Method for separating clay particles in sludge in array pattern mode and preparing adsorption pellets through sodium alginate solidification
By preparing adsorption pellets through array sorting and sodium alginate solidification technology, the problem of low resource utilization rate of dredged sediment was solved, realizing the resource utilization and environmental protection of dredged sediment.
Patent Information
- Application Number
- CN202411041131.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The current technology has a low resource utilization rate of dredged sediment, and its treatment and disposal and the environmental pollution problems it may cause are serious, making it difficult to effectively utilize its adsorption performance for pollutants.
Fine clay particles in silt are sorted by array pattern and then solidified with sodium alginate to prepare adsorption spheres. The process includes calcination, crushing, mixing, cross-linking and drying steps to form sphere materials with good adsorption properties.
This has enabled the resource utilization of dredged sediment, and produced adsorbent materials with good phosphorus adsorption capacity for water purification and covering of polluted sediment, thereby alleviating treatment and disposal pressure and protecting the ecological environment.
Smart Images

Figure CN118976469A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste resource utilization in water conservancy projects and environmental projects, and in particular to a method for sorting clay particles in sludge in an array pattern and preparing adsorption spherical particles through sodium alginate solidification. Background Art
[0002] A large number of dredging projects or environmental dredging projects for the purpose of improving the storage capacity of rivers and lakes, maintaining the ecological environment, and improving the water quality of rivers and lakes have produced a large amount of dredging sludge. The composition of dredging sludge is mainly composed of fine particles such as clay (clay particles account for 16%, and powder particles account for 75%). Among them, clay minerals such as kaolinite and montmorillonite have an adsorption effect on pollutants such as phosphates and have the potential for development and utilization. If the dredging sludge can be simply processed and used as an in-situ adsorption covering material for the treatment of eutrophic rivers and lakes, it can not only alleviate the treatment and disposal pressure of dredging sludge, but also realize the potential value of dredging sludge and achieve the purpose of treating waste with waste. At present, the resource utilization rate of a large amount of dredging sludge is low, and its treatment and disposal and the environmental pollution problems that may be caused are becoming increasingly serious. If it can be prepared as an adsorption material for pollutant phosphorus in rivers and lakes or a covering material for polluted sludge through solidification and granulation and other technologies, it can alleviate the treatment and disposal pressure of dredging sludge, and "treat waste with waste" and give play to the potential value of dredging sludge.
[0003] In view of the need for environmental protection and sustainable development of civil engineering, how to transform dredged sludge, a solid waste, into an environmentally friendly renewable resource for utilization through appropriate methods is an urgent problem to be solved by existing technologies. Summary of the invention
[0004] The present invention aims to provide a method for sorting fine clay particles in sludge in an array manner and preparing adsorption spherical particles by solidification with sodium alginate, so as to solve the technical problem that the solid waste such as dredging sludge is not fully reused in the prior art.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme:
[0006] A method for sorting fine clay particles in sludge in an array pattern and preparing adsorption spherical particles by solidification with sodium alginate, comprising the following steps performed in sequence:
[0007] S1: Enrichment of fine clay particles from dredged sludge;
[0008] S2: fine clay particles are calcined and then crushed to obtain calcined clay particle powder;
[0009] S3: mixing calcined clay particle powder with sodium alginate solution to obtain a mixed solution; adding the mixed solution dropwise into a calcium ion solution, and then allowing the mixed solution to stand in the calcium ion solution to obtain cross-linked composite spherical particles;
[0010] S4: After the cross-linked composite pellets are washed and dried, adsorption pellets are obtained.
[0011] This scheme aims to solve the problem that dredged sludge is difficult to handle and recycle, and the problem that dredged sludge is easily washed away by water when used as a covering material for contaminated sludge. This scheme provides a method for sorting clay particles in sludge in an array pattern and preparing adsorption spherical particles through sodium alginate solidification, and develops an adsorption material with good phosphorus adsorption capacity. This scheme uses an array pattern mud sorting method to obtain clay particles and prepares them into loose, porous spherical materials with good adsorption properties through the cross-linking and solidification of sodium alginate to form a hydrogel. The adsorption spherical materials can be widely used in various water purification projects and in-situ sludge covering projects based on the adsorption principle. It can not only realize the resource utilization of dredging products, but also produce new environmental governance materials. This scheme effectively improves the stability of materials in water bodies and expands the resource utilization channels of dredged sludge, which is of great significance for alleviating the negative impact of dredged sludge on the environment, protecting the ecological environment and promoting sustainable development.
[0012] Further, in S1, the method for enriching fine clay particles from the dredged sludge is: inputting the dredged sludge into the cofferdam, and enriching the fine clay particles through multi-stage overflow;
[0013] According to the order of material flow, the cofferdam is provided with a large gravel particle area, a silt fine sand particle area, a silt particle area, a clay particle area and a fine clay particle area in sequence. Each area is formed by a partition weir and a cofferdam wall, and an overflow port is provided on the partition weir between adjacent areas. Fine clay particles are obtained in the fine clay particle area, and among the fine clay particles, the content of particles with a particle size of less than 5μm is greater than 80%.
