Composite pole piece, preparation method thereof and battery
By introducing cluster electrolytes into the lithium battery electrode sheet, the problem of cumbersome and time-consuming preparation process of conventional lithium battery is solved, and the ionic conductivity without liquid injection is achieved, the thermal stability and safety of the battery are improved, and the battery is reduced. production costs.
Patent Information
- Application Number
- CN202411243863.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-15
AI Technical Summary
The preparation process of conventional lithium batteries is complicated and requires additional electrolyte injection to achieve ionic conductivity, which takes a long time.
A composite electrode sheet is adopted, which contains a current collector and an active material layer located on the surface of the current collector. The active material layer contains cluster electrolytes. Complex molecules generated by complexing reaction between lithium salt and organic solvents, and have ionic conductivity. , no additional electrolyte injection is required.
The preparation process of lithium batteries is simplified, process steps are reduced, production efficiency is improved, and good thermal stability and safety are provided, reducing production costs.
Smart Images

Figure CN118969957A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium battery manufacturing, and in particular to a composite pole piece and a preparation method thereof and a battery. Background Art
[0002] Lithium batteries have the characteristics of high specific energy, long cycle life, high voltage platform, good safety and no memory effect. They have been widely used in 3C digital products and electric transportation vehicles, and are gradually occupying a dominant position in the energy storage field.
[0003] The positive and negative electrodes of conventional lithium batteries are generally composed of electrode active materials, binders, conductive agents and current collectors. When preparing the electrodes, it is necessary to first mix the electrode active materials, binders and conductive agents with a solvent to obtain a slurry, and then evenly apply the slurry to the surface of the current collector, and then vacuum dry the current collector coated with the slurry to completely evaporate the solvent in the slurry to obtain the electrode. The prepared electrodes do not contain any solvents and electrolyte lithium salts. When preparing the battery, a large amount of electrolyte needs to be additionally injected, and the battery needs to be left to stand for a long time to allow the electrolyte to penetrate into the internal pores of the electrode so that the electrode has ionic conductivity, thereby realizing the charging and discharging of the battery. This makes the process of preparing lithium batteries using conventional electrodes more cumbersome and time-consuming.
[0004] Therefore, a pole piece is needed that can omit the step of injecting electrolyte when preparing lithium batteries, so as to simplify the preparation process of lithium batteries. Summary of the invention
[0005] The purpose of the present application is to provide a pole piece that can omit the step of injecting electrolyte when preparing a lithium battery, so as to simplify the preparation process of the lithium battery.
[0006] In a first aspect, the present application provides a composite electrode, comprising a current collector and an active material layer located on at least one side of the current collector, wherein the active material layer comprises a cluster electrolyte, wherein the cluster electrolyte comprises complex molecules generated by complex reaction of cations of a lithium salt with organic solvent molecules, and anions of the lithium salt located in the solvation sheath of the cations.
[0007] In some embodiments, the lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl)imide, lithium di(polyfluoroalkoxysulfonyl)imide, tri(trifluoromethylsulfonyl)methyl lithium, lithium dioxalatoborate and lithium difluorooxalatoborate, and / or the organic solvent includes at least one of a carbonate solvent, a fluorocarbonate solvent, an ether solvent, a fluoroether solvent, a carboxylate solvent, and a sulfite solvent.
[0008] In some embodiments, the active material layer also includes a binder, and the binder includes at least one of polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene copolymer; or the binder includes at least one of nitrile rubber, chloroprene rubber, hydrogenated nitrile rubber, carboxylated nitrile rubber, styrene-butadiene rubber and their derivatives.
[0009] In some embodiments, the active material layer also includes an electrode active material and a conductive agent, the electrode active material is a positive electrode active material or a negative electrode active material; the positive electrode active material includes at least one of lithium cobalt oxide, high-pressure lithium cobalt oxide, lithium iron phosphate, lithium iron manganese phosphate, nickel cobalt manganese ternary material, nickel cobalt aluminum ternary material, lithium-rich manganese-based material and lithium manganese oxide, and the negative electrode active material includes at least one of carbon-based material, silicon-based material, silicon-carbon composite material, lithium titanate, tin-based material, germanium-based material and black phosphorus-based material; the conductive agent includes at least one of electric carbon black, carbon nanotubes, nano-carbon fibers and graphene.
[0010] In some embodiments, the active material layer further includes an additive, wherein the additive includes at least one of a performance optimizer, a flame retardant, a solid electrolyte, and an ion-electron dual-conducting material, wherein the performance optimizer includes vinylene carbonate, vinyl ethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, tris(trimethylsilane) borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, difluorooxalato lithium borate, bis(trifluoromethanesulfonyl imide) lithium, bis(fluorosulfonyl imide) lithium, lithium tetrafluoroborate, bis(oxalic acid) At least one of lithium borate, lithium difluorophosphate, lithium trifluoromethylsulfonate and lithium nitrate; the flame retardant includes at least one of tris(2,2,2-trifluoroethyl)phosphite, tris(4-fluorophenyl)phosphine, tris(2,2,3,3,3-pentafluoropropyl)phosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, dimethyl methylphosphonate, diethyl ethylphosphonate, ethoxy pentafluorocyclotriphosphazene, phenoxy pentafluorocyclotriphosphazene, hexamethoxycyclotriphosphazene and ionic liquid; the solid electrolyte includes at least one of inorganic oxide solid electrolyte, sulfide solid electrolyte and halide solid electrolyte; and the ionic electronic dual-conducting material includes inorganic solid-state ionic electronic dual-conducting material and polymer-based ionic electronic dual-conducting material.
[0011] In a second aspect, the present application also provides a method for preparing a composite electrode, comprising: blending raw materials including a lithium salt and an organic solvent to form a mixture; coating the mixture to at least one side surface of a current collector to form an active material layer on the surface of the current collector; and heating the current collector and / or applying negative pressure to allow the organic solvent molecules in the active material layer to combine with the lithium salt to form a cluster electrolyte in situ, and allowing the organic solvent that has not formed the cluster electrolyte to completely volatilize to obtain the composite electrode, wherein the cluster electrolyte includes complex molecules generated by a complex reaction between cations of the lithium salt and molecules of the organic solvent, and anions of the lithium salt located in the solvation sheath of the cations.
