Tellurate glass with excellent acousto-optic performance, preparation method and application of tellurate glass in acousto-optic modulator
By developing tellurate glass (BaO-TeO2-WO3 series) as an acousto-optical medium, the problem of acousto-optical glass lacking safe and excellent acousto-optical performance in the prior art is solved, and high performance in the visible to mid-infrared band is achieved Acousto-optical materials are suitable for the preparation of acousto-optical devices and exhibit excellent performance in acousto-optical modulator.
Patent Information
- Application Number
- CN202311004461.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-08-10
AI Technical Summary
Existing acoustic and optical materials lack glass materials with excellent acoustic and optical properties and are safe in applications from visible to near infrared bands, especially because the toxicity of arsenic in Ge33As12Se55 glass is not conducive to human health, and the energy loss of passive Q adjustment is large, which limits the Its practical application value.
A tellurate glass (BaO-TeO2-WO3 series) was developed to prepare high glass transition temperature, stability and safety by composition of specific component proportions (such as BaO 14%, TeO2 58%, WO3 28%). The glass is prepared by heating and melting, stirring, quenching, annealing and other steps, and is used as an acousto-optical medium for an acousto-optical modulator.
It realizes high transmittance, large refractive index and low acoustic attenuation coefficient in the visible to mid-infrared band, has excellent acoustic and optical performance, is suitable for the preparation of acousto-optical devices, and does not contain toxic elements, is safe and environmentally friendly, and has a performance comparable to commercial use. Acousto-optical devices.
Smart Images

Figure BDA0004387523850000042 
Figure HDA0004387523860000011 
Figure HDA0004387523860000012
Abstract
Description
Technical Field
[0001] The present invention relates to the field of acousto-optic glass materials, and in particular to a tellurite glass with excellent acousto-optic properties, a preparation method and an application thereof in an acousto-optic modulator. Background Art
[0002] Pulsed lasers, with their unique advantages such as high peak power and large pulse energy, have shown important application prospects in the fields of precision ranging, laser thermonuclear reaction, laser isotope separation, etc. Pulsed lasers are mainly obtained through two channels: passive Q-switching or active Q-switching. In recent years, some saturable absorber materials for passive Q-switched laser output, such as graphene, transition metal dichalcogenides (TMDs), BP and MXenes, have attracted widespread attention due to their low preparation cost and simple preparation process. However, the energy loss of passive Q-switching is very large, which seriously limits its practical application value. Active Q-switching is achieved by controlling the loss of the resonant cavity through an external driving source, mainly including electro-optical Q-switching and acousto-optical Q-switching. Both electro-optical Q-switching and acousto-optical Q-switching can achieve low energy loss, narrow modulation pulse width and stable pulse laser output. However, electro-optical Q-switching has a complex structure and requires a high voltage drive of several thousand volts, which is dangerous and easy to interfere with other adjacent electronic circuits. In contrast, acousto-optical Q-switching has good application prospects in small-volume pulse lasers due to its simple structure, low modulation voltage and convenient operation.
[0003] Currently, the widely used acousto-optic materials include acousto-optic crystals and acousto-optic glass. Compared with crystals, glass has higher practical application value due to its short preparation time and low cost. 33 As 12 Se 55 As two mature acousto-optic glasses, quartz glass is widely used in the manufacture of acousto-optic devices. Quartz glass has excellent resistance to laser damage and stable physical and chemical properties, but its refractive index and elastic properties are not ideal. 33 As 12 Se 55 The elastic coefficient of glass is large, with Ge 33 As 12 Se 55 Acousto-optic modulators with glass as the acousto-optic medium show high diffraction efficiency. Unfortunately, arsenic is toxic and harmful to human health. Currently, there is no acousto-optic glass with excellent acousto-optic performance, practical and safe for visible and near-infrared bands. Therefore, it is very critical to explore a new acousto-optic glass with excellent acousto-optic performance, practical and safe for visible to near-infrared bands. Summary of the invention
[0004] In view of the deficiencies of the prior art, the present invention provides a tellurite glass with excellent acousto-optic properties, a preparation method and its application in an acousto-optic modulator. The tellurite glass (BTW) of the present invention has strong glass-forming ability, a high glass transition temperature, is easy to prepare on a large scale with high quality, does not contain toxic elements, and is safe and environmentally friendly. The glass of the present invention has excellent acousto-optic properties and can be used in the preparation of acousto-optic devices; the transmission band covers the visible to mid-infrared band, has a high refractive index, and a small acoustic attenuation coefficient. The acousto-optic modulator prepared as an acousto-optic medium has excellent device performance.