[0014] Further, in S1, the weir is in the form of an arc surface, including a first weir, a second weir, a third weir and a fourth weir; the first weir is arranged between the gravel large particle area and the silt fine sand particle area, the second weir is arranged between the silt fine sand particle area and the silt particle area, the third weir is arranged between the silt particle area and the clay particle area, and the fourth weir is arranged between the clay particle area and the fine clay particle area;
[0015] The large gravel particle area is connected with two symmetrically distributed silt and fine sand particle areas through the first overflow port on the first weir; the two silt and fine sand particle areas are connected with the same silt particle area through the second overflow ports on their respective second weirs; the silt particle area is connected with two symmetrically distributed clay particle areas through the third overflow port on the third weir; the two clay particle areas are connected with the same fine clay particle area through the fourth overflow ports on their respective fourth weirs.
[0016] Furthermore, in S1, the gravel large particle area is connected to a mud blowing port, and the fine clay particle area is connected to a drainage port; the speed of the dredged sludge entering the cofferdam through the mud blowing port is 5-10m 3 / min; the width of the drain outlet is 150-200cm and the depth is 20-30cm; the width of the overflow outlet is 100-150cm and the depth is 20-30cm.
[0017] Furthermore, in S2, the calcination conditions are 300-800°C and 2-5h; and the particle size of the calcined clay particle powder is 0-5 μm.
[0018] Further, in S3, the mixed solution is sucked into the delivery pipe, and the mixed solution is dripped into the calcium ion solution through the holes on the delivery pipe; after the dripping, the mixed solution is left to stand in the calcium ion solution for 12-36 hours;
[0019] The inner diameter of the delivery pipeline is 80-200 mm; the delivery speed of the mixed liquid in the delivery pipeline is 200-1000 mL / min; and the diameter of the hole is 5-15 mm.
[0020] Further, in S3, the mass ratio of calcined clay particle powder to sodium alginate solution is 30:1-50:1; the concentration of sodium alginate solution is 0.5-2.5%; the calcium ion solution is calcium chloride solution with a concentration of 0.1-0.5 mol / L; and the volume ratio of the mixed solution to the calcium chloride solution is 1:10-1:4.
[0021] Further, in S4, the drying conditions are: 40-80°C, 6-24h.
[0022] The technical solution also provides an adsorption spherical particle prepared by a method of sorting fine clay particles in sludge in an array pattern and preparing the adsorption spherical particle by solidifying with sodium alginate.
[0023] The technical solution also provides a cofferdam for sorting sludge in an array pattern. In accordance with the order of material flow, the cofferdam is provided with a large gravel particle area, a silt fine sand particle area, a silt particle area, a clay particle area and a fine clay particle area in sequence, and each area is formed by a partition weir and a cofferdam wall.
[0024] The weir is in the form of an arc surface, and includes a first weir, a second weir, a third weir and a fourth weir; the first weir is arranged between the gravel large particle area and the silt fine sand particle area, the second weir is arranged between the silt fine sand particle area and the silt particle area, the third weir is arranged between the silt particle area and the clay particle area, and the fourth weir is arranged between the clay particle area and the fine clay particle area;
[0025] The gravel large particle area is connected to two symmetrically distributed silt fine sand particle areas through the first overflow port on the first weir; the two silt fine sand particle areas are connected to the same silt particle area through the second overflow ports on their respective second weirs; the silt particle area is connected to two symmetrically distributed clay particle areas through the third overflow port on the third weir; the two clay particle areas are connected to the same fine clay particle area through the fourth overflow ports on their respective fourth weirs;
[0026] The large gravel particle area is connected to a mud blowing port, and the fine clay particle area is connected to a drainage port.
[0027] In summary, the principle of this technical solution is:
[0028] The desilting sludge involved in this scheme is the sludge removed from the desilting project of rivers, lakes and reservoirs. By setting up a weir in the desilting sludge yard, the fine clay particles are enriched in a specific sedimentation area through multiple overflows, and then the fine clay particles in the desilting sludge are selected. The desilting sludge contains a large number of clay particles, and the clay particles contain a large number of crystal layers, which give them a large specific surface area and a large number of adsorption active sites, and have a good adsorption effect on pollutants such as nitrogen and phosphorus, especially clay particles with a particle size of less than 5μm, because of their better specific surface area, they are more suitable as adsorption pellet raw materials. In this scheme, through array-type sludge sorting, a weir is set up in the desilting sludge yard, and the fine clay particles are enriched in a specific sedimentation area through multiple overflows. After the high-water content desilting sludge enters the sludge yard through the mud blowing port, the flow rate slows down, the large particles in the sludge sink first, and the fine particles enter the next layer of weir through the overflow port. Therefore, after multiple overflows, the fine clay particles are finally enriched in the last layer of weir. Finally, through array-type sludge sorting, the fine clay particles obtained are smaller than 5μm, accounting for more than 80% of the total, and the tail water of the sludge field is discharged from the drain outlet.
