammonia oxidation. The two-dimensional porous structure increases the number of active sites of the catalyst and the contact area with the reactants, significantly improving the catalytic activity. CD can also increase the adsorption of ammonia and stabilize the electronic structure, further increasing the activity and stability of the catalyst.

[0077] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing carbon dot-modified platinum-palladium alloy nanosheets, characterized in that: The following steps are involved: (1) dissolving a platinum salt, a palladium salt and an alkaline substance in an organic solvent to obtain a mixed solution, and subjecting the mixed solution to oxidation treatment to obtain a platinum-palladium oxide; (2) dissolving the platinum-palladium oxide obtained in step (1) and a reducing agent in water, and performing a reduction reaction at 60 to 80° C. to obtain platinum-palladium alloy nanosheets; the reducing agent is morpholine borane or dimethylformamide; (3) The platinum-palladium alloy nanosheets obtained in step (2) are mixed with carbon dots and placed in a heating device for calcination in a mixed gas atmosphere of hydrogen and inert gas to obtain the carbon dot-modified platinum-palladium alloy nanosheets.

2. The preparation method according to claim 1, characterized in that: In step (1), the platinum salt is platinum acetylacetonate, chloroplatinic acid or platinum tetrachloride, and the palladium salt is palladium acetylacetonate or palladium chloride.

3. The preparation method according to claim 1, characterized in that: In step (1), the alkaline substance is potassium carbonate or potassium hydroxide.

4. The preparation method according to claim 1 or 2, characterized in that: In step (1), the molar ratio of the platinum salt to the palladium salt is 1:(0.5-2).

5. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of the platinum palladium oxide to the reducing agent is 1:(5-15).

6. The preparation method according to claim 1, characterized in that: In step (3), the mass of the carbon dots is 1% to 10% of the mass of the platinum-palladium alloy nanosheets.

7. The preparation method according to claim 1, characterized in that: In step (3), the calcination treatment is carried out at 200-300°C.

8. A carbon-dot-modified platinum-palladium alloy nanosheet prepared by the method according to any one of claims 1 to 7.

9. Use of the carbon-dot-modified platinum-palladium alloy nanosheets according to claim 8 in an ammonia oxidation reaction.

10. A catalyst for an ammonia fuel cell, characterized in that: The platinum-palladium alloy nanosheet modified with carbon dots as described in claim 8 is provided.