[0005] The technical solution of the present invention is as follows:
[0006] A tellurite glass with excellent acousto-optical properties comprises the following components in molar percentage: BaO 14%, TeO2 26-76%, WO3 10-60%.
[0007] Preferably according to the present invention, the tellurite glass with excellent acousto-optical properties comprises the following components in molar percentage: BaO 14%, TeO2 46-66%, WO3 20-40%.
[0008] Preferably, the tellurite glass with excellent acousto-optical properties comprises the following components in molar percentage: BaO 14%, TeO 2 58%, WO 3 28%.
[0009] Preferably according to the present invention, the tellurite glass with excellent acousto-optical properties has a glass transition temperature of 450-460°C, a transmittance of 75-85% in the range of 0.43 to 5 μm, a refractive index of 2.1-2.2 at a wavelength of 643 nm, a sound velocity of 3400-3500 m / s, and an acoustic attenuation coefficient of 0.6-0.7 dB / cm.
[0010] The method for preparing the above-mentioned tellurite glass with excellent acousto-optical properties comprises the steps of:
[0011] The raw materials BaCO3, TeO2 and WO3 are mixed in corresponding proportions; the temperature is raised to 800-850°C until the raw materials are in a molten state, and the liquid is stirred to mix evenly, and then allowed to stand at 800-850°C; finally, tellurite glass with excellent acoustic and optical properties is obtained through quenching and annealing.
[0012] According to the present invention, the ratio of the raw materials BaCO3, TeO2, and WO3 is determined according to the tellurite glass composition.
[0013] Preferably according to the present invention, the melting and standing of the raw materials are both carried out in a platinum crucible.
[0014] Preferably, according to the present invention, stirring is performed using a platinum stirring paddle, the stirring speed is 50-70 rpm, and the stirring time is 20-30 h.
[0015] Preferably according to the present invention, the standing time is 8-12h.
[0016] Preferably according to the present invention, the annealing temperature is 350-450° C., and the annealing time is 45-55 h.
[0017] The above-mentioned tellurite glass with excellent acousto-optic properties is used as an acousto-optic medium to prepare an acousto-optic modulator.
[0018] According to the present invention, the structure of the acousto-optic modulator can be based on the prior art. The acousto-optic modulator includes an acousto-optic medium, a piezoelectric transducer and a driving power supply. The connection method of each component is based on the prior art.
[0019] Preferably according to the present invention, the center frequency and radio frequency power of the acousto-optic modulator are 20-200 MHz and 1.2-2.6 W respectively.
[0020] The above-mentioned acousto-optic modulator can be prepared according to the existing method.
[0021] The technical features and beneficial effects of the present invention are as follows:
[0022] 1. The present invention selects metalloid oxide TeO2 and transition metal oxide WO3 with good glass-forming ability as glass formers, selects alkaline earth metal oxide BaO with stable physicochemical properties as glass modifiers, and successfully prepares BaO-TeO2-WO3 tellurite glass. The tellurite glass of the present invention has good forming ability, and the component ratio has a great influence on the properties of the glass. An inappropriate chemical ratio will reduce the forming ability of the glass, such as crystallization, cracking, etc., and will also reduce the acoustic and optical properties of the glass. The specific component types of the present invention can achieve the excellent effects of the present invention. If the component types of the present invention are replaced with similar components such as TiO2, La2O3, etc., the excellent effects of the present invention cannot be achieved, and the glass performance and acoustic and optical properties will be reduced.