[0029] The cross-linking principle and pore-forming step in the preparation process of the adsorption spherical particles of this scheme are: after the mixture of calcined clay particle powder and sodium alginate solution is dripped into calcium chloride solution, calcium alginate hydrogel is formed to embed clay particles to form hydrogel beads. After the drying process removes the water in the hydrogel, the alginate forms a network structure between the clay particles to cross-link and fix the clay particles, accompanied by pore-forming effect, so that the clay particles are cross-linked to form loose porous spherical particles.
[0030] The application cases of the method and the product of the present invention are as follows:
[0031] (1) Adsorption and recovery of phosphorus in eutrophic water bodies: After adsorbing phosphate, the pellets can be recovered and used as phosphorus-rich soil fertilizer.
[0032] (2) Low-disturbance in-situ covering material for contaminated sediments: Due to the loose and porous characteristics of the material, the composite spheres have a low density and sink slowly when placed in the water, causing minimal disturbance to the sediments. In addition, thanks to their regular spherical shape, the composite spheres cover the contaminated sediments evenly, with good covering effects.
[0033] The beneficial effects of the present invention are as follows:
[0034] The present invention creatively combines the cross-linking and curing technology of sodium alginate with the resource utilization of dredged sludge, and prepares the dredged sludge into an adsorption material with good adsorption capacity through a low-cost, simple and easy method and process optimization. This material can also be used as a low-disturbance in-situ covering material for contaminated sludge, and its slow sinking characteristics in the water body can be used to avoid disturbance of the contaminated sludge during the covering process, thereby avoiding secondary pollution and effectively covering the contaminated sludge. The resource utilization of dredged sludge through the above method can not only alleviate the treatment and disposal pressure of dredged sludge, but also realize the potential value of dredged sludge, achieve the purpose of treating waste with waste, have positive significance for protecting the ecological environment, and help further promote the construction of an environmentally friendly and recycling society. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The present invention is a flow chart for preparing the adsorption spherical particles.
[0036] Figure 2 It is a schematic diagram (top view) of the cofferdam for sorting fine clay particles in sludge in an array-like manner according to the present invention.
[0037] Figure 3 It is a side sectional schematic diagram of the granulation conveying pipeline of the present invention.
[0038] Figure 4 Schematic diagram of the cofferdam setting method of comparative example 3 (method 1).
[0039] Figure 5 Schematic diagram of the cofferdam setting method of comparative example 3 (method 2). DETAILED DESCRIPTION
[0040] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the technical means used in the following examples and experimental examples are conventional means well known to those skilled in the art, and the materials, reagents, etc. used can be obtained from commercial sources.
[0041] The figure marks in the drawings of the specification include: gravel large particle area A, first weir A-1, first overflow port A-2, silt fine sand particle area B, second weir B-1, second overflow port B-2, silt particle area C, third weir C-1, third overflow port C-2, clay particle area D, fourth weir D-1, fourth overflow port D-2, fine clay particle area E, mud blowing port 1, drainage port 2, conveying pipeline 3, screw pump 4, hole 5.
[0042] Example 1
[0043] A method for preparing phosphorus adsorption pellets by mixing fine clay particles in dredged sludge with sodium alginate, the specific process is as follows Figure 1 As shown, the general steps are as follows:
[0044] S1 Material selection: A weir is set up in the dredged sludge dump, and the fine clay particles are enriched in a specific sedimentation area through multiple overflows (array-type mud sorting), and the fine clay particles in the dredged sludge are obtained, and the screened fine clay particles are dried.
[0045] S2 pretreatment: calcining and crushing the fine clay particles in the dried dredged sludge to obtain powder. The purpose of this step is to remove ammonia nitrogen and organic pollution contained in the sludge.
[0046] S3 cross-linking and curing: fully mix the above powder, calcium peroxide and sodium alginate solution, suck the mixture into the delivery pipe, and drip the mixed liquid into the calcium chloride solution through the holes on the delivery pipe to form composite pellets in the calcium chloride solution mixture. Then, the composite pellets are placed in the calcium chloride solution to ensure sufficient internal cross-linking.
[0047] S4 Pore formation: After the composite pellets are taken out of the solution, they are rinsed with clean water and dried to remove the water in the hydrogel. The alginate forms a network structure between the sediment particles to cross-link and fix the sediment particles, and pores are formed to form loose porous pellets. The composite pellets are stored in a dry and ventilated place for subsequent use.