[0012] In some embodiments, the lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl)imide, lithium di(polyfluoroalkoxysulfonyl)imide, tri(trifluoromethylsulfonyl)methyl lithium, lithium dioxalatoborate and lithium difluorooxalatoborate, and / or the organic solvent includes at least one of a carbonate solvent, a fluorocarbonate solvent, an ether solvent, a fluoroether solvent, a carboxylate solvent, and a sulfite solvent.
[0013] In some embodiments, the raw material also includes an active material, a conductive agent and a first binder, the first binder is dissolved in the organic solvent, and the first binder includes at least one of nitrile rubber, chloroprene rubber, hydrogenated nitrile rubber, carboxyl nitrile rubber, styrene-butadiene rubber and their derivatives.
[0014] In some embodiments, the method for forming the mixture includes: dissolving the lithium salt in the organic solvent to obtain a cluster electrolyte precursor; dissolving the first binder into the cluster electrolyte precursor to obtain a binding liquid; and adding the active material and the conductive agent to the binding liquid and mixing them evenly to obtain the mixture.
[0015] In some embodiments, the raw material further includes an active material, a conductive agent, and a second binder, wherein the second binder includes at least one of polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene copolymer.
[0016] In some embodiments, the method for forming an active material layer on the surface of the current collector includes: dissolving a lithium salt in an organic solvent to obtain a cluster electrolyte precursor; mixing an active material, a conductive agent, and a second binder to obtain a slurry; applying the slurry to at least one side of the current collector and drying it to form a slurry layer on the surface of the current collector; and uniformly dispersing the cluster electrolyte precursor into the slurry layer through a spraying or infiltration process to form the active material layer.
[0017] In some embodiments, the raw material further includes an additive, the additive including at least one of a performance optimizer, a flame retardant, a solid electrolyte, and an ion-electron dual-conducting material, the performance optimizer including vinyl carbonate, vinyl ethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, tris(trimethylsilane) borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, lithium difluorooxalatoborate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium tetrafluoroborate, bis(oxalatoborate) The invention relates to a novel nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising: a nanostructured carbon nanotube film comprising:
[0018] In a third aspect, the present application further provides a battery, comprising: at least two composite electrodes as described in the first aspect of the present application and a diaphragm arranged between the composite electrodes, wherein the diaphragm is a solid electrolyte diaphragm or a quasi-solid electrolyte diaphragm.
[0019] The beneficial effects of the composite electrode, preparation method thereof, and battery provided in this application include but are not limited to the following:
[0020] The composite electrode provided in the present application has a cluster electrolyte in the active material layer. Under the action of the electric field, the lithium ions in the cluster electrolyte migrate from one lithium salt anion to another lithium salt anion with the assistance of the solvation sheath layer, thereby realizing ion conduction. Therefore, the composite electrode provided in the present application can have ion conductivity without the need for immersion in electrolyte. In the subsequent process of preparing batteries, there is no need to inject electrolyte, thereby reducing the process steps.
[0021] The cluster electrolyte is prepared by heating and / or volatilizing the organic solvent under negative pressure, so that the cluster electrolyte has good thermal stability. Therefore, the composite electrode containing the cluster electrolyte has good thermal stability, and the battery prepared using the composite electrode also has good thermal stability and safety.
[0022] Compared with conventional liquid lithium battery pole pieces, the composite pole pieces provided by the present application have non-volatile and non-flammable electrolytes in the composite pole pieces, so that the battery can obtain better safety under special conditions such as thermal runaway; compared with the pole pieces used in conventional solid-state batteries, the pole pieces used in solid-state batteries require the addition of a large amount of expensive solid electrolyte materials. The composite pole pieces of the present application use cluster electrolytes to achieve the ionic conductivity of the pole pieces, so that the production cost of the composite electrode is also lower than that of the solid-state electrode, and the production process is simpler and more convenient than that of the pole pieces of solid-state batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The following figures describe in detail the exemplary embodiments disclosed in this application. The same reference numerals represent similar structures in several views of the drawings. Those skilled in the art will understand that these embodiments are non-limiting, exemplary embodiments, and the drawings are only for the purpose of illustration and description, and are not intended to limit the scope of this application. Other embodiments may also accomplish the inventive intent in this application. It should be understood that the drawings are not drawn to scale.
[0024] in:
[0025] Figure 1 The present invention is a process flow chart of a method for preparing a composite electrode according to some embodiments of the present application. DETAILED DESCRIPTION
[0026] The following description provides specific application scenarios and requirements of the present application, with the purpose of enabling those skilled in the art to make and use the content in the present application. It will be apparent to those skilled in the art that various local modifications to the disclosed embodiments are apparent, and the general principles defined herein may be applied to other embodiments and applications without departing from the spirit and scope of the present application. Therefore, the present application is not limited to the embodiments shown, but to the widest scope consistent with the claims.
[0027] The present application provides a composite electrode, comprising a current collector and an active material layer located on at least one side of the current collector, wherein the active material layer comprises a cluster electrolyte, wherein the cluster electrolyte comprises complex molecules generated by complex reaction of cations of a lithium salt with organic solvent molecules, and anions of the lithium salt located in the solvation sheath of the cations.
[0028] The composite electrode provided in the present application has a cluster electrolyte in the active material layer. Under the action of the electric field, the lithium ions in the cluster electrolyte migrate from one lithium salt anion to another lithium salt anion with the assistance of the solvation sheath layer, thereby realizing ion conduction. Therefore, the composite electrode provided in the present application can have ion conductivity without the need for immersion in electrolyte. In the subsequent process of preparing batteries, there is no need to inject electrolyte, thereby reducing the process steps.
[0029] The composite electrode and the preparation method thereof provided in the present application will be described in detail below with reference to the embodiments and the accompanying drawings.
[0030] refer to Figure 1 The present application provides a method for preparing a composite electrode, comprising:
[0031] S1: blending raw materials including a lithium salt and an organic solvent to form a mixture;
[0032] S2: applying the mixture to at least one side surface of a current collector to form an active material layer on the surface of the current collector; and
[0033] S3: heating the current collector and / or applying negative pressure to make the organic solvent molecules in the active material layer combine with the lithium salt to form a cluster electrolyte in situ, and completely volatilize the organic solvent that has not formed the cluster electrolyte to obtain the composite electrode.
[0034] The cluster electrolyte includes complex molecules generated by complexation reaction between the cations of the lithium salt and the organic solvent molecules, and anions of the lithium salt located in the solvation sheath of the cations. The solvation sheath described in this application refers to a layer of solvent molecules surrounding the lithium salt cations, i.e., lithium ions, and the organic solvent molecules are tightly combined with the lithium ions through complexation to form a solvation sheath.
