Preparation method of cellulose ether for gypsum mortar
By using multi-stage etherification treatment in gypsum mortar, the problems of gypsum layered cracking, difference in settling time and many bubbles are solved, and the stability and construction performance of gypsum mortar are improved.
Patent Information
- Application Number
- CN202411041387.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
When cellulose ether is used in gypsum mortar, gypsum is prone to cracking layered, obvious differences in settling time, many bubbles and slow thickening.
A preparation method is adopted, including reacting refined cotton powder with liquid alkali, etherifying agent, low boiling point ether substance and low carbon alcohol substance in the reaction kettle, controlling reaction conditions such as pressure, temperature and time, through multiple stages Etherification and oxidation treatment to produce cellulose ethers with gypsum universality.
Reduce gypsum layering and cracking, extend the opening time, reduce the difference in water consumption and condensation time, reduce bubbles, and improve thickening speed.
Smart Images

Figure BDA0004972474410000051 
Figure BDA0004972474410000071 
Figure BDA0004972474410000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of gypsum mortar material preparation and provides a method for preparing cellulose ether for gypsum mortar. Background Art
[0002] Gypsum is a commonly used raw material in building materials. It is divided into desulfurized gypsum and phosphogypsum. As a by-product, gypsum has the characteristics of small shrinkage, large quantity and low price. It is widely used in self-leveling mortar, plastering gypsum, tile adhesive and other materials. However, due to the three-phase instability of gypsum and the diversity of raw materials, gypsum often has problems such as water consumption, variable setting time, and cracking during use.
[0003] The application of cellulose ether in gypsum mortar is mainly reflected in the following aspects: 1) Improving water retention: As a high molecular compound, cellulose ether has excellent water absorption and water retention capacity, which can improve the water retention of gypsum mortar and prevent water loss too quickly, thereby improving construction performance; 2) Improving adhesion: Cellulose ether can increase the adhesion of mortar, improve the bonding strength between mortar and substrate, and help improve the construction quality and durability of mortar; 3) Thickening effect: Cellulose ether can increase the viscosity of mortar, improve the fluidity and operability of mortar, and make it easier to construct and apply; 4) Influence on setting time: The addition of cellulose ether may affect The setting time of gypsum mortar can be controlled to a certain extent by adjusting the dosage of cellulose ether to adapt to different construction requirements; 5) Improve crack resistance: The addition of cellulose ether helps to reduce the shrinkage of gypsum mortar and improve its crack resistance, thereby reducing the occurrence of cracks during construction; 6) Improve construction performance: Cellulose ether can improve the construction performance of gypsum mortar, such as reducing water seepage, extending the operable time of mortar, and improving construction efficiency; Environmental adaptability: 7) Cellulose ether-modified mortar has better adaptability under different environmental conditions, such as temperature changes, which helps to improve the performance stability of mortar in practical applications.
[0004] The purpose of this study is to develop a cellulose ether that has the universality of gypsum, reduces gypsum delamination and cracking, prolongs the gypsum open time, reduces the difference in water consumption and setting time between gypsum batches, has the advantages of less bubbles and faster thickening.
[0005] In summary, the prior art still has the following problems: when cellulose ether is applied to gypsum mortar, gypsum delamination and cracking are likely to occur, the setting time is significantly different, there are many bubbles and the thickening is slow. Summary of the invention
[0006] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a method for preparing cellulose ether for gypsum mortar. When the cellulose ether prepared by the preparation method is applied to gypsum mortar, it has the following advantages:
[0007] It is universally applicable to gypsum, reduces gypsum delamination and cracking, prolongs the opening time of gypsum, reduces the water consumption and setting time differences between gypsum batches, reduces bubbles and thickens quickly.
