Processing method of regenerated carbon black with high dispersion in synthetic rubber
Through multi-stage thermal cracking and crushing processes, the problems of poor dispersion and difficulty in deep processing of recycled carbon black in synthetic rubber are solved, the adsorption capacity and dispersion of the product are improved, and efficient carbon black processing is achieved, which is suitable for synthetic rubber such as D. Styrene rubber and butyl rubber, etc.
Patent Information
- Application Number
- CN202411210597.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
AI Technical Summary
Recycled carbon black is difficult to disperse in synthetic rubber, has a low structure, a small oil absorption value, iodine absorption value and specific surface area, and is prone to block the crusher during deep processing, affecting production capacity and grading effect.
Using multi-stage thermal cracking and crushing processes, including primary thermal cracking and secondary thermal cracking, combined with vibrating screens and iron removal treatment, controlling temperature and negative pressure, using ozone intake, gradually cooling and crushing, and improving the fineness and dispersion of carbon black sex.
Improves the iodine absorption value, specific surface area, toluene transmittance and dispersion of recycled carbon black, solves the problems of high oil absorption value, low production capacity and crusher blockage, enhances the stability and application value of the product, and can be high in synthetic rubber Use in dispersed manner.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of regenerated carbon black materials, and in particular relates to a processing method for highly dispersed regenerated carbon black in synthetic rubber. Background Art
[0002] Regenerated carbon black refers to the rubber blocks or rubber powder extracted from waste tires through steel wire, crushed and iron-removed, which are then subjected to thermal decomposition of the organic components inside by high temperature in an oxygen-deficient or inert gas atmosphere to release volatile products to form solid coke, which is then further processed by slag removal, iron removal, and crushing.
[0003] The regenerated carbon black currently produced in the market has cooled light oil and heavy oil on its surface, and has a high volatility. Even after deep processing, the regenerated carbon black products produced still have small oil absorption value, iodine absorption value and specific surface area, low structural degree, and are difficult to disperse in synthetic rubbers such as styrene-butadiene rubber, EPDM rubber, nitrile rubber, etc., and have no reinforcement effect. The regenerated carbon black in the market is mainly used in natural rubber systems, mainly due to the high self-reinforcement of natural rubber, and it is difficult to distinguish the dispersibility and reinforcement effect of fillers. In addition, during the deep processing of regenerated carbon black, due to its high volatile matter, it is difficult to crush it and is easy to clog the classifier of the crusher, so the crushing capacity is low and has the disadvantages of heavy odor. In view of the above technical problems, the present invention proposes a processing method for highly dispersed regenerated carbon black in synthetic rubber, which effectively solves the technical problems of regenerated carbon black in deep processing and use. Those skilled in the art are in urgent need of developing a processing method for highly dispersed regenerated carbon black in synthetic rubber to meet existing use requirements and market demand. Summary of the invention
[0004] The object of the present invention is to provide a processing method for highly dispersed regenerated carbon black in synthetic rubber to solve the above technical problems.
[0005] A processing method for highly dispersed regenerated carbon black in synthetic rubber comprises the following steps: 1) impurity removal: after the waste tire rubber powder is unpacked by a ton bag unpacking station, it is transported to a vibrating screen to remove gravel impurities larger than 5 mm, and then it is deironed by an iron remover and then enters a material buffer tank for standby use; 2) primary thermal cracking: after the waste tire rubber powder is impurity-removed and deironed, it enters a primary thermal cracking furnace through a conveying device for thermal decomposition treatment to obtain crude carbon black after primary thermal cracking; 3) primary crushing: the crude carbon black after primary thermal cracking is cooled to 64°C-70°C by a spiral cooling and discharging system, and then it is transported to a buffer tank after being treated by a vibrating screen and an iron remover, and then it is transported to a primary crusher for crushing to obtain crude carbon black after primary crushing; 4) Secondary thermal cracking: The crude carbon black after primary crushing enters the secondary thermal cracking furnace through the conveying equipment for pyrolysis treatment; 5) Secondary crushing: The crude carbon black after secondary thermal cracking is cooled to 58~70℃ by a spiral cooling and discharging system, and then transported to a buffer tank after being processed by a vibrating screen and an iron remover, and then transported to a secondary crusher for crushing. After passing the inspection, it is transported to a material buffer tank to obtain recycled carbon black that is highly dispersed in synthetic rubber.
[0006] Furthermore, the waste tire rubber powder is waste all-steel radial tire tread rubber powder.