[0035] Lithium salt cations and organic solvent molecules undergo complexation, and lithium salt anions enter the solvation sheath of lithium salt cations under the Coulomb force between them, so that "lithium salt cations-organic solvent molecules-lithium salt anions" are "bound" together to form a cluster electrolyte. The conductive mechanism of the cluster electrolyte is that under the action of an electric field, lithium ions in the cluster electrolyte migrate from one lithium salt anion to another lithium salt anion with the assistance of the solvation sheath, thereby achieving ion conduction.
[0036] In some embodiments, the lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl) imide, lithium di(polyfluoroalkoxysulfonyl) imide, tri(trifluoromethylsulfonyl) methyl lithium, lithium dioxalate borate and lithium difluorooxalate borate. Generally, lithium salt is dissolved in an electrolyte solvent as an effective component of an electrolyte to prepare a liquid electrolyte to ensure the lithium ion conductivity between the positive and negative electrodes of a lithium battery. The lithium salt in the present application is dispersed in the composite pole piece in the form of a cluster electrolyte, so that the composite pole piece has ionic conductivity without the need for electrolyte infiltration.
[0037] The organic solvent used in the present application is an organic solvent that can dissolve the lithium salt. In some embodiments, the organic solvent includes at least one of a carbonate solvent, a fluorocarbonate solvent, an ether solvent, a fluoroether solvent, a carboxylate solvent, and a sulfite solvent.
[0038] In some embodiments, the carbonate solvent includes at least one of ethylene carbonate, 1,2-dimethylethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dibutyl carbonate and derivatives thereof.
[0039] In some embodiments, the fluorocarbonate solvent includes at least one of fluoroethylene carbonate, bisfluoroethylene carbonate, trifluoromethylethylene carbonate, methyl trifluoroethyl carbonate, fluorodimethyl carbonate and derivatives thereof.
[0040] In some embodiments, the ether solvent includes at least one of tetrahydrofuran, dioxolane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether and derivatives thereof.
[0041] In some embodiments, the fluoroether solvent is a linear fluoroether with the structural formula: R1-O-R2, wherein R1 and R2 may be individually or both methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, isobutyl, tert-butyl, pentyl, isopentyl, etc., and groups in which some or all of the hydrogen atoms are substituted by fluorine.
[0042] In some embodiments, the fluoroether solvent includes at least one of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,3,3,3-hexafluoropropyl-2,2,2-trifluoroethyl ether, 1,1,1,3,3,3-hexafluoropropyl-methyl ether, 1,1,1,2,3,3-hexafluoropropyl-2,2,3,3-tetrafluoropropyl ether and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether.
[0043] In some embodiments, the carboxylate solvent includes at least one of methyl formate, methyl acetate, ethyl acetate and derivatives thereof.
[0044] In some embodiments, the sulfite solvent includes at least one of dimethyl sulfite, diethyl sulfite and derivatives thereof.
[0045] In some embodiments, the raw material also includes an active material, a conductive agent and a first binder, the first binder is dissolved in the organic solvent, and the first binder includes at least one of nitrile rubber, chloroprene rubber, hydrogenated nitrile rubber, carboxyl nitrile rubber, styrene-butadiene rubber and their derivatives.
[0046] The organic solvent used in this application is an organic solvent that can dissolve the lithium salt, and the binder generally used in the preparation process of the pole piece, such as polyvinylidene fluoride binder, cannot be dissolved in such organic solvents. Therefore, if a traditional binder is to be used, it is necessary to use other organic solvents that can dissolve the binder to dissolve the binder first to obtain a binder solution, and then mix the binder solution with the cluster electrolyte precursor, active material and conductive agent. The steps and processes are cumbersome. Therefore, in some embodiments, the present application uses a first binder that is soluble in the organic solvent, thereby avoiding the use of other solvents different from the organic solvent during the preparation process and simplifying the preparation process.
[0047] When the first binder is used to prepare a mixture, the first binder can be directly blended with the organic solvent. Specifically, in some embodiments, the method of forming the mixture includes: dissolving the lithium salt in the organic solvent to obtain a cluster electrolyte precursor; dissolving the first binder into the cluster electrolyte precursor to obtain a binding liquid; and adding the active material and the conductive agent to the binding liquid and mixing them evenly to obtain the mixture. In other embodiments, the method of forming the mixture includes: adding the active material, the conductive agent, the first binder, and the lithium salt to the organic solvent and mixing them evenly to obtain the slurry. In some embodiments, the mixing method is stirring or ball milling.
[0048] In some embodiments, the mass percentages of the active material, the conductive agent, the first binder, the lithium salt and the organic solvent are (20% to 70%): (0.1% to 10%): (0.1% to 10%): (1% to 20%): (15% to 60%).
[0049] In some embodiments, the active material is a positive electrode active material or a negative electrode active material, the positive electrode active material includes at least one of lithium cobalt oxide, high-pressure lithium cobalt oxide, lithium iron phosphate, lithium iron manganese phosphate, nickel cobalt manganese ternary material, nickel cobalt aluminum ternary material, lithium-rich manganese-based material and lithium manganese oxide, and the negative electrode active material includes at least one of carbon-based material, silicon-based material, silicon-carbon composite material, tin-based material, germanium-based material, lithium titanate and black phosphorus-based material.
[0050] In some embodiments, the carbon-based material includes at least one of artificial graphite, natural graphite, mesophase carbon microbeads and hard carbon; the silicon-based material includes at least one of elemental silicon and silicon monoxide; the silicon-carbon composite material includes a complex of elemental silicon and at least one of artificial graphite and natural graphite or a complex of silicon monoxide and at least one of artificial graphite and natural graphite; the tin-based material includes at least one of elemental tin or tin oxide; the germanium-based material includes at least one of elemental germanium or germanium oxide; and / or the black phosphorus-based material includes black phosphorus and antimony-doped black phosphorus.
[0051] In some embodiments, the conductive agent includes at least one of electric carbon black, carbon nanotubes, nanocarbon fibers, and graphene.
[0052] In some embodiments, the active material, the conductive agent, the first binder, and the lithium salt are added to the organic solvent and mixed evenly, and then an additive is added to the organic solvent. The additive is evenly mixed with the active material, the conductive agent, the first binder, the lithium salt and the organic solvent to obtain the slurry.
