High-entropy alkaline earth metal fluoride crystal and preparation method thereof
By introducing Re3+ ions into alkaline earth metal fluoride crystals to form a cluster structure, the problem of difficulty in synthesis of single-phase solid solution of high-entropy materials is solved, and the optical performance of the crystal is regulated and performance improved, forming a low-energy cluster structure and The luminous center enhances the physical and chemical properties of the material.
Patent Information
- Application Number
- CN202411019031.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The synthesis of single-phase solid solutions of high-entropy materials is difficult, which limits its application, especially the formation of single-phase crystals.
By introducing Re3+ ions into the alkaline earth metal fluoride crystal MeF2, a variety of cluster structures and luminescence centers are formed to control the optical properties of the crystals. The high-entropy alkaline earth metal fluoride crystal Re3+:MeF2 is grown by using temperature gradient methods and other methods to control The doping concentration of Re3+ is between 35 at% and 50 at% to form a high entropy effect and a variety of luminescent centers.
The structural regulation of the optical properties of the crystal is achieved, the high entropy performance is improved, the low-energy cluster structure and luminous center are formed, and the physical and chemical properties of the material are enhanced.
Smart Images

Figure CN118957756A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high entropy crystal material, in particular to a high entropy alkaline earth metal fluoride crystal and a preparation method thereof, and belongs to the field of artificial crystal materials. Background Art
[0002] High entropy materials are multi-element materials with highly mixed structures and thus unique physical and chemical properties. Although high entropy materials are excellent candidates for a range of functional materials, the difficulty in synthesizing single-phase solid solutions, especially single-phase crystals, limits the application of such materials. Summary of the invention
[0003] In order to realize the synthesis and performance control of high entropy crystals, the present invention proposes a high entropy crystal Re 3+ :MeF 2 , using rare earth ions in alkaline earth metal fluoride crystals MeF 2 Various cluster structures and luminescence centers are formed in the material, forming a highly disordered configuration, thereby achieving the regulation of the optical properties of the crystal.
[0004] In a first aspect, the present invention provides a high entropy alkaline earth metal fluoride crystal, wherein the chemical formula of the high entropy alkaline earth metal fluoride crystal is Re 3+ :MeF 2 ; wherein Me is one of Ca, Sr and Ba; When Me is Ca or Sr, Re 3+ Yb 3+ 、Nd 3+ 、Tm 3+ 、Ho 3+ , Er 3+ , Pr 3+ 、Sm 3+ 、Eu 3+ , Tb 3+ 、Dy 3+ 、Ce 3+ , Y 3+ ,La 3+ , Gd 3+ 、Lu 3+ Sc 3+ One of; When Me is Ba, Re 3+ Yb 3+ 、Nd 3+ 、Tm 3+ 、Ho 3+ , Er 3+ , Pr 3+ 、Sm 3+ 、Eu 3+ , Tb 3+ 、Ce3+ ,La 3+ , Gd 3+ 、Lu 3+ Sc 3+ One of them.
[0005] The inventors have found through research that fluoride crystals are an ideal laser matrix material due to their wide transmission range, high thermal conductivity, and stable physical and chemical properties. The special alkaline earth fluoride crystal structure makes it easy for trivalent rare earth ions to form a variety of lattice structures in the crystal. When trivalent rare earth ions replace divalent alkaline earth metal ions, the unbalanced charge is replaced by interstitial fluoride ions F i -compensation, and the interstitial fluoride ions can occupy multiple non-equivalent lattice sites, and the local symmetry of the rare earth ions will change accordingly. In addition, the trivalent rare earth ions and the interstitial ions F with a negative charge i -Form a pair of dipoles, the dipoles interact with each other, and clustering together makes the system energy lower. Therefore, rare earth ions can easily form a variety of cluster structures and luminescence centers in alkaline earth fluoride crystals.
[0006] Preferably, when Re 3+ The content is 35at%~50at%.
[0007] Preferably, the configuration entropy of the high entropy alkaline earth metal fluoride crystal is ≥1.5R.
