Extruded foam sheet, and method and device for inspecting extruded foam sheet

By performing image processing and frequency analysis on the extruded foam sheet, the problems of skin bulging and core rupture during vacuum forming are solved, the vacuum forming properties are improved, and a method for predicting thermal shaping is provided.

CN118974150APending Publication Date: 2024-11-15MAXELL LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031185.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, during vacuum forming, the skin layer of the extruded foam sheet is prone to bulge out, the core layer is ruptured, and the appropriateness of thermal shaping is difficult to predict, and effective inspection methods are lacking.

Method used

By irradiating light under the extruded foam sheet, taking an image with the scale scale, performing edge detection and two-dimensional discrete Fourier transformation, determining the difference in brightness frequency distribution, and determining whether vacuum molding can be performed.

Benefits of technology

It is achieved to inhibit the peeling of the skin layer and the rupture of the core layer, improve the vacuum molding property, and provide a method to check the appropriateness of thermal shape in advance to ensure efficient molding of the extruded foam sheet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974150A_ABST
    Figure CN118974150A_ABST
Patent Text Reader

Abstract

The present invention provides an extruded foam sheet capable of obtaining excellent vacuum moldability, and a method and a device for inspecting the extruded foam sheet. In a state in which light is irradiated from below the extruded foam sheet (1), the extruded foam sheet (1) and the scale (10) are simultaneously imaged from above to obtain an image (21). And performing edge processing on the image (21) to obtain an image (22). An image (23) is obtained by subjecting an image (22) to a two-dimensional discrete Fourier transform. The image (23) represents a frequency distribution of brightness in the image (22). An image (24) is obtained by removing the scale (10) from the image (21). An image (25) is obtained by subjecting an image (24) to a two-dimensional discrete Fourier transform. When an image (23) is represented by a two-dimensional spectrum, a first peak (P1), a second peak (P2), and a third peak appearing according to a scale of 1 mm interval of a scale are extracted. When the image (25) is represented by a two-dimensional spectrum, the difference Delta between the brightness value at the position corresponding to the central peak (P0) and the brightness value at the position corresponding to the third peak (P3) is less than 25 when represented by 256 gray scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an extruded foam sheet including a polycarbonate resin, and an inspection method and an inspection device for the extruded foam sheet. Background Art

[0002] In recent years, foamed resins have attracted attention because they can improve convenience and reduce carbon dioxide emissions by making resin molded bodies lightweight. There are two methods for molding foamed resins: physical foaming molding and chemical foaming molding. The chemical foaming molding method uses a chemical foaming agent as a foaming agent. Chemical foaming agents have a high environmental load and are not preferred from the perspective of protecting the global environment. On the other hand, the physical foaming molding method uses physical foaming agents such as nitrogen and carbon dioxide as foaming agents. Physical foaming agents have a small environmental load, so they are preferred from the perspective of protecting the global environment. In the physical foaming molding method, as a method for foaming engineering plastics and super engineering plastics with high heat resistance, there is a method in which the molten resin of engineering plastics and super engineering plastics is shear-kneaded with a high-pressure supercritical fluid to dissolve them.

[0003] Japanese Patent Gazette No. 6139038 (Patent Document 1) discloses a method for manufacturing a foamed molded body using a physical foaming agent such as nitrogen or carbon dioxide at a relatively low pressure instead of a high-pressure supercritical fluid. According to this method, fine foaming cells can be formed in a resin molded body by a relatively simple process using a low-pressure physical foaming agent without using a special high-pressure device. In addition, Patent Document 1 discloses a method for molding a foamed molded body by injection molding and extrusion molding.

[0004] Injection molding can obtain a foaming molded body of complex shape. However, the surface layer of the molten resin flows while cooling and solidifying in the metal mold. At this time, a non-foamed epidermis is formed thinly on the surface layer of the foaming molded body. On the other hand, compared with the injection molding method, the extrusion molding method has fewer restrictions on the size and load of the metal mold, and is suitable for continuously making a foaming molded body of a single shape and a single thickness. In addition, the sheet-like foaming molded body obtained by the extrusion molding method can be shaped into a foaming molded body of a certain degree of complex shape or a foaming molded body of relatively large size by implementing vacuum forming, etc. However, when the molten resin is discharged from the die outlet and cooled and solidified, it is difficult to form an epidermis on the surface layer of the foaming molded body in the extrusion molding method.

[0005] In Patent Document 1, there is no research on the foamed molded body of polycarbonate resin composed of vacuum-formable non-crystalline resin, and there is no research on the rupture of the foamed molded body when heated at a temperature exceeding the glass transition temperature of the polycarbonate resin. Here, in the case of non-foamed resin, for crystalline resin, if heated at a temperature lower than the melting point, it is difficult to cause large deformation even at a temperature higher than the glass transition temperature. However, in the case of non-foamed resin, for non-crystalline resin, thermal deformation is easy to occur when heated at a temperature higher than the glass transition temperature (the glass transition temperature of polycarbonate resin is about 145°C). In view of this, when the foamed molded body containing non-crystalline resin (polycarbonate resin) is heated at a temperature above the glass transition temperature, it is more difficult to suppress its deformation and the rupture accompanying the deformation. It should be noted that the glass transition temperature refers to the secondary transition point observed by differential scanning calorimetry (DSC).

[0006] In addition, the foamed molded body consisting of foamed resin has the problem of mechanical strength reduction due to the low density for the purpose of improving lightness. In particular, the foamed molded body consisting of polycarbonate resin requiring mechanical strength has the problem of mechanical strength significantly reducing compared with the resin molded body consisting of non-foamed resin.

[0007] Japanese Patent Publication No. 8-174780 (Patent Document 2) discloses a polycarbonate extruded resin foam laminate sheet with a high foaming ratio manufactured by a co-extrusion molding method. The polycarbonate extruded resin foam laminate sheet has excellent heating processability, especially deep drawing processability, and is also excellent in appearance design and mechanical strength. Patent Document 2 discloses the heating dimensional change when the polycarbonate extruded resin foam laminate sheet is heated at a relatively low temperature of 170°C.

[0008] Japanese Patent Publication No. 2020-006588 (Patent Document 3) discloses a resin plate. The resin plate can be used as a decorative plate with excellent design by setting the bubbles contained in the resin plate to a predetermined structure, and even if the size of the end face that serves as the light introduction part is small, the light can be spread to a degree that an appropriate number of bubbles can be conspicuous in the light.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent No. 6139038

[0012] Patent Document 2: Japanese Patent Application Laid-Open No. 8-174780

[0013] Patent Document 3: Japanese Patent Application Publication No. 2020-006588 Summary of the invention

[0014] In recent years, when an extruded foam sheet is thermally formed into a desired shape by vacuum forming or the like, it is required to be able to be formed in a short time at a relatively high heating temperature of 200°C or above and from the drawdown (the phenomenon that the molten resin sags due to its own weight) from the viewpoint of improving productivity. However, if an extruded foam sheet having a core layer composed of a foamed resin and a skin layer composed of a non-foamed resin laminated on the main surface of the core layer is heated at a high temperature of 200°C or above, the bubbles in the core layer covered by the skin layer are easily thermally expanded and integrated. As a result, there are problems such as the skin layer bulging from the main surface of the extruded foam sheet and the core layer being broken, which cannot be properly vacuum formed.

[0015] Regarding the unevenness of bubbles contained in the polycarbonate resin laminated foamed resin sheet, Patent Document 2 does not propose a method for suppressing the skin layer from bulging out from the main surface of the extruded foamed sheet during vacuum molding and suppressing the occurrence of cracks in the core layer.

[0016] Patent Document 3 does not propose to improve the vacuum formability of the resin plate.

[0017] Furthermore, when heat-forming an extruded foam sheet into a desired shape, it is important to predict in advance whether heat-forming can be performed appropriately. Patent Documents 1 to 3 do not examine methods for checking whether heat-forming can be performed appropriately.

[0018] An object of the present disclosure is to provide an extruded foam sheet having excellent vacuum formability, and an inspection device and an inspection method for inspecting in advance whether the extruded foam sheet can be appropriately vacuum-formed.

[0019] In order to solve the above-mentioned problems, the present disclosure adopts the following solution. That is, the extruded foam sheet of the present disclosure may contain a polycarbonate resin. In a state where light is irradiated from below the extruded foam sheet, the extruded foam sheet and a scale with 1mm intervals are photographed from above at the same time to obtain a first image. The third image is obtained by performing a two-dimensional discrete Fourier transform on the second image obtained by edge detection processing of the first image, and the fifth image is obtained by performing a two-dimensional discrete Fourier transform on the fourth image obtained by removing the scale from the first image. In the third image and the fifth image, the third image represents the frequency distribution of brightness in the second image, and the fifth image represents the frequency distribution of brightness in the fourth image. When the brightness profile is obtained along the direction of the scale from the center of the third image and represented by a two-dimensional spectrum, the multiple frequency components that appear according to the 1mm interval scale of the ruler are set as the first peak, the second peak and the third peak in sequence from the center position of the third image. When the distance between the 1st peak and the center position of the third image is L, the frequency component with the highest brightness between the position at a distance of L / 5 and the position at a distance of L / 2 from the center position of the third image is set as the central peak. When the brightness profile is obtained linearly from the center of the fifth image toward a direction with higher brightness and expressed in a two-dimensional spectrum, the difference between the brightness at the position corresponding to the central peak and the brightness at the position corresponding to the 3rd peak can be less than 25 when expressed in 256 grayscales.