[0053] In some embodiments, the additive includes at least one of a performance optimizer, a flame retardant, a solid electrolyte, and an ionic-electronic dual-conducting material.
[0054] The performance optimizer is generally used to improve the coulombic efficiency, cycle stability, rate performance of the battery and to improve the capacity of the battery at high or low temperatures. In some embodiments, the performance optimizer includes vinylene carbonate, vinyl ethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane)phosphate, tris(trimethylsilane)phosphite, tris(trimethylsilane)borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, lithium difluorooxalate borate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium tetrafluoroborate, lithium bis(oxalate borate), lithium difluorophosphate, lithium trifluoromethanesulfonate and at least one of lithium nitrate.
[0055] The pole piece may burn under extreme abuse conditions, and adding the flame retardant can further improve the safety of the composite pole piece. In some embodiments, the flame retardant includes at least one of tris(2,2,2-trifluoroethyl)phosphite, tris(4-fluorophenyl)phosphine, tris(2,2,3,3,3-pentafluoropropyl)phosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, dimethyl methylphosphonate, diethyl ethylphosphonate, ethoxy pentafluorocyclotriphosphazene, phenoxy pentafluorocyclotriphosphazene, hexamethoxycyclotriphosphazene and ionic liquid.
[0056] The solid electrolyte can further improve the lithium ion conductivity of the composite electrode, thereby improving the rate performance and cycle life of the battery. In some embodiments, the solid electrolyte includes at least one of an inorganic oxide solid electrolyte, a sulfide solid electrolyte, and a halide solid electrolyte. In some embodiments, the inorganic oxide solid electrolyte includes at least one of LLZO, LLZTO, LATP, and LAGP. In some embodiments, the sulfide solid electrolyte includes Li 10 GeP2S 12 In some embodiments, the halide solid electrolyte comprises at least one of Li3InCl6, Li3YCl3 and Li2ZrCl6.
[0057] The ionic electronic dual-conducting material can further improve the ionic conductivity and electronic conductivity of the composite pole piece, reduce the internal resistance of the battery, and improve the rate performance and cycle life of the battery. In some embodiments, the ionic electronic dual-conducting material includes an inorganic solid-state ionic electronic dual-conducting material and a polymer-based ionic electronic dual-conducting material. In some embodiments, the inorganic solid-state ionic electronic dual-conducting material includes at least one of carbon-coated lithium aluminum titanium phosphate and carbon-coated lithium lanthanum zirconium oxide. In some embodiments, the polymer-based ionic electronic dual-conducting material includes a carbon-grafted PEO-based polymer electrolyte material.
[0058] In some embodiments, the raw material further includes an active material, a conductive agent, and a second binder, wherein the second binder includes at least one of polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene copolymer.
[0059] In addition to using the first binder described in the present application, a second binder that is insoluble in the organic solvent may also be used, that is, the binder required for conventional preparation of pole pieces. Without changing the pole piece preparation process in the prior art, the pole piece is sprayed or infiltrated to generate a cluster electrolyte in situ inside the pole piece.
[0060] Specifically, in some embodiments, the method for forming an active material layer on the surface of the current collector includes: dissolving a lithium salt in an organic solvent to obtain a cluster electrolyte precursor; mixing an active material, a conductive agent and a second binder to obtain a slurry; applying the slurry to at least one side surface of the current collector and drying it to form a slurry layer on the surface of the current collector; and uniformly dispersing the cluster electrolyte precursor into the slurry layer through a spraying or infiltration process to form the active material layer.
[0061] In some embodiments, the method of mixing the active material, the conductive agent and the second binder to obtain the slurry comprises adding the active material, the conductive agent and the second binder to a dispersant and stirring to obtain the slurry. In some embodiments, the dispersant comprises N-methylpyrrolidone.
[0062] In some embodiments, the current collector is copper foil, aluminum foil, nickel foil, stainless steel foil or a conductive plastic film.
[0063] In some embodiments, the heating temperature is 30-120°C, for example, 30°C, 50°C, 70°C, 100°C or 120°C; and the heating time is 2-100h, for example, 2h, 10h, 50h, 80h or 100h.
[0064] In some embodiments, the negative pressure is applied by placing the current collector in a vacuum environment, for example, a vacuum oven.
[0065] In some embodiments, the magnitude of the applied negative pressure is -0.02 MPa to -0.1 MPa, for example, -0.02 MPa, -0.05 MPa or -0.1 MPa.
[0066] During the heating and / or negative pressure process, as the organic solvent in the cluster electrolyte precursor that has not formed the cluster electrolyte evaporates, the cluster electrolyte and the first binder are combined to form a bonding network structure with ionic conductivity. The bonding network structure uniformly covers the active material and the conductive agent, and lithium ions are transmitted between the bonding networks. The composite electrode has ionic conductivity without the need for electrolyte infiltration. In the subsequent battery preparation process, there is no need to inject electrolyte, thereby reducing the process steps.
[0067] The present application also provides a composite electrode, comprising a current collector and an active material layer located on at least one side of the current collector, wherein the active material layer comprises a cluster electrolyte, wherein the cluster electrolyte comprises complex molecules generated by complex reaction of cations of a lithium salt with organic solvent molecules, and anions of the lithium salt located in the solvation sheath of the cations.
[0068] Lithium salt cations and organic solvent molecules undergo complexation, and lithium salt anions enter the solvation sheath of lithium salt cations under the Coulomb force between them, so that "lithium salt cations-organic solvent molecules-lithium salt anions" are "bound" together to form a cluster electrolyte. The conductive mechanism of the cluster electrolyte is that under the action of an electric field, lithium ions in the cluster electrolyte migrate from one lithium salt anion to another lithium salt anion with the assistance of the solvation sheath, thereby achieving ion conduction.
[0069] In some embodiments, the lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl)imide, lithium di(polyfluoroalkoxysulfonyl)imide, tri(trifluoromethylsulfonyl)methyl lithium, lithium bisoxalatoborate, and lithium difluorooxalatoborate.
[0070] In some embodiments, the organic solvent includes at least one of a carbonate solvent, a fluorocarbonate solvent, an ether solvent, a fluoroether solvent, a carboxylate solvent, and a sulfite solvent.
[0071] In some embodiments, the carbonate solvent includes at least one of ethylene carbonate, 1,2-dimethylethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dibutyl carbonate and derivatives thereof.
