High-voltage lithium / carbon fluoride battery electrolyte and battery

By using an electrolyte composed of high donor number solvents and additives, the problems of low voltage and severe heat generation in lithium/carbon fluoride batteries have been solved, improving the battery's voltage and rate performance, making it suitable for high-end equipment and aerospace applications.

CN118943467APending Publication Date: 2024-11-12NANKAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411333135.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Lithium/carbon fluoride batteries suffer from problems such as low voltage, severe heat generation, and poor rate performance in practical applications, which affect their use in high-end equipment and aerospace fields.

Method used

An electrolyte composed of high donor number solvents and high donor number additives, including dimethyl sulfoxide, N-methylpyrrolidone, N-methylimidazolium, triethylamine and ethylenediamine, is used to regulate the solvation structure of the electrolyte, thereby improving the stability of the discharge intermediate phase and battery performance.

Benefits of technology

It improves the voltage and rate performance of lithium/carbon fluoride batteries, suppresses heat generation, enhances battery safety and dynamic performance, and meets the application requirements of high-end equipment and aerospace.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943467A_ABST
    Figure CN118943467A_ABST
Patent Text Reader

Abstract

The invention discloses a high-voltage lithium / carbon fluoride battery electrolyte and a battery. The electrolyte is composed of lithium tetrafluoroborate, a high-donor-number solvent and a high-donor-number additive; the high donor number solvent is dimethyl sulfoxide and N-methyl pyrrolidone; the additive with the high donor number is N-methylimidazole, triethylamine and ethidene diamine. The high-voltage lithium / carbon fluoride battery comprises a positive electrode, a negative electrode, a diaphragm and the high-voltage lithium / carbon fluoride battery electrolyte. According to the invention, the discharge of the Li / CFx battery is creatively changed into a thermodynamic process and a dynamic process, a thermal effect and an electric effect are accompanied with each other in the whole process of battery discharge, a strategy of increasing electrolyte Gibbs free energy to improve the stability of a discharge intermediate phase is provided, the voltage and rate performance of the Li / CFx battery are improved, and the heat production of the battery is inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of primary batteries, in particular to a high-voltage lithium / carbon fluoride battery electrolyte and a battery. Background Art

[0002] In the military and aerospace fields, equipment such as intelligent guided missiles, underwater spacecraft, drones, and ground combat vehicles urgently need reliable and lightweight battery products to improve their combat capabilities and flexibility. Although current secondary lithium-ion batteries have certain advantages, it is still difficult to meet the requirements of high specific capacity and high reliability required for combat readiness or actual combat. In contrast, lithium / carbon fluoride (Li / CF x ) The theoretical energy density of the battery system is as high as 2180Wh / kg. It is the optimal lightweight primary battery based on the redox system. It has the characteristics of stable voltage, low self-discharge rate, long life and good high and low temperature resistance, which can meet the application requirements of high-end civilian instruments, military equipment and aerospace power supply. Therefore, the development of high-voltage lithium / carbon fluoride batteries has scientific and practical significance.

[0003] However, in lithium / carbon fluoride batteries, lithium and carbon fluoride cannot directly generate lithium fluoride and carbon, but first generate an intermediate phase containing lithium, fluorine, carbon and solvent molecules, which changes the Gibbs free energy of the electrochemical reaction. Derived from the Nernst equation -ΔG=zFE, its operating voltage is much lower than the theoretical voltage (4.57V); the first step of battery discharge is electrochemical reaction, and the second step is thermal decomposition reaction. Lithium / carbon fluoride batteries discharge more than lithium metal batteries, and the battery generates more heat; the crystal size of the discharge product lithium fluoride is larger. As the depth of discharge increases, lithium fluoride will block the ion transmission channel, affecting the battery's rate performance. These factors seriously restrict the practical application of lithium / carbon fluoride batteries.

[0004] The donor number (DN) is an indicator that describes the Lewis basicity of solvent molecules or anions, and describes the tendency to donate electrons to electron acceptors. The higher the donor number, the higher the ability and probability of binding with lithium ions, which in turn affects the solvation structure. The higher the donor number, the stronger the Lewis basicity and the stronger the corrosion to lithium metal. Solvents with DN < 20 are called low donor number solvents. Solvents with DN > 30 will directly react with metallic lithium, causing battery gas production and other phenomena, so that they cannot be used as electrolytes alone.