[0008] A method for preparing cellulose ether for gypsum mortar comprises the following steps:
[0009] S1 puts refined cotton powder into the reactor, replaces the air in the reactor, protects with inert gas, and controls the pressure in the reactor;
[0010] S2 adds 32-50% liquid caustic soda, reacts for 5-45 minutes, and the reaction temperature is controlled at 20-45°C;
[0011] S3 adds the first-stage etherifying agent, the pressure in the kettle is controlled at 0.15-0.3MPa, the temperature is controlled at 30-50℃, and the reaction time is 40-90min;
[0012] S4 adds the second-stage etherifying agent, low-boiling-point ethers and low-carbon alcohols, and controls the pressure in the kettle at 0.6-1.0 MPa and the temperature at 40-60°C;
[0013] S5: Raise the reaction pressure to 1.7-2.2 MPa within 30-120 min, and react for 30-90 min at this pressure;
[0014] After S6 recovery is completed, add oxidant into the kettle and stir for 10 to 60 minutes;
[0015] S7 post-processing: neutralization, filter pressing, gel granulation, wet crushing, dry crushing, and packaging to obtain the desired product.
[0016] As a further improvement of this scheme, the inert gas in S1 is any one or two of nitrogen and carbon dioxide;
[0017] The liquid alkali in S2 is sodium hydroxide.
[0018] As a further improvement of this scheme, the first-stage etherifying agent in S3 is any one or more of ethylene oxide, propylene oxide, and butylene oxide.
[0019] As a further improvement of this scheme, the second-stage etherifying agent in S4 is any one or more of methyl chloride, ethyl chloride, and pentyl chloride;
[0020] The low-boiling-point ether substance is any one or more of methyl ether, ethyl ether, methyl ethyl ether, propyl ether, and isopropyl ether;
[0021] Low-carbon alcohol substances: any one or more of methanol, ethanol, propanol, and isopropanol.
[0022] As a further improvement of this scheme, the oxidant in S6 is any one or more of hydrogen peroxide, sodium hypochlorite and the like;
[0023] The feeding amount of refined cotton is 1500-2100kg;
[0024] The molar ratio of refined cotton to 32-50% liquid caustic soda is 1:2.5-6.0, preferably 1:3.5-5.5;
[0025] The molar ratio of refined cotton to the first-stage etherifying agent = 1:0.4-2.0, preferably 1:0.6-1.8;
[0026] The molar ratio of refined cotton to the second-stage etherifying agent = 1:2.0-6.5, preferably 1:2.5-6.0;
[0027] The molar ratio of refined cotton to low-boiling ethers is 1:0.7-2.3, preferably 1:0.9-2.1;
[0028] The molar ratio of refined cotton to low-carbon alcohols is 1:0.70-2.3, preferably 1:0.9-2.1.
[0029] As a further improvement of this scheme, the pressure in the kettle in S1 is controlled at 0.05-0.1 MPa;
[0030] The concentration of the liquid alkali in S2 is 38% to 48%, the temperature is 25 to 35°C, and the reaction time is 10 to 35 minutes.
[0031] As a further improvement of this scheme, the pressure in the autoclave in S3 is controlled at 0.2-0.25 MPa, the temperature is controlled at 35-45°C, and the reaction time is 50-80 min.
[0032] As a further improvement of this scheme, the pressure in the kettle in S4 is controlled at 0.7-0.9 MPa, and the temperature is controlled at 45-55°C.
[0033] As a further improvement of this scheme, in S5, the reaction pressure is increased to 1.8-2.1 MPa within 50-100 min, and the reaction is carried out at this pressure for 50-70 min.
[0034] As a further improvement of this scheme, after the recovery of S6 is completed, an oxidant is added to the kettle and stirred for 20 to 50 minutes.
[0035] Compared with the prior art, the cellulose ether prepared by the method for preparing cellulose ether for gypsum mortar of the present invention has the following beneficial effects:
[0036] The cellulose ether prepared by the present invention is used in lightweight plaster gypsum products, and the open time can be extended to 90 minutes;
[0037] The cellulose ether prepared by the present invention is used in gypsum-based self-leveling mortar to prevent self-leveling bleeding and stratification;
[0038] The cellulose ether prepared by the invention is used in gypsum putty, and the open time of the gypsum putty can be extended to 25 minutes. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is further described below in conjunction with embodiments:
[0040] The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased from the market.