[0007] Furthermore, in the primary thermal cracking process of the waste tire rubber powder: the feed rate of the cracking furnace is controlled at 0.32 t / h~0.6 t / h; the rotation speed of the cracking furnace is 5.2 r / min~6.5 r / min; the temperature of the cracking furnace is 310°C~380°C, and the negative pressure in the furnace is controlled at -0.028~-0.03 MPa.
[0008] Furthermore, the pulverizer speed of the primary pulverization process is 550 rpm / min~850 rpm / min; the mesh size of the coarse carbon black powder of the primary pulverization process is 100~300 meshes.
[0009] Furthermore, the secondary thermal cracking furnace performs a pyrolysis treatment process: the feed rate of the cracking furnace is controlled at 0.40 t / h~0.80 t / h; the rotation speed of the cracking furnace is 4.2 r / min~6.2 r / min; the temperature of the cracking furnace is 420°C~450°C, and the negative pressure in the furnace is controlled at -0.028~-0.03 MPa; the ozone intake rate of the cracking furnace is 10~40 L / min, and the ozone concentration is 5~10 ppm.
[0010] Furthermore, the feed rate of the secondary crushing process is controlled at 2.2-2.9 t / h; the pulverizer speed of the secondary crushing process is 1800-2600 rpm / min; and the mesh size of the coarse carbon black powder of the secondary crushing process is 800-1250 mesh.
[0011] Furthermore, the synthetic rubber is preferably one of styrene-butadiene rubber, butyl rubber or ethylene-propylene-diene rubber.
[0012] Furthermore, the oil absorption value of the regenerated carbon black product is ≥0.81cm 3 / g; the compression oil absorption value of the regenerated carbon black product is ≥0.62×10 -5 m 3 / g; the iodine absorption value of the regenerated carbon black product is ≥119g / kg; the toluene transmittance of the regenerated carbon black product is ≥90%; the nitrogen adsorption specific surface area of the regenerated carbon black product is ≥60m 2 / g; the ash content of the regenerated carbon black product is ≤16.2%; the particle size D99 of the regenerated carbon black product is ≤30μm.
[0013] The first purpose of the present invention is to provide a processing method for highly dispersed regenerated carbon black in synthetic rubber, thereby solving the problem of high light oil and heavy oil content in the regenerated carbon black.
[0014] The second purpose of the present invention is to provide a processing method for highly dispersed regenerated carbon black in synthetic rubber, which effectively solves the problems of low production capacity, clogging of crusher and classifier, and difficulty in granulation during the deep processing of regenerated carbon black.
[0015] The third purpose of the present invention is to provide a processing method for highly dispersed regenerated carbon black in synthetic rubber, which improves the iodine absorption value, specific surface area, toluene transmittance, surface activity and dispersibility of the regenerated carbon black product, making the product quality more stable.
[0016] The fourth purpose of the present invention is to improve the application value of regenerated carbon black, which can be expanded not only in natural rubber, but also in synthetic rubber, such as styrene-butadiene rubber, butyl rubber, EPDM rubber, etc.
[0017] The present invention has the following beneficial effects: The invention discloses a processing method for highly dispersed regenerated carbon black in synthetic rubber, which solves the problem of high light oil and heavy oil content of the regenerated carbon black, and effectively improves the problems of low production capacity, clogging of a crusher and classifier, and difficulty in granulation in the deep processing of the regenerated carbon black. At the same time, the iodine absorption value, specific surface area, toluene transmittance, surface activity and dispersibility of the product are improved, so that the product quality is more stable and can be higher than the industry standard requirements, so that it can not only be used in natural rubber with an expanded filling amount, but also can be used in synthetic rubber with high dispersion, such as styrene-butadiene rubber, butyl rubber, EPDM rubber, etc. DETAILED DESCRIPTION
[0018] The present invention is described below with specific examples, but is not intended to be limiting of the present invention. Example 1
[0019] The tread rubber powder of the all-steel tire is passed through a 5mm swing vibrating screen to remove impurities, and then passed through an iron remover to remove iron filings, and then transported to the material buffer bin. After iron and impurities are removed, the regenerated carbon black enters the primary thermal cracking furnace through the conveying equipment, with a feed rate of 0.32t / h and a rotation speed of 5.2r / min for the activation furnace. The temperature of the primary thermal cracking furnace is set at 310℃, and the negative pressure in the furnace is -0.03MPa. After the thermal cracking is completed, the material is cooled to 70℃ by a three-stage screw cooling conveyor and enters the buffer bin.