[0048] The more specific process and related equipment involved are described as follows:
[0049] In S1, the cofferdam structure with partition weirs used in the array type mud separation is as follows: Figure 2As shown. In the dredged sludge dump (sludge dump), a cofferdam is provided, which includes a large gravel particle area A, a silt fine sand particle area B, a silt particle area C, a clay particle area D, and a fine clay particle area E. Each area is separated by a partition weir. There are four partition weirs, which are, in the order of water flow, the first partition weir A-1, the second partition weir B-1, the third partition weir C-1, and the fourth partition weir D-1. Each partition weir is provided with an overflow port, which includes the first overflow port A-2, the second overflow port B-2, the third overflow port C-2, and the fourth overflow port D-2, which are respectively arranged on the first partition weir A-1, the second partition weir B-1, the third partition weir C-1, and the fourth partition weir D-1. The first overflow port A-2 connects the gravel large particle area A and the silt fine sand particle area B; the second overflow port B-2 connects the silt fine sand particle area B and the silt particle area C; the third overflow port C-2 connects the silt particle area C and the clay particle area D; the fourth overflow port D-2 connects the clay particle area D and the fine clay particle area E. A mud blowing port 1 is provided at one end of the cofferdam close to the gravel large particle area A, and a drainage port 2 is provided at one end of the cofferdam close to the fine clay particle area E.
[0050] More specifically, the gravel large particle area A is formed by the first barrier weir A-1 and the side wall of the cofferdam. There are two silt fine sand particle areas B, and the upper silt fine sand particle area B is used as an example to illustrate that it is formed by the second barrier weir B-1, the first barrier weir A-1, and the side wall of the cofferdam. The silt particle area C is formed by the second barrier weir B-1, the third barrier weir C-1, the first barrier weir A-1, and the side wall of the cofferdam. There are two clay particle areas D, and the upper clay particle area D is used as an example to illustrate that it is formed by the third barrier weir C-1, the fourth barrier weir D-1, and the side wall of the cofferdam. The fine clay particle area E is formed by the third barrier weir C-1, the fourth barrier weir D-1, and the side wall of the cofferdam. It can be seen that the form of the array-type cofferdam is specifically as follows: the gravel large particle area A is connected with two silt and fine sand particle areas B respectively through the first overflow port A-2 on the first weir A-1 (preferably, the two silt and fine sand particle areas B are symmetrically arranged and located on the upper and lower sides); the two silt and fine sand particle areas B are connected with the same silt particle area C respectively through the second overflow ports B-2 on their respective second weirs B-1; the silt particle area C is connected with two clay particle areas D respectively through the third overflow port C-2 on the third weir C-1 (preferably, the two clay particle areas D are symmetrically arranged and located on the upper and lower sides); the two clay particle areas D are connected with the same fine clay particle area E respectively through the fourth overflow ports D-2 on their respective fourth weirs D-1.
[0051] The first weir A-1, the second weir B-1, the third weir C-1, and the fourth weir D-1 are all in the form of arc surfaces, with radians of π, 1 / 3π, 1 / 4π, and 1 / 9π, respectively. The angle between the first weir A-1 and the second weir B-1 is 120°, the angle between the third weir C-1 and the upper and lower side walls of the cofferdam is 60°, and the angle between the third weir C-1 and the fourth weir D-1 is 80°. The dimensions of the first overflow port A-2, the second overflow port B-2, the third overflow port C-2, and the fourth overflow port D-2 are: 100cm-150cm wide (preferably 120cm), 20cm-30cm deep (lower than the upper end of the weir, preferably 25cm). The width of the drain port 2 is 150cm-200cm (preferably 180cm), and the depth is 20cm-30cm (similar to the setting of the overflow port, lower than the upper end of the weir, preferably 25cm). The high-water content dredged sludge enters the gravel large particle area A of the cofferdam through the sludge blowing port 1 (high water content means water content>95%). The diameter of the sludge blowing port 1 is 100-150cm (preferably: 120cm), and it is set at the upper part of the cofferdam (with the cofferdam opening as the top). The flow rate of the high-water content dredged sludge is 5-10m 3 / min (preferably: 8m 3 / min). The size of the cofferdam in this scheme is preferably: 80-120m long, 40-60m wide, 2-3m high (preferably 100m long, 50m wide, 2m high). The radius of the first weir A-1 in the gravel large particle area A is 15-25m (preferably 20m).
[0052] The process of mud separation based on the cofferdam with partition weir (array type mud separation cofferdam) of the above structure is as follows:
[0053] The high-water content dredged sludge enters the gravel and large particle area A of the cofferdam through the mud blowing port 1. The flow rate of the high-water content dredged sludge slows down, and the large particles in the sludge sink first. In the gravel and large particle area A, mainly the large gravel particles settle; the fine particles enter the next area, namely the silt and fine sand particle area B, through the overflow port. In the silt and fine sand particle area B, the flow rate slows down further, and the larger particles continue to settle, mainly the larger silt particles and fine sand particles settle; the finer particles enter the next area, namely the silt particle area C, through the overflow port. In the silt particle area C, the flow rate slows down further, and the larger particles continue to settle, mainly the silt particles settle; the finer particles enter the next area, namely the clay particle area D, through the overflow port. In the clay particle area D, the flow rate slows down further, and the larger particles continue to settle, mainly the larger clay particles settle; the finer clay particles enter the next area, namely the fine clay particle area E, through the overflow port. In the fine clay particle zone E, fine clay particles can be obtained, among which particles smaller than 5 μm account for more than 80% of the total amount. The tail water of the mud field is discharged from the drain outlet 2. The fine clay particles obtained by the above method for downstream processing can reach more than 80% of the total amount of particles smaller than 5 μm (operating cycle 6h) by adopting the above technical scheme. The fine clay particles need to be dried (for example: placed in the open air for natural drying to a moisture content of less than 80%) before the subsequent calcination step can be carried out. The fine clay particle materials mainly composed of montmorillonite, illite and kaolinite can ensure that the produced covering material has good adsorption properties.
