Method for improving center segregation of square billet continuous casting billet

By setting an adjustable elliptical electromagnetic stirrer at the end of the solidification process of billet continuous casting, the molten steel is driven to move in the vertical and casting directions, which solves the problems of center segregation, shrinkage cavities and cracks in the existing technology and improves the quality of the cast billet.

CN118976875AActive Publication Date: 2024-11-19NANJING IRON & STEEL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411029187.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Existing technologies are unable to effectively improve the central segregation, central shrinkage cavity, and central crack of the billet in continuous casting. In particular, the fixed direction of the rotating and traveling wave magnetic field stirrer leads to limited stirring effect and cannot accurately act on the end of the solidification of the continuous casting billet.

Method used

An elliptical electromagnetic stirrer is installed at the end of the solidification of the billet continuous casting to control the pouring temperature of the molten steel at 25℃~35℃ above the liquidus point and to make it at a certain angle with the direction of billet pulling, so as to generate a rotating and continuous or intermittent magnetic field, which drives the incompletely solidified molten steel to move in the vertical and pulling directions.

Benefits of technology

The design of the elliptical electromagnetic stirrer improves the center segregation of the square billet in continuous casting, reduces center shrinkage cavities and porosity, avoids the generation of center cracks, and improves the quality of the cast billet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976875A_ABST
    Figure CN118976875A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving center segregation of a continuous casting billet of a square billet, which comprises the following steps of: controlling the pouring temperature of molten steel to be 25-35 DEG C above a liquid phase point, arranging an elliptical electromagnetic stirrer which forms a certain angle with the casting direction of the continuous casting billet at an accessory of a continuous casting solidification tail end of the square billet, and generating electromagnetic force which forms a certain angle alpha with the casting direction of the continuous casting billet, molten steel which is not completely solidified can move in the vertical throwing direction and can also move in the throwing direction, and therefore center segregation of a square billet continuous casting billet is improved. According to the method, the center segregation of the square billet continuous casting billet is improved, and meanwhile center shrinkage cavities, center porosity and center cracks can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of square billet continuous casting, and in particular to a method for improving the center segregation of square billet continuous casting. Background Art

[0002] The center segregation of continuous casting billets refers to the phenomenon of uneven distribution of components in the solidification process of continuous casting billets, which is mainly caused by the segregation and enrichment of some solutes in the molten steel during the solidification process of the billet due to different solubility. Due to the solidification characteristics of steel products and the limitation of product varieties, it is difficult to fundamentally eliminate the center segregation of continuous casting billets in metallurgical process production. We can only try to control and improve the center segregation of the billet and keep it within the allowable range of billet quality requirements.

[0003] The center segregation of the continuous casting billet is due to the large-scale aggregation of certain solute elements that are prone to cracks (such as P, S and some micro-alloying components such as V, Ti, Nb, etc., which can also be called trace elements or partially called residual elements). It will be accompanied by the generation of center cracks and center shrinkage holes, which will have a serious impact on the internal quality of the steel.

[0004] Center segregation of continuous casting billets is a common quality defect in continuous casting production, and it is also a difficult problem in billet quality that the continuous casting industry is currently committed to studying. Researching and developing new methods to control and improve the center segregation of continuous casting billets is of great significance to improving the quality of continuous casting and increasing continuous casting productivity. In addition to controlling the composition, temperature and pouring conditions of the molten steel, electromagnetic stirring technology at the end of solidification is an effective method to control and improve the center segregation of square billets. Through electromagnetic stirring at the end of solidification, the flow of molten steel in the liquid phase hole of the continuous casting billet can be enhanced, and the reflux and redistribution of the enriched segregated solute can be promoted, which can improve the center segregation of the continuous casting billet to a certain extent. However, whether electromagnetic stirring can accurately act on the end of solidification of the continuous casting billet has become a technical limitation and difficulty in actual operation.

[0005] At present, there are three types of electromagnetic stirrers used for stirring liquid metal in the metallurgical industry and the foundry industry: one is a rotating magnetic field stirrer; one is a traveling wave magnetic field stirrer; and the other is a spiral magnetic field stirrer. At present, the rotating magnetic field and traveling wave magnetic field electromagnetic stirrers are relatively mature in structure and process, and have been applied in metal smelting and continuous casting of molten steel. However, due to the fixed direction of the magnetic field, they can only produce a stirring effect parallel or perpendicular to the direction of the billet drawing. The spiral magnetic field electromagnetic stirrer is still under development, its structure is complex, and it requires special power supply equipment, so it is not used in on-site production. Therefore, it is necessary to develop a new method to improve the center segregation of square billet continuous casting to overcome the above problems. Summary of the invention

[0006] Purpose of the invention: In view of the shortcomings and defects of the prior art, the present invention provides a method for improving the center segregation of square billet continuous casting, thereby improving the center segregation of square billet continuous casting and improving the center shrinkage cavity, center porosity and center crack.