[0020] The coarse coke slag from the primary thermal cracking is transported to the crusher at a speed of 550rpm / min to obtain the coarse coke slag powder from the primary thermal cracking. It is then transported to the secondary thermal cracking furnace at a feed rate of 0.40t / h and a speed of 6.2r / min for the activation furnace. The temperature of the secondary thermal cracking furnace is set at 420℃, the negative pressure in the furnace is -0.03MPa, the ozone intake volume is 10L / min, and the ozone concentration is 5ppm. The material after the secondary thermal cracking is cooled to 70℃ by a three-stage screw cooling conveyor and enters the buffer silo.
[0021] The coarse coke slag powder from the secondary thermal cracking is transported to the crusher with a feed rate of 2.9 t / h and a crusher rotation speed of 1800 rpm / min. The obtained ultrafine regenerated carbon black powder has a mesh size of 800 meshes. Example 2
[0022] The tread rubber powder of the all-steel tire is passed through a 5mm swing vibrating screen to remove impurities, and then passed through an iron remover to remove iron filings, and then transported to the material buffer bin. After iron and impurities are removed, the regenerated carbon black enters the primary thermal cracking furnace through the conveying equipment, with a feed rate of 0.53t / h and a rotation speed of 5.2r / min for the activation furnace. The temperature of the primary thermal cracking furnace is set at 330℃, and the negative pressure in the furnace is -0.028MPa. After the thermal cracking is completed, the material is cooled to 69℃ by a three-stage screw cooling conveyor and enters the buffer bin.
[0023] The coarse coke slag from the primary thermal cracking is transported to the crusher at a speed of 820rpm / min to obtain the coarse coke slag powder from the primary thermal cracking. It is then transported to the secondary thermal cracking furnace at a feed rate of 0.80t / h and a speed of 4.2r / min for the activation furnace. The temperature of the secondary thermal cracking furnace is set at 430℃, the negative pressure in the furnace is -0.028MPa, the ozone intake volume is 20L / min, and the ozone concentration is 5.4ppm. The material after the secondary thermal cracking is cooled to 58℃ by a three-stage screw cooling conveyor and enters the buffer silo.
[0024] The coarse coke slag powder from the secondary thermal cracking is transported to the crusher with a feed rate of 2.2 t / h and a crusher rotation speed of 2600 rpm / min. The obtained ultrafine regenerated carbon black powder has a mesh size of 1250 mesh. Example 3
[0025] The rubber powder of the all-steel tire tread is passed through a 5mm swing vibrating screen to remove impurities, and then passed through an iron remover to remove iron filings, and then transported to the material buffer bin. After iron and impurities are removed, the regenerated carbon black enters the primary thermal cracking furnace through the conveying equipment, with a feed rate of 0.6t / h and a rotation speed of 6.5r / min for the activation furnace. The temperature of the primary thermal cracking furnace is set at 380℃, and the negative pressure in the furnace is -0.03MPa. After the thermal cracking is completed, the material is cooled to 64℃ by a three-stage screw cooling conveyor and enters the buffer bin.
[0026] The coarse coke slag from the primary thermal cracking is transported to the crusher at a speed of 850rpm / min to obtain the coarse coke slag powder from the primary thermal cracking. It is then transported to the secondary thermal cracking furnace at a feed rate of 0.75t / h and a speed of 5.8r / min for the activation furnace. The temperature of the secondary thermal cracking furnace is set at 450℃, the negative pressure in the furnace is -0.03MPa, the ozone intake volume is 40L / min, and the ozone concentration is 10ppm. After the secondary thermal cracking, the material is cooled to 63℃ by a three-stage screw cooling conveyor and enters the buffer silo.
[0027] The coarse coke slag powder from the secondary thermal cracking is transported to the crusher with a feed rate of 2.6 t / h and a crusher rotation speed of 2400 rpm / min. The obtained ultrafine regenerated carbon black powder has a mesh size of 1000 mesh.
[0028] Comparative Example 1 Refer to Example 1, except that no secondary cracking treatment is performed, and the remaining steps are the same. Example 4
[0029] The tread rubber powder of the all-steel tire is passed through a 5mm swing vibrating screen to remove impurities, and then passed through an iron remover to remove iron filings, and then transported to the material buffer bin. After iron and impurities are removed, the regenerated carbon black enters the primary thermal cracking furnace through the conveying equipment, with a feed rate of 0.4t / h and a rotation speed of 6r / min for the activation furnace. The temperature of the primary thermal cracking furnace is set at 330℃, and the negative pressure in the furnace is -0.028MPa. After the thermal cracking is completed, the material is cooled to 70℃ by a three-stage screw cooling conveyor and enters the buffer bin.