[0008] In a second aspect, the present invention provides a method for preparing high entropy alkaline earth metal fluoride crystals, comprising: weighing ReF according to a stoichiometric ratio; 3 and MeF 2 As a raw material, the alkaline earth metal fluoride crystal is grown by using one of the temperature gradient method, the pulling method, the crucible descent method, the heat exchange method, the kyvo method, the top seed method, the flux crystal growth method or the micro-pull-down method.
[0009] Preferably, the parameters of the temperature gradient method include: vacuum degree ≤ 10 -3 Pa; material temperature 1300 ~ 1500 ℃; the cooling rate during crystal growth is 1 ~ 5 ℃ / h; the cooling rate after the growth is completed is 10 ~ 30 ℃ / h.
[0010] Preferably, the parameters of the temperature gradient method also include a crystal growth time of 100 to 300 hours.
[0011] Preferably, PbF is also added to the raw material 2 Used as deoxidizer, PbF 2 The amount of ReF 3 and MeF 2 0.5~2wt% of the total mass.
[0012] Preferably, a graphite porous crucible is used in the growth process of the temperature gradient method.
[0013] Preferably, the crystal obtained after the temperature gradient growth is completed is a single phase.
[0014] In a third aspect, the present invention provides an application of a high entropy alkaline earth metal fluoride crystal in the field of local structure regulation of luminescent ions, wherein the chemical formula of the high entropy alkaline earth metal fluoride crystal is Re 3+ :MeF 2 ; Wherein, Me is one of Ca, Sr, and Ba; Re 3+ Yb 3+ 、Nd 3+ 、Tm 3+ 、Ho 3+ , Er 3+ , Pr 3+ 、Sm 3+ 、Eu 3+ , Tb 3+ 、Dy 3+ 、Ce 3+ , Y 3+ ,La 3+ , Gd 3+ 、Lu 3+ Sc 3+ One of them; Re 3+ The total doping concentration is 35at% to 50at%.
[0015] In a fourth aspect, the present invention provides a method for improving the high entropy performance of alkaline earth metal fluoride crystals, comprising: 2 The total doping concentration introduced is 35at%~50at%Re 3+ , thereby achieving the improvement of high entropy performance; wherein Me is one of Ca, Sr, and Ba; Re 3+ Yb 3+ 、Nd 3+ 、Tm 3+ 、Ho 3+ , Er 3+ , Pr 3+ 、Sm 3+ 、Eu 3+ , Tb 3+ 、Dy 3 + 、Ce 3+ , Y 3+ ,La 3+ , Gd 3+ 、Lu 3+ Sc 3+ One of them.
[0016] Beneficial effects of the present invention: The high entropy alkaline earth metal fluoride crystals prepared in the present invention cause lattice distortion due to the high entropy effect, and form various clusters and luminescence centers, so that the optical properties can be regulated from the structural point of view. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The x% Nd:SrF prepared in Example 1 2 (x=0-40) Powder X-ray diffraction pattern of crystals; Figure 2 The x% Nd:SrF prepared in Example 1 2 (x=0-40) Relationship between crystal configuration entropy and concentration; Figure 3 The rare earth ion cluster structure in the alkaline earth fluoride crystal of Example 2, "La", "Nd" and "Y" are La 3+ 、Nd 3+ , Y 3+ Doped SrF 2 "1" represents the monomer center in the first stage, "2" represents the cubic sublattice cluster in the second stage, and "3" represents the tetragonal anti-prism structure cluster in the third stage. Different cluster structures form high entropy effects and diverse luminescence centers. DETAILED DESCRIPTION
[0018] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0019] In the present disclosure, a high entropy crystal Re is provided. 3+ :MeF 2 . Wherein, Me is one of Ca, Sr and Ba. Re 3+ Yb 3 + 、Nd 3+ 、Tm 3+ 、Ho 3+ , Er 3+ , Pr 3+ 、Sm 3+ 、Eu 3+ , Tb 3+ 、Dy 3+ 、Ce 3+ , Y 3+ ,La 3+ , Gd 3+ 、Lu 3+ Sc 3+ One of them. High doping content Re 3+ Alkaline earth metal fluoride crystals MeF 2Various cluster structures and luminescence centers are formed in the crystal, thereby achieving the regulation of the optical properties of the crystal.