[0023] 2. The tellurite glass of the present invention has a high glass transition temperature, is not easy to deliquesce, has stable physical and chemical properties, is easy to prepare on a large scale with high quality, does not contain toxic elements, and is safe and environmentally friendly. The glass of the present invention has a transmission band covering the visible to mid-infrared band, has a high light transmittance, and has a large refractive index, and a large refractive index is conducive to the occurrence of the elasto-optic effect; the acoustic attenuation coefficient is small, and it has excellent acousto-optic properties, and can be used in the preparation of acousto-optic devices. The acousto-optic modulator prepared with the glass of the present invention as an acousto-optic medium has excellent device performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1This is a photo of BTW glass prepared in Example 1 of the present invention;
[0025] Figure 2 This is a thermal analysis diagram of the BTW glass prepared in Example 1 of the present invention;
[0026] Figure 3 This is a transmission spectrum of the BTW glass prepared in Example 1 of the present invention in the ultraviolet-visible band;
[0027] Figure 4 This is a transmission spectrum diagram of the BTW glass prepared in Example 1 of the present invention in the near infrared band;
[0028] Figure 5 The refractive index diagram of the BTW glass prepared in Example 1 of the present invention;
[0029] Figure 6 Schematic diagram of an acousto-optic modulator using BTW glass as the acousto-optic medium in Experimental Example 1 of the present invention;
[0030] Figure 7 This is a pulse modulation diagram of the acousto-optic modulator using BTW glass as the acousto-optic medium in Experimental Example 1 of the present invention. DETAILED DESCRIPTION
[0031] The present invention is further described below by means of specific examples, but is not limited thereto.
[0032] Unless otherwise specified, the raw materials used in the examples are conventional raw materials and can be obtained commercially; the methods used in the examples are all prior arts unless otherwise specified.
[0033] Example 1
[0034] A tellurite glass with excellent acousto-optical properties comprises the following components in molar percentage: BaO 14%, TeO2 58%, and WO3 28%.
[0035] The method for preparing the above-mentioned tellurite glass with excellent acousto-optical properties comprises the steps of:
[0036] First, according to the composition of the glass, the raw materials BaCO3, TeO2, and WO3 are mixed in corresponding proportions and placed in a platinum crucible. The platinum crucible is placed in a temperature-controlled resistance wire furnace and heated to 800°C to burn the raw materials to a molten state. Then, in order to ensure that the solution is fully mixed, a platinum stirring paddle is immersed in the solution, and the stirring program is set to 60rpm for 24 hours. After the stirring is completed, the stirring paddle is removed from the solution, and the solution is allowed to stand at 800°C for 10 hours. The platinum crucible is then removed from the furnace and quenched to obtain BTW glass. In order to eliminate the thermal stress inside the glass, the glass is annealed at 450°C for 48 hours to obtain a yellow, uniform, transparent, streak-free and bubble-free BTW glass (such as Figure 1 The above preparation processes are all carried out in air.
[0037] BTW glass performance characterization:
[0038] The glass transition temperature of BTW glass was tested by differential temperature scanning method, the heating rate was 5℃ / min, and the atmosphere used was nitrogen. Figure 2 As shown, the glass transition temperature of BTW glass tested by differential temperature scanning method is 457°C, which means that BTW glass always maintains a high thermal stability within the temperature range below 457°C.