[0054] In S2, the dried fine clay particles are calcined at 300-800°C for 2-5 hours (preferably calcined at 550°C for 3 hours). After calcination, the material is crushed into a powder with a particle size of 0-5 μm (excluding 0, preferably <5 μm), thereby obtaining a calcined clay particle powder after the organic matter is removed.
[0055] In S3, the calcined clay particle powder and the sodium alginate solution are fully mixed in a conventional mixer to obtain a mixed solution. The concentration of the sodium alginate solution is 0.5-2.5% (preferably 1%, with a viscosity of 200 mPa·s), and the mass ratio of the calcined clay particle powder to the sodium alginate solution is 30:1-50:1 (preferably 40:1).
[0056] When the pellets are used as sediment covering materials, the sediment is easy to reduce and release phosphorus under anaerobic conditions. This can be achieved by adding calcium peroxide to the pellets to adjust the dissolved oxygen state at the mud-water interface (calcium peroxide reacts with water to release oxygen). Calcium peroxide is an optional ingredient that is added together with the calcined clay particle powder and the sodium alginate solution, and mixed thoroughly to form a mixed solution. The mass percentage of calcium peroxide in the mixed solution is 5%-20%, which is adjusted according to the water conditions.
[0057] After the above mixing operation is completed, the mixed solution is sucked into the delivery pipeline, the structure of which can be seen in Figure 3 . A screw pump 4 is arranged in the delivery pipe 3, which is in the form of a conventional delivery pipe. Slightly different from the conventional method, a plurality of holes 5 are arranged below the delivery pipe 3, which are used to drip the mixed solution into the calcium chloride solution below. Calcium chloride (98%) is used to prepare the calcium chloride solution, and its concentration is 0.1-0.5 mol / L (preferably 0.2 mol / L), and the volume ratio of the mixed solution to the calcium chloride solution is between 1:10 and 1:4. The inner diameter of the delivery pipe 3 is 80-200 mm (preferably 100 mm), the number of holes 5 is set to 20-40 (preferably 30, arranged in a row, located at the lower end of the pipe), and the caliber of the hole 5 is 5-15 mm (preferably 10 mm). The flow rate control of the mixed solution in the delivery pipe 3 is set to 200-1000 mL / min (preferably 500 mL / min).
[0058] The mixed liquid is sucked into the delivery pipe, and the mixed liquid is dripped into the calcium chloride solution through the holes on the delivery pipe. The sodium ions on the sodium alginate G unit exchange with the calcium ions in the solution, and then the dredged sludge is cross-linked and solidified to form composite adsorption pellets. The composite pellets are then placed in the calcium chloride solution for 12-36 hours (preferably 24 hours) to ensure sufficient internal cross-linking. After this step, cross-linked composite pellets are obtained.
[0059] In S4, the cross-linked composite pellets are taken out, rinsed with clean water for 2-3 times, and then dried at 40-80°C for 6-24h (preferably at 60°C for 12h). After drying to remove water from the hydrogel, alginate forms a network structure between the sediment particles to cross-link and fix the sediment particles, accompanied by pore-forming effect, so that the dredged sediment forms loose porous pellets for subsequent use, thereby obtaining the adsorption pellets of this scheme.
[0060] The cross-linking principle and pore-forming step in the preparation process of adsorption spherical particles described in this patent are: after the mixture of calcined clay particle powder and sodium alginate solution is dripped into calcium chloride solution, calcium alginate hydrogel is formed to embed clay particles to form hydrogel beads. After the subsequent drying process removes the water in the hydrogel, alginate forms a network structure between clay particles to cross-link and fix the clay particles, accompanied by pore-forming effect, so that the clay particles are cross-linked to form loose porous spherical particles.
[0061] Experimental example
[0062] Adsorption pellets were prepared using the optimal technical parameters of Example 1 (without adding calcium peroxide). The density of the adsorption pellets when dried was 0.418 g / cm 3 The density when saturated with water is 1.14 g / cm 3During the water absorption process, the sinking speed in the water body is 1-2cm / s. It can be seen that the adsorption pellets have the characteristics of slow sinking after absorbing water. Their slow sedimentation characteristics in water are conducive to reducing the disturbance of river and lake bottom mud during its application.