[0005] Therefore, designing a lithium / carbon fluoride battery electrolyte that can simultaneously increase battery voltage, inhibit heat generation and improve battery rate performance is of great significance for promoting the application of lithium / carbon fluoride batteries in the field of large-scale energy storage. Summary of the invention

[0006] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a high-voltage lithium / carbon fluoride battery electrolyte and a battery.

[0007] The technical solution of the present invention to solve the technical problem of the electrolyte is to provide a high-voltage lithium / carbon fluoride battery electrolyte, characterized in that the electrolyte is composed of lithium tetrafluoroborate, a high donor number solvent and a high donor number additive;

[0008] The high donor number solvents are dimethyl sulfoxide and N-methylpyrrolidone; the high donor number additives are N-methylimidazole, triethylamine and ethylenediamine.

[0009] The technical solution of the present invention to solve the battery technical problem is to provide a high-voltage lithium / carbon fluoride battery, characterized in that the battery includes a positive electrode, a negative electrode, a separator and the high-voltage lithium / carbon fluoride battery electrolyte.

[0010] Compared with the prior art, the present invention has the following beneficial effects:

[0011] (1) The present invention creatively regards the discharge of Li / CFx batteries as two processes, thermodynamics and kinetics, and the thermal effect and electrical effect accompany each other in the whole process of battery discharge. It proposes a strategy to increase the Gibbs free energy of the electrolyte to improve the stability of the discharge intermediate phase, thereby improving the Li / CF x Battery voltage and rate performance, suppressing battery heat generation.

[0012] (2) The present invention introduces a high donor number additive into the electrolyte. The high donor number additive can make the solvation configuration in the electrolyte more compact, generate a more stable intermediate phase during the discharge process, increase the battery voltage from a thermodynamic point of view, and thus increase the battery energy density; the total Gibbs free energy of the reaction is constant, and the use of a high donor number additive can inhibit the decomposition of the intermediate phase and the generation of lithium fluoride, reduce the Gibbs free energy of the thermal decomposition reaction, inhibit the heat generation of the battery, and improve the battery safety performance; the high donor number additive can reduce the size of the discharge product lithium fluoride, avoid large, high-crystalline lithium fluoride blocking the ion channel, accelerate ion transmission, improve the battery rate performance, and improve the battery kinetic performance.

[0013] (3) The present invention screens solvents based on the donor number (DN), mixes high donor number additives with DN>30 with high donor number solvents with DN<30, regulates the solvation structure of the electrolyte, improves the stability of the battery discharge intermediate phase, and enables the battery to have better performance. According to the physical and chemical properties of the solvent, the needs of the battery in different usage scenarios can be met. The use of solvents with lower viscosity and better wettability can make the battery have better rate performance and poor electrolyte performance; the use of solvents with higher dielectric constants can affect the dissociation of lithium salts, which can make the battery have better discharge specific capacity; the use of solvents with better thermal stability and higher boiling point can make the battery operate stably at high temperatures.

[0014] (4) The electrolyte components of the present invention have the advantages of low cost, easy preparation, safety and no pollution, and can be used on a large scale.

[0015] (5) Based on the electrolyte of the present invention, by matching the graphite fluoride positive electrode and the lithium metal negative electrode, the assembled full battery exhibits a higher voltage and a discharge specific capacity close to the theory at room temperature and high temperature, effectively solving the problem of low battery discharge voltage. At the same time, the assembled soft-pack battery and high-capacity battery also achieve high-voltage stable discharge, which is of great significance to promoting the application of lithium / carbon fluoride batteries in the field of large-scale energy storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a desolvation energy test diagram of the electrolytes of Examples 1 to 2 of the present invention and Comparative Examples 1 to 2;

[0017] Figure 2 The electrolyte of Examples 1 to 2 of the present invention and Comparative Examples 1 to 2 7 Li NMR spectrum;

[0018] Figure 3 The discharge curves of the batteries of Examples 3 to 4 and Comparative Examples 3 to 4 of the present invention at a rate of 0.01C are shown;

[0019] Figure 4 The discharge curves of the batteries of Examples 3 to 4 and Comparative Examples 3 to 4 of the present invention at a rate of 0.1C are shown;