[0020] The inspection method of the extruded foam sheet disclosed in the present invention may include: a step of simultaneously photographing the extruded foam sheet and a scale with equally spaced graduations from above while irradiating light from below the extruded foam sheet containing a polycarbonate resin to obtain a first image; a step of obtaining a second image by edge processing the first image; a step of performing a two-dimensional discrete Fourier transform on the second image to obtain a third image representing the frequency distribution of brightness in the second image; a step of obtaining a fourth image by removing the scale from the first image; a step of performing a two-dimensional discrete Fourier transform on the fourth image to obtain a fifth image representing the frequency distribution of brightness in the fourth image; a step of measuring the difference in brightness between the third image and the fifth image based on the frequency distribution of brightness in the second image and the frequency distribution of brightness in the fourth image; and a step of determining that the extruded foam sheet can be vacuum formed when the difference in brightness is lower than a predetermined threshold value.

[0021] The inspection device of the extruded foam sheet disclosed in the present invention may include an image receiving unit and an image processing unit, the image receiving unit receiving a first image obtained by simultaneously photographing the extruded foam sheet and a scale having equal intervals from above in a state where light is irradiated from below the extruded foam sheet containing polycarbonate resin, and the image processing unit processing the first image received by the first image receiving unit. The image processing unit may include an edge processing unit for performing edge processing on the first image to obtain a second image, a first Fourier transform unit for performing two-dimensional discrete Fourier transform on the second image to obtain a third image representing a frequency distribution of brightness in the second image, a second Fourier transform unit for performing two-dimensional discrete Fourier transform on a fourth image obtained by removing the scale from the first image to obtain a fifth image representing a frequency distribution of brightness in the fourth image, a measuring unit for measuring the difference in brightness between the third image and the fifth image based on the frequency distribution of brightness in the second image and the frequency distribution of brightness in the fourth image, and a judging unit for judging that the extruded foam sheet can be vacuum-formed when the difference is below a predetermined threshold.

[0022] According to the present disclosure, it is possible to provide an extruded foam sheet having excellent vacuum formability, and an inspection device and an inspection method for inspecting in advance whether the extruded foam sheet can be appropriately vacuum-formed. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a perspective view showing an extruded foam sheet according to an embodiment of the present disclosure.

[0024] Figure 2 Yes means Figure 1 A photograph of a cross section of an extruded foam sheet is shown.

[0025] Figure 3 It means shooting Figure 1 The diagram shows the state of the extruded foam sheet.

[0026] Figure 4 It's shooting Figure 1 An image of an extruded foam sheet is shown.

[0027] Figure 5 This is a photo showing a scale.

[0028] Figure 6 Yes Figure 4 The image shown is an image after edge processing.

[0029] Figure 7 Yes Figure 6 The image shown is a two-dimensional discrete Fourier transformed image.

[0030] Figure 8 It is represented by a two-dimensional spectrum Figure 7 A graph of the image shown.

[0031] Fig. 9 is from Figure 4 The images shown have the ruler removed.

[0032] Fig.10 Yes Fig. 9 The image shown is a two-dimensional discrete Fourier transformed image.

[0033] Fig.11 It is represented by a two-dimensional spectrum Fig.10 A graph of the image shown.

[0034] Fig.12 yes Figure 1 A cross-sectional view of an extruded foam sheet is shown.

[0035] Fig.13 It is a perspective view showing an extruded foam sheet according to a modified example.

[0036] Fig.14 This is a flow chart showing a method for inspecting an extruded foam sheet.

[0037] Fig.15 This is a block diagram showing an inspection device for an extruded foam sheet.

[0038] Fig.16 It is a perspective view showing a metal mold for vacuum forming. DETAILED DESCRIPTION

[0039] The inventors of the present invention have conducted in-depth research and found that as long as the unevenness of a large number of bubbles contained in an extruded foam sheet is suppressed and the uneven brightness appearing in an image when the main surface of the extruded foam sheet is photographed satisfies a predetermined condition, it is possible to suppress the skin layer from peeling off from the core layer and bulging, and the core layer from rupturing during vacuum forming, that is, it is possible to obtain excellent vacuum formability. The present invention is completed based on such a finding.

[0040] The extruded foam sheet of the present embodiment may contain polycarbonate resin. In the state of irradiating light from the bottom of the extruded foam sheet, the extruded foam sheet and the scale with 1mm intervals are photographed from the top at the same time to obtain a first image. The third image is obtained by performing a two-dimensional discrete Fourier transform on the second image obtained by edge processing the first image, and the fifth image is obtained by performing a two-dimensional discrete Fourier transform on the fourth image obtained by removing the scale from the first image. In the third image and the fifth image, the third image represents the frequency distribution of brightness in the second image, and the fifth image represents the frequency distribution of brightness in the fourth image. When the brightness profile is obtained along the direction of the scale from the center of the third image and represented by a two-dimensional spectrogram, the multiple frequency components that appear according to the scale of 1mm intervals of the scale are set to the first peak, the second peak and the third peak in sequence from the center position of the third image. When the distance between the first peak and the center position of the third image is set to L, the frequency component with the highest brightness between the position at a distance of L / 5 from the center position of the third image and the position at a distance of L / 2 is set to the central peak. When the brightness profile is obtained linearly from the center of the fifth image toward a direction with higher brightness and represented by a two-dimensional spectrum, the difference between the brightness at the position corresponding to the central peak and the brightness at the position corresponding to the third peak can be less than 25 when represented by 256 gray levels.

[0041] Thereby, excellent vacuum formability can be obtained.

[0042] The extruded foam sheet may contain 50% by weight or more of a polycarbonate resin, thereby improving the strength.

[0043] The extruded foam sheet may have a thickness of 1 mm to 5 mm.

[0044] The extruded foam sheet may include a core layer formed of a foamed resin, a first skin layer formed of a non-foamed resin and laminated on one main surface of the core layer, and a second skin layer laminated on the other main surface of the core layer. At least one of the first skin layer and the second skin layer may be composed of a polycarbonate resin.

[0045] The extruded foam sheet may satisfy the following formula (1).

[0046] 0.10≤(t1+t2) / T≤0.5···(1)

[0047] In formula (1), t1 represents the thickness of the first skin layer, t2 represents the thickness of the second skin layer, and T represents the thickness of the extruded foam sheet. Thus, more excellent vacuum formability can be obtained.

[0048] The polycarbonate resin contained in any one of the first skin layer and the second skin layer may have a melt volume rate 1.0 to 5 times that of the polycarbonate resin contained in the core layer. This can provide even better vacuum formability.

[0049] The extruded foam sheet may have a length of 1000 mm or more in the extrusion direction and a length of 1000 mm or more in the width direction perpendicular to the extrusion direction when viewed from above. Even a relatively large extruded foam sheet can have excellent vacuum formability.

[0050] The difference in brightness can be 20 or less when expressed in 256 grayscales. This can provide more excellent vacuum formability.

[0051] The difference in brightness can be 15 or less when expressed in 256 grayscales. This can achieve even better vacuum formability.

[0052] The inspection method of the extruded foam sheet of the present embodiment may include: a step of simultaneously photographing the extruded foam sheet and a scale having equally spaced scales from above to obtain a first image while irradiating light from below the extruded foam sheet containing polycarbonate resin; a step of obtaining a second image of the first image subjected to edge processing; a step of performing a two-dimensional discrete Fourier transform on the second image to obtain a third image representing a frequency distribution of brightness in the second image; a step of obtaining a fourth image with the scale removed from the first image; a step of performing a two-dimensional discrete Fourier transform on the fourth image to obtain a fifth image representing a frequency distribution of brightness in the fourth image; a step of measuring the difference in brightness between the third image and the fifth image based on the frequency distribution of brightness in the second image and the frequency distribution of brightness in the fourth image; and a step of determining that the extruded foam sheet can be vacuum-formed when the difference in brightness is lower than a predetermined threshold value. Thus, before actually vacuum-forming the extruded foam sheet, it is possible to check in advance whether the extruded foam sheet can be properly vacuum-formed.

[0053] In the step of measuring the difference in brightness between the third image and the fifth image, when the brightness profile is obtained along the direction of the scale from the center of the third image and represented in a two-dimensional spectrum, a plurality of frequency components appearing according to the equally spaced scales of the scale are set as the first peak, the second peak and the third peak in sequence from the center position of the third image, when the distance between the first peak and the center position of the third image is set as L, the frequency component with the highest brightness between the position at a distance of L / 5 and the position at a distance of L / 2 from the center position of the third image is set as the central peak, and when the brightness profile is obtained linearly from the center of the fifth image in the direction of higher brightness and represented in a two-dimensional spectrum, the difference in brightness at the position corresponding to the central peak and the position corresponding to the third peak is measured. In the step of determining that the extruded foam sheet can be vacuum-formed, when the brightness difference is represented by 256 grayscales and is less than 25, it can be determined that the extruded foam sheet can be vacuum-formed. Thus, before actually vacuum-forming the extruded foam sheet, it is possible to check in advance whether the extruded foam sheet can be properly vacuum-formed.