[0020] In an optional embodiment, Re 3+ The doping concentration of Re is 35at% to 50at%. 3+ The doping concentration can be 35at%, 40at%, 45at%, 50at%, etc.
[0021] In an optional embodiment, Re 3+ :MeF 2 The configuration entropy of the crystal is ≥1.5R.
[0022] In the present invention, the raw materials are weighed and mixed uniformly according to the molar ratio, wherein PbF 2 It is used as a deoxidizer. Then, a high entropy alkaline earth metal fluoride crystal is grown using a temperature gradient method. The following is an exemplary description of the preparation method of high entropy alkaline earth metal fluoride crystal.
[0023] Ingredients. The raw materials used are MeF 2 (Me=Ca,Sr,Ba),ReF 3 (Re=Yb, Nd, Tm, Ho, Er, Pr, Sm, Eu, Tb, Dy, Ce, Y, La, Gd, Lu, Sc), PbF 2 The raw materials were weighed according to the stoichiometric ratio, ground into powder in a mortar and mixed evenly. 2 The amount of MeF added is 2 and ReF 3 0.5~2.0wt% of the total mass of raw materials
[0024] The mixed raw materials were placed in a graphite porous crucible, placed in a temperature gradient furnace, and evacuated to 10 -3 Pa, raise the temperature from room temperature to 200℃ in 2h, and then keep it warm for 5~10h (to remove moisture and air in the raw materials). Then raise the temperature to 800℃, keep it warm for 5~10h, and then raise the temperature to 1300~1500℃, keep it warm for 10~20h. Finally, slowly cool down at a rate of 1~5℃ / h to grow crystals. After 200~300h, the crystal growth is completed, and then cool down to room temperature at a rate of 10~30℃ / h.
[0025] As an example of the temperature gradient method for growing crystals, the mixed raw materials are placed in a graphite porous crucible, placed in a temperature gradient furnace, and evacuated to 10 -3Pa, raise the temperature from room temperature to 200℃ in 2h, and then keep it for 10h to remove moisture and air in the raw materials. Then raise the temperature to 800℃, keep it for 5h, and then raise the temperature to 1300-1500℃, keep it for 12h. Finally, slowly cool it down at a rate of 1.5℃ / h to grow crystals. After 200h, the crystal growth is completed, and then cool it down to room temperature at a rate of 20℃ / h.
[0026] In the present invention, the structural characteristics of the crystal are analyzed by a neutron diffraction method, and the configuration entropy of the high entropy alkaline earth metal fluoride crystal is calculated to be ≥1.5R.
[0027] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0028] Example 1: x%Nd:SrF 2 Crystal (x = 10, 20, 30, 35, 40, 50, 55) (1) Weigh NdF according to the chemical formula 3 , SrF 2 , PbF 2 The raw materials are ground into powder in a mortar and mixed thoroughly to obtain a mixed powder; (2) placing the mixed powder in a graphite porous crucible and using a temperature gradient method to grow the desired crystal. The parameters of the temperature gradient method include: maintaining a vacuum degree of 10 -3 Pa, after 2 hours, the temperature was raised from room temperature to 200℃, and then kept at this temperature for 10 hours to remove moisture and air in the raw materials; then the temperature was raised to 800℃, kept at this temperature for 5 hours, and then raised to 1480℃, kept at this temperature for 12 hours; then the temperature was slowly lowered at a rate of 1.5℃ / h to grow crystals. After 200 hours of growth, the crystal growth was terminated, and then the temperature was lowered to room temperature at a rate of 20℃ / h.