[0020] Figure 5 The discharge curves of the batteries of Examples 3 to 4 and Comparative Examples 3 to 4 of the present invention at a 1C rate are shown;

[0021] Figure 6 The discharge curves of the batteries of Examples 3 to 4 and Comparative Examples 3 to 4 of the present invention at a rate of 5C are shown;

[0022] Figure 7 This is a constant current intermittent titration technology test curve diagram of the battery of Comparative Example 3 of the present invention;

[0023] Figure 8 This is a constant current intermittent titration technology test curve diagram of the battery of Example 4 of the present invention;

[0024] Fig. 9 The voltage-diffusion coefficient curves of the batteries of Comparative Example 3 and Example 4 of the present invention tested by constant current intermittent titration technology;

[0025] Fig.10 Graphs showing discharge curves of batteries of Example 7 and Example 8 of the present invention at 0.1C and 5C rates;

[0026] Fig.11 This is a SEM image of the surface of the pole piece of Comparative Example 5 of the present invention;

[0027] Fig.12 This is a SEM image of the surface of the pole piece of Comparative Example 6 of the present invention;

[0028] Fig.13 This is a SEM image of the surface of the pole piece of Example 9 of the present invention;

[0029] Fig.14 is a SEM image of the surface of the pole piece of Example 10 of the present invention;

[0030] Fig.15 This is the XRD diagram of the pole piece of Comparative Example 5 of the present invention;

[0031] Fig.16 is the XRD diagram of the pole piece of Example 9 of the present invention;

[0032] Fig.17 It is a ratio diagram of the strength of the Li-F bond and the CF bond in the XPS characterization of the electrode surface of Example 9 of the present invention and Comparative Example 5;

[0033] Fig.18 It is a test curve diagram of adiabatic accelerating calorimeter of the battery of Example 11 of the present invention and Comparative Example 7. DETAILED DESCRIPTION

[0034] The specific embodiments of the present invention are given below. The specific embodiments are only used to further illustrate the present invention in detail and do not limit the protection scope of the present invention.

[0035] The present invention provides a high-voltage lithium / carbon fluoride battery electrolyte (hereinafter referred to as electrolyte), characterized in that the electrolyte consists of lithium tetrafluoroborate, a high donor number solvent and a high donor number additive;

[0036] The high donor number solvent uses a solvent with a relatively high dielectric constant and a donor number close to 30; in order to ensure better battery performance, a solvent with DN>30 is used as a high donor number additive.

[0037] The high donor number solvent is dimethyl sulfoxide (DMSO, DN = 29.8 kcal mol -1 ) and N-methylpyrrolidone (NMP, DN = 27.3 kcal mol -1 ); the high donor number additive is N-methylimidazole (N-MeIM, DN = 47 kcal mol -1 ), triethylamine (TEA, DN = 61 kcal mol -1 ) and ethylenediamine (EDA, DN = 55 kcal mol -1 ).

[0038] Preferably, when the high donor number additive is triethylamine, the high donor number solvent is N-methylpyrrolidone; when the high donor number additive is N-methylimidazole, the high donor number solvent is dimethyl sulfoxide and / or N-methylpyrrolidone (preferably dimethyl sulfoxide); when the high donor number additive is ethylenediamine, the high donor number solvent is dimethyl sulfoxide.

[0039] Preferably, the concentration of lithium tetrafluoroborate is 0.5 to 1 mol / L (preferably 0.5 mol / L); the volume ratio of the high donor number solvent to the high donor number additive is 1 to 4:1 (preferably 4:1).

[0040] Preferably, the electrolyte is prepared by first mixing a high donor number additive and a high donor number solvent evenly to form a co-solvent; and then adding lithium tetrafluoroborate and dissolving the lithium tetrafluoroborate to obtain the electrolyte.

[0041] The present invention also provides a high-voltage lithium / carbon fluoride battery (referred to as battery for short), characterized in that the battery comprises a positive electrode, a negative electrode, a separator and the high-voltage lithium / carbon fluoride battery electrolyte.

[0042] Preferably, the positive electrode active material is a fluorinated carbon material, including fluorinated graphite.