[0041] The products of the embodiments and comparative examples were evaluated using the following performance indicators:
[0042] Technical index requirements of cellulose ether:
[0043]
[0044] Product stability can be expressed by the product qualification rate, and the above indicators are used for testing and evaluation:
[0045] The qualified rate is ≤50%, which is very poor;
[0046] The pass rate is 50% to 70%, poor;
[0047] The pass rate is 70%-90%, which is poor;
[0048] Pass rate: above 90%, good.
[0049] The feeding amount of refined cotton is 2000kg;
[0050] The molar ratio of refined cotton to 32-50% liquid caustic soda is 1:5.5;
[0051] The molar ratio of refined cotton to the first-stage etherifying agent = 1:1.8;
[0052] The molar ratio of refined cotton to the second-stage etherifying agent = 1:3.0;
[0053] The molar ratio of refined cotton to low-boiling-point ethers = 1:1.8;
[0054] The molar ratio of refined cotton to low-carbon alcohols is 1:1.4.
[0055] Example 1
[0056] S1. Put the refined cotton powder into the reactor, replace the air in the reactor, protect it with inert gas (one or two of nitrogen and carbon dioxide are selected as the gas), and control the pressure in the reactor at 0.05-0.1MPa;
[0057] S2, add 38%-48% liquid caustic soda (temperature controlled at 25-35°C), react for 10-35 minutes;
[0058] S3, the first stage etherifying agent is ethylene oxide, the pressure in the kettle is controlled at 0.2-0.25MPa, the temperature is controlled at 35-45℃, and the reaction time is 50-80min;
[0059] S4, the second stage etherification agent is methyl chloride, low boiling point ether substances are not added, low carbon alcohol substances are not added, the pressure in the kettle is controlled at 0.7-0.9MPa, and the temperature is controlled at 45-55℃
[0060] S5. Within 50-100 minutes, the reaction pressure is increased to 1.8-2.1 MPa, and the reaction is carried out at this pressure for 50-70 minutes.
[0061] S6. After the recovery is completed, an oxidant (one or more of hydrogen peroxide, sodium hypochlorite, etc.) is added to the kettle and stirred for 20-50 minutes;
[0062] S7, obtaining the desired product through post-treatment.
[0063] Example 2
[0064] In S3, the first-stage etherifying agent is ethylene oxide, the pressure in the kettle is controlled at 0.2-0.25MPa, the temperature is controlled at 35-45°C, and the reaction time is 50-80min;
[0065] The second-stage etherification agent in S4 is methyl chloride.
[0066] Low boiling point ethers: methyl ether;
[0067] No low-carbon alcohols are added;
[0068] The pressure in the kettle is controlled at 0.7-0.9MPa and the temperature is controlled at 45-55℃.
[0069] The other steps remain the same as those in Example 1.
[0070] Example 3
[0071] In S3, the first-stage etherifying agent is ethylene oxide, the pressure in the kettle is controlled at 0.2-0.25MPa, the temperature is controlled at 35-45°C, and the reaction time is 50-80min;
[0072] The second-stage etherification agent in S4 is methyl chloride.
[0073] Low boiling point ethers: methyl ether;
[0074] Low carbon alcohols: methanol;
[0075] The pressure in the kettle is controlled at 0.7-0.9MPa and the temperature is controlled at 45-55℃.
[0076] The other steps remain the same as those in Example 1.
[0077] Example 4
[0078] In S3, the first-stage etherifying agent is ethylene oxide, the pressure in the kettle is controlled at 0.2-0.25MPa, the temperature is controlled at 35-45°C, and the reaction time is 50-80min;
[0079] The second-stage etherification agent in S4 is methyl chloride.
[0080] Low boiling point ethers: methyl ether, isopropyl ether;
[0081] Low-carbon alcohols: methanol, isopropanol;
[0082] The pressure in the kettle is controlled at 0.7-0.9MPa and the temperature is controlled at 45-55℃.