[0039] The transmission band and transmittance are crucial for acousto-optic materials. If the transmittance of the material is low, it will increase the light loss and have a greater negative impact on the output power of the Q-switched pulsed laser. The transmission spectrum of BTW glass was measured in the range of 300 to 6000 nm using a UV-visible-near infrared micrometer spectrophotometer (20 / 30PV) and a Nicolet NEXUS 670FTIR spectrometer. The test sample size was 4×4×1mm 3 , double-sided polishing. Figure 3 and Figure 4 As shown, BTW glass exhibits a high transmittance (~80%) in the range of 0.43-5 μm, which promotes its application in the visible to mid-infrared band.
[0040] The acousto-optic effect can be regarded as a special elasto-optic effect, which mainly reflects the change of the refractive index of the medium under the action of elastic waves. Therefore, the refractive index plays a vital role in the acousto-optic properties of optical materials. The refractive index of BTW glass was measured using the minimum deviation angle technology. The top angle of the test sample was 23.75°, and the light-transmitting surface was polished. The refractive index of BTW glass at different wavelengths is shown in Table 1. BTW glass has an excellent refractive index of 2.1498 at a wavelength of 643nm, which is much larger than quartz glass (1.47@656nm). Figure 5As shown in the figure, the refractive index dispersion curve of BTW glass was fitted by the least square method, and the corresponding Sellmeier equation is: Where λ and n are the wavelength of incident light and the refractive index of BTW glass at wavelength λ, respectively.
[0041] Table 1. Refractive index of BTW glass at different wavelengths
[0042]
[0043] For acousto-optic modulators, diffraction efficiency and rise time are the two most important device parameters. The greater the sound velocity of the material, the faster the corresponding device response speed and the shorter the rise time. Paradoxically, from the theoretical calculation formula of the material acousto-optic figure of merit, low sound velocity is more conducive to obtaining high diffraction efficiency. Therefore, in order to balance the diffraction efficiency and rise time, an appropriate sound velocity is crucial. The sound velocity and acoustic attenuation coefficient of BTW glass were measured using the UMS-100 ultrasonic echo material characterization system. The test sample size is 6×6×2mm 3 , double-sided polishing. The detection frequency is 5MHz, the sampling frequency is 160MHz, and the repetition frequency is 0.1kHz. The sound velocity of BTW glass is moderate, 3422m / s, which is less than quartz glass (5960m / s) and higher than Ge 33 As 12 Se 55 Glass (2518m / s). Low sound attenuation is essential for excellent performance of acousto-optic materials. The sound attenuation coefficient of BTW glass is 0.653dB / cm, which is less than that of quartz glass (12dB / cm) and Ge 33 As 12 Se 55 Glass (7.1dB / cm).
[0044] Example 2
[0045] A tellurite glass with excellent acousto-optical properties comprises the following components in molar percentage: BaO 14%, TeO2 46%, and WO3 40%.
[0046] The preparation method of the above-mentioned tellurite glass with excellent acousto-optical properties is the same as that of Example 1.
[0047] Example 3
[0048] A tellurite glass with excellent acousto-optical properties comprises the following components in molar percentage: BaO 14%, TeO2 66%, and WO3 20%.
[0049] The preparation method of the above-mentioned tellurite glass with excellent acousto-optical properties is the same as that of Example 1.
[0050] Comparative Example 1
[0051] A tellurite glass, as described in Example 1, except that the chemical composition ratio of the glass is changed, the chemical proportion of barium oxide in the glass is increased, and the molar percentage of the glass is: BaO 30%, TeO2 46%, WO3 24%.
[0052] The preparation method of the above-mentioned tellurite glass is the same as that of Example 1.
[0053] The glass obtained in this comparative example had serious cracks inside and could not be used normally. This shows that the chemical ratio of glass has a great influence on the glass forming ability.
[0054] Comparative Example 2
[0055] A tellurite glass, as described in Example 1, except that BaO is replaced by Bi2O3, the chemical ratio of TeO2 and WO3 is unchanged, and the molar percentage composition of the glass is: Bi2O3 14%, TeO2 58%, WO3 28%.
[0056] The preparation method of the above-mentioned tellurite glass is the same as that of Example 1.