[0029] After taking out the crystal, the X-ray diffraction patterns of different Nd concentrations were tested, such as Figure 1 As shown in the figure, the diffraction peaks and relative intensities of the crystals did not change significantly, indicating that Nd:SrF 2 Maintain a single phase. The structural characteristics of the crystal were analyzed by neutron diffraction method and the configuration entropy was calculated. Figure 2 As shown, 30% Nd:SrF 2 The configuration entropy of the crystal is 1.45R, 35% Nd:SrF 2The configuration entropy of the crystal is 1.59R, 40% Nd:SrF 2 The configurational entropy of the crystal is 1.68R.
[0030] The test and analysis results show that the 35% Nd:SrF grown in the above embodiment 2 and 40% Nd:SrF 2 The crystal is a high-entropy crystal, and the optical properties of rare earth ions can be regulated through the structure, which is expected to achieve a "cocktail" effect in the performance of high-entropy crystals.
[0031] Example 2: x% Re:SrF 2 Crystal (x=35、40、50、55) In this embodiment 2, Re:SrF 2 The preparation process of the crystal is similar to that of Example 1, except that ReF 3 (Re 3+ Yb 3+ 、Tm 3+ 、Ho 3+ , Er 3+ , Pr 3+ 、Sm 3+ 、Eu 3+ , Tb 3+ 、Dy 3+ 、Ce 3+ , Y 3+ ,La 3+ , Gd 3+ 、Lu 3+ or Sc 3 + ), SrF 2 , PbF 2 The raw materials are ground into powder in a mortar and mixed thoroughly to obtain a mixed powder.
[0032] Example 3: x% Tm:CaF 2 Crystal (x=35、40、50) Weigh TmF according to the chemical formula 3 , CaF 2 , PbF 2 The raw materials were ground into powder in a mortar and mixed thoroughly, and then placed in a graphite porous crucible. The desired crystals were grown using a temperature gradient method. The growth and testing process were the same as in Example 1.
[0033] Example 4: x% Re:CaF 2 Crystal (x=35、40、50) In this embodiment 4, Re:CaF 2 The preparation process of the crystal is similar to that of Example 1, except that ReF3 (Re 3+ Yb 3+ 、Nd 3+ 、Ho 3+ , Er 3+ , Pr 3+ 、Sm 3+ 、Eu 3+ , Tb 3+ 、Dy 3+ 、Ce 3+ ,La 3+ , Gd 3+ 、Lu 3+ or Sc 3+ ), CaF 2 , PbF 2 The raw materials are ground into powder in a mortar and mixed thoroughly to obtain a mixed powder.
[0034] Example 5x%La:BaF 2 Crystal (x=35、40、50) Weigh LaF according to the chemical formula 3 , BaF 2 , PbF 2 The raw materials were ground into powder in a mortar and mixed thoroughly, and then placed in a graphite porous crucible. The desired crystals were grown using a temperature gradient method. The growth and testing process were the same as in Example 1.
[0035] Example 6x%Gd:BaF 2 Crystal (x=35、40、50) Weigh GdF according to the chemical formula 3 , BaF 2 , PbF 2 The raw materials were ground into powder in a mortar and mixed thoroughly, and then placed in a graphite porous crucible. The desired crystals were grown using a temperature gradient method. The growth and testing process were the same as in Example 1.
[0036] Example 7x% Er:BaF 2 Crystal (x=35、40、50) Weigh ErF according to the chemical formula 3 , BaF 2 , PbF 2 The raw materials were ground into powder in a mortar and mixed thoroughly, and then placed in a graphite porous crucible. The desired crystals were grown using a temperature gradient method. The growth and testing process were the same as in Example 1.
[0037] Example 8x% Yb:BaF 2 Crystal (x=35、40、50) Weigh YbF according to the chemical formula3 , BaF 2 , PbF 2 The raw materials were ground into powder in a mortar and mixed thoroughly, and then placed in a graphite porous crucible. The desired crystals were grown using a temperature gradient method. The growth and testing process were the same as in Example 1.
[0038] Finally, it is necessary to explain that the above embodiments are only detailed descriptions of the specific implementation of the present invention, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, equal transformations and modifications made according to the above content of the present invention belong to the protection scope of the present invention.