[0083] The other steps remain the same as those in Example 1.
[0084]
[0085] Example 5
[0086] In S3, the first-stage etherifying agent is ethylene oxide and propylene oxide, the pressure in the kettle is controlled at 0.2-0.25MPa, the temperature is controlled at 35-45℃, and the reaction time is 50-80min;
[0087] The second-stage etherification agent in S4 is methyl chloride;
[0088] Low boiling point ethers: methyl ether, isopropyl ether;
[0089] Low-carbon alcohols: methanol, isopropanol;
[0090] The pressure in the kettle is controlled at 0.7-0.9MPa and the temperature is controlled at 45-55℃
[0091] The other steps remain the same as those in Example 1.
[0092] Example 6
[0093] In S3, the first-stage etherifying agent is ethylene oxide and propylene oxide, the pressure in the kettle is controlled at 0.2-0.25MPa, the temperature is controlled at 35-45℃, and the reaction time is 50-80min;
[0094] The second-stage etherifying agent in S4 is methyl chloride and ethyl chloride;
[0095] Low boiling point ethers: methyl ether, isopropyl ether;
[0096] Low-carbon alcohol substances: methanol, isopropanol, the pressure in the kettle is controlled at 0.7-0.9MPa, and the temperature is controlled at 45-55℃
[0097] The other steps remain the same as those in Example 1.
[0098]
[0099]
[0100] From the above embodiments and comparative examples, it can be seen that when low-boiling-point ether substances: methyl ether, isopropyl ether; low-carbon alcohol substances: methanol, isopropyl alcohol, and the first-stage etherifying agent is methyl chloride, and the second-stage etherifying agent is methyl chloride, ethyl chloride, the final product is not only stable, but also has good stability. 1. When used in lightweight plaster gypsum products, the open time can be extended to 90 minutes; 2. When used in gypsum-based self-leveling mortar, self-leveling bleeding and stratification can be prevented; 3. When used in gypsum putty, the open time of gypsum putty can be extended to 25 minutes; 4. Good antibacterial property
[0101] Example 7
[0102] S1. Put the refined cotton powder into the reactor, replace the air in the reactor, and protect it with inert gas (nitrogen is used as the gas, and the pressure in the reactor is controlled at 0.05-0.1MPa;
[0103] S2, add 42% liquid caustic soda (temperature controlled at 25-35°C), react for 10-35 minutes;
[0104] S3, the first stage etherifying agent is ethylene oxide and propylene oxide, the pressure in the kettle is controlled at 0.2-0.25MPa, the temperature is controlled at 35-45℃, and the reaction time is 50-80min;
[0105] S4, the second stage etherifying agent is methyl chloride and ethyl chloride;
[0106] Low boiling point ethers: methyl ether, isopropyl ether;
[0107] Low-carbon alcohols: methanol, isopropanol;
[0108] The pressure in the kettle is controlled at 0.7-0.9MPa and the temperature is controlled at 45-55℃
[0109] S5. Within 30-50 minutes, the reaction pressure is increased to 1.8-2.1 MPa, and the reaction is carried out at this pressure for 50-70 minutes.
[0110] Example 8
[0111] S5. Within 100-120 minutes, the reaction pressure is increased to 1.8-2.1 MPa, and the reaction is carried out at this pressure for 50-70 minutes.
[0112] The other steps remain the same as those in Example 7.
[0113]
[0114] Example 9
[0115] S5. Within 50-100 minutes, the reaction pressure is increased to 1.0-1.8 MPa, and the reaction is carried out at this pressure for 50-70 minutes.
[0116] The other steps remain the same as those in Example 7.
[0117] Example 10
[0118] S5. Within 50-100 minutes, the reaction pressure is increased to 2.1Mpa-2.5Mpa, and the reaction is carried out at this pressure for 50-70 minutes.
[0119] The other steps remain the same as those in Example 7.
[0120]
[0121]
[0122] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent changes made using the present invention are within the patent protection scope of the present invention.