[0057] The tellurite glass obtained in this comparative example has a large amount of crystals visible to the naked eye inside and cannot be used normally. It can be seen that the chemical composition of glass has a great influence on the glass forming ability. BaO is more suitable than Bi2O3 as a chemical modifier of TeO2-WO3 tellurite glass.
[0058] Comparative Example 3
[0059] A tellurite glass, as described in Example 1, except that BaO is replaced by TiO2, and the glass has the following molar percentage compositions: TiO2 14%, TeO2 58%, WO3 28%.
[0060] The preparation method of the above-mentioned tellurite glass is the same as that of Example 1.
[0061] Comparative Example 4
[0062] A tellurite glass, as described in Example 1, except that BaO is replaced by La2O3, and the glass has the following molar percentage compositions: La2O3 14%, TeO2 58%, WO3 28%.
[0063] The preparation method of the above-mentioned tellurite glass is the same as that of Example 1.
[0064] Application Example 1
[0065] The tellurite glass prepared by the method of Example 1 is used as an acousto-optic medium to prepare a free-space acousto-optic modulator.
[0066] Compared with acousto-optic crystals, glass has the characteristics of optical and acoustic isotropy. Therefore, it is more convenient to design and prepare acousto-optic modulators using BTW glass as the acousto-optic medium. 3 The BTW glass sample is used as the acousto-optic medium, and the light-passing and sound-passing surfaces of the medium have been finely polished. The acousto-optic modulator, according to the existing structure, includes an acousto-optic medium, a piezoelectric transducer and a driving power supply; the driving power supply is connected to the piezoelectric transducer; the driving power supply transmits the received RF power signal to the piezoelectric transducer, and the electrical signal is converted into an ultrasonic signal by the piezoelectric transducer and transmitted to the acousto-optic medium; the piezoelectric transducer is connected to the acousto-optic medium through the electrode layer, the bonding layer, and the electrode layer in sequence. Under the action of ultrasonic waves, the refractive index of the acousto-optic medium changes periodically to form an equivalent phase grating, and diffraction occurs when the laser passes through the acousto-optic medium. The piezoelectric transducer uses a 36°Y-cut LiNbO3 crystal as the piezoelectric material; the electrode layer is high-purity gold with a thickness of 2.52μm; the bonding layer is high-purity Sn with a thickness of 4.93μm. Figure 6 is the schematic diagram of the acousto-optic modulator, and RF is the radio frequency driving power supply.
[0067] The center frequency and RF power of the device are set to 100MHz and 2.6W respectively, and the operating wavelength is 1064nm (the device of the present invention can operate at multiple wavelengths such as 633nm, 1064nm, 2100nm, etc.). The diffraction efficiency of the device is 85%. High diffraction efficiency is conducive to the output of high-power Q-switched pulse lasers. The modulation speed of the device is determined by the rise time. The test results show that the rise time and fall time of the BTW glass acousto-optic modulator are 40 and 47ns respectively. Figure 7 As shown in Figure 2, from the perspective of the two main device parameters, diffraction efficiency and rise time, the performance of the AOM using BTW glass as the AOM medium is comparable to that of commercial AOM devices.
[0068] The tellurite glasses prepared by the methods of Examples 2-3 and Comparative Examples 3-4 were used as acousto-optic media to prepare free-space acousto-optic modulators according to the above method, and were tested according to the above method. The diffraction efficiency of the device prepared by the glass of Example 2 was 84%; the diffraction efficiency of the device prepared by the glass of Example 3 was 82%, the diffraction efficiency of the device prepared by the glass of Comparative Example 3 was 60%, and the diffraction efficiency of the device prepared by the glass of Comparative Example 4 was 52%. It can be seen from the above that only the specific component ratio of the present invention combined with the specific component types can achieve the excellent effect of the present invention.