Claims
1. A high entropy alkaline earth metal fluoride crystal, characterized in that: The chemical formula of the high entropy alkaline earth metal fluoride crystal is Re 3+ :MeF2; wherein Me is one of Ca, Sr and Ba, Re 3+ The doping concentration is 35at% to 50at%; When Me is Ca or Sr, Re 3+ Yb 3+ 、Nd 3+ 、Tm 3+ 、Ho 3+ , Er 3+ , Pr 3+ 、Sm 3+ 、Eu 3+ , Tb 3+ 、Dy 3+ 、Ce 3+ , Y 3+ ,La 3+ , Gd 3+ 、Lu 3+ Sc 3+ One of; When Me is Ba, Re 3+ Yb 3+ 、Nd 3+ 、Tm 3+ 、Ho 3+ , Er 3+ , Pr 3+ 、Sm 3+ 、Eu 3+ , Tb 3+ 、Ce 3+ ,La 3+ , Gd 3+ 、Lu 3+ Sc 3+ One of them.
2. The high entropy alkaline earth metal fluoride crystal according to claim 1, characterized in that: The configuration entropy of the high entropy alkaline earth metal fluoride crystal is ≥1.5R.
3. A method for preparing high entropy alkaline earth metal fluoride crystals as claimed in claim 1 or 2, characterized in that: include: ReF3 and MeF2 are weighed as raw materials according to the stoichiometric ratio, and the alkaline earth metal fluoride crystal is grown by a temperature gradient method, a pulling method, a crucible descent method, a heat exchange method, a kyvo method, a top seed crystal method, a flux crystal growth method or a micro-pull-down method.
4. The preparation method according to claim 3, characterized in that: The parameters of the temperature gradient method include: vacuum degree ≤10 -3 Pa; material temperature 1300 ~ 1500 ℃; the cooling rate during crystal growth is 1 ~ 5 ℃ / h; the cooling rate after the growth is completed is 10 ~ 30 ℃ / h.
5. The preparation method according to claim 3 or 4, characterized in that: The parameters of the temperature gradient method also include a crystal growth time of 100 to 300 hours.
6. The preparation method according to any one of claims 3 to 5, characterized in that: PbF2 is also added to the raw materials as a deoxidizer, and the amount of PbF2 added is 0.5-2wt% of the total mass of ReF3 and MeF2.
7. The preparation method according to any one of claims 3 to 6, characterized in that: A graphite porous crucible is used in the growth process of the temperature gradient method; and the crystal obtained after the growth of the temperature gradient method is single-phase.
8. An application of a high entropy alkaline earth metal fluoride crystal in the field of local structure regulation of luminescent ions, characterized in that: The chemical formula of the high entropy alkaline earth metal fluoride crystal is Re 3+ :MeF2; wherein Me is one of Ca, Sr and Ba; Re 3+ Yb 3+ 、Nd 3+ 、Tm 3+ 、Ho 3+ , Er 3+ , Pr 3+ 、Sm 3+ 、Eu 3+ , Tb 3+ 、Dy 3+ 、Ce 3+ , Y 3+ ,La 3+ , Gd 3+ 、Lu 3+ Sc 3+ One of them; Re 3+ The total doping concentration is 35at% to 50at%.
9. A method for improving the high entropy performance of alkaline earth metal fluoride crystals, characterized in that: include: The total doping concentration of 35at% to 50at% Re is introduced into the earth metal fluoride crystal MeF2 3+ , thereby achieving the improvement of high entropy performance; wherein Me is one of Ca, Sr, and Ba; Re 3+ Yb 3+ 、Nd 3+ 、Tm 3+ 、Ho 3+ , Er 3+ , Pr 3+ 、Sm 3+ 、Eu 3+ , Tb 3+ 、Dy 3+ 、Ce 3+ , Y 3+ ,La 3 + , Gd 3+ 、Lu 3+ Sc 3+ One of them.
Citation Information
Cited By
Rare earth fluoride laser crystal doped with trivalent luminous ions regulated and controlled by divalent alkaline earth ions as well as preparation and application of rare earth fluoride laser crystal
CN120291207A