[0072] In some embodiments, the fluorocarbonate solvent includes at least one of fluoroethylene carbonate, bisfluoroethylene carbonate, trifluoromethylethylene carbonate, methyl trifluoroethyl carbonate, fluorodimethyl carbonate and derivatives thereof.
[0073] In some embodiments, the ether solvent includes at least one of tetrahydrofuran, dioxolane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether and derivatives thereof.
[0074] In some embodiments, the fluoroether solvent is a linear fluoroether with the structural formula: R1-O-R2, wherein R1 and R2 may be individually or both methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, isobutyl, tert-butyl, pentyl, isopentyl, etc., and groups in which some or all of the hydrogen atoms are substituted by fluorine.
[0075] In some embodiments, the fluoroether solvent includes at least one of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,3,3,3-hexafluoropropyl-2,2,2-trifluoroethyl ether, 1,1,1,3,3,3-hexafluoropropyl-methyl ether, 1,1,1,2,3,3-hexafluoropropyl-2,2,3,3-tetrafluoropropyl ether and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether.
[0076] In some embodiments, the carboxylate solvent includes at least one of methyl formate, methyl acetate, ethyl acetate and derivatives thereof.
[0077] In some embodiments, the sulfite solvent includes at least one of dimethyl sulfite, diethyl sulfite and derivatives thereof.
[0078] In some embodiments, the active material layer also includes a binder, and the binder includes at least one of polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene copolymer; or the binder includes at least one of nitrile rubber, chloroprene rubber, hydrogenated nitrile rubber, carboxylated nitrile rubber, styrene-butadiene rubber and their derivatives.
[0079] In some embodiments, the active material layer also includes an electrode active material and a conductive agent, the electrode active material is a positive electrode active material or a negative electrode active material; the positive electrode active material includes at least one of lithium cobalt oxide, high-pressure lithium cobalt oxide, lithium iron phosphate, lithium iron manganese phosphate, nickel cobalt manganese ternary material, nickel cobalt aluminum ternary material, lithium-rich manganese-based material and lithium manganese oxide, and the negative electrode active material includes at least one of carbon-based material, silicon-based material, silicon-carbon composite material, lithium titanate, tin-based material, germanium-based material and black phosphorus-based material; the conductive agent includes at least one of electric carbon black, carbon nanotubes, nano-carbon fibers and graphene.
[0080] In some embodiments, the active material layer further includes an additive, wherein the additive includes at least one of a performance optimizer, a flame retardant, a solid electrolyte, and an ion-electron dual-conducting material, wherein the performance optimizer includes vinylene carbonate, vinyl ethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, tris(trimethylsilane) borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, difluorooxalato lithium borate, bis(trifluoromethanesulfonyl imide) lithium, bis(fluorosulfonyl imide) lithium, lithium tetrafluoroborate, bis(oxalic acid) At least one of lithium borate, lithium difluorophosphate, lithium trifluoromethylsulfonate and lithium nitrate; the flame retardant includes at least one of tris(2,2,2-trifluoroethyl)phosphite, tris(4-fluorophenyl)phosphine, tris(2,2,3,3,3-pentafluoropropyl)phosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, dimethyl methylphosphonate, diethyl ethylphosphonate, ethoxy pentafluorocyclotriphosphazene, phenoxy pentafluorocyclotriphosphazene, hexamethoxycyclotriphosphazene and ionic liquid; the solid electrolyte includes at least one of inorganic oxide solid electrolyte, sulfide solid electrolyte and halide solid electrolyte; and the ionic electronic dual-conducting material includes inorganic solid-state ionic electronic dual-conducting material and polymer-based ionic electronic dual-conducting material.
[0081] In some embodiments, the current collector is copper foil, aluminum foil, nickel foil, stainless steel foil or a conductive plastic film.
[0082] The composite electrode provided in the present application has a cluster electrolyte in the active material layer. Under the action of the electric field, the lithium ions in the cluster electrolyte migrate from one lithium salt anion to another lithium salt anion with the assistance of the solvation sheath layer, thereby realizing ion conduction. Therefore, the composite electrode provided in the present application can have ion conductivity without the need for immersion in electrolyte. In the subsequent process of preparing batteries, there is no need to inject electrolyte, thereby reducing the process steps.
[0083] The present application also provides a battery, comprising: at least two composite electrodes provided in the present application, serving as the positive electrode and negative electrode of the battery respectively; and a diaphragm arranged between the composite electrodes, wherein the diaphragm is a solid electrolyte diaphragm or a quasi-solid electrolyte diaphragm.
[0084] Since the composite electrode sheet contains a cluster electrolyte, it can have ion conductivity without being soaked in an electrolyte. In the preparation process of the battery, no electrolyte needs to be added, thereby reducing the process steps.
[0085] In some embodiments, the solid electrolyte membrane includes one or more of a polymer solid electrolyte membrane, an oxide solid electrolyte membrane, a sulfide solid electrolyte membrane, a halide solid electrolyte membrane, and an organic / inorganic composite solid electrolyte membrane. In some embodiments, the polymer electrolyte membrane includes one or more of a polyethylene oxide (PEO)-based solid electrolyte membrane and a polyvinylidene fluoride (PVDF)-based solid electrolyte membrane.
[0086] In some embodiments, the quasi-solid electrolyte membrane includes one or more of a polymer quasi-solid electrolyte membrane, an oxide quasi-solid electrolyte membrane, a sulfide quasi-solid electrolyte membrane, a halide quasi-solid electrolyte membrane, and an organic / inorganic composite quasi-solid electrolyte membrane. In some embodiments, the polymer quasi-solid electrolyte includes one or more of a polyoxyethylene quasi-solid electrolyte membrane, a polyvinylidene fluoride quasi-solid electrolyte membrane, and a polyolefin reference solid electrolyte membrane.
[0087] In some embodiments, the battery may be a pouch-type battery, a cylindrical battery, or a square-type battery.
[0088] The preparation process of traditional lithium batteries is relatively complicated. Currently, there are many steps in the assembly process of lithium batteries. Taking soft-pack lithium batteries as an example, its preparation process mainly includes slurrying, coating, drying, rolling, slitting, die-cutting, lamination, shell packaging, liquid injection, standing, formation and other processes. The purpose of liquid injection is to allow the electrolyte to penetrate into the active material layer of the electrode so that lithium ions can be transmitted between the electrodes. After liquid injection, the battery needs to be left standing for a long time (the standing time at room temperature is greater than 12 hours, and the standing time at high temperature (40-60°C) is greater than 4 hours) to allow the electrolyte to fully infiltrate the active material layer. The process is time-consuming.