[0054] The inspection device for an extruded foam sheet of the present embodiment may include an image receiving unit, which receives a first image obtained by simultaneously photographing an extruded foam sheet and a scale having equally spaced scales from above while irradiating light from below the extruded foam sheet containing a polycarbonate resin, and an image processing unit, which processes the first image received by the first image receiving unit. The image processing unit may include an edge processing unit for performing edge processing on the first image to obtain a second image, a first Fourier transform unit for performing two-dimensional discrete Fourier transform on the second image to obtain a third image representing a frequency distribution of brightness in the second image, a second Fourier transform unit for performing two-dimensional discrete Fourier transform on a fourth image obtained by removing the scale from the first image to obtain a fifth image representing a frequency distribution of brightness in the fourth image, a measuring unit for measuring the difference in brightness between the third image and the fifth image based on the frequency distribution of brightness in the second image and the frequency distribution of brightness in the fourth image, and a judging unit for judging that the extruded foam sheet can be vacuum-formed when the difference is below a predetermined threshold. Thereby, before actually vacuum-forming the extruded foam sheet, it is possible to check in advance whether the extruded foam sheet can be appropriately vacuum-formed.

[0055] The measuring unit may, when obtaining the brightness profile along the direction of the ruler from the center of the third image and representing it in a two-dimensional spectrum, set the multiple frequency components that appear according to the equally spaced scales of the ruler as the first peak, the second peak, and the third peak in sequence from the center position of the third image, and when the distance between the first peak and the center position of the third image is set to L, the frequency component with the highest brightness between the position at a distance of L / 5 and the position at a distance of L / 2 from the center position of the third image is set to the central peak. In this case, when obtaining the brightness profile linearly from the center of the fifth image in the direction of higher brightness and representing it in a two-dimensional spectrum, the difference between the brightness at the position corresponding to the central peak and the brightness at the position corresponding to the third peak is measured. The judging unit may judge that the extruded foam sheet can be vacuum-formed when the brightness difference is represented by 256 grayscales and is less than 25. Thus, before actually vacuum-forming the extruded foam sheet, it is possible to check in advance whether the extruded foam sheet can be properly vacuum-formed.

[0056] Below, use Figures 1 to 13 The embodiment of the extruded foam sheet 1 disclosed in the present invention is specifically described. It should be noted that the same reference numerals are used for the same and corresponding structures in the figures, and the same description is not repeated. It should be noted that in order to make the description easy to understand, the structure is simplified or schematically shown, or a part of the components is omitted in the drawings referred to below.

[0057] The extruded foam sheet 1 contains a polycarbonate resin. The extruded foam sheet 1 contains more than 50% by weight of a polycarbonate resin. The extruded foam sheet 1 has a sheet shape. The extruded foam sheet 1 is formed by extrusion foaming of a molten polycarbonate resin. As long as the resin used in the present disclosure contains a polycarbonate resin, other engineering plastics or super engineering plastics may also be used. Engineering plastics are thermoplastic resins having a deflection temperature under load of more than 100°C. In addition to polycarbonate resin (PC), engineering plastics include, for example, modified polyphenylene ether (m-PPE), syndiotactic polystyrene (SPS), etc. Super engineering plastics are thermoplastic resins having a deflection temperature under load of more than 150°C. Super engineering plastics include, for example, polyphenylene sulfide (PPS), polysulfone (PSF), polyethersulfone (PES), polyarylate (PAR), polyamide-imide (PAI), thermoplastic polyimide (PI), polyetherimide (PEI), liquid crystal polymer (LCP), etc. The thermoplastic resin used in the extruded foam sheet 1 of the present disclosure may include at least one selected from these engineering plastics and super engineering plastics. It should be noted that as the resin material of the present disclosure, any thermoplastic resin that can be extruded can be used. However, by using the above-mentioned engineering plastics and super engineering plastics, it is possible to achieve an increase in strength. In addition, ultraviolet absorbers and anti-aging agents may also be added to the resin material of the extruded foam sheet 1.

[0058] The extruded foam sheet 1 may contain a foaming aid during foam molding. The foaming aid is added to increase the number of bubbles contained in the extruded foam sheet 1 and to increase the melt tension of the molten resin during extrusion molding to achieve micronization of the bubbles. Examples of the foaming aid include a bubble generation nucleating agent.

[0059] like Figure 1 As shown, the extruded foam sheet 1 includes a core layer 2 , a skin layer 3 laminated on one main surface of the core layer 2 , and a skin layer 4 laminated on the other main surface of the core layer 2 .

[0060] The core layer 2 is made of a foamed resin. The core layer 2 can be formed by foaming a molten polycarbonate resin. That is, the core layer 2 has a plurality of bubbles 2a. Figure 2 As shown, a plurality of bubbles 2a are formed relatively evenly in a cross section cut in the thickness direction along a width direction orthogonal to the extrusion direction. That is, the plurality of bubbles of the extruded foam sheet 1 have small unevenness in the cross section in the width direction. It should be noted that the plurality of bubbles 2a, in a cross-sectional view cut in the thickness direction along the direction of the extrusion direction during extrusion molding, mostly have a roughly elliptical shape extending along the extrusion direction. Among the plurality of bubbles 2a contained in the core layer 2, the bubbles contained near the center in the thickness direction of the core layer 2 tend to have a larger bubble diameter than the bubbles 2a contained near the ends in the thickness direction of the core layer 2. The bubble diameters of the plurality of bubbles 2a tend to gradually decrease from the center in the thickness direction of the core layer 2 toward the ends in the thickness direction.

[0061] The skin layer 3 is made of a non-foamed resin. That is, the skin layer 3 is not foamed. The skin layer 3 is extruded from a die outlet in a non-foamed state by a co-extrusion molding method and is integrally laminated with the core layer 2 .

[0062] The skin layer 3 may be made of a thermoplastic resin that can be well bonded to the core layer 2. More specifically, the resin material of the skin layer 3 is preferably the same resin material as the core layer 2. In addition, in order to strengthen the skin layer 3, the skin layer 3 may be composed of a reinforcing resin containing an inorganic filler. By forming the skin layer 3 in this way, the extruded foam sheet 1 can achieve lightweight and improved strength while efficiently improving strength. Examples of inorganic fillers include glass fiber, carbon fiber, aramid fiber, talc, and mica.

[0063] The skin layer 4 is the same as the skin layer 3 except that it is laminated on the other main surface of the core layer 2. Therefore, the specific description of the skin layer 4 is omitted.

[0064] As described above, the core layer 2 has a plurality of bubbles 2a of uneven size in a cross-sectional view along the width direction. This can provide excellent vacuum formability.

[0065] The unevenness of multiple bubbles can be measured as follows. First, Figure 3 As shown in the figure, an extruded foam sheet 1 with a thickness of 3 mm is placed on the upper surface of the light box 100, and a light source with a brightness of 1400 cd / m 2 The main surface of the extruded foam sheet 1 is photographed from above the extruded foam sheet 1 using the camera 200. At this time, the extruded foam sheet 1 and the scale 10 (see FIG. 2 ) are photographed simultaneously. Figure 4 ). When photographing, the ruler 10 is arranged adjacent to the extruded foam sheet 1. At this time, no color correction is performed, and the image is photographed in full color at a specific resolution (2016×1512 pixels). In addition, the distance between the camera lens and the extruded foam sheet 1 is set to 20 cm, and the image is photographed in a manner that the optical axis of the camera lens intersects perpendicularly with the upper surface of the light box 100.

[0066] So, if Figure 4 As shown, since the transmittance varies according to the unevenness of multiple bubbles 2a, an image 21 showing uneven brightness can be obtained. The upper part of the illustrated image 21 shows the main surface of the extruded foam sheet 1, and the darker part shown in the lower part of the image 21 is the scale 10. Regarding the shooting range of the extruded foam sheet 1 in the image 21, the length in the width direction TD is 10 cm, and the length in the extrusion direction MD is 15.6 cm. The shooting range of the image 21 is preferably set in a manner such that the length in the width direction TD is 10 cm to 20 cm and the length in the extrusion direction MD is 15 cm to 25 cm, but as long as the vacuum formability of the extruded foam sheet 1 can be confirmed, it is not necessarily limited to this range. In addition, the resolution of the image 21 is set to be 300 dpi or more when stretched to actual size.

[0067] like Figure 5 As shown, the scale 10 is a 15 cm scale with scales at 1 mm intervals. The scales of the scale 10 are used for calibration of distances in an image. The selection criteria of the scale 10 will be described later.

[0068] Next, edge processing is performed on the image 21. Thus, Figure 6 As shown, image 22 can be obtained. As a result, each scale displayed by the ruler 10 becomes clear. That is, image 22 only needs to make the scale of the ruler 10 clear, and edge processing is performed in a manner such that the SN ratio described later is 2 or more. The edge processing of image 21 can be performed using image processing software such as "ImageJ1.53k".

[0069] Next, a two-dimensional discrete Fourier transform is performed on the image 22. The two-dimensional discrete Fourier transform of the image 22 can be performed using, for example, image processing software "ImageJ1.53k" or the like. Thus, the image 23 after the two-dimensional discrete Fourier transform can be obtained. Figure 7As shown, image 23 shows the frequency distribution of brightness in image 22. There is a slightly white component in the center of the vertical direction (the up and down direction in the figure) of image 23, which is displayed as a straight line at approximately equal intervals along the horizontal direction (the left and right direction in the figure). This is the frequency component of the 1 mm interval scale of the ruler 10.

[0070] The two-dimensional discrete Fourier transform can be expressed by the following equation.

[0071]

[0072] Where f(x,y) represents the image before the two-dimensional discrete Fourier transform, and F(u,v) represents the image after the two-dimensional discrete Fourier transform.

[0073] When displaying a two-dimensional discrete Fourier transformed image, the power spectrum is used. That is, the function represented by the following equation is displayed as a two-dimensional discrete Fourier transformed image.