[0043] Preferably, the preparation method of the positive electrode material is: disperse the carbon fluoride material, the conductive agent conductive carbon black and the binder PVDF in N-methylpyrrolidone in a mass ratio of 7 to 9:0.5 to 2:0.5 to 1 (preferably 8:1:1), mix them evenly and apply them on a carbon-coated aluminum foil (i.e., a carbon layer coated on aluminum) current collector, and obtain it after drying.

[0044] Preferably, the negative electrode is a lithium sheet or a lithium ribbon with a thickness of 50 to 100 μm.

[0045] Preferably, the separator is a PE separator (thickness 25 μm).

[0046] Example 1

[0047] The electrolyte consists of lithium tetrafluoroborate, dimethyl sulfoxide and N-methylimidazole; the concentration of lithium tetrafluoroborate is 0.5 mol L -1 ; The volume ratio of dimethyl sulfoxide and N-methylimidazole is 4:1.

[0048] The specific preparation method is: first, dimethyl sulfoxide and N-methylimidazole are mixed evenly in a volume ratio of 4:1 to form a co-solvent; then lithium tetrafluoroborate is added and dissolved to obtain a lithium tetrafluoroborate concentration of 0.5 mol L -1 of uniform electrolyte.

[0049] Example 2

[0050] The electrolyte consists of lithium tetrafluoroborate, N-methylpyrrolidone and triethylamine; the concentration of lithium tetrafluoroborate is 0.5 mol L -1 ; The volume ratio of N-methylpyrrolidone and triethylamine is 4:1.

[0051] The specific configuration method is: first, N-methylpyrrolidone and triethylamine are mixed evenly at a volume ratio of 4:1 to form a co-solvent; then lithium tetrafluoroborate is added and dissolved to obtain a lithium tetrafluoroborate concentration of 0.5 mol L -1 of uniform electrolyte.

[0052] Comparative Example 1

[0053] The electrolyte is composed of lithium tetrafluoroborate and dimethyl carbonate (DMC, DN = 17.2 kcal mol -1 ) composition; the concentration of lithium tetrafluoroborate is 0.5 mol L -1 .

[0054] Comparative Example 2

[0055] The electrolyte consists of lithium tetrafluoroborate and dimethyl sulfoxide; the concentration of lithium tetrafluoroborate is 0.5 mol L -1 .

[0056] The desolvation energy test was performed on the electrolytes of Examples 1 to 2 and Comparative Examples 1 to 2 ( Figure 1 ), 7 Li NMR spectrum ( Figure 2 ) to characterize the solvation structures of electrolytes with different compositions.

[0057] Depend on Figure 1 It can be seen that the desolvation energies of Examples 1-2 with the addition of triethylamine and N-methylimidazole are higher than those of Comparative Example 2 with only a high donor number solvent and Comparative Example 1 with only dimethyl carbonate.

[0058] Depend on Figure 2 It can be seen that Examples 1 to 2 in which triethylamine and N-methylimidazole were added had a significant effect on Li +The shielding effect is stronger than that of Comparative Examples 1 to 2, and the solvation structure is more compact.

[0059] Example 3

[0060] Positive electrode: Graphite fluoride, conductive carbon black (Super P) and PVDF were mixed evenly in a mass ratio of 8:1:1, dispersed in N-methylpyrrolidone, and stirred for 8 hours until the positive electrode slurry was uniformly obtained; then the positive electrode slurry was evenly coated on a carbon-coated aluminum foil, dried in a drying oven at 80°C for 12 hours, and then cut into positive electrodes with a diameter of 10 mm;

[0061] Negative electrode: lithium sheet, 14mm in diameter and 100μm in thickness;

[0062] Diaphragm: PE diaphragm, SK innovation Co. Ltd;

[0063] Electrolyte: The electrolyte of Example 1 was used.

[0064] Battery assembly: Assemble button cells in the order of negative electrode shell - spring - gasket - negative electrode - electrolyte - diaphragm - electrolyte - positive electrode - positive electrode shell. The battery specification is 2032.

[0065] After the assembled battery was left to rest for 8 hours, a discharge test was performed at room temperature with a cut-off voltage of 1.5 V, and the battery's discharge specific capacity was calculated using graphite fluoride in the positive electrode material as the active substance.

[0066] Example 4

[0067] Positive electrode, negative electrode and separator: the same as in Example 3.

[0068] Electrolyte: The electrolyte of Example 2 was used.