[0089] The pole piece used in the battery provided in the present application can have good lithium ion conductivity without injecting electrolyte, thereby eliminating the step of injecting electrolyte during battery preparation and reducing the battery standing time (3 to 5 hours at room temperature and 1 to 2 hours at high temperature (40 to 60°C)), simplifying the preparation process of lithium batteries and improving battery production efficiency
[0090] The specific implementation methods of the present application are further described below in combination with examples and comparative examples, but the present application is not limited to the following examples. The following examples are all conventional experimental methods unless otherwise specified; the reagents and materials used can be obtained from commercial channels unless otherwise specified.
[0091] Example 1 Preparation of positive electrode sheet
[0092] 9.0g of lithium cobalt oxide positive electrode material, 0.5g of chloroprene rubber, 0.5g of conductive carbon black, 1.3g of lithium bis(trifluoromethylsulfonyl)imide, 2.4g of ethylene carbonate, 2.2g of dimethyl carbonate and 0.33g of fluoroethylene carbonate were mixed evenly, and a uniform mixture was obtained by sufficient mechanical stirring. Then the mixture was evenly coated on an aluminum foil, and the aluminum foil was placed in a vacuum drying oven at 100°C and dried for 3h to obtain a composite electrode sheet, and the composite sheet was rolled and compacted, and cut with a punching and slicing machine to obtain a positive electrode sheet with a diameter of 16mm.
[0093] Example 2 Preparation of positive electrode sheet
[0094] Take 0.6g of nitrile rubber and add it to a solution composed of 5.6g of ethylene carbonate, 4.1g of ethylene glycol dimethyl ether, 1.4g of lithium trifluoromethanesulfonate and 0.2g of vinylene carbonate, and stir to completely dissolve the nitrile rubber to obtain a bonding solution. Add 10.8g of NCM811 positive electrode material and 0.6g of acetylene black to the bonding solution, and stir thoroughly to mix the electrode material, binder and conductive agent to obtain a mixture. Then, the mixture is evenly coated on a carbon-coated aluminum foil. The carbon-coated aluminum foil is placed in a vacuum drying oven at 80°C and dried for 6h to obtain a composite electrode plate, which is rolled and compacted, and cut with a punching slicer to obtain a positive electrode plate with a diameter of 16mm.
[0095] Example 3 Preparation of positive electrode sheet
[0096] 9.4g of lithium iron phosphate positive electrode material, 0.55g of styrene-butadiene rubber, 0.33g of conductive carbon black, 1.2g of lithium bis(trifluoromethylsulfonyl)imide, 0.9g of lithium bis(fluorosulfonyl)imide, 6.5g of ethylene carbonate, 5.1g of ethyl methyl carbonate, 5.9g of diethyl carbonate and 0.2g of lithium difluorooxalate borate were mixed evenly, and a uniform mixture was obtained by ball milling. The mixture was evenly coated on a carbon-coated aluminum foil, and the carbon-coated aluminum foil was placed in a blast drying oven at 120°C and dried for 2h to obtain a composite electrode sheet, and the composite sheet was rolled and compacted, and cut with a punching and slicing machine to obtain a positive electrode sheet with a diameter of 16mm.
[0097] Example 4 Preparation of positive electrode sheet
[0098] 6.5g of lithium iron phosphate positive electrode material, 0.8g of hydrogenated nitrile rubber, 0.8g of conductive carbon black, 2.5g of tris(trifluoromethylsulfonyl)methyl lithium, 3.5g of propylene carbonate, 4.5g of dimethyl carbonate, 7.8g of dibutyl carbonate and 0.45g of trimethyl phosphite were mixed evenly, and a uniform mixture was obtained by ball milling. The mixture was evenly coated on an aluminum foil, and the aluminum foil was placed in a blast drying oven at 100°C and dried for 6h to obtain a composite electrode sheet, and then the composite electrode sheet was rolled and compacted, and cut with a punching slicer to obtain a positive electrode sheet with a diameter of 16mm.
[0099] Example 5 Preparation of positive electrode sheet
[0100] 9.5g of NCM523 positive electrode material, 0.46g of carboxylated nitrile rubber, 0.32g of Ketjen black, 2.1g of lithium bis(fluorosulfonyl)imide, 4.6g of propylene carbonate, 5.8g of ethylene glycol dimethyl ether, 0.13g of vinyl carbonate, and 0.25g of lithium lanthanum zirconium oxide (LLZO) were mixed evenly, and a uniform mixture was obtained by sufficient mechanical stirring. The mixture was then evenly coated on an aluminum foil, and the aluminum foil was placed in a vacuum drying oven at 90°C and dried for 4h to obtain a composite electrode sheet, which was rolled and compacted, and cut with a punching slicer to obtain a positive electrode sheet with a diameter of 16mm.
[0101] Example 6 Preparation of positive electrode sheet
[0102] Take 4.8g of lithium cobalt oxide, 0.6g of conductive carbon black and 8.6g of polyvinylidene fluoride solution (7%, N-methylpyrrolidone as solvent) and mix them evenly by mechanical stirring to prepare electrode slurry. The slurry is evenly coated on aluminum foil, and the aluminum foil is placed in an electric heating blast drying oven for drying and heating at 100°C under normal pressure for 1h to obtain a preliminarily dried electrode plate, and then the preliminarily dried electrode plate is placed in a vacuum drying oven for vacuum heating and drying at 100°C for 8h to obtain a completely dried lithium cobalt oxide electrode.
[0103] 6.2 g of lithium trifluoromethanesulfonate was added to a mixed organic solvent of 14.5 g of ethylene carbonate and 21.3 g of diethyl carbonate, and the mixture was stirred sufficiently to completely dissolve the lithium trifluoromethanesulfonate. The stirring was continued for 2 h to form a cluster electrolyte precursor.
[0104] The lithium cobalt oxide dry electrode was immersed in the cluster electrolyte precursor for 1 minute, then taken out and placed in an electric hot air drying oven for heating and drying at 100°C at normal pressure for 4 hours to obtain a composite electrode sheet. The composite electrode sheet was rolled and compacted, and cut with a punching and slicing machine to obtain a composite positive electrode sheet with a diameter of 16 mm.