[0074] |F(u,v| 2 =ReF(u,v) 2 +ImF(u,v) 2

[0075] like Figure 8 As shown in the graph, the horizontal contour at the center of the vertical direction of the image 23 is represented by a two-dimensional spectrum. The horizontal direction refers to the direction in which the scales of the ruler 10 in the image 22 are arranged, that is, the length direction of the ruler 10, or it can be said to be the direction along the ruler 10. It should be noted that when making the horizontal contour, 10 pixels are accumulated in the vertical direction orthogonal to the horizontal contour to make the contour. The vertical axis of the graph represents the brightness (Gray Value), and the horizontal axis of the graph represents the number of pixels in the horizontal direction of the image 23. It should be noted that the pixels on the horizontal axis represent 1000 pixels from the 508th pixel to the 1508th pixel in the image 23. The smaller the brightness unevenness of the image 22, the gentler the inclination of the resulting graph, and the greater the brightness unevenness of the image 22, the steeper the inclination of the graph. In addition, at this time, from the center of the horizontal axis C of the graph (the center of the image 23) toward the left and right directions, multiple frequency components appear on the outside according to the scales of the ruler 10 at intervals of 1 mm. As shown Figure 8As shown, these frequency components are defined as the primary peak P1, the secondary peak P2, and the tertiary peak P3 in sequence from the center position C of the image 23 toward the outside. In order to clearly determine the peak positions of these primary peaks P1, secondary peaks P2, and tertiary peaks P3, the scale 10 is selected in such a way that the SN ratio of the primary peak P1 is greater than 2, and the above-mentioned edge processing is performed. If a periodic pattern other than the scale is displayed on the scale 10 due to printing, etc., it is difficult to distinguish the peak position equivalent to 1mm intervals. Therefore, it is best to select a scale 10 that is as simple as possible and only displays scales at 1mm intervals. It should be noted that in the case where it is difficult to determine the peak position of the primary peak P1, a Gaussian distribution function can also be used to perform peak fitting to clearly determine the peak position of the primary peak P1.

[0076] Here, the highest peak that appears near the center position C (central value) of the horizontal axis (pixel) is removed from the analysis range as noise. More specifically, when the distance from the center position C of the horizontal axis (pixel) to the pixel position of the first-order peak P1 is set to L, the range from the center of the horizontal axis (the center position C of the image 22) to L / 5 is removed from the analysis range. And, the range outside the range from the pixel central value to L / 5 and to the pixel position of the third-order peak P3 is used as the analysis range. In addition, in the range from the above-mentioned L / 5 position to the L / 2 position, the position with the maximum brightness is defined as the central peak P0.

[0077] Next, the scale 10 is removed from the image 21. Thus, Fig. 9 As shown, image 24 can be obtained. The image 24 is subjected to a two-dimensional discrete Fourier transform using the same method as image 22. Thus, image 25 after a two-dimensional discrete Fourier transform can be obtained. Fig.10 As shown in FIG. 24 , image 25 represents the frequency distribution of brightness in image 24. In image 25, a line with relatively high brightness is observed in the vertical direction at the center of the image. Therefore, a straight line contour is made from the center of image 25 along the direction with relatively high brightness. That is, in image 25, as shown in FIG. Fig.11 As shown in the curve graph, the vertical profile at the center of the horizontal direction is represented by a two-dimensional spectrum. The smaller the brightness unevenness of the image 24, the gentler the slope of the obtained curve graph, and the larger the brightness unevenness of the image 24, the steeper the slope of the curve graph. It should be noted that, as mentioned above, Figure 8 In the graph of , the horizontal axis represents 1000 pixels from the 508th pixel to the 1508th pixel of the image 23. Therefore, Fig.11 The 1008th pixel on the horizontal axis of the graph is equivalent to Figure 8 The 500th pixel on the horizontal axis of the curve graph ranging from 0 to 100.

[0078] When the image 25 is represented by a two-dimensional spectrogram, as Fig.11As shown, when represented by 256 gray levels, the difference Δ between the brightness value at the position (pixel) corresponding to the above-mentioned central peak P0 and the brightness value at the position (pixel) corresponding to the above-mentioned tertiary peak P3 is less than 25. The brightness difference Δ is preferably less than 20, and more preferably less than 15. As a result, the unevenness of bubbles in the cross section along the width direction of the extruded foam sheet 1 can be reduced, and the skin layer 3 or the skin layer 4 can be prevented from peeling off from the core layer 2 and bulging, and cracking in the core layer 2 during vacuum forming, so that excellent vacuum formability can be obtained. It should be noted that the brightness value at the position corresponding to the central peak P0 and the brightness value at the position corresponding to the tertiary peak P3 are set to the average brightness of 20 pixels before and after each peak position. It should be noted that, in general, when the thickness of the extruded foam sheet 1 becomes smaller, the vacuum formability is reduced even if the foaming state of the core layer 2 is the same. That is, it is considered that even if the thickness of the extruded foam sheet 1 changes, if the brightness is 1400cd / m 2 When the light is irradiated, the difference Δ between the brightness value at the position corresponding to the central peak P0 and the brightness value at the position corresponding to the tertiary peak P3 is detected to be the same. Fig.11 In the curve graph, the difference Δ between the brightness value of the position corresponding to the central peak P0 on the left side from the center position C of the image 25 and the brightness value of the position corresponding to the third peak P3 is measured, but the difference Δ between the brightness value of the position corresponding to the central peak P0 on the right side and the brightness value of the position corresponding to the third peak P3 can also be measured in the same way, as long as the brightness difference Δ on at least either side is less than 25.

[0079] The extruded foam sheet 1 is formed into various shapes by vacuum forming. In vacuum forming, after the extruded foam sheet 1 is heated to about 200°C or more and begins to drape, it is covered on a metal mold or the like and vacuum-sucked, thereby being formed. If the extruded foam sheet 1 is to be formed into a more complex shape, or if a relatively large extruded foam sheet 1 having a length of more than 1000 mm in the extrusion direction and a length of more than 1000 mm in the width direction is to be formed, there is a tendency for the heating temperature during vacuum forming to be as high as 200° or more. According to the extruded foam sheet 1, by making the difference Δ between the brightness value at the position corresponding to the central peak P0 and the brightness value at the position corresponding to the tertiary peak P3 less than 25, even if the heating temperature during vacuum forming becomes high, it is possible to prevent the epidermis 3 or the epidermis 4 from peeling off from the core layer 2 and bulging, and causing ruptures in the core layer 2.

[0080] It should be noted that when the epidermis layer 3 and the epidermis layer 4 are colored, or when a decorative sheet is attached to the surface of the epidermis layer 3 and the epidermis layer 4, the above-mentioned accurate brightness unevenness cannot be measured. Therefore, for example, the epidermis layer 3 and the epidermis layer 4 or the decorative sheet are ground using a desktop grinding device (such as EJ200 IN manufactured by Engis Co., Ltd., Japan) to remove them from the extruded foam sheet 1, and the extruded foam sheet 1 is dried after ultrasonic cleaning, and then the brightness unevenness is measured. It should be noted that as long as the epidermis layer 3 and the epidermis layer 4 or the decorative sheet can be removed from the extruded foam sheet 1, the method is not particularly limited. In addition, if a light source that irradiates light vertically to the extruded foam sheet 1 and a camera located on the opposite side of the light source relative to the extruded foam sheet 1 are configured on the production line of the extruded foam sheet 1, the extruded foam sheet 1 can be inspected online.

[0081] In addition, as described above, in order to obtain the brightness unevenness of the extruded foam sheet 1 by photographing, the total light transmittance of the extruded foam sheet 1 is preferably 10% to 60%. The total light transmittance is a value measured by ASTM D1003 (Method A).

[0082] Next, the thickness of the extruded foam sheet 1 and the thickness of each layer of the skin layer 3 and the skin layer 4 will be described. Fig.12 As shown, the extruded foam sheet 1 has a thickness T of 1 to 5 mm. The skin layer 3 has a thickness t1. The skin layer 4 has a thickness t2.

[0083] The thickness t1 of the epidermis layer 3 and the thickness t2 of the epidermis layer 4 are measured as follows. A cross section of the extruded foam sheet 1 cut in the thickness direction along the width direction is observed using a microscope. In the present disclosure, the microscope used is KEYENCE model VHX-60000. The magnification of the microscope can be a magnification of the bubble diameter at the interface between the epidermis layer 3 and the core layer 2 of the extruded foam sheet 1. In the cross-sectional view of the extruded foam sheet 1, among the bubbles present in large quantities, 15 bubbles close to the surface of the extruded foam sheet 1 on each imaginary boundary line when the cross section of the extruded foam sheet 1 is divided into 16 equal parts in the width direction are selected, and the bubbles closest to the surface of the extruded foam sheet 1 are confirmed. Draw an imaginary line passing through the upper end of the nearest bubble and orthogonal to the thickness direction. The inner side in the thickness direction compared to the imaginary line is taken as the core layer 2, and the outer side in the thickness direction is taken as the epidermis layer 3. The boundary between the core layer 2 and the epidermis layer 4 is also defined in the same way, and the thickness t1 of the epidermis layer 3 and the thickness t2 of the epidermis layer 4 are measured. In order to make the thickness T of the extruded foam sheet 1 as uniform as possible during coextrusion molding, the thickness t1 of the skin layer 3 and the thickness t2 of the skin layer 4 are each preferably 0.050 mm or more.

[0084] The thickness of the entire skin layer obtained by adding the thickness t1 of the skin layer 3 and the thickness t2 of the skin layer 4 is preferably 0.10 to 0.5 with respect to the thickness T of the extruded foam sheet 1. That is, the extruded foam sheet 1 satisfies the following formula (1).