[0007] Technical solution: A method for improving the center segregation of square billet continuous casting in the present invention is characterized in that: the pouring temperature of molten steel is controlled at 25°C to 35°C above the liquidus point, and an elliptical electromagnetic stirrer is arranged at a certain angle to the drawing direction of the continuous casting billet near the end of the continuous casting solidification of the square billet to generate an electromagnetic force at a certain angle α to the drawing direction of the continuous casting billet, so that the incompletely solidified molten steel can move both vertically and along the drawing direction, thereby improving the center segregation of the square billet continuous casting.

[0008] Wherein, the elliptical electromagnetic stirrer is installed within a range of 0.5m before and after the liquidus point of the square billet continuous casting machine.

[0009] Wherein, the angle α between the center line of the elliptical electromagnetic stirrer and the casting direction of the continuous casting machine is -45° to 45°.

[0010] The elliptical electromagnetic stirrer generates a clockwise and counterclockwise rotating magnetic field, driving the incompletely solidified molten steel to produce corresponding movement.

[0011] The elliptical electromagnetic stirrer generates continuous and intermittent magnetic fields, driving the incompletely solidified molten steel to move accordingly.

[0012] Wherein, the frequency of the elliptical electromagnetic stirrer is 4 Hz to 9 Hz.

[0013] Wherein, the current intensity of the elliptical electromagnetic stirrer is 0-1200A.

[0014] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: The present invention controls the pouring temperature of molten steel at 25°C to 35°C above the liquidus point, and arranges an elliptical electromagnetic stirrer at a certain angle to the drawing direction of the continuous casting billet at the end attachment of the continuous casting solidification of the square billet, so as to generate an electromagnetic force at a certain angle to the drawing direction of the continuous casting billet, thereby driving the incompletely solidified molten steel to move at a certain angle to the drawing direction of the continuous casting billet, so that the incompletely solidified molten steel can move both vertically and along the drawing direction, thereby improving the center segregation of the square billet continuous casting billet, and at the same time can improve the center shrinkage cavity, center looseness and center crack. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is a structural schematic diagram of the present invention;

[0016] In the figure, 1 is an elliptical electromagnetic stirrer and 2 is a continuous casting billet. DETAILED DESCRIPTION

[0017] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and specific implementation methods.

[0018] The present invention controls the pouring temperature of molten steel at 25°C to 35°C above the liquidus point, and arranges an elliptical electromagnetic stirrer 1 at a certain angle to the drawing direction of the continuous casting billet 2 at the end of the continuous casting solidification of the square billet, so as to generate an electromagnetic force at a certain angle to the drawing direction of the continuous casting billet 2, so that the incompletely solidified molten steel can move both vertically and along the drawing direction, thereby improving the center segregation of the square billet continuous casting billet, and at the same time can improve the center shrinkage cavity, center looseness and center cracks.

[0019] The pouring temperature of the molten steel is controlled at 25 to 35°C above the liquidus point, and the elliptical electromagnetic stirrer 1 is installed within a range of 0.5m before and after the liquidus point of the square billet continuous casting machine. The angle α between the center line of the elliptical electromagnetic stirrer 1 and the casting direction of the continuous casting machine is -45° to 45°. The elliptical electromagnetic stirrer 1 can generate clockwise and counterclockwise rotating magnetic fields, driving the incompletely solidified molten steel to produce corresponding movements. The elliptical electromagnetic stirrer 1 can generate continuous and intermittent magnetic fields, driving the incompletely solidified molten steel to produce corresponding movements. The frequency of the elliptical electromagnetic stirrer 1 is 4Hz to 9Hz, and the current intensity is 0 to 1200A.

[0020] Embodiment 1:

[0021] In the production process of continuous casting of a certain steel square billet, the steel grade has a carbon content of 0.20% low alloy steel. The pouring temperature of the molten steel is controlled at 35°C above the liquidus point, and the elliptical electromagnetic stirrer is installed 0.5m in front of the liquidus point of the square billet continuous casting machine. The angle α between the center line of the elliptical stirrer and the casting direction of the continuous casting machine is 45°. The elliptical electromagnetic stirrer can generate a clockwise rotating magnetic field. The elliptical electromagnetic stirrer generates an intermittent magnetic field, which drives the incompletely solidified molten steel to produce corresponding movement. The frequency of the electromagnetic stirrer is 4Hz and the current intensity is 600A. The low-multiple center segregation of the continuous casting billet is 0.5 level, the center shrinkage cavity is 0.5 level, the center looseness is 0.5 level, and no center cracks are found.