[0105] Example 7 Preparation of positive electrode sheet
[0106] 3.6g NCM622, 0.2g acetylene black and 3.3g polyvinylidene fluoride solution (6%, N,N-dimethylacetamide as solvent) were mixed and mixed evenly by mechanical stirring to prepare electrode slurry. The slurry was evenly coated on aluminum foil, and the aluminum foil was placed in an electric heating blast drying oven for drying and heating at 80°C at normal pressure for 2h to obtain a preliminarily dried electrode sheet, and then the preliminarily dried electrode sheet was placed in a vacuum drying oven for vacuum heating and drying at 100°C for 8h to obtain a completely dried NCM622 electrode.
[0107] Take 5.7 g of lithium bis(trifluoromethylsulfonyl)imide and add it to a mixed solvent consisting of 8.4 g of propylene carbonate, 15.0 g of dimethyl carbonate and 1.5 g of fluoroethylene carbonate. Stir well to completely dissolve the lithium bis(trifluoromethylsulfonyl)imide. Continue stirring for 2 h to form a cluster electrolyte precursor.
[0108] Use a spray gun or other spraying equipment to evenly spray the cluster electrolyte precursor on the NCM622 dry electrode, let it stand for 10 minutes, and then repeat the spraying once to fully infiltrate the electrode with the cluster electrolyte precursor. Place the infiltrated electrode in a vacuum drying oven and heat and dry it at 100°C for 2 hours to obtain a composite electrode sheet. Roll the composite electrode sheet and cut it with a punching machine to obtain a composite positive electrode sheet with a diameter of 16 mm.
[0109] Example 8 Preparation of negative electrode sheet
[0110] 8.9 g of artificial graphite negative electrode material, 0.8 g of chloroprene rubber, 0.7 g of Ketjen black, 1.9 g of lithium bis(fluorosulfonyl)imide, 10.6 g of ethylene carbonate, 8.1 g of ethyl methyl carbonate, 7.8 g of diethyl carbonate and 0.2 g of 1,3-propane sultone were mixed, and the chloroprene rubber was completely dissolved by sufficient mechanical stirring to obtain a uniformly mixed slurry, and then the slurry was evenly coated on a copper foil, and the copper foil was placed in a vacuum drying oven at 90° C. and dried for 4 h to obtain a composite electrode sheet, the composite electrode sheet was roller-compacted, and a negative electrode sheet with a diameter of 17 mm was cut with a punching slicer.
[0111] Example 9 Preparation of Battery
[0112] The positive electrode sheets prepared in Examples 1 to 7 were respectively assembled with the negative electrode sheets prepared in Example 8 in a stacked manner to prepare button batteries. The diaphragm used a polyvinylidene fluoride-based solid electrolyte diaphragm with good ionic conductivity. The battery assembly process is consistent with the conventional button battery assembly process, except that the injection process is omitted. After the battery is sealed, it is placed in a 40°C temperature box for 1 hour. The battery is taken out and cooled to room temperature for electrical performance testing. The battery is numbered according to the embodiment in which the positive electrode sheet used in the battery is located. The test performance of the battery is shown in the following table:
[0113] Table 1 Battery discharge capacity and cycle performance at different rates
[0114]
[0115] As can be seen from Table 1, the positive electrode sheets (Examples 1 to 7) and negative electrode sheets (Example 8) prepared by the technical solution of the present application and the batteries assembled therefrom can be charged and discharged normally without injecting electrolyte, and can fully exert the gram capacity of different battery materials. The reason is that the composite electrode provided by the present application contains a cluster electrolyte, which has good ion conductivity and is evenly distributed in the active material layer, so that lithium ions can be transmitted in the active material layer. Therefore, the composite electrode can achieve ion conductivity without the need for additional injection of electrolyte, thereby achieving normal charging and discharging of the battery.
[0116] The composite electrode provided in the present application contains uniformly distributed cluster electrolytes, which enables the electrode itself to have good ionic conductivity. The cluster electrolyte is prepared by heating the cluster electrolyte precursor and volatilizing the organic solvent under negative pressure, which enables the cluster electrolyte to have good thermal stability. Therefore, the composite electrode containing the cluster electrolyte has good thermal stability, and the battery prepared using the composite electrode also has good thermal stability and safety.
[0117] Compared with conventional liquid lithium battery pole pieces, the composite pole piece provided by this application has a non-volatile and non-flammable electrolyte in the composite pole piece, so the battery can obtain better safety under special conditions such as thermal runaway; compared with the pole pieces used in conventional solid-state batteries, the pole pieces used in solid-state batteries need to add a large amount of expensive solid electrolyte materials. The composite pole piece of this application uses cluster electrolytes to achieve the ionic conductivity of the pole piece, making the production cost of the composite electrode lower than that of the solid-state electrode, and the production process is simpler and more convenient than that of the pole piece of the solid-state battery. Therefore, the composite pole piece provided by the application has laid a solid foundation for the research and development and production of high-performance lithium batteries.
[0118] In summary, after reading the contents of this application, those skilled in the art will appreciate that the aforementioned application contents may be presented only in an exemplary manner and may not be restrictive. Although not explicitly stated herein, those skilled in the art will appreciate that this application is intended to encompass various reasonable changes, improvements and modifications to the embodiments. These changes, improvements and modifications are within the spirit and scope of the exemplary embodiments of this application.
[0119] It should be understood that the term “and / or” used in this embodiment includes any or all combinations of one or more of the associated listed items.
[0120] Similarly, it should be understood that the terms "comprise", "comprising", "including" or "comprising", when used in this application document, indicate the presence of the recorded features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof.
[0121] It should also be understood that although the terms first, second, third, etc. can be used to describe various elements, these elements should not be limited by these terms. These terms are only used to distinguish an element from another element. Therefore, without departing from the teaching of the application, the first element in some embodiments can be called the second element in other embodiments.
Claims
1. A composite pole piece, It is characterized in that It includes a current collector and an active material layer located on at least one side of the current collector, wherein the active material layer includes a cluster electrolyte, and the cluster electrolyte includes complex molecules generated by complex reaction between cations of lithium salt and organic solvent molecules, and anions of the lithium salt located in the solvation sheath of the cations.
2. The composite pole piece according to claim 1, It is characterized in that The lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl)imide, lithium di(polyfluoroalkoxysulfonyl)imide, tri(trifluoromethylsulfonyl)methyl lithium, lithium dioxalatoborate and lithium difluorooxalatoborate, and / or the organic solvent includes at least one of carbonate solvents, fluorocarbonate solvents, ether solvents, fluoroether solvents, carboxylate solvents and sulfite solvents.