[0069] Battery assembly: Same as Example 3.

[0070] After the assembled battery was left to rest for 8 hours, a discharge test was performed at room temperature with a cut-off voltage of 1.5 V, and the battery's discharge specific capacity was calculated using graphite fluoride in the positive electrode material as the active substance.

[0071] Comparative Example 3

[0072] Positive electrode, negative electrode and separator: the same as in Example 3.

[0073] Electrolyte: The electrolyte of Comparative Example 1 was used.

[0074] Battery assembly: Same as Example 3.

[0075] After the assembled battery was left to rest for 8 hours, a discharge test was performed at room temperature with a cut-off voltage of 1.5 V, and the battery's discharge specific capacity was calculated using graphite fluoride in the positive electrode material as the active substance.

[0076] Comparative Example 4

[0077] Positive electrode, negative electrode and separator: the same as in Example 3.

[0078] Electrolyte: The electrolyte of Comparative Example 2 was used.

[0079] Battery assembly: Same as Example 3.

[0080] After the assembled battery was left to rest for 8 hours, a discharge test was performed at room temperature with a cut-off voltage of 1.5 V, and the battery's discharge specific capacity was calculated using graphite fluoride in the positive electrode material as the active substance.

[0081] Depend on Figures 3 to 6 It can be seen that the electrolytes obtained using Examples 1 and 2 have excellent battery performance at different rates of 0.01C, 0.1C, 1C, and 5C. Table 1 shows the battery performance of Examples 3-4 and Comparative Examples 3-4.

[0082] Table 1

[0083] It can be seen from Table 1 that at the rates of 0.01C, 0.1C, 1C, and 5C, Examples 3 and 4 have better battery performance. This is because the electrolytes of Examples 3 and 4 contain high donor number additives, which form a more compact solvation structure. x A more stable intermediate phase is generated during the battery discharge process. The total ΔG before and after the reaction is constant. When a high donor number electrolyte is used, the electrochemical potential of the discharge intermediate phase is lower, and the |ΔG| of the first electrochemical reaction is higher. According to the Nernst equation, its voltage is higher, so that the battery corresponding to the electrolyte using high donor number additives N-methylimidazole and triethylamine has excellent discharge performance at rates of 0.01C, 0.1C, 1C, and 5C.

[0084] Depend on Figures 7-8 It can be seen that the electrolyte of Example 2 has a higher equilibrium potential than the electrolyte of Comparative Example 1. At the same time, as the discharge depth increases, the polarization of the electrolyte of Comparative Example 1 is greater than that of Example 2, and E s With E t The ratio is smaller. Fig. 9 It can be seen that when the same positive electrode graphite fluoride is used, the battery uses the electrolyte of Example 2, and the ion diffusion coefficient is higher.

[0085] Example 5

[0086] The electrolyte consists of lithium tetrafluoroborate, N-methylpyrrolidone and N-methylimidazole; the concentration of lithium tetrafluoroborate is 0.5 mol / L; and the volume ratio of N-methylpyrrolidone to N-methylimidazole is 4:1.

[0087] The specific preparation method is: first, N-methylpyrrolidone and N-methylimidazole are mixed evenly in a volume ratio of 4:1 to form a co-solvent; then lithium tetrafluoroborate is added, and after dissolution, the concentration of lithium tetrafluoroborate is 0.5 mol L -1 of uniform electrolyte.

[0088] Example 6

[0089] The electrolyte consists of lithium tetrafluoroborate, dimethyl sulfoxide and ethylenediamine; the concentration of lithium tetrafluoroborate is 0.5 mol L -1 ; The volume ratio of dimethyl sulfoxide and ethylenediamine is 4:1.

[0090] The specific configuration method is: first, dimethyl sulfoxide and ethylenediamine are mixed evenly at a volume ratio of 4:1 to form a co-solvent; then lithium tetrafluoroborate is added, and after dissolution, the concentration of lithium tetrafluoroborate is 0.5 mol L -1 of uniform electrolyte.

[0091] Example 7

[0092] Positive electrode, negative electrode and separator: the same as in Example 3.

[0093] Electrolyte: The electrolyte of Example 5 was used.

[0094] Battery assembly: Same as Example 3.