[0063] The adsorption spheres produced by this scheme undergo a change in wet density when absorbing water, thus producing the properties of floating-slow sinking-adsorption to the bottom. The adsorption spheres that initially float in the water become more densely wet after absorbing water, and begin to settle, and there is a slow settling that other materials cannot achieve, with a speed of 1-2cm / s. The slow settling and bottoming can adsorb and fix the suspended particles rich in pollutants on the surface of the bottom mud and cover and fix the floating mud, achieving a unique adsorption-fixation-covering effect.
[0064] The adsorption spheres prepared by this scheme were used to test the phosphate adsorption performance. The experimental results showed that when the dosage was 1g / L and the initial phosphate solution concentration was 100mg / L, the equilibrium phosphate adsorption amount reached 8mg / g. The above experimental results show that the adsorption spheres produced by the present invention have excellent adsorption performance for phosphate. This scheme uses dredging sludge, which is different from the sludge produced by ordinary drainage plants. The sludge in the water treatment plant contains substances such as aluminum salt flocculants added in the water production process, so it has a better adsorption effect on phosphorus, and the equilibrium phosphate adsorption amount can obtain a more ideal value. Since the dredging sludge does not contain substances such as aluminum salt flocculants, the effect of the adsorption granules prepared with dredging sludge as raw material is limited. However, in this patent, it is intended to recycle the sludge produced in large quantities by dredging, which is a more environmentally friendly and environmentally friendly material compared to the sludge in the water supply plant. And its adsorption capacity can meet the inhibitory effect on the TP content in river and lake water bodies (<1mg / L).
[0065] Comparative Example 1
[0066] This comparative example tests the effect of different sodium alginate solutions on the formation of adsorption spherical particles. The preparation process refers to the optimal preparation method of Example 1 (without adding calcium peroxide), except that the concentration of the sodium alginate solution is adjusted to 0.5%, 1.5%, 2% and 2.5%.
[0067] The experimental results show that the composite adsorption spheres prepared by 0.5% sodium alginate solution have poor molding effect, and the appearance is water drop-shaped, and the sediment particles are easy to accumulate in the adsorption spheres; the adsorption spheres prepared by 1.5 and 2% sodium alginate solutions form a relatively round sphere, but the sediment particles are still easy to accumulate in the spheres; the 2.5% sodium alginate solution has a high concentration, and the mixed solution before solidification is too viscous, which makes it very easy to block the pipeline during ball making and difficult to prepare and shape. The best effect is the adsorption spheres prepared by solidification with 1% sodium alginate solution (the optimized method of Example 1), which are round and spherical, and the sediment particles are evenly dispersed inside the spheres. This proves that the moderate concentration of sodium alginate solution is an important factor in solidification into spheres: too low a concentration of solution is thin, and it is impossible to effectively cross-link the sediment particles of the water treatment plant. The particles are easy to settle under the action of gravity in the solution and are unevenly distributed, resulting in poor spherical molding effect; and too high a concentration of solution is thick, which also makes it difficult for the sediment particles to be evenly dispersed in the solution, causing the sediment particles to accumulate. The experiment further concluded that the adsorption spheres prepared by solidifying 1% sodium alginate solution have good molding effect, uniform dispersion of soil particles, uniform particle size, unobstructed internal permeable channels, and the best adsorption performance for phosphate.
[0068] Comparative Example 2
[0069] This comparative example is a study on the hole diameter. The optimal preparation method of Example 1 is adopted (the optimal technical parameters of Example 1 are used to prepare the adsorption spheres, without adding calcium peroxide), but the hole diameters are 5mm, 10mm and 15mm, small, medium and large, respectively, for sample preparation comparison. Too small a hole diameter (<5mm) is prone to pore blockage, which is not conducive to batch sample preparation, so experiments were not conducted on smaller hole diameters. When the hole diameter is 10mm, the bottom sinking speed of the adsorption spheres obtained is 1-2cm / s, and the equilibrium adsorption amount of phosphate reaches 8mg / g (see experimental example). The equilibrium adsorption amount decreases with the increase of the finished product particle size, and the bottom sinking speed increases with the increase of the finished product particle size. When using a 15mm diameter hole, the bottom sinking speed of the adsorbed pellets obtained is 2.5-3cm / s, and the phosphate equilibrium adsorption amount is 7.8mg / g; when using a 5mm diameter hole, the bottom sinking speed of the adsorbed pellets obtained is 1.5-1.8cm / s, and the phosphate equilibrium adsorption amount is 8.1mg / g. However, the use of a 5mm diameter will affect the smoothness of the process. In order to ensure the adsorption performance of the finished product (the largest possible equilibrium adsorption amount) and the slow-sinking and covering effect on the bottom mud (the smallest possible bottom sinking speed), 10mm is finally selected as the optimal hole diameter.
[0070] Comparative Example 3
[0071] This comparative example studies the setting method of the partition weir in the cofferdam. Before finally establishing the array-type cofferdam of this solution, the inventor tried various setting methods of the cofferdam.