[0030] The coarse coke slag from the primary thermal cracking is transported to the crusher at a speed of 560rpm / min to obtain the coarse coke slag powder from the primary thermal cracking. It is then transported to the secondary thermal cracking furnace at a feed rate of 0.45t / h and a speed of 6r / min for the activation furnace. The temperature of the secondary thermal cracking furnace is set at 400℃, the negative pressure in the furnace is -0.03MPa, the ozone intake volume is 7L / min, and the ozone concentration is 7ppm. After the secondary thermal cracking, the material is cooled to 70℃ by a three-stage screw cooling conveyor and enters the buffer silo.
[0031] The coarse coke slag powder from the secondary thermal cracking is transported to the crusher with a feed rate of 2.8 t / h and a crusher rotation speed of 1800 rpm / min. The obtained ultrafine regenerated carbon black powder has a mesh size of 800 meshes.
[0032] In order to compare and illustrate the properties of the regenerated carbon black obtained in different embodiments and comparative examples, the properties of the regenerated carbon black obtained in Examples 1 to 4 and Comparative Example 1 were tested, and the test results are shown in Table 1.
[0033] Table 1 Test results of properties of regenerated carbon black of Examples 1 to 4 and Comparative Example 1
[0034] Note: Specific surface area is tested by nitrogen adsorption method according to GB / T10722-2014 Determination of total surface area and external surface area of carbon black; iodine absorption value is tested according to GB / T3780.1-2015 Carbon black Part 1: Iodine absorption value test method; oil absorption value is tested according to GB / T3780.2-2017 Carbon black Part 2: Determination of oil absorption value; volatile matter is tested according to GB / T7047-2006 Determination of volatile matter content of pigment carbon black; ash content is tested according to GB / T3780.10-2017 Carbon black Part 10: Determination of ash content; toluene transmittance is tested according to GB / T3780.15-2016 Carbon black Part 15: Determination of transmittance of toluene extract. Compression oil absorption value refers to GB / T3780.4-2017 Carbon black Part 4: Determination of oil absorption value of compressed specimen.
[0035] In order to compare and illustrate the effects of the regenerated carbon black obtained from different embodiments and comparative examples on the properties of styrene-butadiene rubber, the regenerated carbon black of embodiments 1 to 3 and comparative example 1 were applied to rubber respectively according to the following method, and the mechanical properties of styrene-butadiene rubber were tested. The test results are shown in Table 2.
[0036] The specific rubber material is mixed according to the following components in parts by weight: 100 parts of SBR1502 styrene-butadiene rubber, 50 parts of regenerated carbon black in the examples and comparative examples, 1 part of stearic acid, 3 parts of zinc oxide, 1 part of accelerator NS, 1.75 parts of sulfur, and the vulcanization time is 145°C×50min.
[0037] Table 2 Mechanical properties test results of examples 1 to 3 and comparative example 1 filled with styrene butadiene rubber
[0038] The specific rubber material of the regenerated carbon black obtained in Example 4 was mixed according to the following components in parts by weight: 100 parts of Xinhui CB-01 butyl rubber, 50 parts of regenerated carbon black, 1 part of stearic acid, 3 parts of zinc oxide, 1 part of TMTD, and 1.75 parts of sulfur, and the vulcanization time was 145°C×50min.
[0039] Products: 65 Shore hardness, tensile strength 15.2MPa, 300% elongation at break 7.8MPa, elongation at break 500%, tear strength 36.5N / mm, dispersion grade (Y value) 3.7.
[0040] Comparative Example 1 The rubber material was mixed according to the following components in parts by weight: 100 parts of Cinhui CB-01 butyl rubber, 50 parts of IRB carbon black, 1 part of stearic acid, 3 parts of zinc oxide, 1 part of TMTD, and 1.75 parts of sulfur. The vulcanization time was 145°C×50min.
[0041] Products: 65 Shore hardness, tensile strength 15.2MPa, 300% elongation at break 7.8MPa, elongation at break 500%, tear strength 42.9N / mm, dispersion grade (Y value) 2.6.
[0042] In summary, it can be seen that the obtained regenerated carbon black has excellent performance.