3. The composite pole piece according to claim 1, It is characterized in that The active material layer also includes a binder, which includes at least one of polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene copolymer; or the binder includes at least one of nitrile rubber, chloroprene rubber, hydrogenated nitrile rubber, carboxyl nitrile rubber, styrene butadiene rubber and their derivatives.
4. The composite pole piece according to claim 3, It is characterized in that The active material layer further includes an electrode active material and a conductive agent, wherein the electrode active material is a positive electrode active material or a negative electrode active material; the positive electrode active material includes at least one of lithium cobalt oxide, high-pressure lithium cobalt oxide, lithium iron phosphate, lithium iron manganese phosphate, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium-rich manganese-based material and lithium manganese oxide, and the negative electrode active material includes at least one of carbon-based material, silicon-based material, silicon-carbon composite material, lithium titanate, tin-based material, germanium-based material and black phosphorus-based material; The conductive agent includes at least one of electric carbon black, carbon nanotubes, nanocarbon fibers and graphene.
5. The composite pole piece according to claim 4, It is characterized in that The active material layer further includes an additive, wherein the additive includes at least one of a performance optimizer, a flame retardant, a solid electrolyte, and an ion-electron dual-conducting material. The performance optimizer includes at least one of vinylene carbonate, vinylethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, tris(trimethylsilane) borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, lithium difluorooxalatoborate, lithium bistrifluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, lithium tetrafluoroborate, lithium bisoxalatoborate, lithium difluorophosphate, lithium trifluoromethanesulfonate and lithium nitrate; The flame retardant comprises at least one of tris(2,2,2-trifluoroethyl)phosphite, tris(4-fluorophenyl)phosphine, tris(2,2,3,3,3-pentafluoropropyl)phosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, dimethyl methylphosphonate, diethyl ethylphosphonate, ethoxy pentafluorocyclotriphosphazene, phenoxy pentafluorocyclotriphosphazene, hexamethoxycyclotriphosphazene and ionic liquid; The solid electrolyte includes at least one of an inorganic oxide solid electrolyte, a sulfide solid electrolyte and a halide solid electrolyte; and The ionic-electronic dual-conducting materials include inorganic solid-state ionic-electronic dual-conducting materials and polymer-based ionic-electronic dual-conducting materials.
6. A method for preparing a composite electrode. It is characterized in that include: blending raw materials including a lithium salt and an organic solvent to form a mixture; Applying the mixture to at least one side surface of a current collector to form an active material layer on the surface of the current collector; as well as The current collector is heated and / or negative pressure is applied, so that the organic solvent molecules in the active material layer combine with the lithium salt to form a cluster electrolyte in situ, and the organic solvent that has not formed the cluster electrolyte is completely volatilized to obtain the composite electrode, wherein the cluster electrolyte includes complex molecules generated by the complex reaction between the cations of the lithium salt and the organic solvent molecules, and the anions of the lithium salt located in the solvation sheath of the cations.
7. The preparation method according to claim 6, It is characterized in that The lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl)imide, lithium di(polyfluoroalkoxysulfonyl)imide, tri(trifluoromethylsulfonyl)methyl lithium, lithium dioxalatoborate and lithium difluorooxalatoborate, and / or the organic solvent includes at least one of carbonate solvents, fluorocarbonate solvents, ether solvents, fluoroether solvents, carboxylate solvents and sulfite solvents.
8. The preparation method according to claim 6, It is characterized in that The raw material also includes an active material, a conductive agent and a first binder, the first binder is dissolved in the organic solvent, and the first binder includes at least one of nitrile rubber, chloroprene rubber, hydrogenated nitrile rubber, carboxyl nitrile rubber, styrene butadiene rubber and derivatives thereof.
9. The preparation method according to claim 8, It is characterized in that The method of forming the mixture comprises: dissolving the lithium salt in the organic solvent to obtain a cluster electrolyte precursor; dissolving the first binder into the cluster electrolyte precursor to obtain a binder solution; and The active material and the conductive agent are added into the binder and mixed uniformly to obtain the mixture.
10. The preparation method according to claim 6, It is characterized in that The raw material further includes an active material, a conductive agent and a second binder, wherein the second binder includes at least one of polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene copolymer.
11. The preparation method according to claim 10, It is characterized in that The method for forming an active material layer on the surface of the current collector comprises: Dissolving lithium salt in an organic solvent to obtain a cluster electrolyte precursor; The active material, the conductive agent and the second binder are mixed to obtain a slurry; the slurry is applied to at least one side surface of the current collector and dried to form a slurry layer on the surface of the current collector; the cluster electrolyte precursor is evenly dispersed in the slurry layer through a spraying or infiltration process to form the active material layer.
12. The preparation method according to claim 6, It is characterized in that The raw material further includes an additive, wherein the additive includes at least one of a performance optimizer, a flame retardant, a solid electrolyte, and an ion-electron dual-conducting material. The performance optimizer includes at least one of vinylene carbonate, vinylethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, tris(trimethylsilane) borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, lithium difluorooxalatoborate, lithium bistrifluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, lithium tetrafluoroborate, lithium bisoxalatoborate, lithium difluorophosphate, lithium trifluoromethanesulfonate and lithium nitrate; The flame retardant comprises at least one of tris(2,2,2-trifluoroethyl)phosphite, tris(4-fluorophenyl)phosphine, tris(2,2,3,3,3-pentafluoropropyl)phosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, dimethyl methylphosphonate, diethyl ethylphosphonate, ethoxy pentafluorocyclotriphosphazene, phenoxy pentafluorocyclotriphosphazene, hexamethoxycyclotriphosphazene and ionic liquid; The solid electrolyte includes at least one of an inorganic oxide solid electrolyte, a sulfide solid electrolyte and a halide solid electrolyte; and The ionic-electronic dual-conducting material comprises an inorganic solid-state ionic conductor material and a polymer-based ionic-electronic dual-conducting material.
13. A battery, It is characterized in that include: At least two composite electrodes as claimed in claims 1 to 5 and a diaphragm arranged between the composite electrodes, wherein the diaphragm is a solid electrolyte diaphragm or a quasi-solid electrolyte diaphragm.
Citation Information
Cited By
Preparation method of high-temperature-resistant lithium battery cell
CN120767287A
Electrolyte, and lithium-ion battery and preparation method therefor