[0095] After the assembled battery was left to rest for 8 hours, a discharge test was performed at room temperature with a cut-off voltage of 1.5 V, and the battery's discharge specific capacity was calculated using graphite fluoride in the positive electrode material as the active substance.

[0096] Example 8

[0097] Positive electrode, negative electrode and separator: the same as in Example 3.

[0098] Electrolyte: The electrolyte of Example 6 was used.

[0099] Battery assembly: Same as Example 3.

[0100] After the assembled battery was left to rest for 8 hours, a discharge test was performed at room temperature with a cut-off voltage of 1.5 V, and the battery's discharge specific capacity was calculated using graphite fluoride in the positive electrode material as the active substance.

[0101] Depend on Fig.10It can be seen that at the rates of 0.1C and 5C, Examples 7 and 8 have relatively good battery performance. The dielectric constant of N-methylimidazole used in Example 7 is relatively high, and the battery has a good discharge specific capacity, which can reach 870 mAh g at a rate of 0.1C. -1 The donor number of ethylenediamine used in Example 8 is higher, and the battery has a higher operating voltage, which can reach 2.8V at a rate of 0.1C.

[0102] Example 9

[0103] Battery assembly: Assemble button cells in the order of negative electrode shell - spring - gasket - lithium sheet - electrolyte - diaphragm - electrolyte - positive electrode - positive electrode shell, wherein the electrolyte is the electrolyte of Example 1, the diaphragm is a PE diaphragm, and the battery specification is 2032.

[0104] After the assembled battery was left to rest for 8 hours, a discharge test was performed at a rate of 0.1C at room temperature; after discharging to 1.5V, the battery was disassembled to obtain the discharged electrode.

[0105] Example 10

[0106] The battery assembly is the same as that of Example 9, wherein the electrolyte is the electrolyte of Example 2, the separator is the same as that of Example 9, and the battery specifications are the same as those of Example 9.

[0107] After the assembled battery was left to rest for 8 hours, a discharge test was performed at a rate of 0.1C at room temperature; after discharging to 1.5V, the battery was disassembled to obtain the discharged electrode.

[0108] Comparative Example 5

[0109] The battery assembly is the same as that of Example 9, wherein the electrolyte is the electrolyte of Comparative Example 1, the separator is the same as that of Example 9, and the battery specifications are the same as those of Example 9.

[0110] After the assembled battery was left to rest for 8 hours, a discharge test was performed at a rate of 0.1C at room temperature; after discharging to 1.5V, the battery was disassembled to obtain the discharged electrode.

[0111] Comparative Example 6

[0112] The battery assembly is the same as that of Example 9, wherein the electrolyte is the electrolyte of Comparative Example 2, the separator is the same as that of Example 9, and the battery specifications are the same as those of Example 9.

[0113] After the assembled battery was left to rest for 8 hours, a discharge test was performed at a rate of 0.1C at room temperature; after discharging to 1.5V, the battery was disassembled to obtain the discharged electrode.

[0114] Depend on Figures 11 to 14It can be seen that the discharge product lithium fluoride in Comparative Example 5 is in the form of large crystal blocks; the discharge product lithium fluoride in Comparative Example 6 is in the form of rice grains; the discharge product lithium fluoride in Example 9 is in the form of small spheres; and the discharge product lithium fluoride in Example 10 is in an amorphous shape.

[0115] Depend on Figures 15-16 It can be seen that the XRD signal peak in Comparative Example 5 is wider than that in Example 9, that is, the lattice of the discharge product lithium fluoride in Comparative Example 5 is inferior to that of the lithium fluoride in Example 9.

[0116] Depend on Fig.17 It can be seen that in the XPS characterization, compared with Comparative Example 5, Example 9 has a lower ratio of LiF to CF bond strength during the entire discharge process, indicating that the electrolyte with a high donor number additive has a stronger effect on inhibiting the decomposition of the intermediate phase.

[0117] Embodiment 11

[0118] Positive electrode: Graphite fluoride, conductive carbon black (Super P) and PVDF were mixed evenly in a mass ratio of 8:1:1, dispersed in N-methylpyrrolidone, and stirred for 8 hours until the positive electrode slurry was obtained; then the positive electrode slurry was evenly coated on a carbon-coated aluminum foil, dried in a drying oven at 80°C for 12 hours, and then cut into positive electrodes with a length of 5.5 cm and a width of 4 cm;

[0119] Negative electrode: lithium strip, width 60mm, thickness 100μm;

[0120] Diaphragm: PE diaphragm, SK innovation Co. Ltd;

[0121] Electrolyte: The electrolyte of Example 1 was used.