Claims
1. A method for preparing cellulose ether for gypsum mortar, characterized in that: The following steps are involved: S1 puts refined cotton powder into the reactor, replaces the air in the reactor, protects with inert gas, and controls the pressure in the reactor; S2 adds 32-50% liquid caustic soda, reacts for 5-45 minutes, and the reaction temperature is controlled at 20-45°C; S3 adds the first-stage etherifying agent, the pressure in the kettle is controlled at 0.15-0.3MPa, the temperature is controlled at 30-50℃, and the reaction time is 40-90min; S4 adds the second-stage etherifying agent, low-boiling-point ethers and low-carbon alcohols, and controls the pressure in the kettle at 0.6-1.0 MPa and the temperature at 40-60°C; S5: Raise the reaction pressure to 1.7-2.2 MPa within 30-120 min, and react for 30-90 min at this pressure; After S6 recovery is completed, add oxidant into the kettle and stir for 10 to 60 minutes; S7 post-processing: neutralization, filter pressing, gel granulation, wet crushing, dry crushing, and packaging to obtain the desired product.
2. The method for preparing cellulose ether for gypsum mortar according to claim 1, characterized in that: The inert gas in S1 is either nitrogen or carbon dioxide, or both; The liquid alkali in S2 is sodium hydroxide.
3. The method for preparing cellulose ether for gypsum mortar according to claim 1, characterized in that: The first-stage etherifying agent in S3 is any one or more of ethylene oxide, propylene oxide and butylene oxide.
4. The method for preparing cellulose ether for gypsum mortar according to claim 1, characterized in that: The second-stage etherifying agent in S4 is any one or more of methyl chloride, ethyl chloride, and pentyl chloride; The low-boiling-point ether substance is any one or more of methyl ether, ethyl ether, methyl ethyl ether, propyl ether, and isopropyl ether; Low-carbon alcohol substances: any one or more of methanol, ethanol, propanol, and isopropanol.
5. The method for preparing cellulose ether for gypsum mortar according to claim 1, characterized in that: The oxidant in S6 is any one or more of hydrogen peroxide, sodium hypochlorite and the like; The feeding amount of refined cotton is 1500-2100kg; The molar ratio of refined cotton to 32-50% liquid caustic soda is 1:2.5-6.0, preferably 1:3.5-5.5; The molar ratio of refined cotton to the first-stage etherifying agent = 1:0.4-2.0, preferably 1:0.6-1.8; The molar ratio of refined cotton to the second-stage etherifying agent = 1:2.0-6.5, preferably 1:2.5-6.0; The molar ratio of refined cotton to low-boiling ethers is 1:0.7-2.3, preferably 1:0.9-2.1; The molar ratio of refined cotton to low-carbon alcohols is 1:0.70-2.3, preferably 1:0.9-2.
1.
6. The method for preparing cellulose ether for gypsum mortar according to claim 1, characterized in that: The pressure in the kettle in S1 is controlled at 0.05-0.1 MPa; The concentration of the liquid alkali in S2 is 38% to 48%, the temperature is 25 to 35°C, and the reaction time is 10 to 35 minutes.
7. The method for preparing cellulose ether for gypsum mortar according to claim 1, characterized in that: In S3, the pressure in the autoclave is controlled at 0.2-0.25 MPa, the temperature is controlled at 35-45°C, and the reaction time is 50-80 min.
8. The method for preparing cellulose ether for gypsum mortar according to claim 1, characterized in that: In S4, the pressure in the kettle is controlled at 0.7-0.9 MPa, and the temperature is controlled at 45-55°C.
9. The method for preparing cellulose ether for gypsum mortar according to claim 1, characterized in that: In S5, the reaction pressure is increased to 1.8-2.1 MPa within 50-100 min, and the reaction is carried out at this pressure for 50-70 min.
10. The method for preparing cellulose ether for gypsum mortar according to claim 1, characterized in that: After S6 recovery is completed, add oxidant into the kettle and stir for 20 to 50 minutes.