[0085] 0.10≤(t1+t2) / T≤0.5···(1)

[0086] When the thickness (t1+t2) of the entire epidermis layer is less than 0.10 relative to the thickness T of the extruded foam sheet 1, it is difficult to obtain the reinforcing effect of the non-foamed resin of the epidermis layer on the mechanical strength, and the mechanical strength such as the specific bending modulus is reduced. On the other hand, when the thickness (t1+t2) of the entire epidermis layer is greater than 0.5 relative to the thickness T of the extruded foam sheet 1, the density of the extruded foam sheet 1 becomes larger. As a result, the lightness brought about by foaming is impaired for the extruded foam sheet 1. The ratio of the thickness (t1+t2) of the entire epidermis layer to the thickness T of the extruded foam sheet 1 is preferably in the range of 0.15 to 0.45, and more preferably in the range of 0.2 to 0.4. By making the ratio of the thickness (t1+t2) of the entire epidermis layer to the thickness T of the extruded foam sheet 1 within this range, the specific bending modulus can be improved while achieving the lightweight brought about by the reduction in density. In addition, by making the ratio of the overall thickness of the epidermis layer (t1+t2) to the thickness T of the extruded foam sheet 1 in the range of 0.2 to 0.4, it is possible to improve the secondary processing properties such as vacuum forming while ensuring the thickness of the core layer 2 that makes the bubbles uneven. It should be noted that the specific bending modulus refers to the value obtained by dividing the bending modulus of the extruded foam sheet 1 by the density of the extruded foam sheet 1. That is, it can be said that the larger the specific bending modulus, the better the lightness and mechanical strength. The bending modulus is measured by a three-point bending test (according to ISO178 or JIS7171). At this time, the bending modulus is measured in the atmosphere. The test speed is 10 mm / min.

[0087] In this way, by controlling the density of the extruded foam sheet 1 and the thickness (t1+t2) of the skin layer 3 and the skin layer 4 relative to the thickness T of the extruded foam sheet 1, the expansion and rupture of the surface caused by thermal shaping such as vacuum forming can be suppressed, and excellent mechanical strength can be obtained.

[0088] The melt volume rate (hereinafter referred to as MVR) of the polycarbonate resin contained in the skin layer 3 is the same as or higher than the MVR of the polycarbonate resin contained in the core layer 2. The MVR of the polycarbonate resin contained in the skin layer 3 is 1.0 to 5 times, preferably 1.5 to 3 times, of the MVR of the polycarbonate resin contained in the core layer 2.

[0089] By making the MVR of the resin contained in the skin layer 3 the same as the MVR of the resin contained in the core layer 2 or higher than the MVR of the resin contained in the core layer 2, the temperature of the resin forming the skin layer 3 can be reduced as much as possible immediately after being discharged from the die outlet during extrusion molding. As a result, the viscosity of the skin layer 3 immediately after being discharged from the die outlet can be reduced, so that bulging or cracking of the surface of the skin layer 3 caused by foaming of the resin contained in the core layer 2 can be suppressed. That is, if the ratio of the MVR of the resin contained in the skin layer 3 is less than 1.0 times, it is difficult to reduce the resin temperature, and therefore it is difficult to suppress bulging or cracking of the surface of the skin layer 3. In addition, if the ratio of the MVR of the resin contained in the skin layer 3 is 1.5 times or more, it is easier to suppress bulging or expansion of the surface of the skin layer 3 during extrusion molding, and the preheating time during vacuum molding can be shortened to improve productivity. On the other hand, when the ratio of the MVR in the resin contained in the skin layer 3 is greater than 5 times, if the resin forming the skin layer 3 is to be properly flowed in the mold during extrusion molding, the MVR of the resin forming the core layer 2 needs to be extremely reduced. In addition, if the ratio of the MVR of the resin contained in the skin layer 3 is 3 times or less, the surface area of ​​the extruded foam sheet 1 with excellent appearance design increases. Therefore, the uneven bubbles are easily uniform, and the secondary processing properties of the extruded foam sheet 1 such as vacuum molding can be improved. Therefore, if it is considered to ensure the appropriate fluidity of the core layer 2 and the resin forming the skin layer 3 during extrusion molding, and to control the viscosity to suppress bulging or cracking of the surface of the skin layer 3, the MVR of the polycarbonate resin contained in the skin layer 3 can be 1.0 times to 5 times, preferably 1.5 times to 3 times, relative to the MVR of the polycarbonate resin contained in the core layer 2. This is also the same in the skin layer 4 and the core layer 2.

[0090] It should be noted that the MVR of the resin contained in the skin layer 3 and the core layer 2 is measured by a plastic flow characteristic test (according to JIS K7199, ISO 11443) using a capillary rheometer and a slit rheometer. In the present disclosure, the capillary die length is set to 5 mm, the inner diameter is set to 1 mm, and the measurement temperature is set to 300° C. for measurement.

[0091] It should be noted that the core layer 2 of the present disclosure is preferably foamed using a physical foaming agent such as nitrogen or carbon dioxide with a relatively low pressure as disclosed in the above-mentioned patent document 1, wherein nitrogen is more preferred. As a result, the pressure of the physical foaming agent can be set to a relatively low 1 to 6 MPa, and a plurality of fine bubbles can be formed. As a result, the design of the extruded foam sheet 1 can be improved, and bulging during high temperature and heating during vacuum forming can be more reliably suppressed. The average bubble diameter of the bubbles can be greater than 0.1 mm, can be less than 1.0 mm, and is preferably less than 0.3 mm.

[0092] The extruded foam sheet 1 may contain a plurality of flaky fillers. The flaky fillers are, for example, inorganic fillers such as talc, calcium carbonate, mica, clay, boron nitride, wollastonite, potassium titanate, and glass flakes. The flaky fillers may be subjected to surface treatments such as silane coupling agents, titanate coupling agents, phosphate coupling agents, and fatty acid coupling agents. The flaky fillers have an aspect ratio of more than 5. The aspect ratio is calculated by dividing the average particle size of the flaky filler by the average thickness (average particle size / average thickness). When the aspect ratio of the flaky filler is too small, it is difficult to exert excellent surface smoothness. Therefore, the aspect ratio of the flaky filler is preferably more than 10, more preferably more than 30. However, if the aspect ratio is too large, it is not easy to control the flow rate of the mixed molten resin inside the mold in the manufacturing process described later, and the surface smoothness may deteriorate. In addition, the viscosity of the mixed molten resin during extrusion molding increases, and thermal degradation of the thermoplastic resin may occur due to the heat generated in the extrusion molding device described later. Therefore, the aspect ratio of the flaky filler is preferably less than 50. The specific surface area of ​​the flaky filler is preferably 5 to 20 m 2 When the specific surface area of ​​the flaky filler is too small, the flaky filler slides on the surface and thus has difficulty in exhibiting surface smoothness. When the specific surface area is too large, the resistance of the flaky filler in the molten resin increases, resulting in difficulty in properly orienting the flaky filler.

[0093] The core layer 2 may contain a flaky filler oriented approximately parallel to the boundary surface between the core layer 2 and the skin layer 3 in the vicinity of the boundary with the skin layer 3. The vicinity is an area in the thickness direction of the core layer 2, which is located in the range of 5% of the thickness of the core layer from the boundary surface between the core layer 2 and the skin layer 3. In addition, the bubbles contained in the core layer 2 are in a shape extending along the extrusion direction during extrusion molding. The flaky filler is also oriented approximately parallel to the bubble wall of the bubble extending in the stretching direction, so that the strength of the bubble wall can be improved. As a result, the rupture of the extruded foam sheet 1 along the extrusion direction can be suppressed. It should be noted that the flaky filler is approximately parallel means that in the cross section where the extruded foam sheet 1 is cut in the thickness direction along the extrusion direction during extrusion molding, the flaky filler has an inclination angle of 0° or more and less than 5° relative to the boundary surface between the core layer 2 and the skin layer 3. In other words, it refers to the state in which the surface (main surface) of the flaky filler is relative to the boundary surface between the core layer 2 and the skin layer 3 in an approximately parallel manner. The same applies to the flaky filler oriented in the core layer 2 near the boundary between the core layer 2 and the skin layer 4 .

[0094] The orientation state of the multiple flaky fillers contained in the region near the boundary between the core layer 2 and the epidermis layer 3 is calculated as follows. First, in a cross section in the thickness direction along the extrusion direction during extrusion molding, 50 150×150 μm electron microscope photographs are taken at equal intervals from the front end to the rear end of the extrusion direction of the nearby region and in the center of the thickness direction. Among all the flaky fillers contained in these 50 electron microscope photographs, flaky fillers oriented approximately parallel to the boundary surface between the core layer 2 and the epidermis layer 3 are confirmed. Thus, the proportion of flaky fillers oriented approximately parallel to the multiple flaky fillers contained in the nearby region is calculated.