[0122] Battery assembly: Assemble the soft-pack battery in the order of aluminum-plastic film-negative electrode-electrolyte-diaphragm-electrolyte-positive electrode-aluminum-plastic film, and then vacuum seal it.

[0123] After the assembled battery was left to rest for 8 hours, an adiabatic accelerating calorimeter (ARC) heat generation test was performed with a cutoff voltage of 1.5 V, and the battery's discharge specific capacity was calculated using graphite fluoride in the positive electrode material as the active substance.

[0124] Comparative Example 7

[0125] The battery assembly is the same as that of Example 11, wherein the electrolyte is the electrolyte of Comparative Example 1, and the positive electrode, negative electrode and separator are the same as those of Example 11.

[0126] After the assembled battery was left to rest for 8 hours, an adiabatic accelerating calorimeter (ARC) heat generation test was performed with a cutoff voltage of 1.5 V, and the battery's discharge specific capacity was calculated using graphite fluoride in the positive electrode material as the active substance.

[0127] Depend on Fig.18 It can be seen that the heating rate of Example 11 is slower than that of Comparative Example 7, which further illustrates that the electrolyte with high donor number additive has a higher heating rate in Li / CF x The effect of suppressing heat generation in the battery is better.

[0128] Any matters not described in the present invention are applicable to the prior art.

Claims

1. A high-voltage lithium / carbon fluoride battery electrolyte, characterized in that: The electrolyte consists of lithium tetrafluoroborate, a high donor number solvent and a high donor number additive; The high donor number solvents are dimethyl sulfoxide and N-methylpyrrolidone; the high donor number additives are N-methylimidazole, triethylamine and ethylenediamine.

2. The high-voltage lithium / carbon fluoride battery electrolyte according to claim 1, characterized in that: When the high donor number additive is triethylamine, the high donor number solvent is N-methylpyrrolidone; when the high donor number additive is N-methylimidazole, the high donor number solvent is dimethyl sulfoxide and / or N-methylpyrrolidone; when the high donor number additive is ethylenediamine, the high donor number solvent is dimethyl sulfoxide.

3. The high voltage lithium / carbon fluoride battery electrolyte according to claim 1, characterized in that: The concentration of lithium tetrafluoroborate is 0.5-1 mol / L; the volume ratio of the high donor number solvent to the high donor number additive is 1-4:

1.

4. The high voltage lithium / carbon fluoride battery electrolyte according to claim 1 or 3, characterized in that: The concentration of lithium tetrafluoroborate is 0.5 mol / L; the volume ratio of the high donor number solvent to the high donor number additive is 4:

1.

5. The high-voltage lithium / carbon fluoride battery electrolyte according to claim 1, characterized in that: The electrolyte is prepared by first mixing a high donor number additive and a high donor number solvent evenly to form a co-solvent; then adding lithium tetrafluoroborate and dissolving it to obtain the electrolyte.

6. A high voltage lithium / carbon fluoride battery, characterized in that: The battery comprises a positive electrode, a negative electrode, a separator and the high-voltage lithium / carbon fluoride battery electrolyte according to any one of claims 1 to 5.

7. The high voltage lithium / carbon fluoride battery according to claim 6, characterized in that: The positive electrode active material adopts fluorinated carbon material, including fluorinated graphite.

8. The high voltage lithium / carbon fluoride battery according to claim 6 or 7, characterized in that: The preparation method of the positive electrode material is as follows: disperse the carbon fluoride material, the conductive agent conductive carbon black and the binder PVDF in N-methylpyrrolidone in a mass ratio of 7-9:0.5-2:0.5-1, fully mix them and apply them on the carbon-coated aluminum foil current collector, and obtain the cathode material after drying.

9. The high voltage lithium / carbon fluoride battery according to claim 6, characterized in that: The negative electrode uses a lithium sheet or a lithium belt with a thickness of 50 to 100 μm.

10. The high voltage lithium / carbon fluoride battery according to claim 6, characterized in that: The diaphragm is made of PE.