[0069] Application Example 2
[0070] The tellurite glass prepared by the method of Example 1 is used as an acousto-optic medium to prepare a free-space acousto-optic modulator, as described in Application Example 1, except that the center frequency of the device is set to 200 MHz; other conditions and steps are the same as in Application Example 1.
[0071] The RF power of the device is 2.6W, the center frequency of the device is 200MHz, and the operating wavelength is 1064nm. The rise time and fall time of the device are tested to be 39 and 48ns respectively, which are basically the same as the rise time of the device in Application Example 1. It is worth noting that the diffraction efficiency of the device is only 75% after testing. It can be seen that the center frequency has a great influence on the diffraction efficiency of the device. The acousto-optic modulator using BTW glass as the acousto-optic medium is more suitable for working at a lower center frequency.
[0072] The above-described embodiments are merely examples of the technical solutions of the present invention. The BTW glass and the preparation method of the corresponding acousto-optic modulator involved in the present invention are not limited to the contents described in the above-described embodiments, but are subject to the scope defined in the claims. Any modification, supplement, equivalent replacement or improvement made by technicians in the field of the present invention within the spirit and principle shall be included in the protection scope of the present invention.
Claims
1. A tellurite glass with excellent acousto-optic properties, characterized in that: The composition includes the following molar percentages: BaO 14%, TeO2 26-76%, WO3 10-60%.
2. The tellurite glass with excellent acousto-optical properties according to claim 1, characterized in that: The tellurite glass with excellent acousto-optical properties comprises the following components in molar percentage: BaO 14%, TeO2 46-66%, WO3 20-40%.
3. The tellurite glass with excellent acousto-optical properties according to claim 2, characterized in that: The tellurite glass with excellent acousto-optical properties comprises the following components in molar percentage: BaO 14%, TeO2 58%, WO3 28%.
4. The tellurite glass with excellent acousto-optical properties according to claim 1, characterized in that: The tellurite glass with excellent acousto-optical properties has a glass transition temperature of 450-460°C, a transmittance of 75-85% in the range of 0.43-5 μm, a refractive index of 2.1-2.2 at a wavelength of 643 nm, a sound velocity of 3400-3500 m / s, and an acoustic attenuation coefficient of 0.6-0.7 dB / cm.
5. A method for preparing tellurite glass having excellent acousto-optic properties according to any one of claims 1 to 4, comprising the steps of: The raw materials BaCO3, TeO2 and WO3 are mixed in corresponding proportions; the temperature is raised to 800-850°C until the raw materials are in a molten state, and the liquid is stirred to mix evenly, and then allowed to stand at 800-850°C; finally, tellurite glass with excellent acoustic and optical properties is obtained through quenching and annealing.
6. The method for preparing tellurite glass with excellent acousto-optic properties according to claim 5, characterized in that: The melting and standing of the raw materials are both carried out in a platinum crucible; the stirring is carried out using a platinum stirring paddle, the stirring speed is 50-70 rpm, and the stirring time is 20-30 hours.
7. The method for preparing tellurite glass with excellent acousto-optical properties according to claim 5, characterized in that: The standing time is 8-12 hours; preferably, the annealing temperature is 350-450°C, and the annealing time is 45-55 hours.
8. Use of the tellurite glass with excellent acousto-optic properties as claimed in any one of claims 1 to 4 as an acousto-optic medium in the preparation of an acousto-optic modulator.
9. The use of the tellurite glass with excellent acousto-optical properties according to claim 8, characterized in that: The acousto-optic modulator includes an acousto-optic medium, a piezoelectric transducer and a driving power supply.
10. The use of the tellurite glass with excellent acousto-optical properties according to claim 8, characterized in that: The center frequency and RF power of the AOM are 20-200MHz and 1.2-2.6W respectively.
Citation Information
Patent Citations
Rare-earth blended tungstotellurate glass and its preparing method
CN1587139A
Tellurite glass
JP1987288135A
Tellurite glass and optical amplifier using tellurite glass
JP2004244280A