[0043] Note: Type 1 test specimens with a thickness of 2.0 mm in accordance with GB / T528-2009 are prepared by cutting with a type 1 cutter; the tensile strength, 300% modulus and elongation at break are measured in accordance with the provisions of GB / T528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber, and the moving speed of the clamp is 500 mm / min; the dispersion of carbon black is in accordance with ISO11345-2006 Rapid comparison method for the evaluation of rubber carbon black and carbon black / silicon dioxide dispersions; the relative volume abrasion test is carried out in accordance with the provisions of GB / T9867-2008 Determination of wear resistance of vulcanized rubber or thermoplastic rubber (rotating roller abrader method); the tear strength test is carried out in accordance with the rectangular provisions of GB / T529-2008 Determination of tear strength of vulcanized rubber or thermoplastic rubber.
Claims
1. A processing method for highly dispersed regenerated carbon black in synthetic rubber, characterized in that: The steps include: 1) Impurity removal: After the waste tire rubber powder is unpacked at the ton bag unpacking station, it is transported to the vibrating screen to remove gravel impurities larger than 5mm, and then it is removed by the iron remover and then enters the material buffer tank for standby use; 2) Primary pyrolysis: After the impurities and iron are removed, the waste tire rubber powder enters the primary pyrolysis furnace through the conveying equipment for pyrolysis treatment to obtain crude carbon black after primary pyrolysis; 3) Primary crushing: The crude carbon black after primary thermal cracking is cooled to 64℃~70℃ by a spiral cooling discharging system, and then transported to a buffer tank after being processed by a vibrating screen and an iron remover, and then transported to a primary crusher for crushing to obtain crude carbon black after primary crushing; 4) Secondary thermal cracking: The crude carbon black after primary crushing enters the secondary thermal cracking furnace through the conveying equipment for pyrolysis treatment; 5) Secondary crushing: The crude carbon black after secondary thermal cracking is cooled to 58~70℃ by a spiral cooling and discharging system, and then transported to a buffer tank after being processed by a vibrating screen and an iron remover, and then transported to a secondary crusher for crushing. After passing the inspection, it is transported to a material buffer tank to obtain recycled carbon black that is highly dispersed in synthetic rubber.
2. The method for processing highly dispersed regenerated carbon black in synthetic rubber according to claim 1, characterized in that: The waste tire rubber powder is waste all-steel radial tire tread rubber powder.
3. The method for processing highly dispersed regenerated carbon black in synthetic rubber according to claim 1, characterized in that: The primary thermal cracking process of the waste tire rubber powder: the feed rate of the cracking furnace is controlled at 0.32t / h~0.6t / h; the rotation speed of the cracking furnace is 5.2r / min~6.5r / min; the temperature of the cracking furnace is 310℃~380℃, and the negative pressure in the furnace is controlled at -0.028~-0.03MPa.
4. The method for processing highly dispersed regenerated carbon black in synthetic rubber according to claim 1, characterized in that: The pulverizer speed of the primary pulverization process is 550 rpm / min~850 rpm / min; the mesh size of the coarse carbon black powder of the primary pulverization process is 100~300 meshes.
5. The method for processing highly dispersed regenerated carbon black in synthetic rubber according to claim 1, characterized in that: The secondary thermal cracking furnace performs a pyrolysis treatment process: the feed rate of the cracking furnace is controlled at 0.40 t / h~0.80 t / h; the rotation speed of the cracking furnace is 4.2 r / min~6.2 r / min; the temperature of the cracking furnace is 420°C~450°C, and the negative pressure in the furnace is controlled at -0.028~-0.03 MPa; the ozone intake rate of the cracking furnace is 10~40 L / min, and the ozone concentration is 5~10 ppm.
6. The method for processing highly dispersed regenerated carbon black in synthetic rubber according to claim 1, characterized in that: The feed rate of the secondary pulverization process is controlled at 2.2-2.9 t / h; the pulverizer speed of the secondary pulverization process is 1800-2600 rpm / min; the mesh size of the coarse carbon black powder of the secondary pulverization process is 800-1250 mesh.
7. The method for processing highly dispersed regenerated carbon black in synthetic rubber according to claim 1, characterized in that: The oil absorption value of the regenerated carbon black product is ≥81×10 -5 m 3 / g; the compression oil absorption value of the regenerated carbon black product is ≥62×10 -5 m 3 / g; the iodine absorption value of the regenerated carbon black product is ≥119g / kg; the toluene transmittance of the regenerated carbon black product is ≥90%; the nitrogen adsorption specific surface area of the regenerated carbon black product is ≥60m 2 / g; the ash content of the regenerated carbon black product is ≤16.2%; the particle size D99 of the regenerated carbon black product is ≤30μm.