[0022] Embodiment 2:

[0023] In the production process of continuous casting of a certain steel square billet, the steel grade is low alloy steel with a carbon content of 0.45%. The pouring temperature of the molten steel is controlled at 30°C above the liquidus point, and the elliptical electromagnetic stirrer is installed at the liquidus point of the square billet continuous casting machine. The angle α between the center line of the elliptical stirrer and the casting direction of the continuous casting machine is -25°. The elliptical electromagnetic stirrer can generate a counterclockwise rotating magnetic field. The elliptical electromagnetic stirrer generates an intermittent magnetic field, which drives the incompletely solidified molten steel to produce corresponding movement. The frequency of the electromagnetic stirrer is 9Hz and the current intensity is 900A. The low-multiple center segregation of the continuous casting billet is 0.5 level, the center shrinkage cavity is 0.5 level, the center porosity is 1.0 level, and no center cracks are found.

[0024] Embodiment 3:

[0025] In the production process of continuous casting of a certain steel square billet, the steel grade is low alloy steel with a carbon content of 0.45%. The pouring temperature of the molten steel is controlled at 30°C above the liquidus point, and the elliptical electromagnetic stirrer is installed at the liquidus point of the square billet continuous casting machine. The angle α between the center line of the elliptical stirrer and the casting direction of the continuous casting machine is -45°. The elliptical electromagnetic stirrer can generate a counterclockwise rotating magnetic field. The elliptical electromagnetic stirrer generates a continuous magnetic field, which drives the incompletely solidified molten steel to produce corresponding movement. The frequency of the electromagnetic stirrer is 6Hz and the current intensity is 900A. The low-multiple center segregation of the continuous casting billet is 0.5 level, the center shrinkage cavity is 0.5 level, the center looseness is 0.5 level, and no center cracks are found.

[0026] Embodiment 4:

[0027] In the production process of continuous casting of a certain steel square billet, the steel grade is low alloy steel with a carbon content of 0.9%. The pouring temperature of the molten steel is controlled at 25°C above the liquidus point, and the elliptical electromagnetic stirrer is installed 0.5m after the liquidus point of the square billet continuous casting machine. The angle α between the center line of the elliptical stirrer and the casting direction of the continuous casting machine is -45°. The elliptical electromagnetic stirrer can generate a clockwise rotating magnetic field. The elliptical electromagnetic stirrer generates an intermittent magnetic field, which drives the incompletely solidified molten steel to produce corresponding movement. The frequency of the electromagnetic stirrer is 6Hz and the current intensity is 1200A. The low-multiple center segregation of the continuous casting billet is 0.5 level, the center shrinkage cavity is 0.5 level, the center porosity is 0.5 level, and no center cracks are found.

Claims

1. A method for improving the center segregation of a square billet continuous casting, characterized in that: The pouring temperature of molten steel is controlled at 25°C to 35°C above the liquidus point, and an elliptical electromagnetic stirrer (1) is arranged at a certain angle to the drawing direction of the continuous casting billet (2) near the end of the continuous casting solidification of the square billet to generate an electromagnetic force at a certain angle α to the drawing direction of the continuous casting billet (2), so that the incompletely solidified molten steel can move both vertically and along the drawing direction, thereby improving the center segregation of the square billet continuous casting billet.

2. The method for improving the center segregation of a square billet continuous casting according to claim 1, characterized in that: The elliptical electromagnetic stirrer (1) is installed within a range of 0.5 m before and after the liquidus point of the square billet continuous casting machine.

3. The method for improving the center segregation of a square billet continuous casting according to claim 1, characterized in that: The angle α between the center line of the elliptical electromagnetic stirrer (1) and the casting direction of the continuous casting machine is -45° to 45°.

4. The method for improving the center segregation of a square billet continuous casting according to claim 1, characterized in that: The elliptical electromagnetic stirrer (1) generates a clockwise and counterclockwise rotating magnetic field, driving the incompletely solidified molten steel to produce corresponding movement.

5. The method for improving the center segregation of a square billet continuous casting according to claim 1, characterized in that: The elliptical electromagnetic stirrer (1) generates continuous and intermittent magnetic fields, driving the incompletely solidified molten steel to produce corresponding movements.

6. The method for improving the center segregation of a square billet continuous casting according to claim 1, characterized in that: The frequency of the elliptical electromagnetic stirrer (1) is 4 Hz to 9 Hz.

7. The method for improving the center segregation of a square billet continuous casting according to claim 1, characterized in that: The current intensity of the elliptical electromagnetic stirrer (1) is 0-1200A.

Citation Information

Patent Citations

  • Oblique pole type crystallizer electromagnetic stirring device

    CN109967708A

  • Multi-segment independent adjustable composite magnetic field device and method for controlling flowing of molten metal

    CN115194107A

  • Multi-magnetic-potential electromagnetic magnetic stirring crystallization equipment

    CN215845586U

  • Apparatus for manufacturing metallic slurry

    JP1989138045A

  • Electromagnetic stirring method in mold

    JP1999226710A