[0095] The core layer 2 may contain a flaky filler oriented at an angle of 5° to 90° relative to the surface of the extruded foam sheet 1 in the central region in the thickness direction of the core layer 2. The central region refers to a region with a thickness of 25% from the center in the thickness direction toward the boundary surface between the core layer 2 and the skin layer 3 when the thickness of the core layer 2 is set to 100%. Preferably, more than 40% of the flaky fillers contained in the central region are oriented at an angle of 5° to 90° relative to the surface S of the extruded foam sheet 1. Thus, the moldability of the extruded foam sheet 1 can be improved. More preferably, more than 60%, and further preferably more than 80% of the flaky fillers are oriented at an angle of 5° to 90° relative to the surface. Thus, the moldability of the extruded foam sheet 1 can be further improved. The bubbles contained in the central region of the core layer 2 tend to become larger than the above-mentioned nearby regions during extrusion molding. This is because the central region is difficult to cool after extrusion compared to the nearby regions. If the bubbles are too large, it becomes the main cause of the breakage of the extruded foam sheet 1. As described above, by randomly arranging the flaky filler between the bubbles in an inclined state in the central region, the growth of the bubbles in all directions can be suppressed. Thus, the strength of the extruded foam sheet 1 or the strength during molding, that is, the moldability, can be improved. As a result, when the extruded foam sheet 1 is vacuum-formed into a material to produce a foamed resin molded product, the bubbles contained in the extruded foam sheet 1 can be suppressed from breaking or the extruded foam sheet 1 can be damaged.

[0096] The orientation state of the multiple flaky fillers contained in the central area of ​​the core layer 2 can be calculated as follows. First, 50 microscope photographs are taken at equal intervals at the center of the thickness direction of the core layer 2, as in the case of the nearby area. Among all the flaky fillers contained in these 50 electron microscope photographs, flaky fillers that are oriented at an angle of 5° to 90° relative to the surface of the extruded foam sheet 1 are confirmed. Thus, the proportion of flaky fillers that are oriented at an angle of 5° to 90° relative to the surface of the extruded foam sheet 1 among the multiple flaky fillers contained in the central area is calculated.

[0097] Next, the manufacturing method of the extruded foam sheet 1 is described (not shown). First, resin particles as a resin material are added to the screw cylinder of the main extruder. The resin material is a polycarbonate resin. The resin particles are heated in the screw cylinder to generate a molten resin. Next, a foaming agent is injected into the molten resin from a foaming agent injection bottle installed in the screw cylinder of the main extruder. The foaming agent is dissolved in the molten resin by the above-mentioned screw cylinder, kneaded and evenly dispersed. In this way, a mixed molten resin is generated. The mixed molten resin is discharged from the die outlet to form a core layer 2. At the same time, resin particles as a resin material are respectively added to the screw cylinders of the two auxiliary extruders, heated and melted, thereby generating two molten resins. One of the two molten resins is discharged from the die outlet to form a skin layer 3, and the other is discharged from the die outlet to form a skin layer 4. The mixed molten resin and the two molten resins are merged from their respective extruders in a die, and are discharged from the die outlet in a manner such that the skin layer 3 is stacked on one side of the main surface of the core layer 2 and the skin layer 4 is stacked on the other side of the main surface of the core layer 2. The mixed molten resin foams when it is extruded from the die outlet into the atmosphere. In this way, an extruded foam sheet 1 is manufactured. It should be noted that the foaming method is a physical foaming method using an inert gas such as nitrogen and carbon dioxide as a foaming agent. The extruded foam sheet 1 extruded in this way is transported to a cutting machine by a puller. The cutting machine cuts the extruded foam sheet 1 into a desired shape.

[0098] The extruded foam sheet 1 manufactured in this way can be formed into a desired shape by vacuum forming or the like and used for the following purposes. For example, wide products and parts such as mobile materials such as billboards or automobile exterior materials that require strength, products and parts such as trays for heat-generating components used in the manufacturing process of batteries or accompanying heating processes that require heat resistance, or products and parts that require lightweight, etc. The extruded foam sheet 1 contains polycarbonate resin, which is suitable as a material for molding these products and parts by foaming by co-extrusion molding.

[0099] Products and parts made from the extruded foam sheet 1 can reduce the amount of resin used. As a result, the extruded foam sheet 1 of the present embodiment can contribute to the improvement of resource utilization efficiency, the reduction of transportation burden, the reduction of energy usage and the reduction of CO2 emissions. By providing the extruded foam sheet 1 to society, it can contribute to the realization of Goal 7 (affordable clean energy for all), Goal 9 (creating a foundation for industrial and technological innovation), Goal 11 (building sustainable cities), Goal 12 (responsible consumption and production) and Goal 13 (taking specific measures to address climate change) among the 17 goals of the Sustainable Development Goals (SDGs) formulated by the United Nations.

[0100] (Variation Example)

[0101] In the above embodiment, the skin layer 3 is formed on one main surface of the core layer 2, and the skin layer 4 is formed on the other main surface, but the extruded foam sheet 1 may also be provided with the skin layer 3 only on one main surface of the core layer 2. Fig.13 As shown, the extruded foam sheet 1 may not be provided with the epidermal layer 3 and the epidermal layer 4, but may be composed of a single layer of the core layer 2. That is, the extruded foam sheet 1 may be an extruded foam sheet 1 formed of a foaming resin. It should be noted that, as described above, when the heating temperature during vacuum forming is made high, the extruded foam sheet 1 preferably has the epidermal layer 3 and the epidermal layer 4.

[0102] Next, use Fig.14 The inspection method of the extruded foam sheet 1 of the present disclosure will be described in detail. The methods of obtaining the images 21 to 25 and measuring the brightness difference Δ are as described above, and therefore detailed descriptions thereof will be omitted.

[0103] (Step S1)

[0104] First, the extruded foam sheet 1 is placed on the upper surface of the light box 100, and the main surface of the extruded foam sheet 1 is photographed from above the extruded foam sheet 1 using the camera 200 together with the scale 10. Thus, an image 21 is obtained. At this time, the scale of the scale 10 is not limited to 1 mm intervals, and can be set at equal intervals.

[0105] (Step S2)

[0106] Next, edge processing is performed on the image 21 to obtain an image 22 .

[0107] (Step S3)

[0108] Next, a two-dimensional discrete Fourier transform is performed on the image 22 to obtain an image 23 indicating the frequency distribution of brightness in the image 22 .

[0109] (Step S4)

[0110] On the other hand, the scale 10 is removed from the image 21 to obtain the image 24 .

[0111] (Step S5)

[0112] Next, a two-dimensional discrete Fourier transform is performed on the image 24 to obtain an image 25 indicating the frequency distribution of brightness in the image 24 .

[0113] (Step S6)

[0114] Then, based on the frequency distribution of brightness in the image 22 and the frequency distribution of brightness in the image 24 , the difference Δ between the brightness of the image 23 and the image 25 is measured.

[0115] (Step S7)

[0116] Finally, it is determined whether the brightness difference Δ is lower than a predetermined threshold value. If the brightness difference Δ is lower than the predetermined threshold value, it is determined that the extruded foam sheet 1 can be properly vacuum-formed, and if it is higher than the predetermined threshold value, it is determined that the extruded foam sheet 1 cannot be properly vacuum-formed.

[0117] More specifically, as described above, the above step S6 is as follows: Figure 8 As shown in the curve graph, the horizontal profile at the center of the vertical direction of the image 23 is represented by a two-dimensional spectrum. From the horizontal axis center C of the curve graph (the center of the image 23) toward the left and right directions, multiple frequency components appear on the outside according to the scale of the ruler 10 at equal intervals (for example, 1mm intervals). Figure 8 As shown, these frequency components are set as the first peak P1, the second peak P2 and the third peak P3 in order from the center position C of the image 23 toward the outside. When the distance from the center position C of the horizontal axis (pixel) to the pixel position of the first peak P1 is set to L, the range from the center of the horizontal axis (the center position C of the image 22) to L / 5 is removed from the analysis range. And, the outside of the range from the central value of the pixel to L / 5 and the range to the pixel position of the third peak P3 are used as the analysis range. In addition, in the range from the above-mentioned L / 5 position to the L / 2 position, the position with the maximum brightness is set as the central peak P0. Furthermore, as Fig.11 As shown in the curve graph of , the vertical profile at the center of the horizontal direction of the image 25 is represented by the two-dimensional spectrum. Then, when the image 25 is represented by the two-dimensional spectrum, as shown in Fig.11 As shown, the difference Δ between the brightness value at the position (pixel) corresponding to the above-mentioned central peak P0 and the brightness value at the position (pixel) corresponding to the above-mentioned tertiary peak P3 is measured.

[0118] In the above step S7, more specifically, when the brightness difference Δ is expressed by 256 grayscales, the predetermined threshold value of the brightness difference Δ can be set to 25. That is, when the brightness difference Δ is less than 25, it is determined that the skin layer 3 or the skin layer 4 can be prevented from peeling off from the core layer 2 and bulging, and cracks can be generated in the core layer 2 during vacuum forming, and the extruded foam sheet 1 can be properly vacuum formed. On the other hand, when the brightness difference Δ is greater than 25, it is determined that the extruded foam sheet 1 cannot be properly vacuum formed.

[0119] In this way, according to the inspection method of the extruded foam sheet 1, it is possible to check in advance whether the extruded foam sheet 1 can be properly vacuum-formed without actually performing vacuum forming. It should be noted that, as described above, the threshold value of the brightness difference Δ is preferably 20, and more preferably 15. That is, when the brightness difference Δ is 20 or less or 15 or less, it can be determined that the extruded foam sheet 1 can be more properly vacuum-formed.

[0120] Next, use Fig.15 The inspection device 1000 of the extruded foam sheet 1 disclosed in the present invention is specifically described. The inspection device 1000 includes an image receiving unit 1010 and an image processing unit 1020. It should be noted that, as described above, the camera 200 in the figure photographs the main surface of the extruded foam sheet 1 together with the ruler 10 from above the extruded foam sheet 1 placed on the upper surface of the light box 100. The camera 200 has an image sending unit (not shown). The image sending unit sends the image 21 obtained by photographing the extruded foam sheet 1 and the ruler 10 to the inspection device 1000. It should be noted that the scale of the ruler 10 is not limited to 1 mm intervals, and can be set at equal intervals.