[0072] Method 1: See Figure 4 The cofferdam includes a large gravel particle area A, a silt fine sand particle area B, a silt particle area C, a clay particle area D, and a fine clay particle area E. Each area is separated by a partition weir. There are four partition weirs, in the order of water flow, they are (from right to left): the first partition weir, the second partition weir, the third partition weir, and the fourth partition weir. Each partition weir is provided with an overflow port, which includes the first overflow port (1), the second overflow port (2), the third overflow port (1), and the fourth overflow port (2) which are respectively arranged on the first partition weir, the second partition weir, the third partition weir, and the fourth partition weir. The overflow ports are staggered. For the setting method of the overflow port, please refer to Figure 4 , the size is the same as the preferred parameters in Example 1, the setting of the mud blowing port and the drain port is also the same as the preferred method in Example 1, and the size of the cofferdam is also the same as the optimal method in Example 1. The difference from Example 1 is that the four weirs are arc surfaces and are distributed in parallel, and the radius ratio is 1:2:3:4. After running for 6 hours according to the operation mode of Example 1, the material in the fine clay particle area E was taken for testing, and it was found that the uniformity of the particle size distribution was poor, which was far less than the uniformity of the material in the fine clay particle area E in Example 1. And among the particles obtained in method one, particles smaller than 5μm only accounted for 55%-65% of the total. In the method of Example 1, the particles smaller than 5μm in the material of the fine clay particle area E can account for more than 80% of the total. Therefore, the fine clay particles obtained by method one are not suitable for the subsequent preparation of adsorption spherical particles because of their uneven and large particle sizes.
[0073] Method 2: See Figure 5 , which is different from Example 1, is that the first weir, the second weir, the third weir, and the fourth weir are all planes, not arc surfaces. The overflow port size is the same as the preferred parameters in Example 1, the mud blowing port and the drainage port are also set in the preferred manner of Example 1, and the size of the cofferdam is also the same as the optimal manner of Example 1. Using the cofferdam set in this way, the process was run for 6 hours in the manner of Example 1, and the material in the fine clay particle zone E was taken for testing. It was found that the particle size distribution uniformity was poor, far less than the uniformity of the material in the fine clay particle zone E in Example 1. And among the particles obtained by method 2, particles smaller than 5 μm only accounted for 60%-70% of the total. In the method of Example 1, particles smaller than 5 μm in the material of the fine clay particle zone E can account for more than 80% of the total. Therefore, the fine clay particles obtained by method 2 are not suitable for the subsequent preparation of adsorption spherical particles due to their uneven and large particle size.
[0074] It can be seen that only the arrangement of the array-type cofferdam in Example 1 can ensure that fine clay particles of qualified quality are obtained for subsequent processing. If the fine clay particles cannot reach a level where particles less than 5 μm can account for more than 80% of the total, the phosphate equilibrium adsorption amount of the adsorption pellets prepared subsequently will be significantly reduced, and the bottom sinking rate will be significantly increased, which cannot meet the application requirements. For example, fine clay particles less than 5 μm, which only account for about 65% of the total, are used as raw materials for the preparation of adsorption pellets. The adsorption pellets obtained have poor phosphorus adsorption effect, and the phosphate equilibrium adsorption amount is far less than 8 mg / g, which cannot achieve the purpose of covering and isolating sediment pollutants. The raw material used in the present scheme to prepare the adsorption pellets is dredged sediment, which does not contain substances such as aluminum salt flocculants (which have phosphorus adsorption effects). How to ensure that the adsorption pellets obtained from the raw materials have ideal phosphorus adsorption effects has not been reported in the prior art. The inventors have found for the first time through research that controlling the particle size range of fine clay particles to a certain level (for example, particles less than 5 μm account for more than 80% of the total) can effectively ensure the phosphorus adsorption effect of the adsorption pellets obtained by dredging the bottom mud. Therefore, it is very necessary to adopt the array-type cofferdam of this scheme in the stage of separating and obtaining fine clay particles. If the array-type cofferdam and operation mode of this scheme are not adopted, the initial material for preparing the adsorption pellets will be unqualified and unsuitable for continuing the subsequent preparation of the adsorption pellets.
[0075] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A method for sorting fine clay particles in sludge in an array manner and preparing adsorption spherical particles by solidification with sodium alginate, Features: The method includes the following steps: S1: Enrichment of fine clay particles from dredged sludge; S2: fine clay particles are calcined and then crushed to obtain calcined clay particle powder; S3: mixing calcined clay particle powder with sodium alginate solution to obtain a mixed solution; adding the mixed solution dropwise into a calcium ion solution, and then allowing the mixed solution to stand in the calcium ion solution to obtain cross-linked composite spherical particles; S4: After the cross-linked composite pellets are washed and dried, adsorption pellets are obtained.
2. A method for separating fine clay particles in sludge by array type and preparing adsorption spherical particles by solidification with sodium alginate according to claim 1, Features: In S1, the method for enriching fine clay particles from dredged sludge is as follows: the dredged sludge is input into the cofferdam, and after multi-stage overflow, the fine clay particles are enriched; According to the order of material flow, the cofferdam is provided with a large gravel particle area, a silt fine sand particle area, a silt particle area, a clay particle area and a fine clay particle area in sequence. Each area is formed by a partition weir and a cofferdam wall, and an overflow port is provided on the partition weir between adjacent areas. Fine clay particles are obtained in the fine clay particle area, and among the fine clay particles, the content of particles with a particle size of less than 5μm is greater than 80%.