[0121] The image receiving unit 1010 receives the image 21 transmitted from the image transmitting unit. It should be noted that the camera 200 and the inspection device 1000 are not particularly limited as long as they can be connected via the Internet line or other wireless lines or wired lines and can transmit and receive the image 21.

[0122] The image processing unit 1020 processes the image 21 received by the image receiving unit 1010 so as to check whether the extruded foam sheet 1 can be properly vacuum-formed. The image processing unit 1020 includes an edge processing unit 1021, a first Fourier transform unit 1022, a second Fourier transform unit 1023, a measuring unit 1024, and a determining unit 1025. It should be noted that the acquisition of the images 21 to 25 and the measurement method of the brightness difference Δ in the image processing are as described above, so the detailed description is omitted.

[0123] As described above, the edge processing unit 1021 performs edge processing on the image 21. Thus, the image 22 after the edge processing can be obtained.

[0124] The first Fourier transform unit 1022 performs a two-dimensional discrete Fourier transform on the image 22 after the edge processing. Thus, an image 23 representing the frequency distribution of the brightness of the image 22 can be obtained.

[0125] The second Fourier transform unit 1023 performs a two-dimensional discrete Fourier transform on the image 24 obtained by removing the scale 10 from the image 21. Thus, an image 25 representing the frequency distribution of the brightness of the image 24 can be obtained. It should be noted that the image 24 can be obtained by manually removing the scale 10 from the image 21, or by having the inspection device 1000 detect the scale 10 in the image 21 and automatically removing the scale 10 from the image 21. The image 24 is input to the second Fourier transform unit 1023 and is subjected to a two-dimensional discrete Fourier transform.

[0126] The measuring unit 1024 measures the difference Δ between the brightness of the image 23 and the image 25 based on the frequency distribution of the brightness in the image 22 and the frequency distribution of the brightness in the image 24. More specifically, as described above, Figure 8 As shown in the curve graph, the horizontal profile at the center of the vertical direction of the image 23 is represented by a two-dimensional spectrum. From the horizontal axis center C of the curve graph (the center of the image 23) toward the left and right directions, multiple frequency components appear on the outside according to the scale of the ruler 10 at equal intervals (for example, 1mm intervals). Figure 8 As shown, these frequency components are sequentially set as the first peak P1, the second peak P2, and the third peak P3 from the center position C of the image 23 toward the outside. When the distance from the center position C of the horizontal axis (pixel) to the pixel position of the first peak P1 is set to L, the range from the center of the horizontal axis (the center position C of the image 22) to L / 5 is removed from the analysis range. And, the outside of the range from the central value of the pixel to L / 5 and the range to the pixel position of the third peak P3 are set as the analysis range. In addition, in the range from the above-mentioned L / 5 position to the L / 2 position, the position with the maximum brightness is set as the central peak P0. Furthermore, as Fig.11 As shown in the curve graph of , the vertical profile at the center of the horizontal direction of the image 25 is represented by the two-dimensional spectrum. Then, when the image 25 is represented by the two-dimensional spectrum, as shown in Fig.11 As shown, the difference Δ between the brightness value at the position (pixel) corresponding to the above-mentioned central peak P0 and the brightness value at the position (pixel) corresponding to the above-mentioned tertiary peak P3 is measured.

[0127] The determination unit 1025 determines whether the brightness difference Δ is lower than a predetermined threshold value. When the brightness difference Δ is lower than a predetermined threshold value, it is determined that the extruded foam sheet 1 can be properly vacuum-formed, and when it is above a predetermined threshold value, it is determined that the extruded foam sheet 1 cannot be properly vacuum-formed. More specifically, when the brightness difference Δ is represented by 256 grayscales, the predetermined threshold value of the brightness difference Δ can be set to 25. That is, when the brightness difference Δ is less than 25, it is determined that the skin layer 3 or the skin layer 4 can be prevented from peeling off from the core layer 2 and bulging, and cracks can be generated in the core layer 2 during vacuum forming, and the extruded foam sheet 1 can be properly vacuum-formed. On the other hand, when the brightness difference Δ is greater than 25, it is determined that the extruded foam sheet 1 cannot be properly vacuum-formed. It should be noted that, as described above, the threshold value of the brightness difference Δ is preferably 20, and more preferably 15. That is, when the brightness difference Δ is less than 20 or less than 15, it can be determined that the extruded foam sheet 1 can be more properly vacuum-formed.

[0128] As described above, according to the inspection device 1000 for the extruded foam sheet 1, it is possible to inspect in advance whether the extruded foam sheet 1 can be appropriately vacuum-formed without actually performing vacuum-forming.

[0129] It should be noted that the inspection device 1000 can include a shooting instruction unit (not shown) for instructing the camera 200 to shoot. For example, on the production line of the extruded foam sheet 1, the above-mentioned camera 200 and the inspection device 1000 are set in the process after the extruded foam sheet 1 is produced. The extruded foam sheet 1 conveyed on the production line can also be detected by a sensor, and when the inspection device 1000 receives the detection information sent by the sensor, the shooting instruction unit gives the camera 200 a shooting instruction. The camera 200 shoots the extruded foam sheet 1 conveyed from above, and the extruded foam sheet 1 can be inspected by the above-mentioned functions. In this way, the extruded foam sheet 1 can be inspected on the production line.

[0130] The inspection device 1000 is composed of a computer. The computer has a processor and a memory. The above-mentioned functions can be realized by the processor executing processing according to the program recorded in the memory. A program for making the computer function as the inspection device 1000 or a non-transitory recording medium recording the program may also be included in the present disclosure. It should be noted that the inspection device 1000 may also be composed of two or more computers or one or more applications installed on the computer.

[0131] As mentioned above, although embodiment was described, this disclosure is not limited to the said embodiment, Various changes are possible as long as they do not deviate from the summary.

[0132] (Example)

[0133] As shown in Table 1 below, samples (sheets) of Examples 1 to 9 and Comparative Examples 1 to 5 were prepared. The resin materials used for these samples are polycarbonate resins, specifically, as shown in Table 1, polycarbonate resins "L1225Y", "L1220Y", "L1225Z", "K-1300Y" manufactured by Teijin Limited, or "T2854" which is a mixed resin of polycarbonate resin and ABS, and polycarbonate resins "S-2000" or "S-3000" manufactured by Mitsubishi Engineering-Plastics Corporation. It should be noted that "L11225Z" means polycarbonate resin "L1225 Z100" manufactured by Teijin Limited. The foaming aid shown in Table 1 uses "METABLEN (registered trademark) A-3800" manufactured by Mitsubishi Chemical Corporation. It should be noted that the present disclosure is not limited to these embodiments.

[0134] [Table 1]

[0135]

[0136] (Measurement method of uneven bubbles)

[0137] Based on the above-mentioned method for measuring the unevenness of bubbles, each sample was placed on the upper surface of a light box "NEW5000" manufactured by Fujifilm Corporation and illuminated at a brightness of 1400 cd / m 2 Take pictures. At this time, no color correction is performed, and the main surface of each sample is photographed with a resolution of 24-bit full color and 2016×1512 pixels. As described above, each sample is image processed to find their contours. In Table 1, "brightness difference" represents the difference between the brightness value of the above-mentioned central peak and the brightness value of the tertiary peak. The case where the brightness difference is less than 15 is set to "A", the case where it is less than 25 is set to "B", and the case where it is greater than 25 is set to "C". In addition, the total light transmittance of the samples of Examples 1 to 9 and Comparative Examples 1 to 5 is within the range of 10% to 60%.

[0138] (Evaluation results of uneven bubbles)

[0139] The sample of Example 1 was evaluated as "B", and the samples of Examples 2 to 5 were evaluated as "A". On the other hand, the samples of Comparative Examples 1 to 4 were evaluated as "C".

[0140] (Evaluation method of vacuum formability)

[0141] First, prepare a metal mold for vacuum forming. Fig.16 As shown, the metal mold 300 for vacuum forming has a recessed portion 301 recessed from its upper surface, and the recess 301 has a substantially rectangular shape when viewed from above. The corners of the recess 301 are chamfered with a radius of curvature of 15 mm, the distance between the relatively short sides of the substantially rectangular shape is 200 mm, the distance between the relatively long sides is 80 mm, and the depth of the recess 301 is 30 mm. The samples of Examples 1 to 5 and Comparative Examples 1 to 4 were vacuum formed using the metal mold for vacuum forming. It should be noted that the "CFP-65P Model" manufactured by WAKASAKA Engineering Co., Ltd. was used as a vacuum forming device. After vacuum forming, when the skin layer and the core layer separated, the skin layer expanded, and the core layer ruptured at the above-mentioned corners, it was regarded as poor vacuum formability and evaluated as "C". When the core layer did not rupture but the bubble diameter of the core layer after vacuum forming exceeded 2 mm, it was regarded as good vacuum formability and evaluated as "B". When the core layer did not rupture and the bubble diameter did not change significantly, it was regarded as better vacuum formability and evaluated as "A".

[0142] (Evaluation results of vacuum formability)

[0143] The sample of Example 1 was evaluated as "B", and Examples 2 to 5 were evaluated as "A". On the other hand, Comparative Examples 1 to 4 were evaluated as "C". Thus, it was confirmed that the smaller the difference in brightness, the better the vacuum formability.