3. A method for separating fine clay particles in sludge by array type and preparing adsorption spherical particles by solidification with sodium alginate according to claim 2, Features: In S1, the weir is in the form of an arc surface, including a first weir, a second weir, a third weir and a fourth weir; the first weir is arranged between the gravel large particle area and the silt fine sand particle area, the second weir is arranged between the silt fine sand particle area and the silt particle area, the third weir is arranged between the silt particle area and the clay particle area, and the fourth weir is arranged between the clay particle area and the fine clay particle area; The large gravel particle area is connected with two symmetrically distributed silt and fine sand particle areas through the first overflow port on the first weir; the two silt and fine sand particle areas are connected with the same silt particle area through the second overflow ports on their respective second weirs; the silt particle area is connected with two symmetrically distributed clay particle areas through the third overflow port on the third weir; the two clay particle areas are connected with the same fine clay particle area through the fourth overflow ports on their respective fourth weirs.
4. A method for separating fine clay particles in sludge by array type and preparing adsorption spherical particles by solidification with sodium alginate according to claim 3, Features: In S1, the gravel and large particle area is connected to a mud blowing port, and the fine clay particle area is connected to a drainage port. The speed of the dredged sludge being input into the cofferdam through the mud blowing port is 5-10m 3 / min; the width of the drain outlet is 150-200cm and the depth is 20-30cm; the width of the overflow outlet is 100-150cm and the depth is 20-30cm.
5. A method for separating fine clay particles in sludge by array type and preparing adsorption spherical particles by solidification with sodium alginate according to claim 1, Features: In S2, the calcination conditions are 300-800°C and 2-5h; the particle size of the calcined clay particle powder is 0-5μm.
6. A method for separating fine clay particles in sludge by array type and preparing adsorption spherical particles by solidification with sodium alginate according to claim 1, Features: In S3, the mixed solution is sucked into the delivery pipe, and the mixed solution is dripped into the calcium ion solution through the holes on the delivery pipe; after the dripping, the mixed solution is left to stand in the calcium ion solution for 12-36 hours; The inner diameter of the delivery pipeline is 80-200 mm; the delivery speed of the mixed liquid in the delivery pipeline is 200-1000 mL / min; and the diameter of the hole is 5-15 mm.
7. A method for separating fine clay particles in sludge by array type and preparing adsorption spherical particles by solidification with sodium alginate according to claim 6, Features: In S3, the mass ratio of calcined clay particle powder to sodium alginate solution is 30:1-50:1; the concentration of sodium alginate solution is 0.5-2.5%; the calcium ion solution is calcium chloride solution with a concentration of 0.1-0.5 mol / L; and the volume ratio of the mixed solution to the calcium chloride solution is 1:10-1:
4.
8. A method for separating fine clay particles in sludge by array type and preparing adsorption spherical particles by solidification with sodium alginate according to claim 1, Features: In S4, the drying conditions are: 40-80°C, 6-24h.
9. Adsorption spheres obtained by the method for preparing adsorption spheres by sorting fine clay particles in sludge in an array pattern and solidifying with sodium alginate according to any one of claims 1 to 8.
10. A cofferdam for sorting silt in a pattern. Features: According to the order of material flow, the cofferdam is equipped with large gravel particle area, silt fine sand particle area, silt particle area, clay particle area and fine clay particle area, and each area is formed by the partition weir and the cofferdam wall. The weir is in the form of an arc surface, and includes a first weir, a second weir, a third weir and a fourth weir; the first weir is arranged between the gravel large particle area and the silt fine sand particle area, the second weir is arranged between the silt fine sand particle area and the silt particle area, the third weir is arranged between the silt particle area and the clay particle area, and the fourth weir is arranged between the clay particle area and the fine clay particle area; The gravel and sand particle area is connected with two symmetrically distributed silt and fine sand particle areas through the first overflow port on the first weir; the two silt and fine sand particle areas are connected with the same silt particle area through the second overflow ports on their second weirs; the silt particle area is connected with two symmetrically distributed clay particle areas through the third overflow ports on the third weir; the two clay particle areas are connected with the same fine clay particle area through the fourth overflow ports on their fourth weirs; the gravel and sand particle area is connected with a mud blowing port, and the fine clay particle area is connected with a drainage port.
Citation Information
Patent Citations
Water supply plant sludge-based phosphorus removal particle adsorbent preparation method
CN106540650A
Near-in-situ three-dimensional ecological restoration system and method for dredged sediment of polluted river channel
CN111778920A
Method for preparing adsorption material by using sodium alginate reinforced ditch dredging sludge screening product and prepared adsorption material
CN116371372A
Cited By
Equipment and method suitable for river and lake endogenous pollution bottom mud treatment