[0144] Next, regarding the ratio of the thickness (t1+t2) of the entire epidermis layer to the thickness T of the sample, in the comparison among Examples 1 to 9, when the thickness ratio {(t1+t2) / T} was 0.10 to 0.5, both the difference in brightness and the vacuum formability were evaluated as "B" or higher. In particular, when the thickness ratio was 0.20 to 0.40, there was a tendency for many samples to be evaluated as "A" in terms of the difference in brightness and the vacuum formability. That is, when the thickness ratio was 0.10 to 0.5, the difference in brightness could be reduced, and thus excellent vacuum formability could be obtained. In addition, when the thickness ratio was 0.20 to 0.40, the difference in brightness could be further reduced, and even more excellent vacuum formability could be obtained. It should be noted that the thickness ratio of Comparative Example 5 was 0.032, which was smaller than that of Comparative Examples 1 to 4. Therefore, although the brightness difference and vacuum formability of Comparative Example 5 were evaluated as "C" as those of Comparative Examples 1 to 4, it is considered that the brightness difference and vacuum formability were actually worse than those of Comparative Examples 1 to 4.

[0145] Next, the brightness difference and the evaluation of vacuum formability were confirmed in the MVR ratio of the samples. In the comparison of Examples 1 to 9, when the MVR ratio was 1.0 to 5 times, both the brightness difference and the vacuum formability were evaluated as "B" or above. In particular, when the MVR ratio was 1.0 to 3 times, there was a tendency for many samples to be evaluated as "A" for the brightness difference and the vacuum formability. That is, when the MVR ratio was 1.0 to 5 times, the brightness difference could be reduced, and excellent vacuum formability could be obtained. In addition, when the MVR ratio was 1.0 to 3 times, the brightness difference could be further reduced, and even more excellent vacuum formability could be obtained. It should be noted that the MVR ratio of Comparative Example 5 was 0.7, which was smaller than that of Comparative Examples 1 to 4. Therefore, it is considered that although the brightness difference and the vacuum formability of Comparative Example 5 were evaluated as "C" the same as those of Comparative Examples 1 to 4, the brightness difference and the vacuum formability were actually worse than those of Comparative Examples 1 to 4.

[0146] Description of Reference Numerals

[0147] 1: extruded foam sheet, 2: core layer, 3: skin layer, 4: skin layer, 21: image, 22: image, 23: image, 24: image, 25: image, 1000: inspection device, 1010: image receiving unit, 1020: image processing unit, 1021: edge processing unit, 1022: first Fourier transform unit, 1023: second Fourier transform unit, 1024: measuring unit, 1025: judging unit, P1: 1st peak, P2: 2nd peak, P3: 3rd peak, P0: central peak, Δ: brightness difference, L: distance, T: thickness, t1: thickness, t2: thickness.

Claims

1. An extruded foam sheet comprising a polycarbonate resin, For the extruded foam sheet, The extruded foam sheet and a scale having 1 mm intervals are photographed from above while light is irradiated from below the extruded foam sheet to obtain a first image, and then a second image obtained by edge processing the first image is subjected to two-dimensional discrete Fourier transform to obtain a third image, and a fourth image obtained by removing the scale from the first image is subjected to two-dimensional discrete Fourier transform to obtain a fifth image, In the third image and the fifth image, the third image represents the frequency distribution of brightness in the second image, and the fifth image represents the frequency distribution of brightness in the fourth image, When a brightness profile is obtained along the direction of the ruler from the center of the third image and represented as a two-dimensional spectrum, a plurality of frequency components appearing according to the 1 mm interval scale of the ruler are set as the first peak, the second peak and the third peak in sequence from the center position of the third image, and when the distance between the first peak and the center position of the third image is set as L, the frequency component with the highest brightness between the position at a distance of L / 5 and the position at a distance of L / 2 from the center position of the third image is set as the central peak, In this case, when the brightness profile is obtained linearly from the center of the fifth image toward a direction with higher brightness and represented by a two-dimensional spectrum, the difference between the brightness at the position corresponding to the central peak and the brightness at the position corresponding to the third peak is less than 25 when represented by 256 gray levels.

2. The extruded foam sheet according to claim 1, wherein The extruded foam sheet contains 50% by weight or more of a polycarbonate resin.

3. The extruded foam sheet according to claim 1, wherein The extruded foam sheet has a thickness of 1 to 5 mm.

4. The extruded foam sheet according to claim 1, wherein The total light transmittance of the extruded foam sheet is 10% to 60%.

5. The extruded foam sheet according to claim 1, comprising: A core layer composed of a foamed resin, a first skin layer composed of a non-foamed resin and laminated on one main surface of the core layer, and a second skin layer laminated on the other main surface of the core layer; At least one of the first skin layer and the second skin layer is made of a polycarbonate resin.

6. The extruded foam sheet according to claim 5, which satisfies the following formula (1): 0.10≤(t1+t2) / T≤0.5 ··· (1) In formula (1), t1 represents the thickness of the first skin layer, t2 represents the thickness of the second skin layer, and T represents the thickness of the extruded foam sheet.

7. The extruded foam sheet according to claim 4, wherein: The polycarbonate resin included in any one of the first skin layer and the second skin layer has a melt volume rate that is 1.0 to 5 times that of the polycarbonate resin included in the core layer.

8. The extruded foam sheet according to claim 1, wherein The extruded foam sheet has a length of 1000 mm or more in the extrusion direction, and has a length of 1000 mm or more in the width direction orthogonal to the extrusion direction in a plan view.

9. The extruded foam sheet according to claim 1, wherein: The brightness difference is less than 20 when expressed in 256 grayscales.

10. The extruded foam sheet according to claim 1, wherein The brightness difference is less than 15 when expressed in 256 grayscales.

11. A method for inspecting an extruded foam sheet, comprising: The step of simultaneously photographing the extruded foam sheet and a ruler having equally spaced scales from above while irradiating light from below the extruded foam sheet to obtain a first image, performing edge processing on the first image to obtain a second image, performing a two-dimensional discrete Fourier transform on the second image to obtain a third image representing a frequency distribution of brightness in the second image, removing the scale from the first image to obtain a fourth image, a step of performing a two-dimensional discrete Fourier transform on the fourth image to obtain a fifth image representing a frequency distribution of brightness in the fourth image, a step of determining a brightness difference between the third image and the fifth image based on a frequency distribution of brightness in the second image and a frequency distribution of brightness in the fourth image, and When the brightness difference is lower than a predetermined threshold value, it is determined that the extruded foam sheet can be vacuum-formed.

12. The method for inspecting an extruded foam sheet according to claim 11, wherein: In the step of measuring the brightness difference between the third image and the fifth image, when a brightness profile is obtained along the direction of the ruler from the center of the third image and represented by a two-dimensional spectrum, a plurality of frequency components that appear according to the equally spaced graduations of the ruler are set as a first-order peak, a second-order peak, and a third-order peak in sequence from the center position of the third image, and when the distance between the first-order peak and the center position of the third image is set as L, the frequency component with the highest brightness between a position at a distance of L / 5 and a position at a distance of L / 2 from the center position of the third image is set as a central peak, and when a brightness profile is obtained linearly from the center of the fifth image toward a direction with higher brightness and represented by a two-dimensional spectrum, the difference in brightness between a position corresponding to the central peak and a position corresponding to the third peak is measured; In the step of determining that the extruded foam sheet can be vacuum-formed, when the brightness difference is expressed in 256 grayscales and is less than 25, it is determined that the extruded foam sheet can be vacuum-formed.

13. An inspection device for an extruded foam sheet, comprising: an image receiving unit that receives a first image obtained by simultaneously photographing the extruded foam sheet and a ruler having equally spaced graduations from above while irradiating light from below the extruded foam sheet, and an image processing unit configured to process the first image received by the first image receiving unit; The image processing unit comprises: an edge processing unit, which performs edge processing on the first image to obtain a second image, a first Fourier transform unit configured to perform a two-dimensional discrete Fourier transform on the second image to obtain a third image representing a frequency distribution of brightness in the second image; a second Fourier transform unit configured to perform a two-dimensional discrete Fourier transform on a fourth image obtained by removing the scale from the first image, so as to obtain a fifth image representing a frequency distribution of brightness in the fourth image; a measuring unit that measures a difference in brightness between the third image and the fifth image based on a frequency distribution of brightness in the second image and a frequency distribution of brightness in the fourth image, and A determination unit determines that the extruded foam sheet can be vacuum-formed when the brightness difference is lower than a predetermined threshold value.

14. The inspection device for an extruded foam sheet according to claim 13, wherein: When a brightness profile is obtained along the direction of the ruler from the center of the third image and represented by a two-dimensional spectrum, a plurality of frequency components that appear according to the equally spaced graduations of the ruler are set as a first-order peak, a second-order peak, and a third-order peak in sequence from the center position of the third image, and when the distance between the first-order peak and the center position of the third image is set as L, the frequency component with the highest brightness between a position at a distance of L / 5 and a position at a distance of L / 2 from the center position of the third image is set as a central peak. In this case, when a brightness profile is obtained linearly from the center of the fifth image toward a direction with higher brightness and represented by a two-dimensional spectrum, the measuring unit measures the difference between the brightness at a position corresponding to the central peak and the brightness at a position corresponding to the third peak; When the brightness difference is expressed in 256 grayscales and is less than 25, the determination unit determines that the extruded foam sheet can be vacuum-formed.